Positive pole piece, manufacturing method, secondary battery and electric device
Patent Information
- Application Number
- CN202280093546.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-01
- Publication Date
- 2024-11-26
AI Technical Summary
The hydrofluoric acid generated during the preparation process of lithium hexafluorophosphate in lithium-ion batteries causes an increase in pressure within the battery, affecting cycle performance and safety. The existing positive and negative electrodes have insufficient improvements in resistance to acidic substances.
Adding silicon-containing compound additives with specific average volume particle sizes, such as potassium silicate, sodium silicate, etc., into the positive electrode film layer of the positive electrode sheet can effectively consume hydrogen fluoride in the electrolyte, reduce the DC internal resistance of the battery, and improve cycle performance. .
By reducing the DC internal resistance of the battery, the cycle performance of the lithium-ion battery is significantly improved, and the method has a simple synthesis path, low cost, and is suitable for industrial production.
Smart Images

Figure CN119032440A_ABST
Abstract
Description
Positive electrode sheet, manufacturing method, secondary battery and electrical device Technical Field
[0001] The present application relates to the technical field of lithium batteries, and in particular to a positive electrode sheet, a manufacturing method, a secondary battery and an electrical device. Background Art
[0002] In recent years, the application of lithium-ion batteries has become increasingly widespread. They are widely used in energy storage systems such as hydropower, thermal power, wind power, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and other fields. As lithium-ion batteries have achieved significant development, higher requirements have been placed on their energy density, cycle performance, and safety performance.
[0003] However, lithium-ion battery electrolytes typically use lithium hexafluorophosphate as a lithium salt. During its preparation, the lithium hexafluorophosphate inevitably carries acidic substances such as hydrofluoric acid into the final product. Furthermore, lithium hexafluorophosphate can produce acidic substances such as hydrofluoric acid when in contact with water. When the hydrofluoric acid content in a lithium-ion battery exceeds a certain concentration, it consumes limited lithium ions, increasing the battery's irreversible capacity and increasing internal pressure. As the hydrofluoric acid content increases, the positive and negative electrode structures of the lithium-ion battery may be damaged, reducing performance such as charge and discharge, cycle efficiency, and even leading to safety accidents. Therefore, there is still room for improvement in the acid resistance of the positive and negative electrodes.
[0004] Summary of the Invention
[0005] The present application is made in view of the above-mentioned problems, and its purpose is to provide a positive electrode plate, wherein the positive electrode film layer contains a silicon-containing compound additive of a specific particle size, which significantly reduces the direct current internal resistance (DCR) of the battery and improves the cycle performance of the battery; and the additive has a simple synthesis path, low cost, stable structure, and can be widely used in industrial production.
[0006] In order to achieve the above-mentioned objectives, the present application provides a positive electrode sheet, a manufacturing method, a secondary battery and an electrical device.
[0007] The first aspect of the present application provides a positive electrode sheet, which includes a positive electrode current collector and a positive electrode film layer arranged on at least one side of the positive electrode current collector, wherein the positive electrode film layer contains a positive electrode active material and a x Q·nSi y Q z Silicon compound additives, wherein
[0008] M is one or more of alkali metals, alkaline earth metals, Al, Fe, and Zn;
[0009] Q is one or more of O, F, Cl, Br, I, and At;
[0010] The value of x depends on M;
[0011] The values of y and z depend on Q; and
[0012] m and n are positive integers;
[0013] The silicon-containing compound additive comprises an average volume particle size D v50 The particles are small in size of 0.01-1 μm.
[0014] The positive electrode plate of the present application can consume the hydrogen fluoride present in the electrode liquid by including a silicon-containing compound additive with a specific average volume particle size in its positive electrode film layer, while reducing the direct current internal resistance (DCR) of the battery and improving the cycle performance of the battery.
[0015] In any embodiment, the content of small particles having an average volume particle size Dv50 of 0.01 μm to 1 μm is 50% to 100% based on the total weight of the silicon-containing compound additive. As a result, the small particles react more quickly with hydrogen fluoride in the electrolyte, thereby reducing the direct current resistance (DCR) of the battery and improving the battery's cycling performance.
[0016] In any embodiment, the silicon-containing compound additive comprises 0-40% of 1 μm <D v50 Medium particles ≤ 2μm and 2μm<D with a content of 0-10% v50 Large particles of ≤10 μm, each based on the total weight of the silicon-containing compound additive, react more quickly with hydrogen fluoride in the electrolyte, thereby reducing the direct current resistance (DCR) of the battery and improving the battery's cycle performance.
[0017] In any embodiment, the D of the silicon-containing compound additive is v99 The nanoparticles are smaller than 20 μm. This allows them to react more quickly with hydrogen fluoride in the electrolyte, thereby reducing the direct current resistance (DCR) of the battery and improving its cycle performance.
[0018] In any embodiment, the silicon-containing compound additive comprises at least one of potassium silicate, sodium silicate, lithium silicate, aluminum silicate, lithium fluorosilicate, potassium fluorosilicate, or sodium fluorosilicate. Thus, the silicon-containing compound additive reacts more quickly with hydrogen fluoride in the electrolyte, thereby reducing the direct current resistance (DCR) of the battery and improving the cycle performance of the battery.
[0019] In any embodiment, the content of the silicon-containing compound additive is 0.01%-2% based on the weight of the positive electrode film layer, thereby reacting more quickly with hydrogen fluoride in the electrolyte, thereby reducing the direct current resistance (DCR) of the battery and improving the cycle performance of the battery.
[0020] In any embodiment, the weight ratio of the silicon-containing compound additive to the positive electrode active material is 0.0125%-2.5%, thereby reacting more quickly with hydrogen fluoride in the electrolyte, thereby reducing the direct current resistance (DCR) of the battery and improving the cycle performance of the battery.
[0021] The second aspect of the present application provides a method for preparing a positive electrode sheet, which comprises:
[0022] (1) providing a silicon-containing compound additive;
[0023] (2) mixing the silicon-containing compound additive with a positive electrode active material and a solvent to prepare a positive electrode slurry;
[0024] (3) coating the positive electrode slurry on the positive electrode current collector to form a positive electrode film layer to obtain the positive electrode sheet;
[0025] The silicon-containing compound additive is of formula mM x Q·nSi y Q z ,in
[0026] M is one or more of alkali metals, alkaline earth metals, Al, Fe, and Zn;
[0027] Q is one or more of O, F, Cl, Br, I, and At;
[0028] The value of x depends on M;
[0029] The values of y and z depend on Q; and
[0030] m and n are positive integers;
[0031] The silicon-containing compound additive comprises an average volume particle size D v50 The particles are small in size of 0.01-1 μm.
[0032] Therefore, the method of the present application is simple, low-cost, and convenient for large-scale production and application. The obtained positive electrode plate contains a silicon-containing compound additive with a specific particle size, which can effectively consume the hydrogen fluoride present in the electrode solution, while reducing the direct current internal resistance (DCR) of the battery and improving the cycle performance of the battery.
[0033] In any embodiment, in step (1), the silicon-containing compound additive can be prepared by air flow crushing, ball milling, or reprecipitation. Thus, the silicon-containing compound additive has a simple synthesis path, low cost, and stable structure, and can be better applied to the battery of the present application.
[0034] In any embodiment, in step (2), the silicon-containing compound additive can be deposited on the surface of the positive electrode active material using a deposition method, wherein the deposition method comprises dissolving the silicon-containing compound additive in solvent A to form solution A; dispersing the positive electrode active material in solvent B to form solution B; and then mixing solution A and solution B to deposit the silicon-containing compound additive on the surface of the positive electrode active material. Thus, the silicon-containing compound additive has a simple synthesis path, low cost, and stable structure, and can be better applied to the battery of the present application.
[0035] In any embodiment, the concentration of the silicon-containing compound additive in solution A is 1% to 10% by weight; and the concentration of the positive electrode active material in solution B is 5% to 20% by weight. Thus, the silicon-containing compound additive has a simple synthesis route, low cost, and a stable structure, and can be better applied to the battery of the present application.
[0036] In any embodiment, the solubility of the silicon-containing compound additive in solvent B at room temperature and normal pressure is less than 1 g / 100 g. Thus, the silicon-containing compound additive has a simple synthesis route, low cost, and stable structure, and can be better applied to the battery of the present application.
[0037] A third aspect of the present application provides a secondary battery, characterized in that:
[0038] It includes the positive electrode sheet described in the first aspect of the present application or the positive electrode sheet prepared according to the method described in the second aspect of the present application.
[0039] The fourth aspect of the present application provides an electrical device, characterized in that it includes the secondary battery described in the third aspect of the present application.
[0040] The positive electrode plate of the present application can consume the hydrogen fluoride present in the electrode solution more quickly by including a silicon-containing compound additive with a smaller average volume particle size in its positive electrode film layer, while reducing the direct current internal resistance (DCR) of the battery and improving the cycle performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] FIG1 is an SEM image of a silicon-containing compound additive prepared by a deposition method attached to the surface of a positive electrode active material in one embodiment of the present application; wherein the gray dots in the black box represent the silicon-containing compound additive.
[0042] FIG. 2 is a schematic diagram of a secondary battery according to an embodiment of the present application.
[0043] FIG3 is an exploded view of a secondary battery according to an embodiment of the present application.
[0044] FIG. 4 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.
[0045] Description of reference numerals:
[0046] 5. Secondary battery; 51. Housing; 52. Electrode assembly; 53. Cover; 6. Electrical device. DETAILED DESCRIPTION
[0047] Below, the embodiments of the positive electrode sheet, preparation method, secondary battery and electric device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0048] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0049] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0050] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0051] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0052] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0053] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0054] At present, lithium hexafluorophosphate is commonly used as a lithium salt in lithium-ion battery electrolytes. The lithium hexafluorophosphate used will inevitably carry acidic substances such as hydrofluoric acid into the final product during its preparation process, and lithium hexafluorophosphate can produce acidic substances such as hydrofluoric acid when it comes into contact with water. When the hydrofluoric acid content in a lithium-ion battery exceeds a certain concentration, it will consume limited lithium ions, increase the irreversible capacity of the battery, and at the same time cause the pressure inside the battery to increase. As the hydrofluoric acid content increases, the positive and negative electrode structures of the lithium-ion battery may be destroyed, and its charging and discharging, cycle efficiency and other performance will decrease, and even safety accidents may occur. Therefore, there is still room for improvement in the acid resistance of the positive and negative electrodes. Through extensive research, the inventors found that the positive electrode plate of the first aspect of the present application contains a silicon-containing compound additive with a small average volume particle size in its positive electrode film layer, which significantly reduces the direct current internal resistance (DCR) of the battery and improves the cycle performance of the battery; and the additive has a simple synthesis path, low cost, stable structure, and can be widely used in industrial production.
[0055] Positive electrode
[0056] In some embodiments, the first aspect of the present application provides a positive electrode sheet comprising a positive electrode current collector and a positive electrode film layer disposed on at least one side of the positive electrode current collector, wherein the positive electrode film layer comprises a positive electrode active material and a positive electrode active material.
[0057] mMx Q·nSi y Q z Silicon compound additives, wherein
[0058] M is one or more of alkali metals, alkaline earth metals, Al, Fe, and Zn;
[0059] Q is one or more of O, F, Cl, Br, I, and At;
[0060] The value of x depends on M;
[0061] The values of y and z depend on Q; and
[0062] m and n are positive integers;
[0063] The silicon-containing compound additive comprises an average volume particle size D v50 The particles are small particles of 0.01-1 μm, optionally 0.01-0.8 μm, and further optionally 0.05-0.15 μm.
[0064] The positive electrode plate of the present application includes a silicon-containing compound additive with a specific average volume particle size in its positive electrode film layer, so that the silicon-containing compound additive is evenly dispersed, and the contact area with the hydrogen fluoride present in the electrode liquid is large, which is more conducive to chemical reaction. At the same time, the generated by-products with more stable structures are deposited on the surface of the positive electrode active material, which can reduce the direct current internal resistance (DCR) of the battery and improve the cycle performance of the battery.
[0065] In some embodiments, the average volume particle size D v50 The content of the small particles of 0.01 μm to 1 μm, optionally 0.01 to 0.8 μm, and further optionally 0.05 to 0.15 μm is 50% to 100%, optionally 80% to 100%, based on the total weight of the silicon-containing compound additive. As a result, the small particles react more quickly with hydrogen fluoride in the electrolyte, thereby reducing the direct current resistance (DCR) of the battery and improving the cycle performance of the battery.
[0066] In a preferred embodiment, the silicon-containing compound additive has an average volume particle size D v50 The particle size is 0.01 μm to 1 μm, and the average volume particle size D v50 The particle size is 0.01-0.8 μm, and the average volume particle size D v50 It is composed of small particles of 0.05-0.15μm.
[0067] In some embodiments, the silicon-containing compound additive may further include 1 μm <D v50Medium particles ≤ 2 μm and large particles 2 μm < Dv50 ≤ 10 μm in a content of 0-10%, each based on the total weight of the silicon-containing compound additive, are used to adjust the pore structure of the coating and prevent excessive agglomeration of small-sized silicon-containing compound additives, which may cause poor electrolyte wetting and deteriorate lithium ion transport performance.
[0068] In some embodiments, when the silicon-containing compound additive includes medium particles, the ratio of the medium particles to the small particles is 1:2:8, optionally 1:3-5, based on the weight of the two particles.
[0069] In some embodiments, when the silicon-containing compound additive comprises large particles, the ratio of the large particles to the small particles is 1:5-13, optionally 1:8-10, based on the weight of the two particles.
[0070] In some embodiments, when the silicon-containing compound additive contains both large particles and small particles, the content ratio of large particles, medium particles and small particles is 1:(1.1-4):(4.5-11), and can be optionally 1:(1.5-2.5):(6-8), based on the weight of the particles of the two.
[0071] In some embodiments, the D of the silicon-containing compound additive is v99 The thickness of the nanoparticles is less than 20 μm, and can be less than 10 μm. As a result, the nanoparticles react with hydrogen fluoride in the electrolyte more quickly, thereby reducing the direct current resistance (DCR) of the battery and improving the cycle performance of the battery.
[0072] In this application, D v50 The particle size corresponding to the cumulative volume distribution percentage of the sample starting from the smallest particle size reaches 50%, also known as the average volume particle size; D v90 D is the particle size corresponding to when the cumulative volume distribution percentage of the sample starting from the smallest particle size reaches 90%; v99 It is the particle size corresponding to when the volume cumulative distribution percentage of the sample starting from the smallest particle size reaches 99%.
[0073] The particle size of the above materials has a well-known meaning in the art, and is determined by using a laser particle size analyzer to measure the volume particle size and its distribution of the materials, such as the Mastersizer 3000 laser particle size analyzer produced by Malvern Instruments Ltd., UK.
[0074] In some embodiments, the silicon-containing compound additive may include a silicate or a fluorosilicate, for example, at least one of potassium silicate, sodium silicate, lithium silicate, aluminum silicate, lithium fluorosilicate, potassium fluorosilicate, or sodium fluorosilicate, with potassium silicate or lithium silicate being preferred. This allows the additive to react more quickly with hydrogen fluoride in the electrolyte, thereby reducing the direct current resistance (DCR) of the battery and improving the battery's cycling performance.
[0075] In some embodiments, the silicon-containing compound additive comprises 0.2% to 2%, and optionally 0.5% to 1%, based on the weight of the positive electrode film layer. This allows the silicon-containing compound additive to react more quickly with hydrogen fluoride in the electrolyte, thereby reducing the direct current resistance (DCR) of the battery and improving the battery's cycling performance.
[0076] In some embodiments, the weight ratio of the silicon-containing compound additive to the positive electrode active material is 0.0125%-2.5%, and optionally 0.5%-1.1%. This allows the silicon-containing compound additive to react more quickly with hydrogen fluoride in the electrolyte, thereby reducing the direct current resistance (DCR) of the battery and improving the battery's cycling performance.
[0077] In some optional embodiments, the silicon-containing compound additive is attached to the surface of the positive electrode active material particles and exists as a coating on the surface of the positive electrode active material particles.
[0078] In some embodiments, the silicon-containing compound additive particles are added to the positive electrode film layer by: (1) physically mixing the silicon-containing compound additive with the active material in advance, and then preparing a positive electrode slurry; (2) directly adding the silicon-containing compound additive dispersion to the positive electrode slurry; (3) directly precipitating and depositing the silicon-containing compound additive on the surface of the positive electrode material, and then preparing a positive electrode slurry (preferably, sintering is required later to ensure a stronger bond and more uniform particles); and (4) uniformly coating the silicon-containing compound additive on the surface of the positive electrode active material layer away from the positive electrode current collector to form a silicon-containing compound coating. In this case, the positive electrode film layer includes a positive electrode active material layer and a silicon-containing compound coating arranged on the surface of the positive electrode active material layer on the side contacting the isolation membrane. The thickness of the silicon-containing compound coating is 1-10um, the thickness of the positive electrode active material layer is 50-150um, and the ratio of the thickness of the silicon-containing compound coating to the thickness of the positive electrode active material layer is 0.67%-20%.
[0079] In some embodiments, the average volume particle size Dv50 of the positive electrode active material is 20-100 nm, and the ratio of the Dv50 of the silicon-containing compound to the average volume particle size of the positive electrode active material is 1:20-100, and optionally 1:30-50.
[0080] In some embodiments, the thickness of the positive electrode sheet is 100-250 μm, and the porosity is 20%-35%. The thickness of the positive electrode sheet is the sum of the thickness of the positive electrode current collector and the thickness of the positive electrode film layer (also called the positive electrode active material layer).
[0081] In some embodiments, the second aspect of the present application provides a method for preparing a positive electrode sheet, comprising:
[0082] (1) providing a silicon-containing compound additive;
[0083] (2) mixing the silicon-containing compound additive with a positive electrode active material and a solvent to prepare a positive electrode slurry;
[0084] (3) coating the positive electrode slurry on the positive electrode current collector to form a positive electrode film layer to obtain the positive electrode sheet;
[0085] The silicon-containing compound additive is of formula mM x Q·nSi y Q z ,in
[0086] M is one or more of alkali metals, alkaline earth metals, Al, Fe, and Zn;
[0087] Q is one or more of O, F, Cl, Br, I, and At;
[0088] The value of x depends on M;
[0089] The y and z values depend on Q;
[0090] m and n are positive integers;
[0091] The silicon-containing compound additive comprises an average volume particle size D v50 The particles are small in size of 0.01-1 μm.
[0092] Therefore, the method of the present application is simple, low-cost, and convenient for large-scale production and application. The obtained positive electrode plate contains a silicon-containing compound additive with a specific particle size, which can effectively consume the hydrogen fluoride present in the electrode solution, while reducing the direct current internal resistance (DCR) of the battery and improving the cycle performance of the battery.
[0093] In some embodiments, in step (1), the silicon-containing compound additive provided may be a commercially available silicon-containing compound, or may be prepared by methods known to those skilled in the art.
[0094] In some embodiments, in step (1), the silicon-containing compound additive can be prepared by air flow crushing and reprecipitation. Thus, the silicon-containing compound additive has a simple synthesis path, low cost, and stable structure, and can be better applied to the battery of the present application.
[0095] The average volume particle size D of most commercially available silicon-containing compounds is v50 Typically 50-100 μm, this is too large a particle size for this application.
[0096] In some embodiments, a gas flow milling method can be used to prepare the silicon-containing compound additive having the particle size described herein. The gas flow milling method comprises crushing a commercially available silicon-containing compound through a gas flow mill at a pressure of 0.7-1 MPa and a gas flow rate of 3-20 m³ / min, and then adjusting the average volume particle size of the particles to the desired level after grading and screening.
[0097] In some embodiments, a reprecipitation method can be used to prepare the silicon-containing compound additive having the particle size described herein. The reprecipitation method comprises dissolving a commercially available silicon-containing compound additive in solvent 1 at room temperature and stirring uniformly to form solution 1 having a silicon-containing compound concentration of 1 wt% to 10 wt%; then, while stirring at 400-800 rpm, adding solution 1 to solvent 2, in which the silicon-containing compound is slightly or poorly soluble, to form solution 2 having a concentration of 5 wt% to 20 wt%. During the stirring process, the silicon-containing compound additive reprecipitates, and the average volume particle size of the particles can be adjusted to the desired level.
[0098] In some embodiments, solvent 1 is generally any substance capable of dissolving the silicon-containing compound at room temperature, including, but not limited to, deionized water. Solvent 2 can be a substance known to those skilled in the art that is slightly soluble or insoluble in the silicon-containing compound, including, but not limited to, anhydrous ethanol, N-methylpyrrolidone (NMP), acetone, carbon tetrachloride, and other organic solvents.
[0099] In some embodiments, step (2) comprises mixing the silicon-containing compound additive with a positive electrode active material, a solvent, and optionally a binder or other additives to prepare a positive electrode slurry.
[0100] In some embodiments, in step (2), a deposition method may be used to deposit the silicon-containing compound additive having the particle size described in the present application on the surface of the positive electrode active material.
[0101] In some embodiments, in step (2), the deposition method includes dissolving the silicon-containing compound additive in solvent A to form solution A; dispersing the positive electrode active material in solvent B to form solution B; and then mixing solution A and solution B to deposit the silicon-containing compound additive on the surface of the positive electrode active material. Thus, the silicon-containing compound additive has a simple synthesis path, low cost, and stable structure, and can be better applied to the battery of the present application.
[0102] In some embodiments, the concentration of the silicon-containing compound additive in solution A is 1% to 10% by weight, and the concentration of the positive electrode active material in solution B is 5% to 20% by weight. Thus, the silicon-containing compound additive has a simple synthesis route, low cost, and a stable structure, and can be better applied to the battery of the present application.
[0103] In some embodiments, solvent A is generally any substance that can dissolve the silicon-containing compound at room temperature, including but not limited to deionized water.
[0104] In some embodiments, the solubility of the silicon-containing compound additive in solvent B at room temperature and normal pressure is less than 1 g / 100 g. Therefore, the silicon-containing compound additive has a simple synthesis route, low cost, and stable structure, and can be better applied to the battery of the present application.
[0105] In some embodiments, the solvent B may be a substance known to those skilled in the art that is slightly soluble or insoluble in the silicon-containing compound and poorly soluble or even insoluble in the positive electrode active material, such as but not limited to anhydrous ethanol, NMP, acetone, carbon tetrachloride and other organic solvents.
[0106] In the present application, the term "slightly soluble" means that the solubility of the solute in 100 grams of solvent is 0.01 grams to 1 gram at room temperature and pressure.
[0107] In this application, the term "poorly soluble" means that the solubility of the solute in 100 grams of solvent is less than 0.01 grams at room temperature and pressure.
[0108] In some optional embodiments, the deposition method includes dissolving the silicon-containing compound additive in solvent A to form solution A having a silicon-containing compound additive concentration of 1 wt% to 10 wt%; dispersing the positive electrode active material in solvent B to form solution B; then adding solution A to solution B, stirring and mixing, so that the silicon-containing compound additive is deposited on the surface of the positive electrode active material, filtering, and then sintering at 300-500°C, preferably in air or an inert atmosphere, to obtain a product in which the silicon-containing compound additive is attached to the surface of the positive electrode active material at a desired average volume particle size. The deposition method is similar to the reprecipitation method, except that the precipitated silicon-containing compound additive is directly deposited on the surface of the positive electrode active material particles. The silicon-containing compound additive is in the form of small spherical particles that are evenly distributed on the surface of the positive electrode active material particles.
[0109] In some embodiments, the solvent in step (2) may typically be N-methylpyrrolidone (NMP).
[0110] In some embodiments, in step (2), the positive electrode slurry has a solid content of 40-80 wt % and a viscosity of 5000-25000 mPa·s at room temperature.
[0111] In some embodiments, in step (3), the positive electrode slurry is coated on a positive electrode current collector, dried to form a positive electrode film layer, and then cold-pressed by a cold rolling mill to obtain the positive electrode sheet.
[0112] In some embodiments, the unit area density of the positive electrode film layer is 40-350 g / m2, and the compaction density of the positive electrode sheet is 2.0-3.6 g / cm3, and can be optionally 3.3-3.5 g / cm3.
[0113] The calculation formula of the compacted density is:
[0114] Compacted density = unit area density / (thickness of the electrode after extrusion - thickness of the current collector).
[0115] The mass M of the positive electrode active material per unit area of the positive electrode film layer can be obtained by weighing using a standard balance.
[0116] The thickness T of the positive electrode film layer can be measured using a micrometer, such as a Mitutoyo 293-100 with an accuracy of 0.1 μm. It should be noted that the thickness of the positive electrode film layer described in the present invention refers to the thickness of the positive electrode film layer in the positive electrode sheet after cold pressing and used for battery assembly.
[0117] A third aspect of the present application provides a secondary battery, characterized in that:
[0118] It includes the positive electrode sheet described in the first aspect of the present application or the positive electrode sheet prepared according to the method described in the second aspect of the present application.
[0119] The secondary battery is a lithium ion secondary battery or a sodium ion secondary battery.
[0120] In some embodiments, the initial direct current internal resistance (DCR) of the secondary battery at 25° C. is 1-1.7Ω, optionally 1.05-1.35Ω; and the DCR after 1000 cycles at 25° C. is 2.4-3.8Ω, optionally 2.6-3.0Ω.
[0121] The fourth aspect of the present application provides an electrical device, characterized in that it includes the secondary battery described in the third aspect of the present application.
[0122] The secondary battery and the electric device of the present application will be described below with reference to the accompanying drawings as appropriate.
[0123] Unless otherwise specified, the components, material types, or contents of the batteries mentioned are applicable to both lithium-ion secondary batteries and sodium-ion secondary batteries.
[0124] In one embodiment of the present application, a secondary battery is provided.
[0125] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During the battery's charge and discharge processes, active ions are inserted and removed between the positive and negative electrodes. The electrolyte conducts ions between the positive and negative electrodes. The separator, located between the positive and negative electrodes, primarily prevents short circuits between the positive and negative electrodes while allowing ions to pass through.
[0126] Positive electrode
[0127] The positive electrode sheet is the positive electrode sheet of the first aspect of the present application.
[0128] The positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is arranged on either one or both of the two opposite surfaces of the positive electrode current collector.
[0129] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material on a polymer material substrate. Among them, the metal material includes but is not limited to aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc. Polymer material substrate (such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.)
[0130] In some embodiments, the positive electrode active material may include a positive electrode active material for a battery known in the art.
[0131] As an example, the positive electrode active material of a lithium-ion secondary battery may include at least one of the following materials: a lithium-containing phosphate with an olivine structure, a lithium transition metal oxide, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.
[0132] As an example, the positive electrode active material of a sodium ion secondary battery may include at least one of the following materials: a sodium transition metal oxide, a polyanionic compound, and a Prussian blue compound. However, the present application is not limited to these materials, and other conventionally known materials that can be used as positive electrode active materials for sodium ion batteries may also be used.
[0133] As an optional technical solution of the present application, in the sodium transition metal oxide, the transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Sodium transition metal oxide is, for example, Na x MO2, wherein M is one or more of Ti, V, Mn, Co, Ni, Fe, Cr and Cu, and 0<x≤1.
[0134] As an optional technical solution of the present application, the polyanionic compound can be a compound having sodium ions, transition metal ions and tetrahedral (YO4) n- A class of compounds with anionic units. The transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; Y can be at least one of P, S and Si; n represents (YO4) n- valence.
[0135] Polyanionic compounds can also be sodium ions, transition metal ions, tetrahedral (YO4) n-A class of compounds containing anion units and halogen anions. The transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce; Y can be at least one of P, S, and Si, and n represents (YO4) n- valence state; the halogen may be at least one of F, Cl and Br.
[0136] Polyanionic compounds can also be sodium ions, tetrahedral (YO4) n- Anion unit, polyhedron unit (ZO y ) m+ and an optional halogen anion. Y can be at least one of P, S and Si, and n represents (YO4) n- valence state; Z represents a transition metal, which may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce, and m represents (ZO y ) m+ valence state; the halogen may be at least one of F, Cl and Br.
[0137] Polyanionic compounds include NaFePO4, Na3V2(PO4)3 (sodium vanadium phosphate, abbreviated as NVP), Na4Fe3(PO4)2(P2O7), NaM'PO4F (M' is one or more of V, Fe, Mn and Ni) and Na3(VO y )2(PO4)2F 3-2y At least one of (0≤y≤1).
[0138] Prussian blue compounds can be sodium ions, transition metal ions and cyanide ions (CN - ) compounds. The transition metal may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Prussian blue compounds are, for example, Na a Me b Me' c (CN)6, wherein Me and Me' are each independently at least one of Ni, Cu, Fe, Mn, Co and Zn, 0<a≤2, 0<b<1, 0<c<1.
[0139] The weight ratio of the positive electrode active material in the positive electrode film layer is 80-100 weight %, based on the total weight of the positive electrode film layer.
[0140] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin. The weight ratio of the binder in the positive electrode film layer is 0-20 weight%, based on the total weight of the positive electrode film layer.
[0141] In some embodiments, the positive electrode film layer may further optionally include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. The weight ratio of the conductive agent in the positive electrode film layer is 0-20% by weight, based on the total weight of the positive electrode film layer.
[0142] Negative electrode
[0143] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0144] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0145] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material on a polymer material substrate. Among them, the metal material includes but is not limited to copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver and silver alloys, etc., and the polymer material substrate includes but is not limited to polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE) and other substrates.
[0146] In some embodiments, the negative electrode active material may be a negative electrode active material for batteries known in the art.
[0147] As an example, the negative electrode active material of a lithium-ion secondary battery may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0148] As an example, the negative electrode active material of a sodium ion secondary battery is generally a hard carbon material, a two-dimensional metal carbide or a nitride. Preferably, the negative electrode active material of a sodium ion secondary battery is generally a hard carbon material.
[0149] The weight ratio of the negative electrode active material in the negative electrode film layer is 70-100 weight %, based on the total weight of the negative electrode film layer.
[0150] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS). The binder may be present in the negative electrode film layer in an amount of 0-30% by weight, based on the total weight of the negative electrode film layer.
[0151] In some embodiments, the negative electrode film layer may further include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. The weight ratio of the conductive agent in the negative electrode film layer is 0-20% by weight, based on the total weight of the negative electrode film layer.
[0152] In some embodiments, the negative electrode film layer may further include other additives, such as a thickener (e.g., sodium carboxymethyl cellulose (CMC-Na)). The weight ratio of the other additives in the negative electrode film layer is 0-15% by weight, based on the total weight of the negative electrode film layer.
[0153] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry, wherein the negative electrode slurry has a solid content of 30-70 wt% and a viscosity at room temperature adjusted to 2000-10000 mPa·s; the obtained negative electrode slurry is coated on the negative electrode current collector, and after a drying process, cold pressing, such as with a roller, is obtained. The negative electrode sheet has a unit area density of 50-150 g / m 2 , the compaction density of the negative electrode is 1.2-2.0g / m 3 ; The thickness of the negative electrode sheet is 50-200um, wherein the thickness of the negative electrode collector, such as aluminum foil, is 5-10um.
[0154] The mass M of the negative electrode active material per unit area of the negative electrode film layer can be obtained by weighing using a standard balance.
[0155] The thickness T of the negative electrode film layer or electrode sheet can be measured using a micrometer, for example, a Mitutoyo 293-100 with an accuracy of 0.1 μm. It should be noted that the thickness of the negative electrode film layer referred to in the present invention refers to the thickness of the negative electrode film layer in the negative electrode sheet after cold pressing and used in battery assembly. Throughout this application, the "thickness" mentioned can be measured using the same method as described above.
[0156] electrolytes
[0157] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.
[0158] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.
[0159] In some embodiments, the electrolyte salt of the lithium ion secondary battery can be selected from one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalatophosphate) (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).
[0160] The electrolyte salt of the sodium ion secondary battery can be selected from one or more of sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, sodium trifluoromethanesulfonate, sodium tetrafluoroborate, sodium difluorophosphate, sodium perchlorate, and sodium chloride.
[0161] The concentration of the electrolyte salt is usually 0.5-5 mol / L.
[0162] In some embodiments, the solvent can be selected from one or more of fluoroethylene carbonate (FEC), ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS) and diethyl sulfone (ESE).
[0163] In some embodiments, the electrolyte may optionally include other additives. For example, the other additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0164] Isolation film
[0165] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0166] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0167] In some embodiments, the isolation film has a thickness of 5-20 μm, optionally 5-15 μm.
[0168] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.
[0169] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0170] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0171] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG2 shows a secondary battery 5 having a square structure as an example.
[0172] In some embodiments, referring to Figure 3, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0173] In some embodiments, secondary batteries can be assembled into a battery module. The number of secondary batteries contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.
[0174] In the battery module, the plurality of secondary batteries 5 can be arranged in sequence along the length of the battery module. Of course, they can also be arranged in any other manner. The plurality of secondary batteries 5 can further be fixed by fasteners.
[0175] Optionally, the battery module may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.
[0176] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.
[0177] A battery pack may include a battery box and multiple battery modules disposed within the battery box. The battery box comprises an upper box body and a lower box body. The upper box body can be placed over the lower box body to form an enclosed space for accommodating the battery modules. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0178] In addition, the present application also provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.
[0179] As the electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.
[0180] Figure 4 shows an example of an electric device. This device can be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery, a battery pack or battery module can be used.
[0181] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.
[0182] Example
[0183] In order to make the technical problems, technical solutions and beneficial effects solved by this application clearer, the application will be further described in detail below with reference to the embodiments and drawings. Obviously, the described embodiments are only a part of the embodiments of this application, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is in no way intended to limit the present application and its applications. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0184] If no specific techniques or conditions are specified in the examples, the experiments were carried out according to the techniques or conditions described in the literature in the field or according to the product instructions. All reagents or instruments used without specifying the manufacturer are commercially available conventional products.
[0185] 1. Preparation of positive electrode sheet
[0186] Preparation Example 1
[0187] (1) Provide 500 g of commercially available potassium silicate (purchased from Maclean's Reagent Network, CAS No. 1312-76-1, Product No. P850160, D v50 Average particle size 70 μm);
[0188] (2i) 10 g of the commercially available potassium silicate was added to 190 g of deionized water and stirred to dissolve to prepare a solution A with a potassium silicate concentration of 5 wt %; 2 kg of the positive electrode active material LiMn with an average volume particle size of 5 μm was added. 0.5 Ni 0.3 Co 0.2 The O2 substance is dispersed in 1800g of solvent NMP to prepare solution B; then, solution A is added to solution B while stirring at 800rpm, and the mixture is stirred and mixed. At the same time as solution A is added, the potassium silicate additive is redeposited, so that the potassium silicate additive is deposited on the surface of the positive electrode active material; vacuuming is carried out with a filtration equipment, and after filtration and drying at room temperature, it is sintered in nitrogen at 500°C for 4h to obtain potassium silicate particles with an average volume particle size of 200nm deposited on the surface of the positive electrode active material.
[0189] (2ii) The product prepared in step (2) (a positive electrode active material having potassium silicate particles with an average volume particle size of 200 nm deposited on the surface), conductive carbon black SP, and binder PVDF were dispersed in a solvent NMP at a weight ratio of 98:1:1 and mixed uniformly to obtain a positive electrode slurry;
[0190] (3) The positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil. After drying and cold pressing, the positive electrode sheet is obtained. The coating amount per unit area is 0.27g / 1540.25mm 2 The thickness of the positive electrode is 150um.
[0191] The relevant parameters of the products are summarized in Table 1.
[0192] Preparation Example 2
[0193] The steps of Example 1 were repeated, except that in step (2i), the concentration of the silicon-containing compound in solution A was 1 wt %, and the total concentration of the solution after mixing was still 10 wt %. Potassium silicate particles with an average volume particle size of 100 nm were deposited on the surface of the positive electrode active material.
[0194] Preparation Example 3
[0195] The steps of Preparation Example 1 were repeated, except that in step (2i), the concentration of the silicon-containing compound in Solution A was 10 wt %, to obtain potassium silicate particles with an average volume particle size of 500 nm deposited on the surface of the positive electrode active material.
[0196] Preparation Example 4
[0197] The steps of Preparation Example 1 were repeated, except that in step (2i), the concentration of the silicon-containing compound in Solution A was 0.5 wt %, to obtain potassium silicate particles with an average volume particle size of 50 nm deposited on the surface of the positive electrode active material.
[0198] Preparation Example 5
[0199] The steps of Preparation Example 1 were repeated, except that in step (2i), the concentration of the silicon-containing compound in solution A was 5%, and the amount of solvent B was 800 g; potassium silicate particles with an average volume particle size of 1 μm deposited on the surface of the positive electrode active material were obtained.
[0200] Preparation Example 6
[0201] The steps of Preparation Example 1 were repeated, except that in step (2i), the concentration of the silicon-containing compound in solution A was 15%, and the amount of solvent B was 600 g; potassium silicate particles with an average volume particle size of 2 μm deposited on the surface of the positive electrode active material were obtained.
[0202] Preparation Example 7
[0203] The steps of Example 1 were repeated, except that commercially available potassium fluorosilicate (purchased from MacLean Reagent Network, CAS No. 16871-90-2, Product No. P816423, D v50 Average particle size 150um).
[0204] Preparation Example 8
[0205] The steps of Example 1 were repeated, except that commercially available sodium silicate (McLean Reagent Network, CAS No. 1344-09-8, Product No. S871944, Dv50 average particle size 150 μm) was provided in step (1).
[0206] Preparation Example 9
[0207] The steps of Example 1 were repeated, except that commercially available aluminum silicate (McLean Reagent Network, CAS No. 1302-93-8, Product No. A823215, Dv50 average particle size 6.5 μm) was provided in step (1).
[0208] Preparation Example 10
[0209] The steps of Preparation Example 1 were repeated, except that in step (2i) the positive electrode active material was Na2FePO4.
[0210] Preparation Example 11
[0211] Potassium silicate powder (composition shown in Table 1) was dispersed in an NMP solution and then ultrasonically homogenized to form a 10% potassium silicate dispersion. The positive electrode active material, potassium silicate dispersion, conductive carbon black SP, and PVDF binder were added to the NMP solvent in the order of 97:1:1:1 by weight and mixed to obtain a positive electrode slurry.
[0212] Preparation Example 12
[0213] (1) LiMn 0.5 Ni 0.3 Co 0.2 O2, conductive carbon black SP and binder PVDF are dispersed in solvent NMP in a weight ratio of 98:1:1 and mixed evenly to obtain a positive electrode slurry;
[0214] (2) Potassium silicate powders with Dv50 of 200 nm, 1 μm, and 5 μm were dispersed in a solvent NMP at a weight ratio of 7:2:1, and 2% of a binder PVDF was added. The mixture was stirred evenly to obtain a potassium silicate slurry.
[0215] (3) The positive electrode slurry was evenly coated on the positive electrode current collector aluminum foil. After drying, the potassium silicate slurry was evenly coated on the surface of the positive electrode active material layer. After cold pressing, the positive electrode sheet was obtained. The coating amount per unit area was 0.27 g / 1540.25 mm 2 .
[0216] The thickness of the positive electrode active material layer is 150 μm, and the thickness of the potassium silicate layer is 10 μm.
[0217] Comparative Example 1
[0218] (1) LiMn 0.5 Ni 0.3 Co 0.2 O2, conductive carbon black SP and binder PVDF are dispersed in solvent NMP in a weight ratio of 98:1:1 and mixed evenly to obtain a positive electrode slurry;
[0219] (2) The positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil. After drying and cold pressing, the positive electrode sheet is obtained. The coating amount per unit area is 0.27g / 1540.25mm 2 The thickness of the positive electrode film is 150um.
[0220] Comparative Example 2
[0221] Potassium silicate powder (composition shown in Table 1) with a particle size of ≥1 μm was dispersed in an NMP solution and then ultrasonically homogenized to form a 10% potassium silicate dispersion. The positive electrode active material, potassium silicate dispersion, conductive carbon black SP, and PVDF binder were added in the order of 97:1:1:1 by weight into the NMP solvent and mixed to obtain a positive electrode slurry.
[0222] The positive electrode slurry was evenly coated on the positive electrode current collector aluminum foil, and after drying and cold pressing, the positive electrode sheet was obtained. The coating amount per unit area was 0.27g / 1540.25mm 2 .
[0223] Comparative Example 3
[0224] Potassium silicate powder (composition shown in Table 1) with only 20% small particles was dispersed in an NMP solution and then ultrasonically homogenized to form a 10% potassium silicate dispersion. The positive electrode active material, potassium silicate dispersion, conductive carbon black SP, and PVDF binder were added in the order of 97:1:1:1 by weight into the NMP solvent and mixed thoroughly to obtain a positive electrode slurry.
[0225] The positive electrode slurry was evenly coated on the positive electrode current collector aluminum foil, and after drying and cold pressing, the positive electrode sheet was obtained. The coating amount per unit area was 0.27g / 1540.25mm 2 .
[0226] Comparative Example 4
[0227] The steps of Example 1 were repeated, except that (i) in step (1), 10 g of commercially available potassium silicate was added to 190 g of deionized water at room temperature and dissolved and stirred at 400 rpm; 1800 g of anhydrous ethanol was stirred at 800 rpm, and the potassium silicate solution was added dropwise thereto while stirring, so that potassium silicate gradually precipitated; after continuous stirring for 0.5 h, the solution was filtered and dried to obtain potassium silicate; (ii) step (2i) was not performed; and (iii) in step (2ii), the potassium silicate prepared above and the positive electrode active material LiMn were mixed. 0.5 Ni 0.3 Co 0.2 The O2 material, conductive carbon black SP and binder PVDF were dispersed into the solvent NMP in a weight ratio of 1:97:1:1 and mixed evenly to obtain a positive electrode slurry.
[0228] Comparative Example 5
[0229] The steps of Comparative Example 4 were repeated, except that in step (1), 2 kg of commercially available potassium silicate was added to a jet mill at room temperature and pulverized at 1 MPa. 3The mixture was crushed under an air flow of 1.5747 W / min for 2 h to obtain potassium silicate particles.
[0230] The different product parameters of each embodiment and comparative example are shown in Table 1.
[0231] Table 1 Related parameters of silicon-containing compounds in the positive electrode sheets of various preparation examples and comparative examples
[0232]
[0233]
[0234] 2. Application Examples
[0235] Example 1
[0236] 1) Preparation of positive electrode sheet
[0237] The positive electrode sheet prepared in Example 1 was used.
[0238] 2) Preparation of negative electrode sheet
[0239] The negative electrode active material graphite, thickener sodium carboxymethyl cellulose, binder styrene butadiene rubber, and conductive agent acetylene black were mixed in a mass ratio of 97:1:1:1, and deionized water was added to obtain a negative electrode slurry under the action of a vacuum mixer; the negative electrode slurry was evenly coated on a copper foil; the copper foil was dried at room temperature and then transferred to a 120°C oven for drying for 1 hour, and then supercooled pressed and cut to obtain a negative electrode sheet, the coating amount per unit area of which was 0.17g / 1540.25mm 2 .
[0240] 3) Isolation film
[0241] A 12 μm thick polypropylene isolation film (provided by Celgard) was selected.
[0242] 4) Preparation of electrolyte
[0243] The organic solvent is a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC), with the volume ratio of EC, EMC, and DEC being 20:20:60. In an argon atmosphere glove box with a water content of <10 ppm, fully dried lithium salt LiPF6 is dissolved in the organic solvent and mixed thoroughly to obtain an electrolyte solution. The concentration of the lithium salt is 1 mol / L.
[0244] 5) Preparation of batteries
[0245] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator placed between the positive and negative electrode sheets to serve as an isolation. After winding into a square bare battery cell, an aluminum-plastic film is placed in it. After baking at 80°C to remove water, 150g of the corresponding non-aqueous electrolyte is injected and sealed. After standing, hot and cold pressing, formation, clamping, and capacity division, a finished battery with a capacity of 50Ah is obtained.
[0246] The secondary batteries of Examples 2-12 and the secondary batteries of Comparative Examples 1-3 were prepared in a similar manner to the secondary battery of Example 1, but using the positive electrode sheets of the corresponding preparation examples.
[0247] 3. Battery performance test
[0248] 1. DC internal resistance test
[0249] Adjust the battery capacity to 50% SOC: In a 25°C environment, charge and discharge the lithium-ion battery at a fixed rate of 1 / 3C (1C = battery rated capacity), with a charge and discharge voltage range of 2.5-4.35V. Repeat this step three times. The third discharge capacity is recorded as the battery nominal capacity Cn. Start charging at 1 / 3Cn to half of the nominal capacity, and adjust the battery SOC to 50% SOC.
[0250] In a 25°C environment, discharge the above battery with 4Cn for 30s. Record the voltage values before and after discharge as V0 and V1 respectively. (V0-V1) / 4Cn is recorded as the initial internal resistance DCR of the battery at 25°C.
[0251] Note: The resistance values are measured based on the battery cells in Example 1. The resistance values of batteries in different modes are different.
[0252] 2. Cycle life and cycle DCR test:
[0253] The test temperature is 25°C. The battery is charged at a constant current of 1 cm / min to 4.35V, then charged at a constant voltage of 0.05 cm / min. After 30 minutes of rest, the battery is discharged at a rate of 0.33 cm / min to 2.5V. The capacity obtained in this step is used as the initial capacity, and the battery is cycled through a 1 cm / min charge / 0.33 cm / min discharge cycle. The capacity at each step is calculated as the ratio of the initial capacity to the capacity retention rate. The number of cycles at which the capacity retention rate reaches 85% after 25 cycles is considered the cycle life performance of the lithium-ion battery. During the cycling process, the DC internal resistance at the corresponding cycle temperature is tested every 1000 cycles.
[0254] 4. Test results of various embodiments and comparative examples
[0255] Batteries of various examples and comparative examples were prepared according to the above methods, and various performance parameters were measured. The results are shown in Table 2 below.
[0256] Table 2 Battery performance of each embodiment and comparative example
[0257] No. Initial DCR / Ω at 25℃ DCR / Ω after 1000 cycles at 25℃ Number of cycles 11.322.9337193521.22.667201031.443.2004187541.082.4003210051.4883.30708180061.6323.62712172571.3923.09372183081.5363.41376177091 .7283.840481680101.432.93372000111.3923.093721890121.2482.773681950Comparison 12.45.671500Comparison 22.2084.907281620Comparison 32.044.53391650Comparison 42.22724.9499521620Comparison 52.2444.987291575
[0258] It can be seen from Table 1 and Table 2 that when the silicon compound additive contains small particles and the average volume particle size D of the small particles is V50 Under smaller conditions, the battery of the present invention has good technical effects. For example, after 1000 cycles at 25°C, the DCR of the battery can reach 2.67Ω. When the capacity retention rate drops to 80%, the number of cycles of the battery can even reach more than 2000 cycles. Compared with the comparative example 1 without adding the silicon compound additive, the cycle life is increased by more than 30%.
[0259] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A positive electrode sheet comprising a positive electrode current collector and a positive electrode film layer disposed on at least one side of the positive electrode current collector, wherein the positive electrode film layer comprises a positive electrode active material and a x Q·nSi y Q z Silicon compound additives, wherein M is one or more of alkali metals, alkaline earth metals, Al, Fe, and Zn; Q is one or more of O, F, Cl, Br, I, and At; The value of x depends on M; The values of y and z depend on Q; and m and n are positive integers; The silicon-containing compound additive comprises an average volume particle size D v50 The particles are small in size of 0.01-1 μm.
2. The positive electrode sheet according to claim 1, characterized in that: The content of small particles having an average volume particle size Dv50 of 0.01 μm to 1 μm is 50% to 100% based on the total weight of the silicon compound-containing additive.
3. The positive electrode sheet according to claim 1 or 2, characterized in that: The silicon compound additive comprises 0-40% of 1 μm <D v50 Medium particles ≤ 2μm and 2μm<D with a content of 0-10% v50 Large particles of ≤10 μm, each based on the total weight of the silicon-containing compound additive.
4. The positive electrode sheet according to any one of claims 1 to 3, characterized in that: The silicon compound additive D v99 Less than 20 μm.
5. The positive electrode sheet according to any one of claims 1 to 4, characterized in that: The silicon-containing compound additive comprises at least one of potassium silicate, sodium silicate, lithium silicate, aluminum silicate, lithium fluorosilicate, potassium fluorosilicate or sodium fluorosilicate.
6. The positive electrode sheet according to any one of claims 1 to 5, characterized in that: The content of the silicon-containing compound additive is 0.2%-2%, based on the weight of the positive electrode film layer.
7. The positive electrode sheet according to any one of claims 1 to 6, characterized in that: The weight ratio of the silicon-containing compound additive to the positive electrode active material is 0.25-2.5:
1.
8. A method for preparing a positive electrode sheet, comprising: (1) providing a silicon-containing compound additive; (2) mixing the silicon-containing compound additive with a positive electrode active material and a solvent to prepare a positive electrode slurry; (3) coating the positive electrode slurry on the positive electrode current collector to form a positive electrode film layer to obtain the positive electrode plate; the silicon-containing compound additive is of formula mM x Q·nSi y Q z ,in M is one or more of alkali metals, alkaline earth metals, Al, Fe, and Zn; Q is one or more of O, F, Cl, Br, I, and At; The value of x depends on M; The values of y and z depend on Q; and m and n are positive integers; The silicon-containing compound additive comprises an average volume particle size D v50 The particles are small in size of 0.01-1 μm.
9. The method according to claim 8, characterized in that In step (1), the silicon-containing compound additive can be prepared by a gas flow crushing method or a reprecipitation method.
10. The method according to claim 8 or 9, characterized in that In step (2), the silicon-containing compound additive may be deposited on the surface of the positive electrode active material by a deposition method; wherein the deposition method comprises dissolving the silicon-containing compound additive in solvent A to prepare solution A; The positive electrode active material is dispersed in solvent B to prepare solution B; solution A is then mixed with solution B, so that the silicon-containing compound additive is deposited on the surface of the positive electrode active material.
11. The method according to claim 10, characterized in that The concentration of the silicon-containing compound additive in solution A is 1 wt % to 10 wt %; the concentration of the positive electrode active material in solution B is 5 wt % to 20 wt %.
12. The method according to claim 10 or 11, characterized in that The solubility of the silicon-containing compound additive in the solvent B at room temperature and normal pressure is less than 1 g / 100 g.
13. A secondary battery, characterized in that: The invention comprises the positive electrode sheet according to any one of claims 1 to 7 or the positive electrode sheet prepared by the method according to any one of claims 8 to 12.
14. An electrical device, characterized in that: The secondary battery according to claim 13 is included.