Alkaline electrochemical generator with zinc anode
By adding wetting agents and defoaming agents to the electrolyte, the hydrophilic characteristics of the film are improved, and the problems of dendrite and passivation of zinc electrodes in alkaline environments are solved, the number of cycles and stability of the battery is improved, and the industry is satisfied. Cycling requirements for batteries.
Patent Information
- Application Number
- CN202380023580.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-17
- Filing Date
- 2023-02-10
- Publication Date
- 2024-11-26
AI Technical Summary
Zinc electrodes are prone to form dendrite and passivation layers in an alkaline environment, resulting in limited battery cycles and cannot meet the needs of industrial batteries. The existing technology increases internal resistance or complicated processes and is not environmentally friendly.
By adding ionic and non-ionic wetting agents to the electrolyte, combined with defoaming agents, the hydrophilic characteristics of the film are improved, the solid-liquid contact surface between the zinc electrode and the electrolyte is enhanced, dendrites are prevented from growing and passivating, and the battery is extended Cycle life.
It significantly improves the number of cycles of zinc electrodes and battery stability, extends the cycle life, reduces the quality loss of the battery, and improves the capacity retention ability of the battery.
Smart Images

Figure CN119032434A_ABST
Abstract
Description
[0001] The present invention relates to the field of alkaline electrochemical generators, more specifically batteries. It is particularly relevant to secondary electrochemical generators with zinc anodes, such as nickel-zinc, zinc-manganese dioxide, silver-zinc, zinc-air secondary electrochemical generators, and batteries with completely soluble or partially soluble cathodes, such as zinc-iodine, zinc-bromine, zinc-ferrocyanide, zinc-manganese oxide batteries, the purpose of which is to achieve high cycle times through the zinc electrode. Background Art
[0002] Zinc (820Ah / kg, 5845Ah / I) has energy properties such as electronegativity (1.65V), low cost and easy recycling, making it the first choice for electrochemical generator anode materials: Moreover, the theoretical mass energy of nickel-zinc and zinc-air batteries is 334Wh / kg and 1320Wh / kg respectively. In fact, the mass energy of prismatic nickel-zinc batteries can reach 80Wh / kg, which is two to three times that of lead batteries.
[0003] However, despite the presence of zinc in alkaline batteries and Zinc is widely used in batteries, but apart from limited-life silver-zinc batteries used primarily in military applications and, more recently, the first industrial nickel-zinc batteries, zinc is rarely found in industrial-grade alkaline batteries.
[0004] In alkaline environments, zinc dissolves in the form of zincates and is prone to dendrite growth when a zinc anode battery is charged, resulting in a short circuit between electrodes of opposite polarity.
[0005] Furthermore, during the charge and discharge cycles, the negative electrode area where zinc is deposited changes: moreover, a densification phenomenon occurs, which reduces the porosity of the electrode and thus the working capacity at the corresponding current density in actual battery use. Other factors affecting the zinc anode include the precipitation of zinc oxide, which forms a passivation layer that reduces the active surface area of the electrode. Much research work has been devoted to understanding the deposition and dissolution mechanisms of zinc in alkaline environments, and a large number of patents have been filed to provide solutions:
[0006] - the use of additives, added to the electrolyte or incorporated into the anode active material, aimed at reducing the solubility of zincates, which constitute the main subject of the patent;
[0007] - Mechanical treatment methods are also described, which enable the electrolyte to circulate alone or the zinc electrode to be dispersed in the electrolyte to ensure uniform zinc deposition, preventing dendrite growth;
[0008] - using pulsed current, with or without polarity reversal, enabling at least partial dissolution of the dendritic growth;
[0009] - Finally, a separator is used to limit or eliminate the diffusion of zincate ions from the anode to the cathode: for example a multi-layer microporous separator or an ion exchange membrane.
[0010] These technical solutions can be implemented individually or in combination, but they only provide partial solutions and in some cases increase internal resistance, increase battery cost or complicate implementation. In addition, some have suggested adding lead or cadmium to the anode active material, but this is obviously unacceptable for pollution reasons.
[0011] In the case where the electrolyte is mainly composed of potash, some progress has been made by adding some additives, such as the small nickel-zinc (NiZn) cylindrical batteries currently available on the market. However, the number of cycles obtained does not meet the needs of industrial batteries and stationary application batteries, which need to guarantee at least 1000 and 2000 deep charge and discharge cycles, respectively, with a discharge depth of 80% or more.
[0012] The first breakthrough was achieved by adding a conductive ceramic, preferably titanium nitride (TiN), to the zinc electrode, described in patent FR 2 788 887 (filed on January 27, 1999 by SCPS), which allowed a cycle number of more than 1000 and a depth of discharge of more than 80%. The second significant progress was achieved by adding SiO2 to the electrolyte, described in patent FR 3 099 851 (filed on August 9, 2019 by Sunergy), which allowed a cycle number of more than 2000 and a depth of discharge of more than 80%.
[0013] The capacity loss of NiZn batteries during cycling has historically been mainly related to the formation of zinc dendrites, which ultimately lead to short circuits. Subsequent research by SCPC, under patent FR 2 788 887, succeeded in eliminating this dendrite formation, allowing cycles of more than 1000 cycles. Since then, the capacity loss of NiZn batteries has been mainly caused by redistribution of active materials, densification, drying out and passivation of the zinc electrode. Sunergy research, under patent FR 3 099 851, demonstrates a new solution that overcomes these limitations of NiZn battery stability, allowing cycles of more than 2000 cycles. With the improvement of the stability of the zinc electrode, the capacity loss is related to other parameters, in addition to those mentioned above, such as the stability of the hydrophilic properties of the membrane.
[0014] The present invention aims to provide a new solution to overcome the limitations of batteries based on zinc electrodes in terms of their ability to provide a large number of cycles by improving the stabilization of the hydrophilic properties of the membrane while maintaining the more than 2000 cycles achieved.
[0015] For this purpose, experiments were conducted to add wetting agents to the electrolyte. The purpose was to improve the solid-liquid interface of the active materials of the nickel and zinc electrodes and prevent possible degradation of the hydrophilic properties of the membrane. It was assumed that part of the wetting agent that was soluble or suspended in the electrolyte would eventually adhere to the pores of the membrane, allowing the membrane to maintain its hydrophilic properties for a longer time.
[0016] An examination of the prior art for zinc anode systems shows that there are several patents and studies that mention the use of wetting agents. For example, Rossler et al., in patent US 4 195 120 filed on November 3, 1978, show that hydrogen evolution in a battery having a zinc anode can be reduced or eliminated by adding a wetting agent to the battery, the wetting agent being an ethylene oxide polymer, an alkyl adduct ester phosphate. The wetting agent is added in such a way that when the electrolyte wets the anode, the wetting agent can be directly or indirectly adsorbed on the surface of the zinc anode material, thereby preventing the release of hydrogen gas. The wetting agent is ideally present in the battery in an amount of 0.001% to 5% by weight of the zinc component. The wetting agent described herein is soluble or dispersible in water and alkaline electrolytes. The wetting agent can be added directly to the zinc electrode, or indirectly to the electrolyte or cathode. Through the electrolyte, the wetting agent can be deposited on the surface of the zinc, while through the cathode, the wetting agent can penetrate the membrane and be deposited on the zinc.
[0017] In Chinese patent application CN111048846 filed on December 18, 2019, a wetting agent is mentioned, which is selected from sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium chloride, tetrabutylammonium bromide, one or more compounds from tetrabutylammonium hydroxide, tetrabutylammonium chloride and perfluorosurfactant, which makes it possible to increase the number of charge and discharge cycles from 100 to 600 times by reducing common limiting factors such as short circuit, dissolution, deformation, densification, passivation of zinc electrode and hydrogen evolution.
[0018] An article published by JiLing Zhu et al. in 1998 (Journal of Power Sources, Vol. 72, 1998, pp. 231-235) mentioned the effects of different types of perfluorinated ionic wetting agents, including the hydrocarbon chain-containing wetting agent CTAB, on the electrochemical behavior of zinc. The results show that these wetting agents can be used as a substitute for mercury to reduce corrosion in zinc batteries. The study also showed that zinc deposition was improved to a certain extent in the presence of these wetting agents. The morphology of electrodeposited zinc shows that these wetting agents can bring more uniform and dense deposition, thereby reducing the growth of dendrites. FC-170C and CTAB are the most effective inhibitors. These ionic wetting agents can still adhere to zinc during the strong polarization associated with hydrogen evolution, while non-ionic wetting agents will not. Cationic wetting agents can be adsorbed by the electrostatic attraction between the molecular polar groups and the zinc electrode surface, so when the zinc electrode potential is below -1.80V, the rate of hydrogen evolution increases more slowly in the presence of FC-135 or CTAB. The shift in the deposition onset potential and the maximum potential of the cathode current indicates that the zinc deposition is inhibited to some extent in the presence of the wetting agent. The reason is that the wetting agent is adsorbed on the surface of the zinc electrode, forming a layer that has an inhibitory effect on the electroreduction process of zincate ions. Therefore, these wetting agents can slow down the zinc deposition rate of zincate when the electrode is charged, thereby weakening the growth of dendrites.
[0019] An article published by MA Deyab in 2015 (Journal of Power Sources, Vol. 292, 2015, pp. 66-71) mentioned the effect of polyoxyethylene (40) nonylphenol ether as a nonionic surfactant (PNE) as a corrosion inhibitor in alkaline electrolyte (7.0 M KOH).
[0020] Prior art studies on wetting agent addition are all related to the study of reducing hydrogen evolution and zinc corrosion. Summary of the invention
[0021] The present invention aims to provide a rechargeable alkaline electrochemical generator with a zinc anode, which can improve the capacity stability of the battery and extend its cycle life.
[0022] This object is achieved in particular by enhancing and stabilizing the hydrophilic properties of the membrane, which makes it possible to reduce the surface tension and improve the contact of the electrolyte with the solid surface.
[0023] In more detail, the present invention relates to an alkaline electrochemical generator with a zinc anode according to statement 1 below:
[0024] 1. An alkaline electrochemical generator with a zinc anode, comprising an electrolyte, the electrolyte being an alkaline aqueous solution having a molar concentration of hydroxide ions between 4M and 15M and comprising:
[0025] a) at least one wetting agent, the electrolyte concentration is 0.1 g / l
[0026] and 50 g / l; and
[0027] b) at least one defoaming agent in an amount between 10 mg and 1000 mg per kg of electrolyte.
[0028] Advantageous features of the alkaline electrochemical generator with zinc anode according to statement 1 above are indicated in the following statements 2 to 11:
[0029] 2. Alkaline electrochemical generator with zinc anode according to statement 1, wherein it comprises at least one ionic wetting agent and at least one non-ionic wetting agent.
[0030] 3. An alkaline electrochemical generator with a zinc anode according to statement 1 or 2, wherein the ionic wetting agent contained is bis(2-ethylhexyl)phosphate.
[0031] 4. Alkaline electrochemical generator with zinc anode according to one of statements 1 to 3, comprising at least one nonionic wetting agent selected from alkyl polyglucosides and polyethylene glycol ethers and alkylphenol ethers, especially octylphenol ethers.
[0032] 5. Alkaline electrochemical generator with zinc anode according to one of statements 1 to 4, wherein the defoaming agent is selected from polyorganosiloxanes.
[0033] 6. Alkaline electrochemical generator with zinc anode according to one of statements 1 to 5, wherein the molar concentration of the alkaline solution is between 7M and 12M.
[0034] 7. Alkaline electrochemical generator with zinc anode according to one of statements 1 to 6, wherein the concentration of the one or more wetting agents in the electrolyte is between 1 g / l and 25 g / l.
[0035] 8. Alkaline electrochemical generator with zinc anode according to one of statements 1 to 7, wherein the concentration of the defoaming agent in the electrolyte is between 100 mg and 500 mg per kg of electrolyte.
[0036] 9. Alkaline electrochemical generator with zinc anode according to one of statements 1 to 8, wherein the electrolyte also contains silicate.
[0037] 10. Alkaline electrochemical generator with zinc anode according to one of statements 1 to 9, wherein the electrolyte further comprises zincate.
[0038] 11. Alkaline electrochemical generator with zinc anode according to one of statements 1 to 10, wherein the electrolyte further comprises borates, phosphates and / or fluorides.
[0039] According to another aspect, the present invention also relates to the following method for preparing an alkaline electrochemical generator with a zinc anode in accordance with statement 12:
[0040] 12. A method for producing an alkaline electrochemical generator with a zinc anode according to one of statements 1 to 11, comprising the step of introducing a hydroxide of lithium, sodium and / or potassium when preparing the electrolyte.
[0041] Other features and advantages of the present invention will now be described in detail in the following disclosure with reference to the accompanying drawings, which schematically show:
[0042] [ Figure 1 ]: Discharge capacity curve of NiZn element, 8Ah cycle, 8A charging for 1 hour, 8A IV discharge, discharge depth 100%;
[0043] [ Figure 2 ]: Discharge capacity curve of NiZn element, 8Ah cycle, 8A charge for 1 hour, 8A IV discharge, discharge depth 100%; and
[0044] [ Figure 3 ]: Discharge capacity curve of NiZn component, 8Ah cycle, 8A charging for 1 hour, 8A 1V discharge, discharge depth 100%. DETAILED DESCRIPTION
[0045] The battery with zinc anode is manufactured according to methods known to those skilled in the art. The electrode is plate-shaped and consists of a current collector and an active material. The active material may contain compounds that do not participate in the electrochemical reaction, but these compounds can ensure functions such as electron conduction or provide a mechanical connection between the active element and the current collector, or ensure the function of retaining the products of the electrochemical reaction.
[0046] For zinc anodes, in addition to polymers such as PTFE, polyethylene glycol, polyvinyl alcohol, styrene-butadiene polymers, carboxymethyl cellulose, etc. as binders for the electrode components, calcium hydroxide can be used to limit the formation of soluble zincates, as well as conductive ceramics as described in patent FR 2 788 887.
[0047] The diaphragm separates the anode compartment from the cathode compartment: it can be a felt, a porous membrane or an ion exchange membrane, and a combination of felt and porous membranes can be used. The diaphragm is usually a hydrophobic polymer membrane, which is made hydrophilic by adding one or more wetting agents. Depending on the manufacturing method, the battery with zinc anode can be prismatic, cylindrical or filter plate battery using bipolar cells.
[0048] The present invention is particularly suitable for manufacturing nickel-zinc storage batteries, and its main features are as follows.
[0049] According to a preferred embodiment, a nickel-zinc storage battery is manufactured by combining a plasticized nickel electrode with a zinc electrode containing an organic binder.
[0050] 1) Nickel Electrode
[0051] The current collector for the nickel electrode is preferably a nickel metal foam with very fine pores. Some foams are called "battery grade" and are available from suppliers such as Sumitomo Electric Industries (Japan) and Corun (China). The thickness of the foam is selected according to the required surface capacity of the nickel electrode, usually between 1.2 mm and 2 mm, but the thickness can be precisely adjusted by calendering to achieve the required surface capacity.
[0052] The active material consists of nickel hydroxide, preferably also containing coprecipitated zinc and cobalt. To increase the volume capacity, the particles are preferably spherical or quasi-spherical. The particles can be coated with cobalt oxide and hydroxide, which are converted into conductive cobalt oxyhydroxide when forming a battery (Oshitani et al., J. Electrochem.
[0053] Soc. 1989 136, 6, 1590).
[0054] Conductive additives (fibers, metal powders) may also be added to the nickel hydroxide powder.
[0055] The above ingredients are mixed with deionized water to which carboxymethyl cellulose has been added to form a slurry. A polymer binder such as PTFE in the form of a suspension can be added at this production stage or later after filling the current collector, more specifically nickel foam, with the active slurry soaked in the suspension.
[0056] The filling of the nickel foam can be carried out on a laboratory scale by pressing the slurry into the thickness of the support with a doctor blade, and on an industrial scale by injecting the slurry into the foam under pressure.
[0057] After drying, the electrodes are compressed to ensure adhesion between the current collector, active material and additives, and cut to the desired size.
[0058] 2) Zinc electrode
[0059] The current collector for the zinc electrode can be in the form of a perforated metal foil, woven mesh, expanded foil or metal foam. Copper is preferred for its conductivity but must be covered with a metal protector: zinc, tin or an alloy.
[0060] The zinc electrode is manufactured by preparing a slurry containing zinc oxide and various additives in advance:
[0061] Electronic conductors: metallic zinc, carbon, copper, conductive ceramics, etc. in powder or filament form.
[0062] Anti-corrosion agents: indium, bismuth, etc.
[0063] Compounds that react with zincate: calcium hydroxide, barium hydroxide, etc.
[0064] The liquid phase is deionized water or alcohol, to which carboxymethylcellulose is added as a binder and thickener. Other binders may be added as mentioned in patent application EP 1 715 536.
[0065] Depending on the chosen technique, a high viscosity slurry can be prepared and applied by pressure to both sides of the metal support to form a "sandwich" structure, or a medium viscosity slurry can be prepared, the current collector is immersed in it, and then the excess slurry is removed, the electrode thickness is adjusted with a scraper, and then a drying operation is performed. Finally, a dry powder mixed with a binder can also be used and pressed onto a metal support to form an electrode.
[0066] 3) Electrolyte
[0067] Preferably, a concentrated alkaline solution is used, the molar concentration of hydroxide ions being between 4 and 15 M (4 to 15 mol / l), preferably between 4 and 12 M. Alkalinity is provided by potassium hydroxide, sodium hydroxide and lithium hydroxide, which can be used alone or in mixture.
[0068] The electrolyte may also contain zincates and silicates, as mentioned in patent FR 3 099 851. The electrolyte may also contain borates, phosphates and fluorides, as described in patent US 5 215 836, either alone or in combination.
[0069] According to the present invention, the amount of wetting agent added to the electrolyte is between 0.1 g / l and 50 g / l, preferably between 1 g / l and 25 g / l; the amount of defoaming agent added to the electrolyte (in mg / kg electrolyte) is between 10 mg and 1000 mg. The wetting agent is especially selected from ionic wetting agents, bis (2-ethylhexyl) phosphate and non-ionic wetting agents such as alkyl polyglucosides, especially The defoaming agent is selected from the group of products related to the polyorganosiloxane chemical family. These wetting agents and defoaming agents can be used alone or in combination.
[0070] In order to illustrate the working principle and the definitions of the invention, NiZn elements 1 to 11 with a capacity of 8 Ah were implemented according to the general description provided above. The composition of the zinc electrodes of elements 1 to 4 differs from that of elements 5 to 11. The nickel electrodes of all elements are the same. The electrolyte used is a concentrated alkaline solution of hydroxide ions with a molar concentration of 10 M, with the addition of silicates, as described in patent FR 3 099 851. For elements 3, 4 and 8 to 11, the electrolyte is modified by the addition of wetting agents and defoamers. These elements are equipped with low-pressure valves of 0.2 bar. The battery is cycled with a constant current of 8 A, corresponding to a C-rate of charging for 1 hour corresponding to 100% charge and complete discharge when the voltage reaches 1 V. Table 1 summarizes the parameters that distinguish elements 1 to 11 and the number of cycles achieved with a capacity exceeding 70% of the rated capacity (Cn).
[0071]
[0072] Table 1: NiZn battery characteristics, nominal capacity 8Ah, cycle charge 8A 1h, 100% discharge 8A 1V, the symbol > indicates that the experiment is still in progress.
[0073] Example 1 (control group):
[0074] NiZn elements 1 to 4 with a nominal capacity of 8 Ah were implemented in the same manner as the general description provided above. The composition of the zinc electrodes of elements 1 to 4 differed from that of elements 5 to 11. The nickel electrodes of all elements were identical. The electrolyte used was a concentrated alkaline solution with a molar concentration of 10 M hydroxide ions, with the addition of silicate, as described in patent FR 3 099 851.
[0075] For these elements, two membranes, A and B, were used. Membrane A is a polypropylene microporous membrane with a thickness of 25 μm, to which a wetting agent was added. The gas permeability of this membrane A, expressed in Guerley, is relatively high, exceeding 1000, enabling it to act as a gas barrier to ensure thermal stability and limit the recombination of oxygen on the surface of the zinc electrode. The zinc electrode was covered with two layers of the membrane superimposed to form a thickness of 50 μm. Membrane B is a polypropylene microporous membrane with a thickness of 40 μm, to which a wetting agent was added. The gas permeability of this membrane B, expressed in Guerley, is lower than that of membrane A, ranging between 450 and 750. This wide range indicates that there are uniformity defects in the membrane layer to which the wetting agent is added. The zinc electrode surface is covered with only one layer of this membrane B.
[0076] Element 1, equipped with membrane A, showed 2240 cycles before the capacity fell below 70% of 8 Ah. Element 2, equipped with membrane B, resulted in zero capacity after a formation phase, characterized by 3 12-hour charge cycles at C / 10 rate and discharge cycles at C / 5 rate until the battery voltage reached 1.2 V.
[0077] Element 3 is the previous element 2, with 4 wetting agents added to the electrolyte, three of which are Brands BG-10, CG-110, X-100 and di(2-ethylhexyl) phosphate wetting agents. The four wetting agents were introduced into element 2 to make element 3, with a total concentration of 21.3 g / l. No defoamer was added. Figure 1 The change in discharge capacity of batteries 1 and 3 with the number of cycles was compared.
[0078] After the addition of the wetting agent, element 2, which originally had zero capacity, became element 3, achieving 2180 cycles, a result comparable to element 1. Thus, the wetting agent added to the electrolyte was able to deposit in situ on the membrane in the cell, allowing the otherwise incompatible membrane to function properly, with a life comparable to that obtained with membrane A; membrane A had no significant defects in its wetting agent attachment. This first experiment was therefore conclusive of the ability of the wetting agent introduced into the electrolyte to attach to the membrane and restore its hydrophilicity.
[0079] However, two problems incompatible with long-term operation were noted, the first being the formation of a large amount of foam, which could overflow from the battery and cause leakage, and the second being a significantly large mass loss. Thus, after 2000 cycles, elements 1 and 3 lost 8% and 44% of the electrolyte mass, respectively. When the electrolyte mass loss exceeds about 20%, water needs to be added to prevent a capacity drop due to battery drying out.
[0080] Example 2 (present invention):
[0081] Element 4 with a nominal capacity of 8 Ah was implemented in the same manner as the general description provided above. The zinc and nickel electrodes and the membrane A of element 4 were identical to those of element 1. The electrolyte used was a concentrated alkaline solution with a molar concentration of hydroxide ions of 10 M, to which was added a silicate as described in patent FR 3 099 851, and to which were added 4 wetting agents, 3 of which were Brands BG-10, CG-110, X-100 and di(2-ethylhexyl) phosphate wetting agents. The total concentration of the 4 wetting agents is 21.3 g / l. A defoamer from the polyorganosiloxane chemical family is added to the electrolyte at a level of 100 mg per kg of electrolyte. The battery is cycled at a constant current of 8 A, equivalent to a C rate, with a voltage of 1 V at the end of charge for 1 hour and discharge.
[0082] Figure 1The discharge capacity of cells 1, 3 and 4 was compared as a function of the number of cycles. Even though membrane A had no obvious defects in its wetting agent attachment, the results obtained for more than 3500 cycles showed that the wetting agent added to the electrolyte significantly improved the cycle life of this battery, being able to attach to membrane A and maintain or restore its hydrophilicity. The addition of a defoamer significantly reduced the formation of foam. After 2000 cycles, the mass loss was 21%, about 3 times that of element 1, which had a mass loss of 8% in the absence of a wetting agent. The larger mass loss was compensated by simply adding water, and a greater number of cycles was shown by the addition of a wetting agent and a defoamer to the electrolyte.
[0083] Example 3 (control group and the present invention):
[0084] Element 5 (control) with a nominal capacity of 8 Ah was implemented in the same manner as the general description provided above. It had the same nickel electrodes and membrane A as element 1, but the composition of its zinc electrode was different. The electrolyte used was a concentrated alkaline solution with a molar concentration of 10 M hydroxide ions, with the addition of silicate, as described in patent FR 3 099 851.
[0085] Element 6 (invention) is the same as element 5, but 4 wetting agents are added to the electrolyte, 3 of which are TRITON brand BG-10, CG-110, X-100 and di(2-ethylhexyl)phosphate wetting agent. The total concentration of the 4 wetting agents is 21.3 g / l. A defoamer from the polyorganosiloxane chemical family is added to the electrolyte in an amount of 100 mg per kg of electrolyte.
[0086] Element 7 (present invention) is the same as element 5, but two kinds of Brand wetting agents, BG-10 and X-100. The total concentration of the two wetting agents is 21.3 g / l. A defoamer from the polyorganosiloxane chemical family is added to the electrolyte in an amount of 100 mg per kg of electrolyte.
[0087] The three batteries were cycled at a constant current of 8 A, equivalent to a C rate, with a voltage of 1 V reached after 1 h of charging and at the end of discharge. Figure 2 The discharge capacity of batteries 5, 6 and 7 was compared with the cycle number.
[0088] Compared to Component 5, the addition of the wetting agent increased the cycle number of Component 6 by 44% to 2500 cycles, while the cycle number of Component 7 increased by 95% to 3400 cycles.
[0089] The addition of defoamers significantly reduced the formation of foam. After 2000 cycles, the mass loss of components 5, 6 and 7 was 18%, 57% and 45%, respectively, i.e. the mass loss of components with wetting agents was 2 to 3 times higher than that of components without wetting agents. The larger mass loss can be compensated by simply adding water and a higher number of cycles can be shown by adding wetting agents and defoamers to the electrolyte.
[0090] Example 4 (present invention):
[0091] To limit the foam formation caused by the addition of wetting agents, the amount of defoamer was doubled from 100 to 200 mg per kg of electrolyte.
[0092] To limit mass loss, the amount of wetting agent was reduced.
[0093] The new three sets of elements evaluated the effect of lower wetting agent concentrations, with elements 8, 9 and 10 having wetting agent concentrations of 10.65 g / l, 7.1 g / l and 5.3 g / l respectively.
[0094] Cells 8, 9 and 10 were identical to cell 5 except for the addition of a wetting agent and a defoaming agent. These cells were cycled at a constant current of 8 A, equivalent to a C rate, with a voltage of 1 V reached after 1 hour of charge and at the end of discharge.
[0095] The cycle numbers shown in Table 1 are 1740, 2120, 2220, 2520 and 2500 for elements 5, 8, 9, 10 and 6, respectively, indicating that even with lower concentrations of wetting agent, its effect is maintained. By reducing the concentration of wetting agent and increasing the amount of defoamer, foam formation and mass loss are significantly reduced, with mass losses of 11.8%, 9.3% and 13% for elements 8, 9 and 10 after 2000 cycles, respectively.
[0096] Example 5 (present invention):
[0097] Our analysis shows that strong oxygen recombination on the zinc electrode surface may accelerate the shedding of the wetting agent on the membrane. Sometimes, the heat release accompanying this reaction leads to a drop in the battery voltage at the end of charge, which is often referred to as "negative delta V" in the prior art.
[0098] To limit this phenomenon, the structure of the zinc electrode was slightly modified in element 11.
[0099] Apart from this modification, element 11 is identical to element 8 and similar to elements 5 and 6, with the addition of four wetting agents to the electrolyte, three of which are Brands, namely BG-10, CG-110, X-100, and a bis(2-ethylhexyl) phosphate wetting agent. The total concentration of the four wetting agents in component 11 is 10.65 g / l, which is half of that in component 6. A defoaming agent with a chemical composition of polyorganosiloxane is added to the electrolyte at a concentration of 200 mg per kg of electrolyte, which is twice that of component 6.
[0100] Element 11 was cycled at a constant current of 8 A, equivalent to a C rate, charging for 1 hour and discharging until the voltage reached 1 V.
[0101] Figure 3 The discharge capacity of batteries 5, 6 and 11 is compared with the change in cycle number.
[0102] According to this combination, the capacity stability of element 11 is further improved, exceeding 3350 cycles, and the test is still in progress. The mass loss after 2000 cycles of elements 5, 6 and 11 is 18%, 57% and 4%, respectively, indicating that the formation of foam and mass loss after the addition of wetting agent are improved and compatible with extended water addition cycles. Compared with the results measured for element 8, the performance improvement of element 11 - 65% reduction in mass loss at 2000 cycles and at least 55% increase in the number of cycles - highlights the enhanced stability associated with the authors of the present invention to reduce the consequences caused by oxygen recombination, further stabilizing the preservation of the wetting agent in the electrolyte and membrane.
[0103] Among the numerous experiments conducted by the inventors of the present invention, only a portion of which is listed in Table 1, it is shown that the selection of the concentration of the wetting agent and the defoaming agent can achieve good results in a wide range. The optimal concentration depends mainly on the characteristics of the membrane used, the alkalinity level of the electrolyte, the formula and preparation method of the electrode, the configuration of the battery, and the cycle conditions. The results show that the overall concentration of the wetting agent is between about 0.1 and 50 grams per liter of electrolyte, and the concentration of the defoaming agent is between about 10 and 1000 milligrams per kilogram of electrolyte.
[0104] At the zinc electrode, zinc metal is formed during charging by reducing zincate ions in solution. The zinc deposits surround the particles where they originate.
[0105] During the discharge of the zinc electrode, the zinc is converted to zincate ions, partially exposing its surface, which is then covered by a zinc oxide deposit that is characteristic of the active anode material in the discharged state. During the exposing phase, materials deposited or trapped in the zinc are also released into the electrolyte and redeposited in situ or elsewhere, especially on the membrane.
[0106] This release from the electrolyte is favored in cases where the zinc affinity for the wetting agent is low, which is the case for non-ionic wetting agents. Due to the close proximity of the membrane to the zinc electrode surface, this mechanism may deliver the wetting agent to the membrane and stabilize its hydrophilicity over time.
[0107] This phenomenon is similar to the self-repair mechanism of the membrane.
Claims
1. An alkaline electrochemical generator with a zinc anode, comprising an electrolyte, the electrolyte being an alkaline aqueous solution having a molar concentration of hydroxide ions between 4M and 15M and comprising: a) at least one wetting agent, the electrolyte concentration is 0.1 g / l and 50 g / l; and b) at least one defoaming agent in an amount between 10 mg and 1000 mg per kg of electrolyte; Features: - the electrolyte contains an ionic wetting agent, namely bis(2-ethylhexyl) phosphate; and / or - the electrolyte comprises at least one nonionic wetting agent selected from alkyl polyglucosides and polyethylene glycol ethers and alkyl phenol ethers; and / or - The defoaming agent is selected from polysiloxane.
2. An alkaline electrochemical generator with a zinc anode according to claim 1, comprising at least one ionic wetting agent and at least one non-ionic wetting agent.
3. Alkaline electrochemical generator with zinc anode according to one of claims 1 and 2, wherein the molar concentration of the alkaline solution is between 7M and 12M.
4. Alkaline electrochemical generator with zinc anode according to one of claims 1 to 3, wherein the concentration of the one or more wetting agents in the electrolyte is between 1 g / l and 25 g / l.
5. Alkaline electrochemical generator with zinc anode according to one of claims 1 to 4, wherein the concentration of the defoaming agent in the electrolyte is between 100 mg and 500 mg per kg of electrolyte.
6. Alkaline electrochemical generator with zinc anode according to one of claims 1 to 5, wherein the electrolyte further comprises silicate.
7. An alkaline electrochemical generator with a zinc anode according to any one of claims 1 to 6, wherein the electrolyte further comprises zincate.
8. An alkaline electrochemical generator with a zinc anode according to any one of claims 1 to 7, wherein the electrolyte further comprises borates, phosphates and / or fluorides.
9. A method for producing an alkaline electrochemical generator with a zinc anode according to one of claims 1 to 8, comprising a step of introducing lithium, sodium and / or potassium hydroxides when preparing the electrolyte.
Citation Information
Patent Citations
Nickel-zinc battery
CN111048846A
secondary alkali electrochemical generators with zinc anode
FR3099851A1
Hydrogen evolution inhibitors for cells having zinc anodes
US4195120A
Alkaline galvanic cells
US5215836A