High-entropy rare earth-based hexaboride ceramic material as well as preparation method and application thereof
Through the preparation of high-entropy rare earth-based hexaboride ceramic materials, the problem of insufficient solar energy absorption and infrared emissivity of existing solar system materials is solved, efficient solar energy absorption and storage is achieved, and the stability and efficiency of the system are improved.
Patent Information
- Application Number
- CN202410402685.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-03
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-04-03
AI Technical Summary
The existing solid particulate materials of concentrated solar systems such as alumina and cordierite have poor performance in solar energy absorption and infrared emissivity, which limits the application of solar thermal power generation technology.
High-entropy rare earth-based hexaboride materials are prepared by solid phase reaction method, and the concept of high entropy is introduced to obtain high-entropy rare earth-based hexaboride ceramic materials with high solar energy absorption and high infrared emissivity, which are used in concentrated solar energy systems.
It realizes efficient solar energy absorption and infrared emission, improves the efficiency and stability of the light-concentrating solar system, reduces system complexity, and enhances commercial competitiveness.
Smart Images

Figure CN119059824A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of solar energy absorption materials and infrared radiation materials, and relates to a high-entropy rare earth-based hexaboride ceramic material, a preparation method and application thereof, and specifically relates to a high-entropy rare earth-based hexaboride with high solar energy absorption rate and high infrared emissivity, a preparation method and application thereof. Background Art
[0002] In recent years, due to the depletion of fossil fuels, the increase of greenhouse effect, climate change and energy security issues in countries with small fossil energy reserves, renewable energy has received widespread attention. Solar power generation is becoming increasingly dominant, and the global power system is gradually transforming towards low-carbon. Concentrated solar power (CPS) system is a power generation method that collects solar energy and directly uses it as a heat source for power cycle. However, the alternation of day and night and weather changes greatly limit the application of solar thermal power generation technology. The combination of CPS technology and thermal energy storage (TES) technology is an attractive solution. At the same time, direct solar absorption and heat storage based on solid particles have received increasing attention in high-temperature concentrated solar power generation. CPS system solid particles not only need to have excellent optical properties, thermophysical properties, stability and other characteristics, but also need to have high solar absorptivity, high infrared emissivity, high specific heat and good stability. At present, the most studied CPS system solid particles such as alumina, cordierite, mullite, black silicon carbide, quartz and ceramic sintered bauxite particles are used as heat transfer fluid (HFT) and TES materials. Rare earth lanthanum hexaboride was once found to be a potential material for use as a concentrated solar absorber, but its solar absorptivity and infrared emissivity are insufficient. Summary of the invention
[0003] In order to improve the above technical problems, the present invention provides a high-entropy rare earth-based hexaboride with high solar absorptivity and high infrared emissivity, and a preparation method and application thereof. The present invention introduces the concept of high entropy through a solid-phase reaction method to obtain a high-entropy rare earth-based hexaboride material that can be used for solar absorption and infrared radiation.
[0004] In order to achieve the above object, the present invention adopts the following technical solution:
[0005] The present invention provides a high entropy boride material having the following general chemical formula: RE(AE) x B6, wherein: RE is selected from at least three of the rare earth elements La, Nd, Sm, Eu, Gd, Dy, Ho, Yb, Tm, Lu, Sc and Y, AE is selected from one of the alkaline earth elements Be, Mg, Ca, Sr, Ba and Ra, x is 0.2 to 0.5, exemplarily, x = 0.2, 0.25, 0.3, 0.4 or x = 0.5.
[0006] According to an embodiment of the present invention, the high entropy boride material is a high entropy rare earth-based hexaboride ceramic material, which has high solar energy absorptivity and high infrared emissivity.
[0007] Preferably, the average solar energy absorption rate of the high entropy boride material is 82-88%, exemplified by 82.68%, 85.61%, and 87.75%.
[0008] Preferably, the near-infrared emissivity of the high-entropy boride material is 80-90%, exemplified by 83.63%, 85.23%, and 88.76%.
[0009] Preferably, the mid- and far-infrared emissivity of the high-entropy boride material is 90-95%, exemplified by 91.12%, 93.01%, and 94.36%.
[0010] According to an embodiment of the present invention, the particle size of the high entropy boride material is D 90 ≤2.5μm.
[0011] According to an embodiment of the present invention, the high entropy boride material is La 0.25 Sm 0.25 Ce 0.25 Eu 0.25 B6, La 0.25 Sm 0.25 Ce 0.25 Ba 0.25 B6 and La 0.2 Sm 0.2 Ce 0.2 Eu 0.2 Ba 0.2 At least one of B6.
[0012] Preferably, the high entropy rare earth-based hexaboride ceramic material is a typical CsCl-type cubic structure.
[0013] According to an embodiment of the present invention, the high entropy boride material is prepared from raw materials including B4C, RE2O3 and AECO3 by a solid phase reaction method, wherein RE and AE have the definitions and selections as described above.
[0014] The present invention also provides a method for preparing the high entropy boride material, comprising: mixing B4C with RE2O3 and AECO3, and preparing the high entropy boride material by a solid phase reaction method. In the present invention, the chemical reaction process of obtaining the high entropy boride material by reacting B4C with RE2O3 and AECO3 is as follows:
[0015] 4RE2O3+7B4C=4REBO3+REB6+7C (1)
[0016] 4REBO3+7C+5B4C=4REB6+12CO (2)
[0017] (1)+(2):4RE2O3+12B4C=5REB6+12CO
[0018] According to an embodiment of the present invention, the solid phase reaction further comprises grinding the mixed raw materials. For example, the grinding time may be more than 0.5 h.
[0019] According to an embodiment of the present invention, the preparation method further comprises pressing the ground mixed raw materials. For example, the pressing pressure is 3-5MPa, exemplified by 3MPa, 4MPa, 4.5MPa, 5MPa; the pressing time is 10-60s, exemplified by 20s, 30s, 40s; the pressing method can be dry pressing.
[0020] According to an embodiment of the present invention, the sintering temperature of the solid phase reaction is 1500-1700°C, exemplified by 1500°C, 1600°C, and 1700°C; the sintering time of the solid phase reaction is 1-4h, exemplified by 2h, 2.5h, and 3h; the heating rate of the solid phase reaction is 1-10°C / min, exemplified by 5°C / min.
[0021] According to an embodiment of the present invention, the preparation method further comprises crushing, grinding and screening the product after the solid phase reaction to obtain a powder of high entropy ceramic. Preferably, the screening uses a standard sieve of 200 to 400 meshes.
[0022] According to an embodiment of the present invention, the molar ratio of the total molar amount of RE (rare earth element) and AE (alkaline earth element) to boron carbide is 2:(3-3.45), and exemplarily is 2:3.3.
[0023] The present invention also provides the use of the high entropy boride material in solar energy absorption and storage, preferably in a concentrated solar energy system, for example, for converting solar energy into heat energy and then into electrical energy.
[0024] The present invention also provides a concentrated solar power (CPS) system, which contains the high entropy boride material.
[0025] Beneficial effects of the present invention:
[0026] In order to achieve the integration of heat absorption and energy storage and to achieve service at higher temperatures, a high entropy method is used to prepare high entropy hexaboride ceramics to improve their solar absorptivity and infrared emissivity. High entropy ceramics have high entropy effect, hysteresis diffusion effect, lattice distortion effect and "cocktail" effect, which make high entropy borides have slower grain growth rate, better high temperature stability and better infrared emission performance.
[0027] Applying high entropy ceramics to concentrated solar power systems can achieve high solar absorption rates of 0.28 to 2.5 μm and high infrared emissivity of 2.5 to 25 μm, creating new materials that combine heat absorption and energy storage, thereby reducing the complexity of solar power generation systems, achieving high-efficiency power cycles, and improving the commercial competitiveness of CPS systems. In view of this:
[0028] (1) The preparation process of the high-entropy rare earth-based hexaboride of the present invention is simple, and the synthesized high-entropy ceramic powder has small grains (D 90 ≤2.5μm) and evenly distributed.
[0029] (2) The high entropy rare earth hexaboride of the present invention has good optical properties, namely high solar absorptivity and high infrared emissivity as well as good high-temperature thermal stability due to lattice distortion and hysteresis diffusion effects.
[0030] (3) The present invention adopts a high-temperature solid-phase method to prepare high-entropy rare earth-based hexaboride ceramic materials. The preparation process is simple and the operating conditions are controllable, which is easy to promote and apply in industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The present invention is a process flow chart for preparing the high entropy rare earth-based hexaboride ceramic powder with high solar water absorption and high infrared emissivity.
[0032] Figure 2 For the (La synthesized in Examples 1-3 of the present invention 0.25 Sm 0.25 Ce 0.25 Eu 0.25 B6)、(La 0.25 Sm 0.25 Ce 0.25 Ba 0.25 B6), and (La 0.2 Sm 0.2 Ce 0.2 Eu 0.2 Ba 0.2 B6) XRD pattern of high entropy rare earth hexaboride ceramic powder.
[0033] Figure 3 Where a, b, and c are respectively (La0.25 Sm 0.25 Ce 0.25 Eu 0.25 B6)、(La 0.25 Sm 0.25 Ce 0.25 Ba 0.25 B6) and (La 0.2 Sm 0.2 Ce 0.2 Eu 0.2 Ba 0.2 B6) EDS element distribution diagram of high entropy ceramics.
[0034] Figure 4 (La synthesized in Examples 1-3 of the present invention 0.25 Sm 0.25 Ce 0.25 Eu 0.25 B6)、(La 0.25 Sm 0.25 Ce 0.25 Ba 0.25 B6) and (La 0.2 Sm 0.2 Ce 0.2 Eu 0.2 Ba 0.2 B6) UV-visible-near-infrared reflectance spectrum of high-entropy ceramics.
[0035] Figure 5 is the ((La synthesized in Examples 1-3 of the present invention 0.25 Sm 0.25 Ce 0.25 Eu 0.25 B6)、(La 0.25 Sm 0.25 Ce 0.25 Ba 0.25 B6) and (La 0.2 Sm 0.2 Ce 0.2 Eu 0.2 Ba 0.2 B6) Bar graph of the average solar absorptivity in the near-infrared band and the mid- and far-infrared emissivity of high-entropy ceramics. DETAILED DESCRIPTION
[0036] The technical solutions in the embodiments of the present invention will be described clearly and completely below. It should be understood that the following embodiments are only exemplary illustrations and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the invention are included in the scope that the present invention is intended to protect.
[0037] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0038] Example 1
[0039] like Figure 1 As shown, a high entropy rare earth-based hexaboride ceramic material with high solar absorptivity and high infrared emissivity, and its preparation method is as follows:
[0040] (1) Weigh 0.025 mol of La2O3 (lanthanum oxide), 0.025 mol of Sm2O3 (samarium oxide), 0.025 mol of Eu2O3 (europium oxide) powder, 0.05 mol of CeO2 (cerium oxide) and 0.33 mol of B4C powder respectively, transfer all the raw materials into an agate mortar, and grind for more than 40 minutes until they are completely mixed;
[0041] (2) The mixture powder ground evenly in step (1) is tableted, using a tableting mold with a diameter of 15 mm, setting the tableting machine pressure to 4 MPa, and pressing time to 40 s to obtain embryo A;
[0042] (3) The embryo A obtained in step (2) was synthesized in an argon atmosphere under normal pressure, with a synthesis temperature of 1600° C., a heating rate of 5° C. / min, and a holding time of 2 h to obtain a high entropy ceramic La 0.25 Sm 0.25 Ce 0.25 Eu 0.25 B6;
[0043] (4) The high entropy ceramic synthesized in step (3) is crushed, ground and sieved (400 mesh) to obtain a high entropy ceramic powder.
[0044] like Figure 2 As shown, the high entropy rare earth hexaboride ceramic material La prepared in this embodiment 0.25 Sm 0.25 Ce 0.25 Eu 0.25 The XRD pattern of B6 is basically consistent with the standard card of single phase in the ICDD database, and there is no impurity peak, which shows that the high entropy rare earth hexaboride prepared in this example is a single-phase solid solution of CsCl type body-centered cubic structure.
[0045] like Figure 3 As shown, the high entropy rare earth hexaboride ceramic material La prepared in this embodiment 0.25 Sm 0.25 Ce 0.25 Eu 0.25EDS element distribution diagram of B6. It can be seen from the figure that the high entropy rare earth-based hexaboride ceramic material La prepared in this embodiment 0.25 Sm 0.25 Ce 0.25 Eu 0.25 The rare earth elements in B6 are evenly distributed without segregation.
[0046] like Figure 4 As shown, the high entropy rare earth hexaboride ceramic material La prepared in this embodiment 0.25 Sm 0.25 Ce 0.25 Eu 0.25 The reflectivity spectrum of B6 at 0.28-2.5 μm, and its solar absorptivity is calculated by the following formula:
[0047]
[0048] Where: S(λ) is the solar emission spectrum, integrated between λ = 0.28 μm and λ = 2.5 μm. It is found that its average solar absorption rate is as high as 82.68%, which is nearly half higher than that of single-phase LaB6 (54.05%).
[0049] like Figure 5 As shown, the high entropy rare earth hexaboride ceramic material La prepared in this embodiment 0.25 Sm 0.25 Ce 0.25 Eu 0.25 The average infrared emissivity of B6 in the near-infrared and far-infrared, that is, the solar energy absorption rate, is significantly enhanced compared with single-phase LaB6, and the mid-infrared and far-infrared emissivity is also slightly enhanced, reaching 83.63% and 91.12% respectively.
[0050] Example 2
[0051] like Figure 1 As shown, a high entropy rare earth-based hexaboride ceramic material with high solar absorptivity and high infrared emissivity, and its preparation method is as follows:
[0052] (1) Weigh 0.025 mol of La2O3 (lanthanum oxide), 0.025 mol of Sm2O3 (samarium oxide), 0.05 mol of CeO2 (cerium oxide) and 0.05 mol of BaCO3 (barium carbonate), add 0.33 mol of B4C powder, transfer all the raw materials into an agate mortar, and grind for more than 45 minutes until they are completely mixed;
[0053] (2) The mixture powder ground evenly in step (1) is tableted, using a tableting mold with a diameter of 15 mm, setting the tableting machine pressure to 4.5 MPa, and pressing time to 30 s to obtain embryo B;
[0054] (3) The embryo B obtained in step (2) was synthesized in an argon atmosphere under normal pressure, with a synthesis temperature of 1600° C., a heating rate of 5° C. / min, and a holding time of 2.5 h to obtain a high entropy ceramic La 0.25 Sm 0.25 Ce 0.25 Ba 0.25 B6;
[0055] (4) The high entropy ceramic synthesized in step (3) is crushed, ground and sieved (400 mesh) to obtain a high entropy ceramic powder.
[0056] like Figure 2 As shown, the high entropy rare earth-alkaline earth hexaboride ceramic material La prepared in this embodiment 0.25 Sm 0.25 Ce 0.25 Ba 0.25 The XRD pattern of B6 is basically consistent with the standard card of single phase in the ICDD database, and there is no impurity peak, which shows that the high entropy rare earth hexaboride prepared in this example is a single-phase solid solution of CsCl type body-centered cubic structure.
[0057] like Figure 3 As shown, the high entropy rare earth hexaboride ceramic material La prepared in this embodiment 0.25 Sm 0.25 Ce 0.25 Ba 0.25 EDS element distribution diagram of B6. It can be seen from the figure that the high entropy rare earth-based hexaboride ceramic material La prepared in this embodiment 0.25 Sm 0.25 Ce 0.25 Ba 0.25 The rare earth elements in B6 are evenly distributed without segregation.
[0058] like Figure 4 As shown, the high entropy rare earth hexaboride ceramic material La prepared in this embodiment 0.25 Sm 0.25 Ce 0.25 Ba 0.25 The reflectivity spectrum of B6 at 0.28-2.5 μm was obtained, and its solar absorptivity was calculated in the same way as in Example 1, and it was found that its average solar absorptivity was as high as 85.61%.
[0059] like Figure 5 As shown, the high entropy rare earth hexaboride ceramic material La prepared in this embodiment 0.25 Sm 0.25 Ce 0.25 Ba 0.25The average infrared emissivity of B6 in the near-infrared and far-infrared, that is, the solar energy absorption rate, is significantly enhanced compared with single-phase LaB6, and the mid-infrared and far-infrared emissivity are also slightly enhanced, reaching 85.23% and 94.36% respectively.
[0060] Example 3
[0061] like Figure 1 As shown, a high entropy rare earth-based hexaboride ceramic material with high solar absorptivity and high infrared emissivity, and its preparation method is as follows:
[0062] (1) Weigh 0.02 mol of La2O3 (lanthanum oxide), 0.02 mol of Sm2O3 (samarium oxide), 0.02 mol of Eu2O3 (europium oxide) powder, 0.04 mol of CeO2 (cerium oxide), 0.04 mol of BaCO3 and 0.33 mol of B4C powder respectively, transfer all the raw materials into an agate mortar, and grind for more than 50 min until they are completely mixed;
[0063] (2) tabletting the uniformly ground mixture powder of step (1), using an edible tabletting die with a diameter of 15 mm, setting the tabletting machine pressure to 5 MPa, and pressing for 20 s to obtain embryo C;
[0064] (3) The embryo C obtained in step (2) was synthesized in an argon atmosphere under normal pressure, with a synthesis temperature of 1600° C., a heating rate of 5° C. / min, and a holding time of 3 h to obtain a high entropy ceramic La 0.2 Sm 0.2 Ce 0.2 Eu 0.2 Ba 0.2 B6;
[0065] (4) The high entropy ceramic synthesized in step (3) is crushed, ground and sieved (400 mesh) to obtain a high entropy ceramic powder.
[0066] like Figure 2 As shown, the rare earth-based high entropy hexaboride ceramic material La prepared in this embodiment 0.2 Sm 0.2 Ce 0.2 Eu 0.2 Ba 0.2 The XRD pattern of B6 is basically consistent with the standard card of single phase in the ICDD database, and there is no impurity peak, which shows that the high entropy rare earth hexaboride prepared in this example is a single-phase solid solution of CsCl type body-centered cubic structure.
[0067] like Figure 3 As shown, the rare earth-based high entropy hexaboride ceramic material La prepared in this embodiment 0.2 Sm0.2 Ce 0.2 Eu 0.2 Ba 0.2 EDS element distribution diagram of B6. It can be seen from the figure that the high entropy rare earth-based hexaboride ceramic material La prepared in this embodiment 0.2 Sm 0.2 Ce 0.2 Eu 0.2 Ba 0.2 The rare earth elements in B6 are evenly distributed without segregation.
[0068] like Figure 4 As shown, the high entropy rare earth hexaboride ceramic material La prepared in this embodiment 0.2 Sm 0.2 Ce 0.2 Eu 0.2 Ba 0.2 The reflectivity spectrum of B6 at 0.28-2.5 μm was calculated using the same method as in Example 1, and it was found that its average solar absorptivity was as high as 87.75%.
[0069] like Figure 5 As shown, the high entropy rare earth hexaboride ceramic material La prepared in this embodiment 0.2 Sm 0.2 Ce 0.2 Eu 0.2 Ba 0.2 The average infrared emissivity of B6 in the near-infrared and far-infrared, that is, the solar energy absorption rate, is significantly enhanced compared with single-phase LaB6, and the mid-infrared and far-infrared emissivity is also slightly enhanced, reaching 88.76% and 93.01% respectively.
[0070] The above is an exemplary description of the embodiments of the present invention. However, the protection scope of the present invention is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A high entropy boride material, characterized in that: It has the following general chemical formula: RE(AE) x B6, wherein: RE is selected from at least three of the rare earth elements La, Nd, Sm, Eu, Gd, Dy, Ho, Yb, Tm, Lu, Sc and Y, AE is selected from one of the alkaline earth elements Be, Mg, Ca, Sr, Ba and Ra, and x is 0.2 to 0.
5.
2. The high entropy boride material according to claim 1, characterized in that The average solar energy absorption rate of the high entropy boride material is 82-88%. Preferably, the near infrared emissivity of the high entropy boride material is 80-90%. Preferably, the mid- and far-infrared emissivity of the high-entropy boride material is 90-95%. Preferably, the particle size of the high entropy boride material is D 90 ≤2.5μm.
3. The high entropy boride material according to claim 1, characterized in that: The high entropy boride material is La 0.25 Sm 0.25 Ce 0.25 Eu 0.25 B6, La 0.25 Sm 0.25 Ce 0.25 Ba 0.25 B6 and La 0.2 Sm 0.2 Ce 0.2 Eu 0.2 Ba 0.2 At least one of B6.
4. The high entropy boride material according to any one of claims 1 to 3, characterized in that: The high entropy boride material is prepared from raw materials including B4C, RE2O3 and AECO3 through a solid phase reaction method.
5. The method for preparing the high entropy boride material according to any one of claims 1 to 4, characterized in that: The preparation method comprises mixing B4C, RE2O3 and AECO3, and then preparing the high entropy boride material through a solid phase reaction method.
6. The preparation method according to claim 5, characterized in that: The method further comprises grinding the mixed raw materials before the solid phase reaction. Preferably, the preparation method further comprises pressing the ground mixed raw materials into a shape. Preferably, the pressing pressure is 3-5 MPa, and the pressing time is 10-60 s.
7. The preparation method according to claim 5 or 6, characterized in that: The sintering temperature of the solid phase reaction is 1400-1800° C.; the sintering time of the solid phase reaction is 1-4 hours.
8. The preparation method according to any one of claims 5 to 7, characterized in that: The molar ratio of the total molar amount of RE (rare earth element) and AE (alkaline earth element) to boron carbide is 2:(3-3.45).
9. Use of the high entropy boride material according to any one of claims 1 to 4 in solar energy absorption and storage, preferably in a concentrated solar energy system, for example, for converting solar energy into heat energy and then into electrical energy.
10. A concentrated solar energy system, characterized in that: It contains the high entropy boride material according to any one of claims 1 to 4.
Citation Information
Patent Citations
High-entropy transition-rare earth metal diboride ceramic material and preparation method thereof
CN114507074A
High-entropy rare earth co-doped nano low-heat-transfer powder material and preparation method thereof
CN114524440A
Medium-high-entropy ceramic material as well as preparation method and application thereof
CN114560699A
Metal-based composite material, and preparation method therefor and use thereof
WO2023174159A1
Cited By
High-temperature self-lubricating high-entropy rare earth boride ceramic material and preparation method thereof
CN119684008A
A high-temperature self-lubricating high-entropy rare earth boride ceramic material and its preparation method
CN119684008B