Rolling method for improving grain size of steel for steering gear rack

By closing the cooling water pipe and using a cold bed insulation cover for isothermal normalization during the rolling process of steel for steering racks, the crystal mixing problem caused by insufficient AlN dispersion is solved, and the grain size is refined and annealing is avoided The process improves the delivery rate.

CN119056864AInactive Publication Date: 2024-12-03NANJING IRON & STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411134313.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The isothermal normalization time of the steel for the steering gear rack after induction heating shortens, resulting in insufficient dispersion and precipitation of AlN, and a crystal mixing phenomenon, resulting in the breakage of the steel parts during impact and fatigue tests, requiring annealing treatment, increasing production costs and extending the lead time .

Method used

Close the cooling water pipe during the rolling process to ensure high-temperature controlled rolling, and use a cold bed insulation cover to perform isothermal normalization to ensure that AlN fully disperses in the steel, refines the grains, and avoids the annealing process.

Benefits of technology

By controlling the rolling and cooling temperature, the austenite grain size is refined, the crystal mixing phenomenon is avoided, the annealing process is saved, and the delivery rate is improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a rolling method for improving the grain size of steel for a steering gear rack, which comprises the following steps: 1) before rolling, all water tanks are offline, and a cooling water pipe of a roller way is closed, so that water is prevented from being splashed on the surface of the steel in the rolling process, and the local crystal mixing condition caused by uneven cooling is avoided; (2) the speed of a rough rolling last rack rolling mill is 0.6 m / s, it is guaranteed that the reducing sizing temperature is 980 DEG C or above, and high-temperature controlled rolling is conducted; and (3) a heat preservation cover of the cooling bed is lowered in advance, the cooling bed moves at 40 s / step, the steel for the steering gear rack stays in the heat preservation cover for 20 min or above, when the surface temperature of the steel is lowered to 500 DEG C, the moving speed of the cooling bed is manually controlled, the steel is moved out of the heat preservation cover, the isothermal normalizing effect is achieved, it is guaranteed that AlN is fully dispersed in the steel, and the grain boundary pinning effect is achieved to refine grains. The problem that the grain size of the steel for the bar steering gear rack with the diameter being 40-80 mm is too large is solved, the effect of refining grains is achieved, and the situation that the steel for the steering gear rack needs an annealing procedure due to coarse grains is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of steel smelting, and in particular to a rolling method for improving the grain size of steel for a steering gear rack. Background Art

[0002] With the development of new energy vehicles, the demand for steel for automotive steering racks is also gradually increasing. The automotive steering rack plays a transmission role through gear meshing and needs to withstand strong impact during the operation of the car. Steering rack steel needs to have a good grain size to ensure strong impact and fatigue performance.

[0003] Steering rack steel is an important component of automobile transmission and has a good market demand. This steel has high requirements for austenite grain size to ensure strong impact and fatigue performance. Steering rack steel chemical composition: C: 0.38-0.43, Mn: 0.62-0.81, Si: 0.17-0.35, Mo: 0.16-0.25, Cr: 0.95-1.12, Ni: ≤0.15, Cu: ≤0.20, P+S+Al+N<0.18, Fe remainder; Steering rack steel refines grains through the dispersion precipitation of AlN along the grain boundaries, which hinders the migration of grain boundaries. However, as the downstream customers' processes changed, gas furnace heating was changed to induction heating, and the isothermal normalizing time was shortened from the original 120 minutes to 30 minutes, resulting in serious lack of AlN dispersion and precipitation, and the occurrence of mixed crystal phenomenon. The rotor rack broke during the impact and fatigue tests. In order to solve the mixed crystal problem, annealing treatment is usually required, which not only increases production costs, but also prolongs the delivery cycle.

[0004] Therefore, it is necessary to develop new technologies to solve the mixed crystal problem. Summary of the invention

[0005] Purpose of the invention: In view of the shortcomings and defects of the prior art, the present invention provides a rolling method for improving the grain size of steering rack steel, which solves the problem of large grain size of Φ40-80mm bar steering rack steel, achieves the effect of refining the grains, and avoids the need for annealing process for steering rack steel due to coarse grains.

[0006] Technical solution: A rolling method for improving the grain size of a steering rack steel of the present invention is characterized in that it comprises the following steps:

[0007] 1) Before rolling, all water tanks are offline and roller cooling water pipes are closed to prevent water from splashing onto the steel surface during rolling, which may cause uneven cooling and local mixed crystals;

[0008] 2) The speed of the rough rolling mill is 0.6m / s, ensuring that the sizing temperature is above 980℃, and high temperature controlled rolling is carried out;

[0009] 3) The cooling bed lowers the insulation cover in advance and moves at 40s / step. The steering rack steel stays in the insulation cover for more than 20min. When the surface temperature of the steel drops to 500℃, the moving speed of the cooling bed is manually controlled to move the steel out of the insulation cover to play the role of isothermal normalizing, ensuring that AlN is fully dispersed in the steel and plays the role of pinning grain boundaries to refine the grains.

[0010] Wherein, the diameter of the steel used for the steering gear rack is 40mm-80mm.

[0011] Among them, during the rolling, a 320mm×480mm cross-section billet smelted in an electric furnace is heated and kept at 1240°C for billet opening and rolling into a 180×180 billet, and then heated and rolled into steel for steering racks to produce Φ40mm-80mm round steel.

[0012] During the rolling, a heating furnace, high-pressure water descaling, 23 horizontal and vertical alternating short stress line rolling mills, 4 three-roller KOCKS rolling mills, 5 flying shears and 7 water tanks for online controlled cooling are configured online, and a heat preservation cover is provided above the cooling bed.

[0013] Wherein, the steering gear rack steel includes the following components in percentage by mass: C: 0.38%-0.43%, Mn: 0.62%-0.81%, Si: 0.17%-0.35%, Mo: 0.16%-0.25%, Cr: 0.95%-1.12%, Ni≤0.15%, Cu≤0.20%, P+S+Al+N<0.18%, Fe balance.

[0014] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: During the production process, the present invention can ensure the dispersion and precipitation of AlN in the steel by controlling the rolling and post-rolling cooling method, which plays a role in pinning the grain boundaries to achieve the effect of grain refinement, thereby avoiding the need for annealing process of steering rack steel due to coarse grains.

[0015] According to detection, the present invention controls the rolling temperature and the cooling temperature, the austenite grain size is in the range of 6-8, there is no mixed crystal phenomenon, the annealing process is saved, and the delivery rate is improved. DETAILED DESCRIPTION

[0016] The technical solution of the present invention is further described below in conjunction with specific implementation methods.

[0017] The rolling method for improving the grain size of the steel for the steering rack of the present invention comprises the following steps:

[0018] 1) Before rolling, all water tanks are offline and the roller cooling water pipes are closed to prevent water from splashing onto the steel surface during rolling, causing uneven cooling and local mixed crystals.

[0019] 2) The speed of the final stand of rough rolling is 0.6 m / s to reduce the temperature loss during rolling, ensure that the sizing temperature is above 980 °C, and perform high temperature controlled rolling to ensure that AlN is completely dissolved during controlled rolling.

[0020] 3) The cooling bed lowers the insulation cover in advance and moves at 40s / step. The steering rack steel stays in the insulation cover for more than 20min. When the surface temperature of the steel drops to 500℃, the moving speed of the cooling bed is manually controlled to move the steel out of the insulation cover to play the role of isothermal normalizing, ensuring that AlN is fully dispersed in the steel and plays the role of pinning grain boundaries to refine the grains.

[0021] The present invention adopts 320mm×480mm cross-section billet smelted in an electric furnace, and heats and insulates to 1240℃ to open and roll into 180×180 billet, and then heats and rolls into steel for steering rack to produce Φ40mm-80mm round steel. The online configuration includes a heating furnace, high-pressure water descaling, 23 horizontal and vertical alternating short stress line rolling mills, 4 three-roller KOCKS rolling mills, 5 flying shears and 7 water tanks for online controlled cooling, and a heat preservation cover is provided above the cooling bed.

[0022] The steering gear rack steel includes the following components in percentage by mass: C: 0.38%-0.43%, Mn: 0.62%-0.81%, Si: 0.17%-0.35%, Mo: 0.16%-0.25%, Cr: 0.95%-1.12%, Ni≤0.15%, Cu≤0.20%, P+S+Al+N<0.18%, Fe balance.

[0023] According to detection, the present invention controls the rolling temperature and the cooling temperature, the austenite grain size is in the range of 6-8, there is no mixed crystal phenomenon, the annealing process is saved, and the delivery rate is improved.

Claims

1. A rolling method for improving the grain size of steel for steering rack, characterized in that: The steps include: 1) Before rolling, all water tanks are offline and roller cooling water pipes are closed to prevent water from splashing onto the steel surface during rolling, which may cause uneven cooling and local mixed crystals; 2) The speed of the rough rolling mill is 0.6m / s, ensuring that the sizing temperature is above 980℃, and high temperature controlled rolling is carried out; 3) The cooling bed lowers the insulation cover in advance and moves at 40s / step. The steering rack steel stays in the insulation cover for more than 20min. When the surface temperature of the steel drops to 500℃, the moving speed of the cooling bed is manually controlled to move the steel out of the insulation cover to play the role of isothermal normalizing, ensuring that AlN is fully dispersed in the steel and plays the role of pinning grain boundaries to refine the grains.

2. The rolling method for improving the grain size of the steering rack steel according to claim 1, characterized in that: The diameter of the steel used for the steering gear rack is 40mm-80mm.

3. The rolling method for improving the grain size of the steering rack steel according to claim 2, characterized in that: During the rolling, a 320mm×480mm cross-section billet smelted in an electric furnace is heated and kept at 1240°C for billet opening and rolling into a 180×180 billet, which is then heated and rolled into steel for a steering rack to produce Φ40mm-80mm round steel.

4. The rolling method for improving the grain size of the steering rack steel according to claim 3, characterized in that: During the rolling, a heating furnace, high-pressure water descaling, 23 horizontal and vertical alternating short stress line rolling mills, 4 three-roller KOCKS rolling mills, 5 flying shears and 7 water tanks for online controlled cooling are configured online, and a heat preservation cover is provided above the cooling bed.

5. The rolling method for improving the grain size of the steering rack steel according to claim 1, characterized in that: The steering rack steel comprises the following components in percentage by mass: C: 0.38%-0.43%, Mn: 0.62%-0.81%, Si: 0.17%-0.35%, Mo: 0.16%-0.25%, Cr: 0.95%-1.12%, Ni≤0.15%, Cu≤0.20%, P+S+Al+N<0.18%, and Fe balance.

Citation Information

Patent Citations

  • High-carbon, sulfur-containing and easy-cutting type ferritic stainless steel and production method thereof

    CN106591742A

  • Manufacturing method of medium-carbon CrMo steel wire rod free of annealing and drawing

    CN110004376A

  • Steel for 12.9-grade large-sized and high-toughness wind power bolt and production method

    CN111676423A

  • High-strength steel for corrosion-resistant fastener for ocean wind power and production method

    CN111945063A

  • Method for improving bending degree of mining chain steel bar

    CN118455279A