Delayed mechanical distribution imaging material based on thermal excitation, preparation method and application

By introducing Dy3+ and polydimethylsiloxane composite into mechanical luminescent materials, a delayed mechanical distribution imaging material based on thermal excitation was prepared, which solved the problem of insufficient time-lapse luminescence and stress afterglow of mechanical luminescent materials, and realized mechanical storage and super long continuous luminescence under thermal excitation, suitable for a variety of application fields.

CN119060730AInactive Publication Date: 2024-12-03SHAANXI MUGUANG GEZHI TECHNOLOGY CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411159781.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing mechanical luminescent materials exhibit instantaneous luminescence, short life, and limited stress afterglow duration, limiting their use in mechanical visualization and applications.

Method used

Using a delayed mechanical distribution imaging material based on thermal excitation, the chemical formula is M9-xN(PO4)7:xR, Dy3+ is introduced as the luminescence center, and prepared by high-temperature sintering and grinding, combined with polydimethylsiloxane (PDMS) Combination, achieving super long continuous luminescence under the afterglow.

Benefits of technology

It realizes ultra-long continuous luminescence under mechanical storage and thermal excitation conditions, can effectively record and visualize the mechanical distribution, and is suitable for precision component detection, road and bridge early warning, extends application time and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060730A_ABST
    Figure CN119060730A_ABST
Patent Text Reader

Abstract

The invention discloses a delayed mechanical distribution imaging material based on thermal excitation, a preparation method and application, the chemical general formula of the imaging material is M9-xN (PO4) 7: xDy < 3 + >, the prepared and formed imaging material is high in luminous intensity under mechanical stimulation, delayed mechanical distribution imaging based on thermal excitation stimulation after a force-induced afterglow phenomenon is finished can be achieved, and the imaging material has a good application prospect. According to the delayed mechanical distribution imaging material, quantitative visual delayed mechanical distribution imaging is achieved through force-induced afterglow under mechanical storage and continuous luminescence under the thermal excitation condition, thermal excitation continuous luminescence based on force-induced afterglow is achieved, and super-long visual information reading can be achieved; the method can be used for detection of blind areas in precision parts, mechanical distribution detection, visual early warning of highways and bridges and other fields, can effectively record the mechanical distribution condition in a delayed manner, and is not limited by time and space.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of luminescent materials, and in particular to a delayed mechanical distribution imaging material based on thermal excitation, a preparation method and an application thereof. Background Art

[0002] Luminescent materials refer to materials that can absorb energy and convert it into light radiation (non-equilibrium radiation). Such materials are widely used in many fields, such as lighting, display, information communication, medicine, etc. There are many ways for luminescent materials to emit light, the main types of which are photoluminescence, cathode ray luminescence, electroluminescence, thermoluminescence, photoluminescence, radioluminescence, etc. With the continuous emergence and mature application of new preparation technologies, the performance of luminescent materials will be further improved and optimized. This will provide a broader space and prospect for the application of luminescent materials in various fields.

[0003] Mechanoluminescence (ML) is a phenomenon in which light is emitted under mechanical stimulation such as fracture, friction, compression, abrasive force and stretching. ML directly bridges the gap between luminescence and mechanics, however, most current ML materials essentially exhibit transient luminescence with a short lifetime. Developing long-life ML, namely Pers-ML, is an effective way to overcome the shortcomings of ML transient luminescence. The persistent luminescence characteristics after mechanical stimulation can undoubtedly enable the display and visualization of mechanics for a period of time, which can be easily observed by the naked eye or an ordinary camera. Therefore, it has high convenience and practicality in applications related to mechanical visualization. However, only a small number of stress luminescent materials currently have the phenomenon of stress afterglow, and the duration of stress afterglow is usually limited. After the stress afterglow disappears, the material cannot be used again, which limits the application range of luminescent materials. Summary of the invention

[0004] In response to the above-mentioned problems, the present invention aims to provide a delayed mechanical distribution imaging material based on thermal excitation, a preparation method and an application. Under the conditions of mechanical storage and thermal excitation, the imaging material can achieve ultra-long continuous luminescence based on force-induced afterglow, and can be used for blind spot detection inside precision parts, mechanical distribution detection, visual early warning of highway bridges and other fields.

[0005] In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is as follows: a delayed mechanical distribution imaging material based on thermal excitation, the chemical formula of the imaging material is: 9-x N(PO4)7:xR, wherein the R element is an element that enables the imaging material to have secondary delayed mechanical distribution imaging under thermal excitation conditions.

[0006] Preferably, the R element is Dy 3+ .

[0007] Preferably, 0.01≦x≦0.3.

[0008] Preferably, M is selected from one or a combination of Ca, Sr, Ba, Mg and Zn; and N is selected from one or a combination of Al, Ga, Y, Gd, Lu and Sc.

[0009] The preparation method of the time-delayed mechanical distribution imaging material based on thermal excitation comprises the following steps:

[0010] S1, according to the chemical formula M 9-x The molar ratio of N(PO4)7:xR is as follows: the raw materials of each component are weighed respectively, and the R element is selected from the element that has the secondary time-delay mechanical distribution imaging of the imaging material under thermal excitation conditions, preferably Dy 3+ , 0.01≦x≦0.3; M is selected from one or a combination of Ca, Sr, Ba, Mg and Zn; N is selected from one or a combination of Al, Ga, Y, Gd, Lu and Sc.

[0011] S2, adding anhydrous ethanol to the raw materials of each component weighed in step S1, and then grinding thoroughly for 30 minutes to mix evenly;

[0012] S3, sintering the ground and mixed raw materials in S2 at high temperature in air, and then cooling to room temperature;

[0013] S4, grinding the product sintered at high temperature in step S3, and then molding the imaging material.

[0014] Application of a thermally stimulated delayed mechanical distribution imaging material, the chemical formula of the imaging material is: M 9-x N(PO4)7:xDy 3+ , 0.01≦x≦0.3; the temperature of thermal excitation is 400K-600K.

[0015] Preferably, the imaging material is used for at least one of the following: internal blind spot detection of precision parts, mechanical distribution detection, visual warning of highway bridges, electronic skin and wearable devices.

[0016] The beneficial effects of the present invention are:

[0017] 1. The thermally stimulated time-delayed mechanical distribution imaging material prepared by the present invention is prepared by introducing Dy 3+ As the luminescent center, the powder is compounded with PDMS to prepare the required composite elastomer, and under the conditions of mechanical storage and thermal stimulation, thermally stimulated continuous luminescence based on force-induced afterglow can be achieved. It can achieve ultra-long visual information reading, which can be used for internal blind spot detection of precision parts, mechanical distribution detection, visual warning of highway bridges and other fields, and can effectively delay the recording of mechanical distribution without being restricted by time and space.

[0018] 2. The time-delay mechanical distribution imaging composite device prepared by mixing the imaging material prepared by the present invention with polydimethylsiloxane (PDMS) has a high luminescence intensity under mechanical stimulation, and can realize time-delay mechanical distribution imaging under thermal excitation after the end of the force-induced afterglow phenomenon. The time-delay mechanical distribution imaging material realizes quantitative visualization time-delay mechanical distribution imaging through force-induced afterglow under mechanical storage and continuous luminescence under thermal excitation conditions.

[0019] 3. The imaging material provided by the present invention removes the doped rare earth ion Dy 3+ , and the other raw materials are cheap, which reduces the production and application cost of the imaging material and can be widely used. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a flow chart of the method for preparing the time-delayed mechanical distribution imaging material of the present invention.

[0021] Figure 2 The present invention is a flow chart of a method for preparing a composite elastic film of the imaging material.

[0022] Figure 3 It is the XRD spectrum of the delayed mechanical distribution imaging material of Example 1 of the present invention and the international crystal diffraction standard card JCPDS:48-1192.

[0023] Figure 4 The emission spectrum of the imaging material prepared in Example 1 of the present invention (under 351nm excitation, the emission spectrum shows four peaks at 481nm, 572nm, 670nm, and 755nm, corresponding to 4 F 9 / 2 → 6 H 15 / 2 , 4 F 9 / 2 → 6 H 13 / 2 , 4 F 9 / 2 → 6 H 11 / 2 , 4 F 9 / 2 → 6 H 9 / 2 + 6 F 9 / 2 transition).

[0024] Figure 5 The excitation spectrum of the imaging material prepared in Example 1 of the present invention (under 571nm monitoring, in the range of 275-420nm, respectively, belongs to Dy 3+ of 6 H 15 / 2 → 4 K13 / 2 , 6 H 15 / 2 → 4 K 15 / 2 , 6 H 15 / 2 → 6 P 7 / 2 + 4 M 15 / 2 ).

[0025] Figure 6 It is a comparative diagram of the stress luminescence intensity and stress afterglow duration of the imaging materials prepared in Examples 1-6 of the present invention under thermal excitation.

[0026] Figure 7 Dy doped in this invention 3+ With Dy doping 3+ Comparison diagram of brightness and afterglow duration under thermal excitation.

[0027] Figure 8 The figure is a graph showing the brightness of the imaging material of the present invention at different thermal actuation temperatures.

[0028] Fig. 9 This is the linear relationship between the strain and the luminescence intensity of the imaging material prepared in Example 1 of the present invention (the photon intensity is collected during the stretching process).

[0029] Fig.10 This is a graph showing the relationship between the luminescence time and luminescence intensity of the imaging material prepared in Example 1 of the present invention (the graph shows three stages. After the transient mechanoluminescence (ML) ends, there will be a stress afterglow phenomenon. After the stress afterglow disappears, the composite elastomer is heated to achieve the effect of brightness recovery, realize delayed mechanical distribution imaging under thermal excitation, and achieve a secondary imaging effect).

[0030] Fig.11 The changes in the thermal release curve of the imaging material prepared in Example 1 of the present invention when heated at different temperatures (the heating temperature is 100° C.-400° C., and the stored carriers can be discharged to the maximum extent within this temperature range, and the luminescence effect is better).

[0031] Fig.12 A composite elastic film prepared by mixing the imaging material prepared in Example 1 of the present invention with PDMS (a photo taken when the letter M was being written. After the stress afterglow completely disappeared, the writing track can be presented again after heating treatment).

[0032] Fig.13 This is a comparison chart of the thermal release curve test of the composite elastomer prepared by mixing the imaging material prepared in Example 1 of the present invention with PDMS before and after stretching. DETAILED DESCRIPTION

[0033] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0034] See attached Figures 1 to 13 The delayed mechanical distribution imaging material based on thermal actuation shown in the figure has a chemical formula of: M 9-x N(PO4)7:xR, wherein the R element is an element that enables the imaging material to have secondary delayed mechanical distribution imaging under thermal excitation conditions, and the element is preferably Dy 3+ Dy is a rare earth element and serves as the luminescence center of the molding material. Compared with currently known luminescent materials, it has mechanical distribution imaging under secondary delay (luminescence) under thermal excitation and is not affected by the short duration of stress afterglow, which makes the imaging material have a wide range of applications without restrictions.

[0035] The molar mass of Dy is: 0.01≦x≦0.3. Within this range, the imaging material has better luminous intensity and afterglow duration under thermal excitation, as shown in the following embodiments. The raw material of Dy is Dy2O3.

[0036] M is selected from one or a combination of Ca, Sr, Ba, Mg and Zn, such as Ca compound CaCO3; N is selected from one or a combination of Al, Ga, Y, Gd, Lu and Sc, such as Al compound Al2O3.

[0037] The present invention also provides a method for preparing a thermally stimulated time-delayed mechanical distribution imaging material, comprising the following steps:

[0038] S1, according to the chemical formula M 9-x N(PO4)7:xDy 3+ Weigh the raw materials of each component according to the molar stoichiometric ratio;

[0039] S2, adding anhydrous ethanol to the raw materials of each component weighed in step S1, and then grinding thoroughly for 30 minutes to mix evenly;

[0040] S3, placing the ground and mixed raw materials in S20 in a corundum crucible, and sintering them at high temperature in an air atmosphere with a resistance furnace, with a heating rate of 5°C / min; the high temperature holding temperature is 1100-1300°C, preferably 1200°C / min; the heat preservation time is 5-7h, preferably 6h; and then cooling to room temperature.

[0041] S4, grinding the product sintered at high temperature in step S3 to form the time-delayed mechanical distribution imaging material.

[0042] Example 1

[0043] According to the molar ratio, weigh CaCO3: 0.8636g, Al2O3: 0.0485g, H6NO4P: 0.7727g, Dy2O3: 0.0018g respectively; add anhydrous ethanol to the weighed raw materials in a mortar and grind and mix them evenly. Then put them into a corundum crucible and perform high-temperature solid-phase synthesis in an air atmosphere.

[0044] In this embodiment, the sintering temperature is 1100° C., the sintering time is 5 hours, and after sintering, the material is cooled to room temperature and then ground to obtain the time-delayed mechanical distribution imaging material.

[0045] Example 2

[0046] According to the molar ratio, CaCO3: 0.8616g, Al2O3: 0.0485g, H6NO4P: 0.7727g, Dy2O3: 0.0054g were weighed respectively; the weighed raw materials were added with anhydrous ethanol in a mortar and fully ground and mixed. Then, they were loaded into a corundum crucible, and then high-temperature solid-phase synthesis was carried out in an air atmosphere.

[0047] In this embodiment, the sintering temperature is 1150° C., the sintering time is 6 hours, and after sintering, the material is cooled to room temperature and then ground to obtain the time-delayed mechanical distribution imaging material.

[0048] Example 3

[0049] According to the molar ratio, CaCO3: 0.8595g, Al2O3: 0.0485g, H6NO4P: 0.7727g, Dy2O3: 0.0090g were weighed respectively; the weighed raw materials were added with anhydrous ethanol in a mortar and fully ground and mixed. The raw materials were loaded into a corundum crucible, and then high-temperature solid-phase synthesis was carried out in an air atmosphere.

[0050] In this embodiment, the sintering temperature is 1200° C., the sintering time is 6 hours, and after sintering, the material is cooled to room temperature and then ground to obtain the time-delayed mechanical distribution imaging material.

[0051] Example 4

[0052] According to the molar ratio, CaCO3: 0.8548g, Al2O3: 0.0485g, H6NO4P: 0.7727g, Dy2O3: 0.0177g were weighed respectively; the weighed raw materials were added with anhydrous ethanol in a mortar and fully ground and mixed. Then, they were loaded into a corundum crucible, and then high-temperature solid-phase synthesis was carried out in an air atmosphere.

[0053] In this embodiment, the sintering temperature is 1300° C., the sintering time is 6 hours, and then the material is cooled to room temperature and ground to obtain the time-delayed mechanical distribution imaging material.

[0054] Example 5

[0055] According to the molar ratio, CaCO3: 0.8454g, Al2O3: 0.0485g, H6NO4P: 0.7727g, Dy2O3: 0.0356g were weighed respectively; the weighed raw materials were added with anhydrous ethanol in a mortar and fully ground and mixed. Then, they were loaded into a corundum crucible, and then high-temperature solid-phase synthesis was carried out in an air atmosphere.

[0056] In this embodiment, the sintering temperature is 1200° C., the sintering time is 7 hours, and then the material is cooled to room temperature and ground to obtain the time-delayed mechanical distribution imaging material.

[0057] Example 6

[0058] According to the molar ratio, CaCO3: 0.8355g, Al2O3: 0.0485g, H6NO4P: 0.7727g, Dy2O3: 0.0531g were weighed respectively; the weighed raw materials were added with anhydrous ethanol in a mortar and fully ground and mixed. Then, they were loaded into a corundum crucible, and then high-temperature solid-phase synthesis was carried out in an air atmosphere.

[0059] The sintering temperature of this embodiment is 1300° C., the sintering time is 5 hours, and then the material is cooled to room temperature and ground to obtain the time-delayed mechanical distribution imaging material.

[0060] The testing method of the relevant data in the embodiment of the present invention is as follows:

[0061] X-ray diffraction (XRD) tests were performed on a D2PHASER desktop X-ray diffractometer produced by Bruker, Germany. Cu target Kα radiation (Kα: ). The working voltage is 30Kv and the current is 10mA. The test adopts step scanning with a step length of 0.02° and a scanning range of 5° to 80°.

[0062] ML spectra were captured by an OceanInstrument (QEpro) during stretching using a multi-mode mechanoluminescence detection system (QKLN-ML-2).

[0063] like Figure 6 As shown, the chemical formula of the phosphor is Ca9Al(PO4)7:Dy 3+ , pure phosphor was prepared by high temperature solid phase method, and Dy 3+ As the luminescent center, the powder is compounded with PDMS to prepare the desired composite elastomer, such as Figure 6The figure shows the stress luminescence intensity and stress afterglow duration comparison of the composite elastic body under mechanical stimulation of strain of 180%. The comparison results show that when 0.01≤x≤0.3, the composite elastic body has good stress luminescence intensity and stress afterglow duration. When x=0.1, the stress luminescence intensity and stress afterglow duration are better.

[0064] For this application, Dy 3+ As a luminescent element, it is different from Tb selected in the prior art. 3+ For example Figure 7 As shown, doped Ca9Al(PO4)7:Tb 3+ It also has stress afterglow characteristics, and selects the best doping concentration Ca9Al(PO4)7:0.4Tb 3+ With Ca9Al(PO4)7:0.1Dy 3+ Compare and dope Dy 3+ The stress afterglow duration and brightness under thermal excitation are better than those of doped Tb 3+ Therefore, the present invention adopts Dy 3+ Doped as a luminescent center.

[0065] On the basis of the above, the present invention also provides a method for preparing a composite device for time-delayed mechanical distribution imaging of strain based on the time-delayed mechanical distribution imaging material, that is, a method for preparing a composite elastic film of the time-delayed mechanical distribution imaging material (prepared in Example 1) and polydimethylsiloxane (PDMS), comprising the following steps:

[0066] S5, 2.5 g of PDMS (Sylgard 184, Dow Corning) based resin and 0.2 g of curing agent were thoroughly mixed in a Petri dish with a diameter of 60 mm;

[0067] S6. After adding 1.25 g of time-lapse mechanical distribution imaging material into the culture dish, place it on a magnetic stirrer at room temperature and continue stirring for 8 min.

[0068] S7, pour the mixture in step 60 into a rectangular mold (length, width, inner depth are 60mm, 30mm, 3mm respectively) and let it stand for 10 minutes to eliminate bubbles;

[0069] S8. Curing at 80° C. for 80 minutes to obtain a composite elastic film, i.e., a time-delayed mechanical distribution imaging composite device.

[0070] The application of the composite device for time-lapse mechanical distribution imaging prepared above, such as Figure 8As shown, the composite elastic film can display the mechanical distribution for a long time through stress afterglow after being subjected to external mechanical stimulation. At the same time, after the stress afterglow disappears, some carriers are stored in the traps. Through the auxiliary means of thermal stimulation, the stress distribution information can be reproduced with a time delay, and the force conditions can be accurately distinguished according to the brightness, and thus can be applied to the field of time-delay mechanical distribution imaging technology.

[0071] The time-lapse mechanical distribution imaging material realizes stress information brightness reproduction through thermal excitation, and its principle is as follows:

[0072] like Fig. 9 As shown, it is the photon number intensity under a single stretching cycle. Since different strains correspond to different luminescence intensities, the luminescence intensity gradually increases with the increase of deformation. After linear fitting, the fitting factor is 0.9839, which proves that the linear response is good and can be realized as a high-precision strain-delay mechanical distribution imaging based on mechanoluminescence.

[0073] like Fig.10 As shown in the figure, the thermal release curves of the composite elastomer under different heating temperatures after stretching were tested, and the formula The trap depth is calculated. Under heating at different temperatures, carriers in traps of different depths can be discharged, and the corresponding shallow trap strength gradually decreases.

[0074] like Fig.11 As shown, there are three stages, I is the stress luminescence stage, II is the stress afterglow stage, and III is the brightness recovery stage when the composite elastomer is heated. The heating process corresponds to the process of carriers being released outward. As the heating time gradually increases, the carriers are gradually emptied and the brightness gradually disappears.

[0075] like Fig.12 As shown, this is a stress luminescence photograph of the letter M when the composite elastomer is written. There will be a stress afterglow phenomenon after the stress luminescence ends. Heating the composite elastomer can restore the brightness and achieve a secondary imaging effect.

[0076] based on Figure 9-12 A rare earth ion is introduced into the ML material, and different luminescence intensities correspond to different strain levels. At the same time, the stress afterglow phenomenon exists, which can delay the recording of the force distribution. The stress afterglow of previous materials is usually short, and the present invention can achieve delayed mechanical distribution imaging based on mechanical storage. Mechanical storage is achieved by the change of the thermal release curve after stress stimulation. After stretching, the trap can be filled so that the carriers are stored in the trap, and then the carriers are released outward through thermal excitation to achieve brightness recovery, thereby realizing delayed mechanical distribution imaging.

[0077] Before this, the optical time-delay mechanical distribution imaging technology based on force-induced afterglow was short-lived and could not break the limitations of time and space. Compared with the short-term mechanical information storage of stress afterglow before, the present invention uses mechanical storage to store carriers in traps, and releases carriers outward through thermal excitation to achieve time-delay mechanical distribution imaging. The composite elastomer can be placed at room temperature for a long time, greatly improving the time-delay mechanical distribution imaging. In the blind spot non-destructive testing inside precision parts, it can effectively delay the recording of mechanical distribution, breaking the limitations of time and space.

[0078] Based on the above embodiments, the present invention also provides an application of a thermally stimulated time-delayed mechanical distribution imaging material, such as Figure 8 As shown, under mechanical stimulation, the traps are filled with carriers. After the stress afterglow disappears, some carriers still exist inside the traps, which are released relatively slowly under thermal disturbance at room temperature. Thermal stimulation can accelerate the release of carriers. After the afterglow brightness ends, the composite elastomer is subjected to heat treatment at different temperatures. It can be seen from the figure that as the temperature gradually increases, the brightness increases, the decay rate also accelerates, and the maintenance time becomes shorter.

[0079] like Fig.13 As shown in the figure, under mechanical stimulation, the traps are filled with carriers. After comparing the thermal release curves before and after the composite elastomer is stretched, it can be seen that there is an obvious thermal release peak. The position of the peak is determined by Gaussian fitting. The fitting results show that there are three traps. The storage capacity of the trap for carriers is closely related to the peak intensity. That is, the temperature corresponding to the horizontal axis represents the temperature at which the carriers can be released outward. At room temperature, room temperature thermal disturbance can cause the carriers in the shallow traps to be released slowly and continuously, and the carriers in the deep traps remain basically unchanged. Heating at the temperature corresponding to the thermal release peak can cause the carriers in the trap to be released quickly.

[0080] comprehensive Figure 8 , 13 , by comparing different heating temperatures, it is concluded that the thermal excitation heating temperature of the imaging material is 400K-600K.

[0081] Furthermore, the imaging material is used for at least one of the following: internal blind spot detection of precision parts, mechanical distribution detection, visual warning of highway bridges, electronic skin and wearable devices. Specifically, when detecting the internal blind spot of precision parts (the imaging material can be coated on the parts or prepared as a film and attached to the parts), afterglow appears when the parts are stressed, and the afterglow may be lost during the process of disassembling the parts and transferring them to the detection equipment. Therefore, the secondary delay of the parts can be achieved again through thermal excitation, and the parts can be monitored through the secondary delay without being restricted by time and space.

[0082] The principle of the present invention is that the delayed mechanical distribution imaging material based on thermal excitation disclosed in the present invention is to introduce a rare earth ion Dy into its matrix. 3+ , realizing ultra-long mechanical information storage. The delayed mechanical distribution imaging material is prepared into a composite device, and different luminescence intensities corresponding to different strain levels provide a basis for recording mechanical distribution. After the stress afterglow disappears, the carriers are released slowly under room temperature thermal disturbance. Thermal excitation means are used to accelerate the discharge of carriers, realizing thermal excitation delayed mechanical distribution imaging based on force-induced afterglow, which can effectively realize internal blind spot detection of precision parts, mechanical distribution detection, visual warning of highway bridges and other fields.

[0083] The above shows and describes the basic principle, main features and advantages of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention claimed.

Claims

1. A time-delayed mechanical distribution imaging material based on thermal excitation, characterized in that: The chemical formula of the imaging material is: 9-x N(PO4)7:xR, wherein the R element is an element that enables the imaging material to have secondary delayed mechanical distribution imaging under thermal excitation conditions.

2. The imaging material according to claim 1, characterized in that: The R element is Dy 3+ .

3. The imaging material according to claim 2, characterized in that: 0.01≦x≦0.3。 4. The imaging material according to claim 3, characterized in that: M is selected from one or a combination of Ca, Sr, Ba, Mg and Zn; N is selected from one or a combination of Al, Ga, Y, Gd, Lu and Sc.

5. A method for preparing a time-delayed mechanical distribution imaging material based on thermal excitation, characterized in that: The following steps are involved: S1, according to the chemical formula M 9-x The molar stoichiometric ratio in N(PO4)7:xR is to weigh the raw materials of each component respectively, and the R element is selected from the element that the imaging material has secondary time-delay mechanical distribution imaging under thermal excitation conditions; S2, adding anhydrous ethanol to the raw materials of each component weighed in step S1, and then grinding thoroughly for 30 minutes to mix evenly; S3, sintering the ground and mixed raw materials in S2 at high temperature in air, and then cooling to room temperature; S4, grinding the product sintered at high temperature in step S3, and then molding the imaging material.

6. The preparation method according to claim 5, characterized in that: The R element is Dy 3+ .

7. The preparation method according to claim 6, characterized in that: 0.01≦x≦0.3。 8. The preparation method according to claim 7, characterized in that: M is selected from one or a combination of Ca, Sr, Ba, Mg and Zn; N is selected from one or a combination of Al, Ga, Y, Gd, Lu and Sc.

9. Application of a thermally stimulated time-delayed mechanical distribution imaging material, characterized in that: The chemical formula of the imaging material is: 9-x N(PO4)7:xDy 3+ , 0.01≦x≦0.3; the temperature of thermal excitation is 400K-600K.

10. The use according to claim 9, characterized in that: The imaging material is used for at least one of the following: internal blind spot detection of precision parts, mechanical distribution detection, visual warning of highway bridges, electronic skin and wearable devices.

Citation Information

Cited By

  • Stress distribution delay imaging film and preparation method and application thereof

    CN120574424A

  • A stress distribution time-lapse imaging film and a preparation method and application thereof

    CN120574424B