Secondary battery and electric device
Patent Information
- Application Number
- CN202280095080.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-25
- Publication Date
- 2024-11-26
AI Technical Summary
It is difficult for existing secondary batteries to balance high energy density and service life when improving kinetic performance, and increasing energy density often affects kinetic performance and storage performance.
By using a first carbon-based material with both a pore structure and a second carbon-based material with a carbon coating layer on part of the surface in the negative electrode film layer, the layer spacing, gram capacity and powder compaction density are adjusted to form a reasonable Pore structure and active ion transport performance.
It achieves both good dynamic performance and storage performance under the premise of high energy density, and extends the service life of the battery.
Smart Images

Figure CN119032438A_ABST
Abstract
Description
Secondary batteries and electrical devices Technical Field
[0001] The present application belongs to the field of battery technology, and specifically relates to a secondary battery and an electrical device. Background Art
[0002] In recent years, secondary batteries have been widely used in energy storage systems such as hydropower, thermal, wind, and solar power stations, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and other fields. As the scope of secondary battery applications expands, so too have the increasing demands placed on their performance. For example, the requirement for secondary batteries to balance various performance requirements, such as energy density, dynamic performance, and service life, has become increasingly challenging. However, existing technologies face the following challenges: improving the dynamic performance of secondary batteries often struggles to balance their energy density; and increasing their energy density often compromises their dynamic performance and service life.
[0003] Summary of the Invention
[0004] The present application is developed in view of the above-mentioned technical problems, and its purpose is to provide a secondary battery and an electrical device, which can enable the secondary battery to have good dynamic performance and storage performance while having high energy density.
[0005] A first aspect of the present application provides a secondary battery, comprising a negative electrode plate, wherein the negative electrode plate comprises a negative electrode current collector and a negative electrode film layer formed on at least one surface of the negative electrode current collector and comprising a negative electrode active material, wherein the negative electrode active material comprises a first carbon-based material and a second carbon-based material, wherein the first carbon-based material has a pore structure, and at least a portion of the surface of the second carbon-based material has a carbon coating layer.
[0006] The inventors discovered through in-depth research that by making the negative electrode active material in the negative electrode film layer include a first carbon-based material and a second carbon-based material at the same time, the first carbon-based material has a pore structure, and at least part of the surface of the second carbon-based material has a carbon coating layer, the high capacity and high compaction density characteristics of the first carbon-based material and the good kinetic characteristics of the second carbon-based material can be fully utilized, thereby enabling the negative electrode plate to have a high compaction density, low volume change and high active ion transport performance, and thus the secondary battery using the negative electrode plate can have good kinetic performance and storage performance while having high energy density.
[0007] In any embodiment of the present application, the interlayer spacing of the 002 crystal plane of the second carbon-based material is greater than the interlayer spacing of the 002 crystal plane of the first carbon-based material. By adjusting the interlayer spacing of the 002 crystal plane of the second carbon-based material to be greater than the interlayer spacing of the 002 crystal plane of the first carbon-based material, it is beneficial for the secondary battery to achieve both high energy density and good dynamic performance.
[0008] In any embodiment of the present application, the gram capacity of the second carbon-based material is less than the gram capacity of the first carbon-based material. By combining the first carbon-based material having a high capacity with the second carbon-based material having a carbon coating layer, it is beneficial for the secondary battery to have both high energy density and good kinetic performance.
[0009] In any embodiment of the present application, the powder compaction density of the second carbon-based material under a pressure of 5000 kg is less than the powder compaction density of the first carbon-based material under a pressure of 5000 kg. By combining the second carbon-based material having a low powder compaction density with the first carbon-based material having a high powder compaction density, it is beneficial for the negative electrode film layer to have a reasonable pore structure and enable the negative electrode film layer to have good active ion transport performance and electron transport performance, thereby facilitating the secondary battery to have high energy density and good cycle performance and kinetic performance.
[0010] In any embodiment of the present application, the peak intensity ratio of the D peak to the G peak in the Raman spectrum of the second carbon-based material is D / I G Greater than the peak intensity ratio I of the D peak and the G peak in the Raman spectrum of the first carbon-based material D / I G By adjusting the I D / I G Greater than the I of the first carbon-based material D / I G On the one hand, it is beneficial to improve the overall surface stability of the negative electrode active material, reduce the occurrence of side reactions, and improve storage performance; on the other hand, it is also beneficial for the secondary battery to have good kinetic performance.
[0011] In any embodiment of the present application, the second carbon-based material includes secondary particles. Optionally, the number of secondary particles in the second carbon-based material is greater than or equal to 50%. When the second carbon-based material includes an appropriate proportion of secondary particles, the active ion channels in the negative electrode film layer can be increased, the active ion insertion path can be shortened, thereby further improving the kinetic performance of the secondary battery, and can also reduce polarization and side reactions, thereby enabling the secondary battery to have good storage performance.
[0012] In any embodiment of the present application, the peak intensity ratio of the D peak to the G peak in the Raman spectrum of the second carbon-based material is D / I G is ≥0.23, and can be 0.23-0.41. By adjusting the I D / I GWithin the above range, the second carbon-based material has better active ion transport performance, which is beneficial to improving the kinetic performance of the secondary battery.
[0013] In any embodiment of the present application, the powder compaction density of the second carbon-based material under a pressure of 5000 kg is ≥1.65 g / cm 3 , optional 1.65g / cm 3 -1.90g / cm 3 By adjusting the powder compaction density of the second carbon-based material within the above range, it is beneficial to form a reasonable pore structure between the particles of the negative electrode film layer, thereby facilitating the secondary battery to have both high energy density and good dynamic performance.
[0014] In any embodiment of the present application, the interlayer spacing of the 002 crystal plane of the second carbon-based material is ≤0.336217 nm, and can be optionally 0.335787 nm-0.336217 nm. By adjusting the interlayer spacing of the second carbon-based material within the above range, it is beneficial to the rapid deintercalation of active ions, thereby improving the active ion transport performance of the negative electrode film layer; in addition, the second carbon-based material can also have high surface stability and high specific capacity, thereby reducing the occurrence of side reactions.
[0015] In any embodiment of the present application, the specific surface area of the second carbon-based material is ≥0.90m 2 / g, optional 0.9m 2 / g-2.5m 2 By adjusting the specific surface area of the second carbon-based material within the above range, it is beneficial to the rapid deintercalation of active ions, thereby further improving the kinetic performance of the secondary battery. It is also beneficial to reduce the occurrence of side reactions and the consumption of active ions by SEI film formation, thus helping the secondary battery to achieve both high initial coulombic efficiency and good cycle performance and storage performance.
[0016] In any embodiment of the present application, the volume distribution particle size Dv50 of the second carbon-based material is ≥10 μm, and can be optionally 10 μm-22 μm. When the volume distribution particle size Dv50 of the second carbon-based material is within the above range, the specific surface area of the second carbon-based material can be reduced, the occurrence of side reactions can be reduced, and the storage performance and / or cycle performance of the secondary battery can be improved. In addition, it is also beneficial to improve the transport performance of active ions and electrons, thereby further improving the kinetic performance of the secondary battery.
[0017] In any embodiment of the present application, the particle size distribution (Dv90-Dv10) / Dv50 of the second carbon-based material is ≤1.65, and can be optionally 0.9-1.65. When the particle size distribution (Dv90-Dv10) / Dv50 of the second carbon-based material is within the above range, its particle stacking performance is good, which is beneficial to improving the compaction density of the negative electrode film layer and improving the energy density of the secondary battery; in addition, it is also beneficial to form a reasonable pore structure between the particles of the negative electrode film layer, improving the active ion and electron transport performance, and thus improving the kinetic performance of the secondary battery.
[0018] In any embodiment of the present application, the tap density of the second carbon-based material is ≥0.85 g / cm 3 , optional 0.9g / cm 3 -1.25g / cm 3 When the tap density of the second carbon-based material is within the above range, it can increase the compaction density of the negative electrode film layer and improve the energy density of the secondary battery. In addition, it is also conducive to the formation of a reasonable pore structure between the particles of the negative electrode film layer, improving the active ion and electron transport performance, and thus improving the kinetic performance of the secondary battery.
[0019] In any embodiment of the present application, the gram capacity of the second carbon-based material is ≥340 mAh / g, and can be optionally 340 mAh / g-360 mAh / g. By adjusting the gram capacity of the second carbon-based material within the above range, on the one hand, the energy density of the secondary battery can be improved, and on the other hand, the second carbon-based material can also have good active ion transport performance, thereby also helping to improve the kinetic performance of the secondary battery.
[0020] In any embodiment of the present application, the second carbon-based material includes at least one of artificial graphite and natural graphite. Optionally, the second carbon-based material includes artificial graphite.
[0021] In any embodiment of the present application, the first carbon-based material includes one or more pores with an area greater than or equal to 0.1 μm 2 The pore structure may include one or more pores with an area of 0.12 μm 2 -2.5μm 2 When the first carbon-based material includes a pore structure having the above-mentioned pore area, the pore structure can reserve the required expansion space for its particle volume change, thereby further reducing the risk of particle breakage and generation of new interfaces, thereby reducing the occurrence of side reactions and improving the storage performance of the secondary battery.
[0022] In any embodiment of the present application, the first carbon-based material includes an outer region and an inner region located inside the outer region, wherein the outer region refers to a region extending from the surface of the first carbon-based material particle to the interior of the particle by a distance of 0.25L, where L refers to the minor axis length of the first carbon-based material particle, the total pore area of the outer region is denoted as S1, the total pore area of the inner region is denoted as S2, and S2>S1. When the first carbon-based material further satisfies S2>S1, the first coulombic efficiency of the secondary battery can be improved, and the storage performance of the secondary battery can be further improved.
[0023] In any embodiment of the present application, 1.5≤S2 / S1≤500, optionally, 2≤S2 / S1≤450. When S2 / S1 is also within the above range, the secondary battery can better achieve both high energy density and good storage performance.
[0024] In any embodiment of the present application, the area of the pore structure in the outer region of the first carbon-based material is less than or equal to 0.15 μm 2 , can be selected to be less than or equal to 0.13μm 2 By controlling the area of the pore structure in the outer region of the first carbon-based material within the above range, the outer region of the first carbon-based material can have a dense structure, thereby effectively improving the structural stability of the first carbon-based material and preventing the electrolyte from penetrating into the pore structure inside the first carbon-based material particles as much as possible, thereby effectively improving the storage performance of the secondary battery.
[0025] In any embodiment of the present application, the inner region of the first carbon-based material includes one or more areas greater than or equal to 0.15 μm 2 The pore structure may include one or more pores with an area of 0.15 μm 2 -2.0μm 2 By making the internal region of the first carbon-based material include a pore structure of the aforementioned size, sufficient and stable expansion space can be reserved for the volume change of the first carbon-based material particles, thereby reducing the risk of first carbon-based material particles breaking and the occurrence of side reactions. On the other hand, the compaction density of the negative electrode film layer can also be improved.
[0026] In any embodiment of the present application, at least a portion of the surface of the first carbon-based material has a carbon coating layer.
[0027] In any embodiment of the present application, the first carbon-based material includes primary particles. Optionally, the number of primary particles in the first carbon-based material accounts for greater than or equal to 50%. When the first carbon-based material includes an appropriate proportion of primary particles, it can have higher structural stability, reduce the occurrence of side reactions, thereby improving the storage performance of the secondary battery, and further increase the compaction density of the negative electrode film layer, thereby improving the energy density of the secondary battery.
[0028] In any embodiment of the present application, the specific surface area of the first carbon-based material is ≤2.3m 2 , optional 0.7m 2 / g-2.3m 2 The first carbon-based material has a lower specific surface area, thereby reducing the consumption of active ions in SEI film formation, reducing the occurrence of side reactions, and improving the initial coulombic efficiency and storage performance of the secondary battery.
[0029] In any embodiment of the present application, the volume distribution particle size Dv50 of the first carbon-based material is ≥6.0 μm, and can be optionally 6.0 μm-25.0 μm.
[0030] In any embodiment of the present application, the volume distribution particle size Dv90 of the first carbon-based material is ≥16.0 μm, and can be optionally 16.0 μm-40.0 μm.
[0031] When the volume distribution particle size Dv50 and / or Dv90 of the first carbon-based material is within the above range, it is beneficial to improve the transmission performance of active ions and electrons, thereby improving the kinetic performance of the secondary battery. In addition, it can also reduce the specific surface area of the first carbon-based material, reduce the occurrence of side reactions, and improve the storage performance of the secondary battery.
[0032] In any embodiment of the present application, the particle size distribution (Dv90-Dv10) / Dv50 of the first carbon-based material is ≤1.55, and can be optionally 0.9-1.55. When the particle size distribution (Dv90-Dv10) / Dv50 of the first carbon-based material is within the above range, its particle packing performance is good, which is beneficial to improving the compaction density of the negative electrode film layer and improving the energy density of the secondary battery; in addition, it is also beneficial to form a reasonable pore structure between the particles of the negative electrode film layer, improving the active ion and electron transport performance, and improving the kinetic performance of the secondary battery.
[0033] In any embodiment of the present application, the tap density of the first carbon-based material is ≥0.8 g / cm 3 , optional 0.8g / cm 3 -1.20g / cm 3When the tap density of the first carbon-based material is within the above range, it can increase the compaction density of the negative electrode film layer and improve the energy density of the secondary battery. It is also conducive to forming a reasonable pore structure between the particles of the negative electrode film layer, improving the active ion and electron transport performance, and thus improving the kinetic performance of the secondary battery.
[0034] In any embodiment of the present application, the powder compaction density of the first carbon-based material under a pressure of 5000 kg is ≤ 2.10 g / cm 3 , optional 1.85g / cm 3 -2.10g / cm 3 When the powder compaction density of the first carbon-based material is within the above range, the compaction density of the negative electrode film layer can be increased, thereby increasing the energy density of the secondary battery. This is also conducive to forming a reasonable pore structure between the particles of the negative electrode film layer, thereby improving the active ion and electron transport performance, and thus improving the kinetic performance of the secondary battery.
[0035] In any embodiment of the present application, the interlayer spacing of the 002 crystal plane of the first carbon-based material is ≤0.335916nm, and can be 0.335576nm-0.335916nm. When the interlayer spacing of the first carbon-based material is within the above range, its specific capacity is higher, which is conducive to improving the energy density of the secondary battery.
[0036] In any embodiment of the present application, the gram capacity of the first carbon-based material is ≥358 mAh / g, and can be 358 mAh / g-370 mAh / g. When the gram capacity of the first carbon-based material is within the above range, the energy density of the secondary battery can be improved.
[0037] In any embodiment of the present application, the X-ray diffraction pattern of the first carbon-based material has a diffraction peak of the 3R phase 101 crystal plane. When the first carbon-based material has a diffraction peak of the 3R phase 101 crystal plane, more active sites may exist on the surface of the first carbon-based material particles, which can accelerate the transmission of active ions.
[0038] In any embodiment of the present application, the X-ray diffraction pattern of the first carbon-based material does not have a diffraction peak of the 3R phase 012 crystal plane. When the first carbon-based material does not have a diffraction peak of the 3R phase 012 crystal plane, its internal defects are relatively small, which can reduce the consumption of active ions and improve the initial coulombic efficiency and storage performance of the secondary battery.
[0039] In any embodiment of the present application, in a thermogravimetric analysis test of the first carbon-based material in an air atmosphere, the weight loss rate of the first carbon-based material between 35°C and 790°C is ≤50%, and can optionally be 16%-43%. The first carbon-based material has a lower weight loss rate between 35°C and 790°C, at which time it has fewer surface defects and / or bulk defects, which can reduce the consumption of active ions in SEI film formation and reduce the consumption of active ions during storage of the secondary battery, thereby improving the storage performance of the secondary battery.
[0040] In any embodiment of the present application, in the thermogravimetric analysis test of the first carbon-based material in an air atmosphere, the temperature corresponding to the maximum weight loss rate of the first carbon-based material is recorded as T max , then T max Greater than or equal to 795°C, optionally 805°C-850°C. The first carbon-based material has a temperature T corresponding to a high maximum weight loss rate. max At this time, it has good thermal stability and low reactivity, which can reduce the consumption of active ions in SEI film formation and reduce the consumption of active ions in the storage process of secondary batteries, thereby improving the storage performance of secondary batteries.
[0041] In any embodiment of the present application, the mass proportion of the first carbon-based material in the negative electrode active material is ≥30wt%, and can be 30wt%-80wt%. When the content of the first carbon-based material is within the above range, the energy density of the secondary battery can be improved, and the secondary battery can also have good dynamic performance.
[0042] In any embodiment of the present application, the volume distribution particle size Dv50 of the negative electrode active material is ≥6 μm, and can be optionally 6 μm-23 μm. When the volume distribution particle size Dv50 of the negative electrode active material is within the above range, it is beneficial to improve the transport performance of active ions and electrons, thereby further improving the kinetic performance of the secondary battery, and can also reduce the occurrence of side reactions and improve the storage performance of the secondary battery.
[0043] In any embodiment of the present application, the particle size distribution (Dv90-Dv10) / Dv50 of the negative electrode active material is ≥0.9, and can optionally be 0.9-1.55. When the particle size distribution (Dv90-Dv10) / Dv50 of the negative electrode active material is within the above range, its particle packing performance is good, which is beneficial for increasing the compaction density of the negative electrode film layer, thereby further improving the energy density of the secondary battery. In addition, it is also beneficial for forming a reasonable pore structure between the particles in the negative electrode film layer, thereby improving the dynamic performance of the secondary battery.
[0044] In any embodiment of the present application, the degree of graphitization of the negative electrode active material is ≥92%, and can be optionally 92%-96%. By adjusting the degree of graphitization of the negative electrode active material within the above range, the negative electrode active material is advantageously provided with high gram capacity and good active ion transport performance, thereby facilitating the secondary battery to achieve both high energy density and good kinetic performance.
[0045] In any embodiment of the present application, the gram capacity of the negative electrode active material is ≥350 mAh / g, and can be 350 mAh / g-365 mAh / g. By adjusting the gram capacity of the negative electrode active material within the above range, it is beneficial to improve the energy density of the secondary battery.
[0046] In any embodiment of the present application, the negative electrode film layer further comprises a silicon-based material. The silicon-based material can improve the pore structure in the negative electrode film layer, facilitate electrolyte infiltration and retention, and enhance the dynamic performance of the secondary battery; it can also increase the negative electrode capacity, thereby further improving the energy density of the secondary battery.
[0047] In any embodiment of the present application, the mass proportion of the silicon-based material in the negative electrode film layer is less than or equal to 20%. This can improve the dynamic performance and energy density of the secondary battery while ensuring good cycle performance and storage performance.
[0048] In any embodiment of the present application, the porosity of the negative electrode film layer is ≥15.5%, and can be optionally 15.5%-38%. This is beneficial for the negative electrode film layer to have both high capacity and suitable pore structure, and further beneficial for the secondary battery to have both high energy density and good storage performance and dynamic performance.
[0049] In any embodiment of the present application, the compaction density of the negative electrode film layer is ≥1.40 g / cm 3 , optional 1.40g / cm 3 -1.80g / cm 3 This is beneficial for the negative electrode film layer to have both high capacity and high active ion and electron transport performance, and further beneficial for the secondary battery to have both high energy density and good storage performance and kinetic performance.
[0050] In any embodiment of the present application, the surface density of the negative electrode film layer is ≥5.5 g / cm 2 , optional 6.0g / cm 3 -19.5g / cm 2 This is beneficial for the negative electrode film layer to have both high capacity and high active ion and electron transport performance, and further beneficial for the secondary battery to have both high energy density and good storage performance and kinetic performance.
[0051] In any embodiment of the present application, the OI value of the negative electrode film layer is ≤38, and can be 8-38. This is beneficial to improving the active ion embedding performance of the negative electrode film layer and also enables the negative electrode film layer to have a lower thickness rebound rate, thereby facilitating the secondary battery to have good storage performance and dynamic performance.
[0052] A second aspect of the present application provides an electrical device comprising the secondary battery according to the first aspect of the present application.
[0053] The electric device of the present application includes the secondary battery provided by the present application, and thus has at least the same advantages as the secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] To more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on the drawings without inventive effort.
[0055] FIG1 is a schematic diagram of a cross-sectional image of a particle of a first carbon-based material of the present application.
[0056] FIG. 2 is a schematic diagram of an embodiment of a secondary battery of the present application.
[0057] FIG3 is an exploded schematic diagram of an embodiment of a secondary battery of the present application.
[0058] FIG4 is a schematic diagram of an embodiment of a battery module of the present application.
[0059] FIG5 is a schematic diagram of an embodiment of a battery pack of the present application.
[0060] FIG. 6 is an exploded schematic diagram of the embodiment of the battery pack shown in FIG. 5 .
[0061] FIG. 7 is a schematic diagram of an embodiment of an electric device including the secondary battery of the present application as a power source.
[0062] In the accompanying drawings, which are not necessarily drawn to scale, reference numerals are as follows: 1 battery pack, 2 upper housing, 3 lower housing, 4 battery module, 5 secondary battery, 51 housing, 52 electrode assembly, 53 cover plate, 100 first carbon-based material, 101 outer region, 102 inner region. DETAILED DESCRIPTION
[0063] Below, the embodiments of the secondary battery and the electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0064] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0065] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of the present application.
[0066] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of this application.
[0067] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0068] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0069] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0070] Unless otherwise specified, the terms used in this application have the common meanings generally understood by those skilled in the art.
[0071] Unless otherwise specified, the values of the parameters mentioned in this application can be measured using various test methods commonly used in the art, for example, they can be measured according to the test methods given in this application.
[0072] Unless otherwise specified, in this application, the term "active ions" refers to ions that can be intercalated and extracted back and forth between the positive electrode and the negative electrode of a secondary battery, including but not limited to lithium ions.
[0073] In this application, the terms "plurality" and "multiple" refer to two or more.
[0074] The inventors have discovered that the key to improving the kinetic performance of secondary batteries, especially their rapid charging capabilities, lies in improving the kinetic performance of the negative electrode. Currently, most approaches to improving the kinetic performance of the negative electrode are to reduce the coating weight of the negative electrode film or to reduce the compaction density of the negative electrode film. However, numerous studies have shown that these methods of improving the kinetics of the negative electrode only improve the kinetic performance of the battery in the early stages of charging to a certain extent, and have no significant effect on improving the kinetic performance of the battery in the final stages of charging. This results in the secondary battery's kinetic performance failing to be effectively improved, and even makes it impossible to actually charge the secondary battery at a high rate. Furthermore, the energy density of the secondary battery will also be significantly reduced.
[0075] When the energy density of a secondary battery is increased by, for example, increasing the compaction density of the negative electrode film layer, the kinetic performance of the secondary battery is often deteriorated. In addition, the electrolyte wetting characteristics of the negative electrode film layer deteriorate under high compaction density, and the risk of negative electrode active material particles breaking increases, thereby increasing side reactions inside the battery, which in turn affects the storage performance of the secondary battery.
[0076] Therefore, it is difficult for current secondary batteries to achieve both high energy density and good dynamic and storage performance.
[0077] The inventors further conducted extensive research and cleverly improved the composition of the negative electrode film layer, breaking the above bottleneck.
[0078] Specifically, a first aspect of the embodiments of the present application provides a secondary battery.
[0079] The present application does not have any particular restrictions on the type of secondary battery. For example, the secondary battery can be a lithium-ion battery, etc. In general, a secondary battery includes a positive electrode sheet, a negative electrode sheet, and an electrolyte, etc. During the charge and discharge process of the secondary battery, active ions are embedded and extracted back and forth between the positive electrode sheet and the negative electrode sheet, and the electrolyte plays a role in conducting active ions between the positive electrode sheet and the negative electrode sheet. The present application does not have any particular restrictions on the type of the electrolyte, and it can be selected according to actual needs. For example, the electrolyte can be selected from at least one of a solid electrolyte and a liquid electrolyte (i.e., an electrolyte). Secondary batteries using electrolytes, and some secondary batteries using solid electrolytes, may also include an isolation membrane, which is arranged between the positive electrode sheet and the negative electrode sheet to play an isolation role.
[0080] [Negative electrode]
[0081] The negative electrode plate includes a negative electrode current collector and a negative electrode film layer formed on at least one surface of the negative electrode current collector and including a negative electrode active material, the negative electrode active material includes a first carbon-based material and a second carbon-based material, the first carbon-based material has a pore structure, and at least part of the surface of the second carbon-based material has a carbon coating layer.
[0082] In the present application, "the first carbon-based material has a pore structure" means that the first carbon-based material has a pore structure that can be directly observed from a cross-sectional image (for example, a scanning electron microscope image with a magnification of 1000 times), that is, the pore structure in the main structure of the raw material used to prepare the first carbon-based material is not completely filled.
[0083] The inventors have discovered that when at least part of the surface of the second carbon-based material has a carbon coating (e.g., a coating comprising amorphous carbon), its kinetic performance is better, facilitating the rapid deintercalation of active ions. However, the second carbon-based material has a relatively low gram capacity and compaction density, which can affect the compaction density of the negative electrode film layer and the energy density of the secondary battery. The first carbon-based material has a porous structure and a relatively high compaction density, which can increase the compaction density of the negative electrode film layer and the energy density of the secondary battery. At the same time, the porous structure can also reserve the required expansion space for particle volume changes, reducing the risk of particle breakage and the formation of new interfaces, thereby reducing the occurrence of side reactions.
[0084] The inventors discovered through in-depth research that by making the negative electrode active material in the negative electrode film layer include a first carbon-based material and a second carbon-based material at the same time, the first carbon-based material has a pore structure, and at least part of the surface of the second carbon-based material has a carbon coating layer, the high capacity and high compaction density characteristics of the first carbon-based material and the good kinetic characteristics of the second carbon-based material can be fully utilized, thereby enabling the negative electrode plate to have a high compaction density, low volume change and high active ion transport performance, and thus the secondary battery using the negative electrode plate can have good kinetic performance and storage performance while having high energy density.
[0085] In some embodiments, the interlayer spacing of the 002 crystal plane of the second carbon-based material is greater than the interlayer spacing of the 002 crystal plane of the first carbon-based material. The larger interlayer spacing of the second carbon-based material is conducive to the rapid deintercalation of active ions, while the smaller interlayer spacing of the first carbon-based material leads to a higher specific capacity. Therefore, by adjusting the interlayer spacing of the 002 crystal plane of the second carbon-based material to be greater than the interlayer spacing of the 002 crystal plane of the first carbon-based material, it is beneficial for the secondary battery to have both high energy density and good dynamic performance.
[0086] In some embodiments, the gram capacity of the second carbon-based material is less than the gram capacity of the first carbon-based material. By combining the first carbon-based material having a high capacity with the second carbon-based material having a carbon coating layer, it is beneficial for the secondary battery to have both high energy density and good kinetic performance.
[0087] In some embodiments, the powder compaction density of the second carbon-based material under a pressure of 5000 kg is less than the powder compaction density of the first carbon-based material under a pressure of 5000 kg. The powder compaction density of the first carbon-based material is relatively high, which is conducive to the formation of a good electron conduction network in the negative electrode film layer, and the powder compaction density of the second carbon-based material is relatively low, which is conducive to the negative electrode film layer having good electrolyte infiltration characteristics. Therefore, by combining the second carbon-based material with a low powder compaction density with the first carbon-based material with a high powder compaction density, it is beneficial for the negative electrode film layer to have a reasonable pore structure, and the negative electrode film layer to have both good active ion transmission performance and electron transmission performance, which is beneficial for the secondary battery to have both high energy density and good cycle performance and kinetic performance.
[0088] In some embodiments, the peak intensity ratio of the D peak to the G peak in the Raman spectrum of the second carbon-based material is 1 D / I G Greater than the peak intensity ratio I of the D peak and the G peak in the Raman spectrum of the first carbon-based material D / I G . The second carbon-based material I D / I G The larger the particle size, the more active sites it has on the particle surface, which is beneficial to the rapid deintercalation of active ions. D / I G Small, thus the surface stability of the particles is high, can reduce the occurrence of side reactions. Therefore, by adjusting the I of the second carbon-based material D / I G Greater than the I of the first carbon-based material D / I G On the one hand, it is beneficial to improve the overall surface stability of the negative electrode active material, reduce the occurrence of side reactions, and improve storage performance; on the other hand, it is also beneficial for the secondary battery to have good kinetic performance.
[0089] In some embodiments, the second carbon-based material includes secondary particles. Optionally, the amount of the secondary particles in the second carbon-based material is greater than or equal to 50%, for example, it can be 50%-95%, 60%-100%, 65%-85%, 70%-100%, 75%-90%, 75%-85%, 80%-100%, 80%-90%, 85%-95%, or 90%-100%. When the second carbon-based material contains an appropriate proportion of secondary particles, the active ion channels in the negative electrode film layer can be increased, and the active ion embedding path can be shortened, thereby further improving the kinetic performance of the secondary battery, and reducing polarization and side reactions, so that the secondary battery can also have good storage performance.
[0090] In some embodiments, the second carbon-based material is all secondary particles, that is, the number of the secondary particles in the second carbon-based material accounts for 100%.
[0091] In the present application, the number ratio of secondary particles in the second carbon-based material refers to: randomly taking a test sample in the negative electrode film layer, randomly taking multiple test areas in the test sample, using a scanning electron microscope to obtain images of the multiple test areas, and counting the ratio of the number of second carbon-based materials with secondary particle morphology in each image to the total number of second carbon-based material particles. The average value of multiple statistical results is the number ratio of secondary particles in the second carbon-based material.
[0092] In some embodiments, the peak intensity ratio of the D peak to the G peak in the Raman spectrum of the second carbon-based material is 1 D / I G is ≥0.23, and can be 0.23-0.41. By adjusting the I D / I G Within the above range, the second carbon-based material has better active ion transport performance, which is beneficial to improving the kinetic performance of the secondary battery.
[0093] In some embodiments, the powder compaction density of the second carbon-based material under a pressure of 5000 kg is ≥1.65 g / cm 3 , optional 1.65g / cm 3 -1.90g / cm 3 By adjusting the powder compaction density of the second carbon-based material within the above range, it is beneficial to form a reasonable pore structure between the particles of the negative electrode film layer, thereby facilitating the secondary battery to have both high energy density and good dynamic performance.
[0094] In some embodiments, the interlayer spacing of the 002 crystal plane of the second carbon-based material is ≤0.336217nm, and can be optionally 0.335787nm-0.336217nm. By adjusting the interlayer spacing of the second carbon-based material within the above range, it is beneficial to the rapid deintercalation of active ions, thereby improving the active ion transport performance of the negative electrode film layer; in addition, the second carbon-based material can also have high surface stability and high gram capacity, thereby reducing the occurrence of side reactions. Therefore, the secondary battery can take into account high energy density as well as good kinetic performance and storage performance.
[0095] In some embodiments, the specific surface area of the second carbon-based material is ≥0.90 m 2 / g, optional 0.9m 2 / g-2.5m 2 / g,0.95m 2 / g-2.45m 2By adjusting the specific surface area of the second carbon-based material within the above range, it is beneficial to the rapid deintercalation of active ions, thereby further improving the kinetic performance of the secondary battery. It is also beneficial to reduce the occurrence of side reactions and the consumption of active ions by SEI film formation, thus helping the secondary battery to achieve both high initial coulombic efficiency and good cycle performance and storage performance.
[0096] In some embodiments, the volume distribution particle size Dv50 of the second carbon-based material is ≥10 μm, optionally 10 μm-22 μm, and optionally 11.5 μm-20.0 μm. When the volume distribution particle size Dv50 of the second carbon-based material is within the above range, the specific surface area of the second carbon-based material can be reduced, the occurrence of side reactions can be reduced, and the storage performance and / or cycle performance of the secondary battery can be improved. In addition, it is also beneficial to improve the transport performance of active ions and electrons, thereby further improving the kinetic performance of the secondary battery.
[0097] In some embodiments, the particle size distribution (Dv90-Dv10) / Dv50 of the second carbon-based material is ≤1.65, and can optionally be 0.9-1.65. When the particle size distribution (Dv90-Dv10) / Dv50 of the second carbon-based material is within the above range, its particle packing performance is good, which is beneficial to improving the compaction density of the negative electrode film layer and the energy density of the secondary battery. In addition, it is also beneficial to form a reasonable pore structure between the particles of the negative electrode film layer, improving the active ion and electron transport performance, and thus improving the kinetic performance of the secondary battery.
[0098] In some embodiments, the tap density of the second carbon-based material is ≥0.85 g / cm 3 , optional 0.85g / cm 3 -1.25g / cm 3 , 0.9g / cm 3 -1.25g / cm 3 When the tap density of the second carbon-based material is within the above range, it can increase the compaction density of the negative electrode film layer and improve the energy density of the secondary battery. In addition, it is also conducive to the formation of a reasonable pore structure between the particles of the negative electrode film layer, improving the active ion and electron transport performance, and thus improving the kinetic performance of the secondary battery.
[0099] In some embodiments, the gram capacity of the second carbon-based material is ≥340 mAh / g, and can be 340 mAh / g to 360 mAh / g, or 345 mAh / g to 360 mAh / g. By adjusting the gram capacity of the second carbon-based material within the above range, on the one hand, the energy density of the secondary battery can be improved, and on the other hand, the second carbon-based material can also have good active ion transport performance, thereby also helping to improve the kinetic performance of the secondary battery.
[0100] In some embodiments, the second carbon-based material comprises at least one of artificial graphite and natural graphite. Alternatively, the second carbon-based material comprises artificial graphite.
[0101] In some embodiments, more than 80% of the surface of the second carbon-based material is covered with a carbon coating layer. Optionally, 90%-100% of the surface of the graphite is covered with a carbon coating layer.
[0102] In some embodiments, the carbon in the coating layer comprises amorphous carbon, which facilitates rapid deintercalation of active ions. The carbon may be formed by carbonization of an organic carbon source. The organic carbon source may be any carbonaceous material known in the art suitable for coating, for example, one or more of coal tar, petroleum asphalt, phenolic resin, coconut shell, and the like.
[0103] In some embodiments, the second carbon-based material comprises artificial graphite in the form of secondary particles, and at least a portion of the surface of the artificial graphite has a carbon coating. Optionally, the amount of artificial graphite in the form of secondary particles in the second carbon-based material is greater than or equal to 50%, for example, 50%-95%, 60%-100%, 65%-85%, 70%-100%, 75%-90%, 75%-85%, 80%-100%, 80%-90%, 85%-95%, or 90%-100%.
[0104] In the present application, the quantitative ratio of artificial graphite with secondary particle morphology in the second carbon-based material refers to: randomly taking a test sample in the negative electrode film layer, randomly taking multiple test areas in the test sample, using a scanning electron microscope to obtain images of the multiple test areas, and counting the ratio of the number of artificial graphite with secondary particle morphology in each image to the total number of particles of the second carbon-based material. The average value of multiple statistical results is the quantitative ratio of artificial graphite with secondary particle morphology in the second carbon-based material.
[0105] In some embodiments, the first carbon-based material includes at least one pore with an area greater than or equal to 0.1 μm 2 The pore structure may include one or more pores with an area of 0.12 μm 2 -2.5μm 2 When the first carbon-based material includes a pore structure having the above-mentioned pore area, the pore structure can reserve the required expansion space for its particle volume change, thereby further reducing the risk of particle breakage and generation of new interfaces, thereby reducing the occurrence of side reactions and improving the storage performance of the secondary battery.
[0106] In some embodiments, the first carbon-based material includes an external region and an internal region located inside the external region, wherein the external region refers to a region extending 0.25L from the particle surface of the first carbon-based material to the interior of the particle, L refers to the short axis length of the first carbon-based material particle, the total pore area of the external region is denoted as S1, the total pore area of the internal region is denoted as S2, and S2>S1.
[0107] When the first carbon-based material also satisfies S2>S1, the first carbon-based material further has the following characteristics: the number of pores in the internal region is large and / or the pore size is large, while the number of pores in the external region is small and / or the pore size is small. The pore structure in the internal region of the first carbon-based material can reserve the required expansion space for the volume change of the particles, thereby reducing the risk of particles breaking to produce new interfaces, reducing the rebound rate of the thickness of the negative electrode film layer, and thus reducing the occurrence of side reactions; the number of pores in the external region of the first carbon-based material is small and / or the pore size is small, thereby making the first carbon-based material particles have a stable structure and avoiding the electrolyte from penetrating into the pore structure inside the first carbon-based material particles as much as possible, thereby further reducing the occurrence of side reactions and reducing the consumption of active ions by the SEI film formation inside the particles. Therefore, when the first carbon-based material also satisfies S2>S1, it can improve the first coulombic efficiency of the secondary battery and further improve the storage performance of the secondary battery.
[0108] In some embodiments, 1.2≤S2 / S1≤500, 1.5≤S2 / S1≤500, 2≤S2 / S1≤450, 2.2≤S2 / S1≤400, 2.4≤S2 / S1≤300, 2.5≤S2 / S1≤250, 2.6≤S2 / S1≤200, 2.8≤S2 / S1≤150, and 3.0≤S2 / S1≤100. The inventors found in further research that when S2 / S1 is also within the above range, the secondary battery can better balance high energy density and good storage performance.
[0109] In the present application, the total pore area S1 of the outer region and the total pore area S2 of the inner region of the first carbon-based material can be obtained by testing a cross-sectional image of the first carbon-based material.
[0110] In the present application, the cross-sectional image of the first carbon-based material includes a cross-sectional image passing through the center of the first carbon-based material particle. "Particle center" refers to the range within a radius of 0.1 μm extending from the geometric center of the particle to the particle surface.
[0111] In this application, the minor axis length of a particle refers to the minimum value when a line connecting two points on the particle surface passes through the geometric center of the particle.
[0112] FIG1 is a schematic diagram of a cross-sectional image of a particle of the first carbon-based material 100 of the present application, and the cross-sectional image passes through the center of the particle of the first carbon-based material 100. As shown in FIG1 , L represents the length of the minor axis of the particle of the first carbon-based material 100, and the region extending from the surface of the particle of the first carbon-based material 100 to the interior of the particle by a distance of 0.25L is the outer region 101, and the region inside the outer region 101 is the inner region 102.
[0113] A cross-section polisher (e.g., IB-09010 CP argon ion cross-section polisher from JEOL, Japan) can be used to prepare the cross-section of the first carbon-based material; then, referring to JY / T010-1996, a scanning electron microscope (e.g., Sigma 300 scanning electron microscope from ZEISS, Germany) can be used to scan the cross-section of the first carbon-based material; finally, image processing software (e.g., AVIZO) can be used to calculate the total pore area S1 of the outer region and the total pore area S2 of the inner region of the first carbon-based material.
[0114] In some embodiments, the short axis length L of the first carbon-based material particle satisfies L≥4μm, optionally, 4μm≤L≤25μm, 4μm≤L≤20μm, 6μm≤L≤20μm, 8μm≤L≤20μm, 8μm≤L≤18μm, 8μm≤L≤16μm.
[0115] In some embodiments, the area of the pore structure in the outer region of the first carbon-based material is less than or equal to 0.15 μm 2 , can be selected to be less than or equal to 0.13μm 2 In further research, the inventors also found that by controlling the area of the pore structure in the outer region of the first carbon-based material within the above range, the outer region of the first carbon-based material can have a dense structure, thereby effectively improving the structural stability of the first carbon-based material and avoiding the electrolyte from penetrating into the pore structure inside the first carbon-based material particles as much as possible, thereby effectively improving the storage performance of the secondary battery. Of course, this application does not intend to limit the area of all pore structures in the outer region of the first carbon-based material to be less than or equal to 0.15 μm 2 For example, the area of the pore structure can be controlled to be less than or equal to 0.15 μm by more than 95%, or more than 99%. 2 .
[0116] In some embodiments, the inner region of the first carbon-based material includes at least one area greater than or equal to 0.15 μm 2 The pore structure may include one or more pores with an area of 0.15 μm 2 -2.0μm 2The inventors also discovered in further research that by including the aforementioned pore structure in the interior region of the first carbon-based material, sufficient and stable expansion space can be reserved for the volume changes of the first carbon-based material particles, thereby reducing the risk of first carbon-based material particle breakage and the occurrence of side reactions. Furthermore, the compaction density of the negative electrode film layer can be increased.
[0117] In some embodiments, at least a portion of the surface of the first carbon-based material has a carbon coating layer. Optionally, more than 80% of the surface of the first carbon-based material is covered with the carbon coating layer, and further, 90%-100% of the surface of the first carbon-based material is covered with the carbon coating layer.
[0118] In some embodiments, the carbon in the coating layer includes amorphous carbon and / or crystalline carbon with a graphitization degree between 68% and 90%, thereby further improving the dynamic performance of the secondary battery.
[0119] In some embodiments, the first carbon-based material may also not have a carbon coating layer. The first carbon-based material of the present application has a relatively stable surface. When the surface does not have a carbon coating layer, it is beneficial to maintain its low side reaction activity and reduce the occurrence of side reactions, thereby further improving the cycle performance and / or storage performance of the secondary battery.
[0120] In some embodiments, the first carbon-based material includes primary particles, and the amount of the primary particles in the first carbon-based material is greater than or equal to 50%, for example, 55%-95%, 60%-100%, 65%-90%, 65%-80%, 70%-100%, 75%-90%, 80%-100%, 90%-100%, or 95%-100%. When the first carbon-based material contains an appropriate proportion of primary particles, it can have higher structural stability, reduce the occurrence of side reactions, thereby improving the storage performance of the secondary battery, and further, can also increase the compaction density of the negative electrode film layer, thereby improving the energy density of the secondary battery.
[0121] In some embodiments, the first carbon-based material may be composed entirely of primary particles, that is, the primary particles in the first carbon-based material account for 100%.
[0122] In the present application, the number ratio of primary particles in the first carbon-based material refers to: randomly selecting a test sample in the negative electrode film layer, randomly selecting multiple test areas in the test sample, using a scanning electron microscope to obtain images of the multiple test areas, and counting the ratio of the number of first carbon-based materials with primary particle morphology in each image to the total number of first carbon-based material particles. The average value of multiple statistical results is the number ratio of primary particles in the first carbon-based material.
[0123] In some embodiments, the specific surface area of the first carbon-based material is ≤2.3 m 2 , optional 0.7m 2 / g-2.3m 2 / g,0.7m 2 / g-2.1m 2 / g,0.7m 2 / g-1.8m 2 / g,0.7m 2 / g-1.7m 2 / g,0.7m 2 / g-1.6m 2 / g,0.7m 2 / g-1.5m 2 / g,0.7m 2 / g-1.4m 2 / g,0.7m 2 / g-1.3m 2 / g,0.7m 2 / g-1.25m 2 The first carbon-based material has a lower specific surface area, thereby reducing the consumption of active ions in SEI film formation, reducing the occurrence of side reactions, and improving the initial coulombic efficiency and storage performance of the secondary battery.
[0124] In some embodiments, the volume distribution particle size Dv50 of the first carbon-based material is ≥6.0 μm, and can be optionally 6.0 μm-25.0 μm.
[0125] In some embodiments, the volume distribution particle size Dv90 of the first carbon-based material is ≥16.0 μm, and can be optionally 16.0 μm-40.0 μm.
[0126] When the volume distribution particle size Dv50 and / or Dv90 of the first carbon-based material is within the above range, it is beneficial to improve the transmission performance of active ions and electrons, thereby improving the kinetic performance of the secondary battery. In addition, it can also reduce the specific surface area of the first carbon-based material, reduce the occurrence of side reactions, and improve the storage performance of the secondary battery.
[0127] In some embodiments, the particle size distribution (Dv90-Dv10) / Dv50 of the first carbon-based material is ≤1.55, and can optionally be 0.9-1.55. When the particle size distribution (Dv90-Dv10) / Dv50 of the first carbon-based material is within the above range, its particle packing performance is good, which is beneficial for improving the compaction density of the negative electrode film layer and the energy density of the secondary battery. In addition, it is also beneficial for forming a reasonable pore structure between the particles of the negative electrode film layer, improving the active ion and electron transport performance, and improving the kinetic performance of the secondary battery.
[0128] In some embodiments, the tap density of the first carbon-based material is ≥0.8 g / cm 3 , optional 0.8g / cm 3 -1.20g / cm 3 When the tap density of the first carbon-based material is within the above range, it can increase the compaction density of the negative electrode film layer and improve the energy density of the secondary battery. It is also conducive to forming a reasonable pore structure between the particles of the negative electrode film layer, improving the active ion and electron transport performance, and thus improving the kinetic performance of the secondary battery.
[0129] In some embodiments, the powder compaction density of the first carbon-based material under a pressure of 5000 kg is ≤ 2.10 g / cm 3 , optional 1.85g / cm 3 -2.10g / cm 3 When the powder compaction density of the first carbon-based material is within the above range, the compaction density of the negative electrode film layer can be increased, thereby increasing the energy density of the secondary battery. This is also conducive to forming a reasonable pore structure between the particles of the negative electrode film layer, thereby improving the active ion and electron transport performance, and thus improving the kinetic performance of the secondary battery.
[0130] In some embodiments, the interlayer spacing of the 002 crystal plane of the first carbon-based material is ≤0.335916 nm, and can be 0.335576 nm-0.335916 nm. When the interlayer spacing of the first carbon-based material is within the above range, its specific capacity is higher, which is conducive to improving the energy density of the secondary battery.
[0131] In some embodiments, the gram capacity of the first carbon-based material is ≥358 mAh / g, and can be 358 mAh / g-370 mAh / g. When the gram capacity of the first carbon-based material is within the above range, the energy density of the secondary battery can be improved.
[0132] In some embodiments, the X-ray diffraction pattern of the first carbon-based material has a diffraction peak of the 3R phase 101 crystal plane.
[0133] In some embodiments, the X-ray diffraction pattern of the first carbon-based material does not have a diffraction peak of the 3R phase 012 crystal plane. In the X-ray diffraction pattern of the first carbon-based material, the 2θ of the diffraction peak of the 3R phase 101 crystal plane is in the range of 43°-44°, and the 2θ of the diffraction peak of the 3R phase 012 crystal plane is in the range of 46°-47°.
[0134] 3R (Rhombohedral) phase crystalline carbon is rhombohedral phase crystalline carbon with an ABCABC… stacking structure; 2H (Hexagonal) phase crystalline carbon is hexagonal phase crystalline carbon with an ABAB… stacking structure.
[0135] During the research process, the inventors discovered that when the first carbon-based material has a diffraction peak of the 3R phase 101 crystal plane, there may be more active sites on the surface of the first carbon-based material particles, which can accelerate the transmission of active ions; when the first carbon-based material does not have a diffraction peak of the 3R phase 012 crystal plane, its internal defects are still relatively small, which can reduce the consumption of active ions and improve the first coulombic efficiency and storage performance of the secondary battery.
[0136] In some embodiments, in a thermogravimetric analysis test of the first carbon-based material in an air atmosphere, the weight loss rate of the first carbon-based material between 35°C and 790°C is ≤50%, optionally 10%-50%, or 16%-43%. The first carbon-based material has a lower weight loss rate between 35°C and 790°C, at which time it has fewer surface defects and / or bulk defects, which can reduce the consumption of active ions in SEI film formation and reduce the consumption of active ions during storage of the secondary battery, thereby improving the storage performance of the secondary battery.
[0137] In some embodiments, in a thermogravimetric analysis test of the first carbon-based material in an air atmosphere, the temperature corresponding to the maximum weight loss rate of the first carbon-based material is recorded as T max , then T max Greater than or equal to 795°C, optionally 800°C-855°C, 805°C-850°C. The first carbon-based material has a temperature T corresponding to a high maximum weight loss rate. max At this time, it has good thermal stability and low reactivity, which can reduce the consumption of active ions in SEI film formation and reduce the consumption of active ions in the storage process of secondary batteries, thereby improving the storage performance of secondary batteries.
[0138] The thermogravimetric analysis (TG) test of the first carbon-based material can be carried out with reference to JY / T 014-1996. The present application can also be carried out under the following conditions: the sample weighing mass is 10±0.05 mg, the purge gas is air and the air flow rate is 60 mL / min, the heating rate is 5°C / min, and the test temperature range is 35°C-950°C. The test instrument can be the NETZSCH STA 449F3 synchronous thermal analyzer of the German NETZSCH Instrument Company. The temperature T corresponding to the maximum weight loss rate of the first carbon-based material is max is the peak temperature of the thermogravimetric differential curve of the first carbon-based material.
[0139] In some embodiments, the mass proportion of the first carbon-based material in the negative electrode active material is ≥30wt%, and can be 30wt%-80wt%. When the content of the first carbon-based material is within the above range, the energy density of the secondary battery can be increased, and the secondary battery can also have good dynamic performance.
[0140] In some embodiments, the volume distribution particle size Dv50 of the negative electrode active material is ≥6 μm, and can be optionally 6 μm-23 μm. The volume distribution particle size, particle size distribution, mass content and other parameters of the first carbon-based material and / or the second carbon-based material can be adjusted so that the volume distribution particle size of the negative electrode active material is within the above range. When the volume distribution particle size Dv50 of the negative electrode active material is within the above range, it is beneficial to improve the transport performance of active ions and electrons, thereby further improving the kinetic performance of the secondary battery. In addition, it can also reduce the occurrence of side reactions and improve the storage performance of the secondary battery.
[0141] In some embodiments, the particle size distribution (Dv90-Dv10) / Dv50 of the negative electrode active material is ≥0.9, and can be optionally 0.9-1.55. The volume distribution particle size, particle size distribution, mass content and other parameters of the first carbon-based material and / or the second carbon-based material can be adjusted to make the particle size distribution of the negative electrode active material within the above range. When the particle size distribution (Dv90-Dv10) / Dv50 of the negative electrode active material is within the above range, its particle stacking performance is better, which is beneficial to improve the compaction density of the negative electrode film layer, thereby further improving the energy density of the secondary battery; in addition, it is also beneficial to form a reasonable pore structure between the particles of the negative electrode film layer, thereby improving the dynamic performance of the secondary battery.
[0142] In some embodiments, the degree of graphitization of the negative electrode active material is ≥92%, optionally 92%-96%. The degree of graphitization, mass content, and other parameters of the first carbon-based material and / or the second carbon-based material can be adjusted to ensure that the degree of graphitization of the negative electrode active material is within the above range. By adjusting the degree of graphitization of the negative electrode active material within the above range, the negative electrode active material is advantageously provided with high gram capacity and good active ion transport performance, thereby facilitating the secondary battery to achieve both high energy density and good kinetic performance.
[0143] In some embodiments, the gram capacity of the negative electrode active material is ≥350 mAh / g, and can be optionally 350 mAh / g-365 mAh / g. The gram capacity, mass content, and other parameters of the first carbon-based material and / or the second carbon-based material can be adjusted to keep the gram capacity of the negative electrode active material within the above range. By adjusting the gram capacity of the negative electrode active material within the above range, the energy density of the secondary battery can be improved.
[0144] In some embodiments, the negative electrode film layer may further include other negative electrode active materials known in the art in addition to the first carbon-based material and the second silicon-based material described above. For example, the negative electrode film layer may also include a silicon-based material. The silicon-based material can improve the pore structure in the negative electrode film layer, facilitate electrolyte infiltration and retention, and enhance the dynamic performance of the secondary battery. It can also increase the negative electrode capacity, thereby further improving the energy density of the secondary battery. Optionally, the silicon-based material may include one or more of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite, and silicon alloy.
[0145] In some embodiments, when the negative electrode film layer further includes a silicon-based material, the mass proportion of the silicon-based material in the negative electrode film layer is less than or equal to 20%, for example, 1%-20%, 1%-15%, 1%-10%, 1.5%-8%, 2%-6%, or 3%-7%. This can improve the kinetic performance and energy density of the secondary battery while ensuring good cycling performance and storage performance.
[0146] In some embodiments, the negative electrode film layer may further optionally include a negative electrode conductive agent. The present application does not particularly limit the type of the negative electrode conductive agent. As examples, the negative electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0147] In some embodiments, the negative electrode film layer may further optionally include a negative electrode binder. The present application does not particularly limit the type of the negative electrode binder. As examples, the negative electrode binder may include one or more of styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS).
[0148] In some embodiments, the negative electrode film layer may further include other additives. For example, the other additives may include a thickener, such as sodium carboxymethyl cellulose (CMC), a PTC thermistor material, and the like.
[0149] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).
[0150] The negative electrode film layer is typically formed by coating a negative electrode slurry onto a negative electrode current collector, followed by drying and cold pressing. The negative electrode slurry is typically formed by dispersing the negative electrode active material, an optional conductive agent, an optional binder, and other optional additives in a solvent and stirring until uniformly mixed. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP) or deionized water.
[0151] The negative electrode plate does not exclude other additional functional layers in addition to the negative electrode film layer. For example, in some embodiments, the negative electrode plate described in the present application further includes a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode film layer and disposed on the surface of the negative electrode current collector; in some embodiments, the negative electrode plate described in the present application further includes a protective layer covering the surface of the negative electrode film layer.
[0152] In some embodiments, the porosity of the negative electrode film is ≥15.5%, and can be 15.5%-38%. This helps the negative electrode film to achieve both high capacity and suitable pore structure, and thus helps the secondary battery to achieve both high energy density and good storage performance and dynamic performance.
[0153] In some embodiments, the compaction density of the negative electrode film layer is ≥1.40 g / cm 3 , optional 1.40g / cm 3 -1.80g / cm 3 This is beneficial for the negative electrode film layer to have both high capacity and high active ion and electron transport performance, and further beneficial for the secondary battery to have both high energy density and good storage performance and kinetic performance.
[0154] In some embodiments, the surface density of the negative electrode film layer is ≥5.5 g / cm 2 , optional 6.0g / cm 3 -19.5g / cm 2 This is beneficial for the negative electrode film layer to have both high capacity and high active ion and electron transport performance, and further beneficial for the secondary battery to have both high energy density and good storage performance and kinetic performance.
[0155] In some embodiments, the OI value of the negative electrode film is ≤38, and can be 8-38. This helps improve the active ion embedding performance of the negative electrode film and also enables the negative electrode film to have a lower thickness rebound rate, thereby facilitating the secondary battery to have both good storage performance and dynamic performance.
[0156] The negative electrode current collector has two surfaces that face each other in the thickness direction, and the negative electrode film is disposed on either or both of the two opposing surfaces of the negative electrode current collector. It should be noted that the negative electrode film parameters (e.g., compacted density, surface density, porosity, OI value, etc.) given in this application refer to the parameters of the negative electrode film on a single side of the negative electrode current collector. When the negative electrode film is disposed on both sides of the negative electrode current collector, the parameters of the negative electrode film on either side satisfy the requirements of this application and are considered to fall within the scope of protection of this application.
[0157] In this application, the specific surface area of a material (e.g., a first carbon-based material, a second carbon-based material, etc.) is a well-known meaning in the art and can be measured using instruments and methods known in the art. For example, it can be measured using the nitrogen adsorption specific surface area analysis test method according to GB / T 19587-2017 and calculated using the BET (Brunauer Emmett Teller) method. The test instrument can be a Tri-Star 3020 specific surface area pore size analyzer from Micromeritics, USA.
[0158] In the present application, whether there is a coating layer on the surface of a material (eg, the first carbon-based material, the second carbon-based material, etc.) can be determined by transmission electron microscopy.
[0159] In this application, the interlayer spacing of the 002 crystal plane of a material (e.g., the first carbon-based material and the second carbon-based material) has a meaning well known in the art and can be measured using instruments and methods known in the art. For example, an X-ray diffractometer (e.g., a Bruker D8 Discover) can be used for testing. The test can refer to JIS K 0131-1996 and JB / T 4220-2011 to obtain the interlayer spacing of the C(002) crystal plane in the material's crystal structure.
[0160] In this application, the graphitization degree of the negative electrode active material is a well-known meaning in the art and can be tested using instruments and methods known in the art. For example, an X-ray diffractometer (such as Bruker D8 Discover) can be used for testing. The test can refer to JIS K 0131-1996 and JB / T 4220-2011 to obtain the average interlayer spacing d of the C(002) crystal plane in the material crystal structure. 002 Then according to the formula g=(0.344-d 002) / (0.344-0.3354)×100% to calculate the degree of graphitization. In the above formula, d 002 It is the average interlayer spacing of the C(002) planes in the material's crystal structure expressed in nanometers (nm).
[0161] In this application, the volume distribution particle size Dv10, Dv50, and Dv90 of the material (e.g., the first carbon-based material, the second carbon-based material, the negative electrode active material, etc.) are well-known in the art, and respectively represent the particle size corresponding to when the cumulative volume distribution percentage of the material reaches 10%, 50%, and 90%, and can be measured using instruments and methods known in the art. For example, it can be measured using a laser particle size analyzer with reference to GB / T 19077-2016. The test instrument can be a Mastersizer 3000 laser particle size analyzer from Malvern Instruments Ltd., UK.
[0162] In this application, the powder compaction density of a material (e.g., the first carbon-based material, the second carbon-based material, etc.) is a well-known meaning in the art and can be measured using instruments and methods known in the art. For example, it can be measured using an electronic pressure testing machine (e.g., a UTM7305 electronic pressure testing machine) with reference to GB / T 24533-2009. An exemplary test method is as follows: 1 g of sample powder is weighed and added to a container with a bottom area of 1.327 cm 2 In the mold, pressurize to 5000kg, maintain pressure for 30s, then release the pressure, maintain for 10s, and then record and calculate the powder compaction density of the material under 5000kg pressure.
[0163] In this application, the tap density of a material (e.g., a first carbon-based material, a second carbon-based material, etc.) is a well-known meaning in the art and can be measured using instruments and methods known in the art. For example, it can be measured using a powder tap density tester with reference to GB / T 5162-2006. The test instrument can be Dandong Baxter BT-301, and the test parameters are as follows: vibration frequency 250 ± 15 times / min, amplitude 3 ± 0.2 mm, vibration number 5000 times, and graduated cylinder 25 mL.
[0164] In this application, the I of the material (eg, the first carbon-based material, the second carbon-based material, etc.) D / I G Raman spectrometer can be used for testing. D The Raman spectrum of the material is 1350±50cm -1 The D peak intensity at I G The Raman spectrum of the material is 1580±50cm -1The test conditions are: excitation wavelength 532nm, grating 600 lines, objective lens 50 times, integration time 10s, accumulation times 3 times, surface scanning, obtain the D peak and G peak intensity of 100 points, calculate the I of 100 points D / I G , remove the largest and smallest 30 I D / I G The average value of the remaining 40 points is the I D / I G The testing instrument may be a Horiba LabRAM HR800 Raman spectrometer.
[0165] In this application, primary particles and secondary particles have meanings well known in the art. Primary particles refer to non-agglomerated particles. Secondary particles refer to agglomerated particles formed by the aggregation of two or more primary particles. Primary particles and secondary particles can be distinguished using scanning electron microscopy (SEM) images.
[0166] In this application, the gram capacity of materials (such as the first carbon-based material, the second carbon-based material, the negative electrode active material, etc.) has a meaning well known in the art and can be tested using methods known in the art. An exemplary test method is as follows: the sample powder is mixed evenly with the conductive agent carbon black (Super P), the binder polyvinylidene fluoride (PVDF) in a mass ratio of 91.6:1.8:6.6 and the solvent N-methylpyrrolidone (NMP) to form a slurry; the prepared slurry is applied on the surface of the negative electrode current collector copper foil, dried in an oven and set aside; ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then LiPF6 is dissolved in the above organic solvent to a concentration of 1 mol / L The electrolyte was then added to a lithium metal sheet as the counter electrode and a polyethylene (PE) film as the separator. The cells were assembled into CR2430 button cells in an argon-protected glove box with the electrolyte. The resulting button cells were left to rest for 12 hours and then discharged at 0.05C to 0.005V at 25°C. The cells were then left to rest for 10 minutes and then discharged again at 50μA to 0.005V. The cells were left to rest for 10 minutes and then discharged again at 10μA to 0.005V. The cells were then charged at 0.1C to 2V, and the charge capacity was recorded. The ratio of the charge capacity to the sample mass is the gram capacity of the corresponding material (e.g., the first carbon-based material, the second carbon-based material, the negative electrode active material, etc.).
[0167] In this application, the areal density of the negative electrode film layer has a meaning well known in the art and can be tested using methods known in the art. For example, a negative electrode sheet coated on one side and cold pressed can be taken (if it is a double-sided coated negative electrode sheet, the negative electrode film layer on one side can be wiped off first), punched into small discs with an area of S1, weighed, and recorded as M1. Then, the negative electrode film layer of the weighed negative electrode sheet is wiped off, and the weight of the negative electrode current collector is weighed and recorded as M0. The areal density of the negative electrode sheet = (M1-M0) / S1.
[0168] In this application, the compacted density of the negative electrode film layer is well known in the art and can be measured using methods known in the art. The compacted density of the negative electrode film layer = the surface density of the negative electrode film layer / the thickness of the negative electrode film layer. The thickness of the negative electrode film layer is well known in the art and can be measured using methods known in the art, such as using a micrometer (e.g., Mitutoyo 293-100, with an accuracy of 0.1 μm).
[0169] In the present application, the porosity of the negative electrode film layer has a well-known meaning in the art and can be measured using methods known in the art. An exemplary test method is as follows: take a negative electrode sheet that has been coated on one side and cold-pressed (if it is a negative electrode sheet coated on both sides, the negative electrode film layer on one side can be wiped off first), punch it into small disc samples of a certain area, and calculate the apparent volume V1 of the negative electrode sheet; refer to GB / T24586-2009, use an inert gas (such as helium or nitrogen) as a medium, adopt a gas replacement method, and use a true density tester to measure the true volume V2 of the negative electrode sheet. The porosity of the negative electrode film layer = (V1-V2) / V1×100%. Multiple negative electrode sheet samples with good appearance and no powder falling on the edges (such as 30 pieces) can be taken for testing, and the results are averaged, thereby improving the accuracy of the test results. The testing instrument can be a Micromeritics AccuPyc II 1340 true density tester.
[0170] In this application, the OI value of the negative electrode film layer has a well-known meaning in the art and can be tested using instruments and methods known in the art. For example, an X-ray diffractometer (such as Bruker D8 Discover) can be used for testing. The test can refer to JIS K 0131-1996 and JB / T 4220-2011 to obtain an X-ray diffraction pattern of the negative electrode sheet. According to OI value = I 004 / I 110 The OI value of the negative electrode film layer is calculated. 004 is the integrated area of the diffraction peak of the 004 crystal plane of crystalline carbon in the negative electrode film layer, I 110 It is the integrated area of the diffraction peak of the 110 crystal plane of crystalline carbon in the negative electrode film layer.
[0171] In the X-ray diffraction analysis test of this application, a copper target can be used as the anode target, and CuKα rays can be used as the radiation source. The ray wavelength is The scanning 2θ angle range was 20°-80°, and the scanning rate was 4° / min.
[0172] It should be noted that the various parameter tests on the negative electrode active material or the negative electrode film layer can be performed by sampling and testing the prepared secondary battery according to the following steps.
[0173] Discharge the secondary battery (for safety reasons, the secondary battery is generally fully discharged). Disassemble the secondary battery, remove the negative electrode, and soak the negative electrode in dimethyl carbonate for a certain period of time (e.g., 2-10 hours). Then remove the negative electrode and dry it at a certain temperature and time (e.g., 60°C for more than 4 hours). After drying, remove the negative electrode. Samples can now be taken from the dried negative electrode to test the aforementioned parameters related to the negative electrode film, such as the surface density, compacted density, porosity, and OI value of the negative electrode film.
[0174] The dried negative electrode sheet is baked at a certain temperature and time (for example, 400°C for more than 2 hours), and a sample of the negative electrode active material is taken from any area of the baked negative electrode sheet (a blade can be used for scraping powder sampling); the collected negative electrode active material is sieved (for example, sieved with a 200-mesh sieve) to finally obtain a sample that can be used to test the parameters of the above-mentioned negative electrode active materials.
[0175] In the present application, the first active material and the second active material mentioned above can be obtained commercially, or can also be prepared by the following method of the present application.
[0176] In some embodiments, the preparation method of the first carbon-based material includes: step 1, providing a raw material having a plurality of pore structures; step 2, uniformly mixing the raw material and the filler material in a predetermined proportion, then keeping the mixture at a first temperature T1 for a first time t1, and cooling to room temperature to obtain an intermediate; step 3, keeping the obtained intermediate at a second temperature T2 for a second time t2, and obtaining the first carbon-based material.
[0177] In some embodiments, in step 1, the raw material for preparing the first carbon-based material includes natural graphite. Alternatively, the natural graphite includes one or more of flake graphite, natural spherical graphite, and microcrystalline graphite, and more preferably includes natural spherical graphite.
[0178] "Natural spherical graphite" refers to natural graphite with a spherical or quasi-spherical shape, and not all natural graphite particles are controlled to be ideal spheres. In some embodiments, natural spherical graphite with a desired particle size and morphology can be obtained by pre-treating flake graphite. Optionally, the pre-treatment includes crushing, classification, spheroidization, purification, and other processes.
[0179] In some embodiments, in step 1, the volume distribution particle size Dv50 of the raw material may be 6.0 μm-25.0 μm.
[0180] In some embodiments, in step 1, the specific surface area of the raw material may be ≥2.5m 2 / g, optional 2.5m 2 / g-10.0m 2 When the specific surface area of the raw material is within the above range, it is beneficial to carry out subsequent filling processing and obtain the first carbon-based material with the required specific surface area. It is also beneficial for the first carbon-based material to have both high capacity and high first coulombic efficiency. In addition, it is also beneficial for the first carbon-based material to have better kinetic properties.
[0181] In some embodiments, in step 2, the softening point temperature of the filling material is 90° C.-150° C. Optionally, the softening point temperature of the filling material is 94° C.-146° C., 94° C.-142° C., 94° C.-138° C., 94° C.-134° C., 94° C.-130° C., 104° C.-146° C., 104° C.-142° C., 104° C.-138° C., 104° C.-134° C., 104° C.-130° C.
[0182] In some embodiments, in step 2, the volume distribution particle size Dv50 of the filler material is less than or equal to 6 μm, and can be selected from 1 μm-6 μm, 1 μm-5 μm, 2 μm-5 μm, and 3 μm-5 μm. This facilitates the filler material to be melted by heat and filled into the pore structure of the raw material, and also helps to improve the dispersion uniformity of the filler material and the raw material.
[0183] In some embodiments, in step 2, the coking value of the filler material is 15%-40%, and optionally 18%-34%. In this application, the coking value of the filler material is well known in the art and can be measured using instruments and methods known in the art. For example, it can be measured in accordance with GB / T 8727-2008.
[0184] In some embodiments, in step 2, the filling material includes one or more of coal tar, petroleum asphalt, polymer compounds and resins, and may optionally include one or more of coal tar and petroleum asphalt.
[0185] In some embodiments, in step 2, the mass ratio of the filling material to the raw material is (10-40):100, and can be optionally (10-32):100, (10-30):100, (10-25):100, (10-20):100, (12-30):100, (14-28):100, (15-25):100.
[0186] In step 2, by adjusting one or more parameters such as the type, softening point, coking value, and addition amount of the filling material within the above-mentioned range, it is beneficial to adjust the number of pores and / or pore size in the outer and inner areas of the first carbon-based material within a suitable range, which is beneficial to adjust the S2 / S1 of the first carbon-based material within a suitable range.
[0187] By adjusting the type, softening point, coking value, addition amount and other parameters of the filling material within the above range, the viscosity of the filling material is not high after being heated and melted, and it maintains good fluidity. At the same time, it is not easy to adhere to the raw material particles, which can reduce the agglomeration of the raw material particles in the subsequent preparation process. This can also reduce the problems of increased surface defects of the first carbon-based material particles and increased surface active sites due to the need to add a depolymerization process.
[0188] In some embodiments, in step 2, the heating process of uniformly mixing the raw material and the filling material in a predetermined ratio and then heating the mixture to the first temperature T1 may be a staged heating process.
[0189] In some embodiments, the staged temperature increasing process includes a first temperature increasing process, a second temperature increasing process, and a third temperature increasing process.
[0190] In some embodiments, the first temperature raising process is to raise the temperature to 200° C.-250° C. and keep the temperature at this temperature for 0.5 h-3 h.
[0191] In some embodiments, the second temperature raising process is to raise the temperature to 450°C-550°C and keep the temperature at this temperature for 0-2 hours. When the holding time is 0 hours, it means that when the temperature is raised to the range of 450°C-550°C, no holding treatment is performed, but the temperature is continued to rise to the first temperature T1.
[0192] In some embodiments, the third temperature raising process is to raise the temperature to the first temperature T1 and keep the temperature at the first time t1.
[0193] In the staged heating process, the temperature is first raised to 200℃-250℃. Since the heating temperature is higher than the softening point of the filling material, the filling material is melted and softened by the heat. Keeping it warm for 0.5h-3h allows it to flow and fill into the pore structure of the raw material; then the temperature is raised to 450℃-550℃. At this time, the melted and softened filling material undergoes a carbonization reaction, gradually forming a semi-coke state and turning into a viscous liquid or solid, thereby preventing the filling material from entering the entire pore structure of the raw material; finally, the temperature is raised to the first temperature. At this time, the filling material undergoes a carbonization reaction, thereby enabling the pore structure occupied by the filling material to be effectively filled.
[0194] In some embodiments, in step 2, the temperature is raised to the first temperature T1 at a rate of 1°C / min-10°C / min. For example, the heating rate can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min or any range thereof. Alternatively, the heating rate is 1.5°C / min-8°C / min, 1.5°C / min-6°C / min, 2°C / min-6°C / min, 2°C / min-5°C / min
[0195] In some embodiments, the heating rate of the first heating process may be 1°C / min-10°C / min, optionally 1.5°C / min-8°C / min, 1.5°C / min-6°C / min, 2°C / min-6°C / min, or 2°C / min-5°C / min.
[0196] In some embodiments, the heating rate of the second heating process may be 1° C. / min-10° C. / min, and may be optionally 2° C. / min-8° C. / min.
[0197] In some embodiments, the heating rate of the third heating process may be 1° C. / min-10° C. / min, and may be optionally 2° C. / min-8° C. / min.
[0198] In some embodiments, in step 2, the first temperature T1 is 700° C.-1200° C. For example, the first temperature T1 can be 700° C., 750° C., 800° C., 850° C., 900° C., 950° C., 1000° C., 1050° C., 1100° C., 1200° C., or any range thereof. Alternatively, the first temperature T1 is 750° C.-1100° C., 800° C.-1100° C., 850° C.-1100° C., 900° C.-1100° C., or 850° C.-1000° C.
[0199] In some embodiments, in step 2, the first time t1 is 1 hour to 5 hours. For example, the first time t1 can be 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, or any range thereof. Optionally, the first time t1 is 2 hours to 4 hours.
[0200] In some embodiments, in step 2, the heat treatment can be carried out in a device capable of programmed temperature increase, such as a medium frequency furnace, a roller kiln, a rotary kiln, a push plate kiln, a vertical granulation kettle, a horizontal granulation kettle, a vertical reactor, a horizontal reactor or a drum furnace.
[0201] In some embodiments, in step 2, the heat treatment atmosphere may be a protective gas atmosphere, which may include one or more of nitrogen, argon, and helium.
[0202] In step 2, by adjusting one or more of the heating rate, the first temperature, the first time, the heating process, etc. within the above-mentioned range, it is beneficial to adjust the number of pores and / or the pore size in the outer area and the inner area of the first carbon-based material within a suitable range, and thus it is beneficial to adjust the S2 / S1 of the first carbon-based material within a suitable range.
[0203] In some embodiments, in step 3, the second temperature T2 is 2070° C.-2700° C. Optionally, the second temperature T2 is 2070° C.-2570° C., 2070° C.-2510° C., 2070° C.-2450° C., 2070° C.-2360° C., 2140° C.-2570° C., 2140° C.-2510° C., 2140° C.-2450° C., 2140° C.-2360° C.
[0204] In some embodiments, in step 3, the second time t2 is 1.5 hours to 6 hours. For example, the second time t1 can be 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, 5.5 hours, 6 hours, or any range thereof. Optionally, the second time t2 is 2 hours to 5 hours.
[0205] In some embodiments, in step 3, the heat treatment may be performed in a medium frequency furnace, a box-type graphitization furnace, an Acheson graphitization furnace, a continuous graphitization furnace, or an inner-string graphitization furnace.
[0206] In some embodiments, in step 3, the medium frequency furnace and the continuous graphitization heat treatment atmosphere may be a protective gas atmosphere. The protective gas may include one or more of nitrogen, argon, and helium.
[0207] In step 3, by adjusting one or more of the second temperature and the second time within the above range, it is beneficial to adjust the content of disordered carbon in the first carbon-based material to be within a suitable range, which is beneficial for the first carbon-based material to have a suitable graphitization degree, interlayer spacing and I D / I G wait.
[0208] In the preparation method of the first carbon-based material, by adjusting one or more of the parameters of natural graphite, the parameters of the filler material, the heating rate, the first temperature, the first time, the heating process, the second temperature, the second time, etc. within the above range, it is beneficial to adjust the S2 / S1, I D / I G , graphitization degree, gram capacity, specific surface area, particle size, powder compaction density, tap density, weight loss rate and other parameters.
[0209] In some embodiments, the second carbon-based material is prepared by mixing a raw material with an organic carbon source and then carbonizing the mixture to form a carbon coating on at least a portion of the surface of the particles, thereby obtaining the second carbon-based material. The raw material comprises at least one of artificial graphite and natural graphite, and may optionally comprise artificial graphite.
[0210] In some embodiments, the organic carbon source may be a carbon-containing material known in the art that is suitable for coating, for example, it may include one or more of coal tar, petroleum asphalt, phenolic resin, coconut shell, etc.
[0211] In some embodiments, the carbonization temperature is 900°C-1300°C.
[0212] In the preparation method of the second carbon-based material, by adjusting one or more parameters of the raw material parameters (such as particle size, specific surface area, particle size distribution, gram capacity, etc.), the amount of organic carbon source added, the carbonization temperature, the carbonization time, etc., it is beneficial to adjust the I of the second carbon-based material. D / I G , graphitization degree, interlayer spacing, gram capacity, particle size, specific surface area, powder compaction density, tap density and other parameters.
[0213] [Positive electrode]
[0214] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector. For example, the positive electrode current collector has two surfaces that are opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposing surfaces of the positive electrode current collector.
[0215] The positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).
[0216] The positive electrode film layer generally comprises a positive electrode active material, an optional binder and an optional conductive agent. The positive electrode film layer is generally formed by coating a positive electrode slurry on the positive electrode current collector, drying and cold pressing. The positive electrode slurry is generally formed by dispersing a positive electrode active material, an optional conductive agent, an optional binder and any other components in a solvent and stirring evenly. The solvent may be N-methylpyrrolidone (NMP), but is not limited thereto. As an example, the binder for the positive electrode film layer may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin. As an example, the conductive agent for the positive electrode film layer includes one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0217] The positive electrode active material may be a positive electrode active material for a secondary battery known in the art.
[0218] When the secondary battery of the present application is a lithium-ion battery, the positive electrode active material may include, but is not limited to, one or more of lithium-containing transition metal oxides, lithium-containing phosphates, and their respective modified compounds. Examples of the lithium transition metal oxide may include, but are not limited to, one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. Examples of the lithium-containing phosphate may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and their respective modified compounds.
[0219] In some embodiments, in order to further improve the energy density of the secondary battery, the positive electrode active material for the lithium ion battery may include a general formula of Li a Ni b Coc M d O e A f One or more of lithium transition metal oxides and their modified compounds thereof. 0.8 ≤ a ≤ 1.2, 0.5 ≤ b < 1, 0 < c < 1, 0 < d < 1, 1 ≤ e ≤ 2, 0 ≤ f ≤ 1, M is selected from one or more of Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, and B, and A is selected from one or more of N, F, S, and Cl.
[0220] In some embodiments, by way of example, the positive electrode active material for a lithium-ion battery may include one or more of LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523), LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811), LiNi 0.85 Co 0.15 Al 0.05 O2, LiFePO4, and LiMnPO4.
[0221] In the present application, the modified compounds of the above positive electrode active materials may be doping modification and / or surface coating modification of the positive electrode active materials.
[0222] [Electrolyte]
[0223] In some embodiments, the electrolyte uses an electrolytic solution, and the electrolytic solution includes an electrolyte salt and a solvent.
[0224] The type of the electrolyte salt is not specifically limited and can be selected according to actual needs.
[0225] When the secondary battery of the present application is a lithium ion battery, as an example, the electrolyte salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobisoxalatophosphate (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).
[0226] The type of the solvent is not specifically limited and can be selected according to actual needs. In some embodiments, for example, the solvent may include ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE). One or more.
[0227] In some embodiments, the electrolyte may further optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, or additives capable of improving certain properties of the secondary battery, such as additives that improve the overcharge performance of the secondary battery, additives that improve the high-temperature performance of the secondary battery, and additives that improve the low-temperature power performance of the secondary battery.
[0228] [Isolation film]
[0229] The present application has no particular limitation on the type of the isolation membrane, and any known porous isolation membrane with good chemical stability and mechanical stability can be selected.
[0230] In some embodiments, the material of the isolation membrane may include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The isolation membrane may be a single-layer film or a multi-layer composite film. When the isolation membrane is a multi-layer composite film, the materials of each layer may be the same or different.
[0231] In some embodiments, the positive electrode sheet, the separator, and the negative electrode sheet can be formed into an electrode assembly through a winding process or a lamination process.
[0232] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0233] In some embodiments, the outer packaging can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0234] The present application has no particular limitation on the shape of the secondary battery, which can be cylindrical, square, or any other shape. FIG2 shows a secondary battery 5 with a square structure as an example.
[0235] In some embodiments, as shown in FIG3 , the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 is used to cover the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation film can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is impregnated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, which can be adjusted according to demand.
[0236] The preparation method of the secondary battery of the present application is well known. In some embodiments, a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte can be assembled to form a secondary battery. As an example, the positive electrode sheet, separator, and negative electrode sheet can be formed into an electrode assembly through a winding process or a lamination process. The electrode assembly is placed in an outer packaging, dried, and then injected with electrolyte. The secondary battery is then vacuum packaged, allowed to stand, formed, and shaped.
[0237] In some embodiments of the present application, the secondary batteries according to the present application can be assembled into a battery module. The battery module can contain multiple secondary batteries, and the specific number can be adjusted according to the application and capacity of the battery module.
[0238] Figure 4 is a schematic diagram of an exemplary battery module 4. As shown in Figure 4 , within the battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured using fasteners.
[0239] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.
[0240] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0241] Figures 5 and 6 are schematic diagrams of an exemplary battery pack 1. As shown in Figures 5 and 6, the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 covers the lower case 3 and forms an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 may be arranged in any manner within the battery box.
[0242] The present application also provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack of the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device can be, but is not limited to, a mobile device (such as a mobile phone, a tablet computer, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship, a satellite, an energy storage system, etc.
[0243] The electrical device may select a secondary battery, a battery module or a battery pack according to its usage requirements.
[0244] Figure 7 is a schematic diagram of an exemplary electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of this device, a battery pack or battery module may be used.
[0245] As another example, the electric device may be a mobile phone, a tablet computer, a laptop computer, etc. Such an electric device is usually required to be lightweight and thin, and may use a secondary battery as a power source.
[0246] Example
[0247] The following examples describe the present disclosure in more detail. These examples are intended to be illustrative only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing. The instruments used in the examples are commercially available.
[0248] In the following examples and comparative examples, the first carbon-based material can be prepared by the following method of the present application.
[0249] In the following embodiments and comparative examples, except for comparative example 3 in which the second carbon-based material is artificial graphite without a coating layer, the other second carbon-based materials are all artificial graphite with a carbon coating layer, and all of them can be purchased commercially.
[0250] The flake graphite is mechanically crushed, classified, spheroidized and purified to obtain natural spherical graphite. The obtained natural spherical graphite is mixed with petroleum asphalt, and the mixed material is placed in a programmable temperature raising device for staged temperature raising heat treatment, and then cooled to room temperature to obtain an intermediate. The obtained intermediate is placed in a graphitization furnace for heat treatment, and then demagnetized and sieved to obtain the first carbon-based material. In the above process, the preparation process of the first carbon-based material given above in this application can be used for regulation and control, so that the parameters such as S2 / S1, interlayer spacing, volume distribution particle size Dv50 of the first carbon-based material are within the range shown in Table 1.
[0251] The S2 / S1 ratio of the first carbon-based material was measured using the following method. A sample preparation binder was mixed evenly with the first carbon-based material powder, then coated onto copper foil and dried at 60°C for 30 minutes. The sample was cut into 6 mm x 6 mm pieces and attached to the sample stage of a CP-type argon ion cross-section polisher. A plasma beam was used to cut the sample, obtaining a cross section of the first carbon-based material, with the cross section passing through the center of the first carbon-based material particle. The testing instrument can be an IB-09010 CP-type argon ion cross-section polisher from JEOL, Japan. The cross section of the first carbon-based material was scanned using a scanning electron microscope. The test method can refer to JY / T010-1996. The testing instrument can be a Sigma 300 scanning electron microscope from ZEISS, Germany. The area extending 0.25 L from the surface of the first carbon-based material particle to the interior of the particle is designated as the outer region, and the area inside the outer region is designated as the inner region. L represents the minor axis length of the first carbon-based material particle. The total pore area S1 of the outer region of the first carbon-based material and the total pore area S2 of the inner region of the first carbon-based material are calculated using image processing software, which may be AVIZO.
[0252] The secondary batteries of Examples 1-29 and Comparative Examples 1-3 were all prepared according to the following method.
[0253] The negative electrode active material (a mixture of the first and second carbon-based materials, see Table 1 for details), conductive carbon black (Super P), thickener sodium carboxymethyl cellulose, and binder styrene-butadiene rubber were thoroughly stirred and mixed in an appropriate amount of deionized water at a weight ratio of 96.4:1:1.2:1.4 to form a negative electrode slurry. The negative electrode slurry was coated on both surfaces of the negative electrode current collector copper foil, dried, and cold pressed to obtain a negative electrode sheet.
[0254] LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523) is mixed with carbon black (Super P), a conductive agent, and polyvinylidene fluoride (PVDF) as a binder in a weight ratio of 96:2:2. An appropriate amount of NMP solvent is added and stirred evenly to obtain a positive electrode slurry. The positive electrode slurry is then coated on both surfaces of the positive electrode current collector aluminum foil. After drying and cold pressing, a positive electrode sheet is obtained.
[0255] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then LiPF6 is dissolved in the above organic solvent to prepare an electrolyte with a concentration of 1 mol / L.
[0256] A polyethylene film is used as an isolation film and is placed in order with the positive electrode sheet and the negative electrode sheet prepared above, so that the isolation film is located between the positive electrode sheet and the negative electrode sheet to play an isolation role. The electrode assembly is then wound to obtain an electrode assembly; the electrode assembly is placed in an outer package, dried, and then injected with electrolyte. After vacuum packaging, standing, formation, shaping and other processes, a secondary battery is obtained.
[0257] Performance Testing
[0258] (1) Fast charging performance test of secondary batteries
[0259] At 25°C, the secondary battery was charged to 4.3V at a constant current of 0.33C, then charged to a current of 0.05C at a constant voltage. After standing for 5 minutes, the secondary battery was discharged to 2.8V at a constant current of 0.33C, and its actual capacity was recorded as C0.
[0260] Then the secondary battery is charged with constant current at 1.0C0, 1.3C0, 1.5C0, 1.8C0, 2.0C0, 2.3C0, 2.5C0, 3.0C0 in sequence to a negative electrode cutoff potential of 4.3V or 0V (whichever is reached first). After each charge, it is discharged to 2.8V at 1C0. The SOC (State of Charge) at different charge rates is recorded. The charge rate-negative electrode potential curve under different SOC states was drawn, and the charge rate corresponding to the negative electrode potential of 0 V under different SOC states was obtained after linear fitting. The charge rate is the charging window under the SOC state, which is recorded as C10% SOC, C20% SOC, C30% SOC, C40% SOC, C50% SOC, C60% SOC, C70% SOC, and C80% SOC, respectively. The charging time T of the secondary battery from 10% SOC to 80% SOC (assuming that the secondary battery does not undergo lithium deposition) is calculated according to the formula (60 / C20% SOC + 60 / C30% SOC + 60 / C40% SOC + 60 / C50% SOC + 60 / C60% SOC + 60 / C70% SOC + 60 / C80% SOC) × 10%, and the unit is min. The shorter the charging time, the better the dynamic performance of the secondary battery.
[0261] (2) Storage performance test of secondary batteries
[0262] At 25°C, the prepared secondary battery was charged at a constant current of 1C to 4.3V, then charged at a constant voltage to a current of 0.05C. After standing for 5 minutes, the secondary battery was discharged at a constant current of 1C to 2.8V. The discharge capacity at this time was recorded, which was the discharge capacity before storage.
[0263] At 25°C, the prepared secondary battery was charged at a constant current of 1C to 4.3V, and then charged at a constant voltage to a current of 0.05C. The secondary battery was then stored in a thermostat at 60°C for 180 days. Capacity retention (%) of the secondary battery after 180 days of storage at 60°C = discharge capacity after storage / discharge capacity before storage × 100%.
[0264] As can be seen from Table 1, by making the negative electrode active material in the negative electrode film layer include a first carbon-based material having a pore structure and a second carbon-based material having a carbon coating layer on at least a portion of its surface, the secondary battery can have both good kinetic performance and storage performance while having a high energy density.
[0265] Based on the test results of Example 1, Comparative Example 1 and Comparative Example 2, it can be seen that the first carbon-based material and the second carbon-based material can produce a synergistic effect, so that the battery has a longer storage life while having a high energy density.
[0266] In Comparative Example 3, the second carbon-based material without a carbon coating layer is used in combination with the first carbon-based material, and the kinetic performance and storage performance of the battery are poor.
[0267] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.
[0268]
[0269]
Claims
1. A secondary battery comprising a negative electrode plate, wherein the negative electrode plate comprises a negative electrode current collector and a negative electrode film layer formed on at least one surface of the negative electrode current collector and comprising a negative electrode active material, wherein the negative electrode active material comprises a first carbon-based material and a second carbon-based material, wherein the first carbon-based material has a pore structure, and at least a portion of the surface of the second carbon-based material has a carbon coating layer.
2. The secondary battery according to claim 1, wherein The interlayer spacing of the crystal plane of the second carbon-based material 002 is greater than the interlayer spacing of the crystal plane of the first carbon-based material 002.
3. The secondary battery according to claim 1 or 2, wherein The gram capacity of the second carbon-based material is less than the gram capacity of the first carbon-based material.
4. The secondary battery according to any one of claims 1 to 3, wherein: The powder compaction density of the second carbon-based material under a pressure of 5000 kg is less than the powder compaction density of the first carbon-based material under a pressure of 5000 kg.
5. The secondary battery according to any one of claims 1 to 4, wherein: The peak intensity ratio of the D peak to the G peak in the Raman spectrum of the second carbon-based material is D / I G Greater than the peak intensity ratio I of the D peak and the G peak in the Raman spectrum of the first carbon-based material D / I G .
6. The secondary battery according to any one of claims 1 to 5, wherein: The second carbon-based material includes secondary particles; optionally, the secondary particles in the second carbon-based material account for greater than or equal to 50%.
7. The secondary battery according to any one of claims 1 to 6, wherein: The second carbon-based material satisfies at least one of the following conditions: (1) The peak intensity ratio of the D peak to the G peak in the Raman spectrum of the second carbon-based material is D / I G ≥0.23, optional range is 0.23-0.41; (2) The powder compaction density of the second carbon-based material under a pressure of 5000 kg is ≥1.65 g / cm 3 , optional 1.65g / cm 3 -1.90g / cm 3 ; (3) The interlayer spacing of the 002 crystal plane of the second carbon-based material is ≤0.336217 nm, and can be selected from 0.335787 nm to 0.336217 nm; (4) The specific surface area of the second carbon-based material is ≥0.90 m 2 / g, optional 0.9m 2 / g-2.5m 2 / g; (5) The volume distribution particle size Dv50 of the second carbon-based material is ≥10 μm, and can be selected from 10 μm to 22 μm; (6) The particle size distribution of the second carbon-based material (Dv90-Dv10) / Dv50 is ≤1.65, and can be optionally 0.9-1.65; (7) The tap density of the second carbon-based material is ≥0.85 g / cm 3 , optional 0.9g / cm 3 -1.25g / cm 3 ; (8) The gram capacity of the second carbon-based material is ≥340 mAh / g, and can be optionally 340 mAh / g-360 mAh / g.
8. The secondary battery according to any one of claims 1 to 7, wherein: The second carbon-based material includes at least one of artificial graphite and natural graphite; optionally, the second carbon-based material includes artificial graphite.
9. The secondary battery according to any one of claims 1 to 8, wherein: The first carbon-based material includes at least one pore with an area greater than or equal to 0.1 μm 2 The pore structure may include one or more pores with an area of 0.12 μm 2 -2.5μm 2 pore structure.
10. The secondary battery according to any one of claims 1 to 9, wherein: The first carbon-based material includes an external region and an internal region located inside the external region, the external region refers to a region extending from the particle surface of the first carbon-based material to the interior of the particle by a distance of 0.25L, L refers to the short axis length of the first carbon-based material particle, the total pore area of the external region is recorded as S1, the total pore area of the internal region is recorded as S2, and S2>S1, optionally, 1.5≤S2 / S1≤500, 2≤S2 / S1≤450.
11. The secondary battery according to claim 10, wherein The area of the pore structure in the outer region of the first carbon-based material is less than or equal to 0.15 μm 2 , can be selected to be less than or equal to 0.13μm 2 and / or, The inner region of the first carbon-based material includes at least one area greater than or equal to 0.15 μm 2 The pore structure may optionally include one or more pores with an area of 0.15 μm 2 -2.0μm 2 pore structure.
12. The secondary battery according to any one of claims 1 to 11, wherein: At least a portion of the surface of the first carbon-based material has a carbon coating layer.
13. The secondary battery according to any one of claims 1 to 12, wherein: The first carbon-based material includes primary particles; optionally, the primary particles in the first carbon-based material account for greater than or equal to 50%.
14. The secondary battery according to any one of claims 1 to 13, wherein: The first carbon-based material satisfies at least one of the following conditions: (1) The specific surface area of the first carbon-based material is ≤2.3m 2 , optional 0.7m 2 / g-2.3m 2 / g; (2) the volume distribution particle size Dv50 of the first carbon-based material is ≥6.0 μm, and can be selected from 6.0 μm to 25.0 μm; (3) the volume distribution particle size Dv90 of the first carbon-based material is ≥16.0 μm, and can be selected from 16.0 μm to 40.0 μm; (4) the particle size distribution of the first carbon-based material (Dv90-Dv10) / Dv50 is ≤1.55, and can be optionally 0.9-1.55; (5) The tap density of the first carbon-based material is ≥0.8 g / cm 3 , optional 0.8g / cm 3 -1.20g / cm 3 ; (6) The powder compaction density of the first carbon-based material under a pressure of 5000 kg is ≤ 2.10 g / cm 3 , optional 1.85g / cm 3 -2.10g / cm 3 ; (7) The interlayer spacing of the 002 crystal plane of the first carbon-based material is ≤0.335916 nm, and can be selected from 0.335576 nm to 0.335916 nm; (8) The gram capacity of the first carbon-based material is ≥358 mAh / g, and can be selected from 358 mAh / g to 370 mAh / g; (9) The X-ray diffraction pattern of the first carbon-based material has a diffraction peak of the 101 crystal plane of the 3R phase; (10) The X-ray diffraction pattern of the first carbon-based material does not have a diffraction peak of the 012 crystal plane of the 3R phase; (11) In a thermogravimetric analysis test of the first carbon-based material in an air atmosphere, the weight loss rate of the first carbon-based material between 35° C. and 790° C. is ≤50%, and can be optionally 16%-43%; (12) In the thermogravimetric analysis test of the first carbon-based material in air atmosphere, the temperature corresponding to the maximum weight loss rate of the first carbon-based material is recorded as T max , then T max Greater than or equal to 795℃, optional 805℃-850℃.
15. The secondary battery according to any one of claims 1 to 14, wherein: The mass proportion of the first carbon-based material in the negative electrode active material is ≥30 wt %, and can be optionally 30 wt %-80 wt %.
16. The secondary battery according to any one of claims 1 to 15, wherein: The negative electrode active material satisfies at least one of the following conditions: (1) The volume distribution particle size Dv50 of the negative electrode active material is ≥6 μm, and can be selected from 6 μm to 23 μm; (2) The particle size distribution of the negative electrode active material (Dv90-Dv10) / Dv50 is ≥0.9, and can be optionally 0.9-1.55; (3) The graphitization degree of the negative electrode active material is ≥92%, and can be optionally 92%-96%; (4) The gram capacity of the negative electrode active material is ≥350 mAh / g, and can be optionally 350 mAh / g-365 mAh / g.
17. The secondary battery according to any one of claims 1 to 16, wherein: The negative electrode film layer further includes a silicon-based material; optionally, the silicon-based material accounts for less than or equal to 20% by mass in the negative electrode film layer.
18. The secondary battery according to any one of claims 1 to 17, wherein: The negative electrode film layer satisfies at least one of the following conditions: (1) The porosity of the negative electrode film layer is ≥15.5%, and can be selected from 15.5% to 38%; (2) The compaction density of the negative electrode film is ≥1.40 g / cm 3 , optional 1.40g / cm 3 -1.80g / cm 3 ; (3) The surface density of the negative electrode film layer is ≥5.5g / cm 2 , optional 6.0g / cm 3 -19.5g / cm 2 ; (4) The OI value of the negative electrode film layer is ≤38, and can be optionally 8-38.
19. An electrical device comprising the secondary battery according to any one of claims 1 to 18.
Citation Information
Patent Citations
Negative electrode material for non-aqueous electrolyte secondary battery and non-aqueous electrolyte secondary battery using same
CN102362380A
Graphite material, carbon material for battery electrode, and battery
CN102844918A
Carbon material and negative electrode for nonaqueous secondary battery and nonaqueous secondary battery
CN103460459A
Negative electrode active material for lithium secondary battery, negative electrode containing same for lithium secondary battery, and lithium secondary battery
CN111602274A
Non-aqueous electrolyte secondary cell
CN112292773A