Smelting method of low-nitrogen molten steel with high scrap ratio
Through converter dual process smelting and CO2 spraying coal powder technology, the problem of increased liquid nitrogen content in the high scrap steel ratio is solved, efficient nitrogen content control and scrap steel ratio improvement are achieved, and environmental protection performance of the steelmaking process is improved.
Patent Information
- Application Number
- CN202411198781.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-29
AI Technical Summary
In the traditional long blast furnace + converter process, after increasing the scrap steel ratio, the liquid nitrogen content of the steel increases significantly and fluctuates greatly, making it difficult to control, affecting the efficiency and environmental performance of the steelmaking process.
The converter double-process smelting steel is used to smelter the steel, and the first scrap steel is added through the first converter and CO2 is used as carrier gas to spray coal powder. After carbonization is increased, the semi-steel liquid is entered into the second converter and the second scrap steel smelting, and in the second converter Continue to use CO2 as carrier gas to spray coal powder to reduce the nitrogen content of the steel liquid.
The liquid nitrogen content of the steel is significantly reduced on the basis of high scrap steel ratio, which improves the smelting efficiency and nitrogen removal effect, better kinetic conditions, lower the O content of the converter end point and the slag T.Fe, and the scrap steel ratio can be increased to 35%. ~75%, liquid nitrogen content of steel is ≤0.0018%.
Smart Images

Figure CN119061227A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of converter steelmaking, and in particular to a method for smelting molten steel with a high scrap steel ratio and low nitrogen content. Background Art
[0002] In the traditional "blast furnace + converter" long process, more than 80% of carbon emissions come from the pre-iron process. Therefore, increasing the scrap steel ratio and reducing the molten iron ratio in steelmaking production will be one of the main measures to reduce carbon emissions in the future.
[0003] At present, the measures to increase the scrap ratio mainly include improving efficiency and reducing temperature drop, increasing the temperature of molten iron entering the furnace, and adding heat supplement to the converter. After the scrap ratio of the converter is increased, the nitrogen content increases significantly and the nitrogen content fluctuates greatly. The main reasons are as follows: the molten iron ratio is reduced, the total amount of carbon-oxygen reaction in the converter is reduced, the amount of bubbles in the carbon-oxygen reaction is reduced, and the denitrification is more difficult; the scrap steel itself has a high nitrogen content, which increases the total amount of nitrogen brought in; the sources and types of scrap steel are many, and the quality is difficult to control, which causes large fluctuations in nitrogen. Therefore, reducing the nitrogen content of molten steel on the basis of ensuring a high scrap ratio during smelting is a technical problem that needs to be solved urgently. Summary of the invention
[0004] The present application provides a smelting method for molten steel with a high scrap steel ratio and low nitrogen content, so as to solve the technical problem in the prior art that it is difficult to reduce the nitrogen content of molten steel while ensuring a high scrap steel ratio during smelting.
[0005] The present application provides a smelting method of low-nitrogen molten steel with a high scrap steel ratio, the method comprising:
[0006] Performing a first converter smelting on the molten iron and the first scrap steel to obtain a first semi-steel liquid;
[0007] Carburizing the first semi-steel molten steel to obtain a second semi-steel molten steel; and
[0008] The second semi-steel molten steel and the second scrap steel are subjected to a second converter smelting, and pulverized coal is injected using CO2 as a carrier gas to reduce the nitrogen content of the molten steel, thereby obtaining a converter molten steel.
[0009] Optionally, the amount of the first scrap steel added is 250 Kg / t·steel to 450 Kg / t·steel.
[0010] Optionally, the amount of the second scrap steel added is 100 Kg / t·steel to 300 Kg / t·steel.
[0011] Optionally, the first converter smelting time is t1, t1 is 10min to 15min; wherein,
[0012] When the first converter smelting time is less than 5 minutes, pure CO2 is blown from the converter bottom;
[0013] When the smelting time of the first converter is 5min~t1, CO2 is used as a carrier gas to inject pulverized coal at the bottom of the converter.
[0014] Optionally, for a converter with a tonnage of 300t, the flow rate of CO2 is 2500Nm 3 / h~4500Nm 3 / h, the flow rate of the coal powder is 200Kg / min~400Kg / min.
[0015] Optionally, the second converter smelting time is t2, and t2 is 13min to 20min; wherein,
[0016] When the smelting time of the second converter is less than 12 minutes, CO2 is used as carrier gas to inject pulverized coal at the bottom of the converter;
[0017] When the smelting time of the second converter is 12min~t2, pure argon gas is blown from the bottom of the converter.
[0018] Optionally, relative to a converter with a tonnage of 300t, the flow rate of CO2 is (3500+t2×500)Nm 3 / h, the flow rate of the coal powder is (300+t2×50)kg / min, and the flow rate of the argon gas is 1000Nm 3 / h~3000Nm 3 / h.
[0019] Optionally, the mass fraction of C in the second semi-steel liquid is 1.5% to 2.5%; and the tapping temperature of the second semi-steel liquid is 1350°C to 1450°C.
[0020] Optionally, in the converter steel liquid, the mass fraction of C is 0.02% to 0.06%, the mass fraction of N is ≤0.0018%, and the mass fraction of O is 0.03% to 0.05%; and the tapping temperature of the converter steel liquid is 1550°C to 1700°C.
[0021] Optionally, the carburization is carried out by adding a carbon material to the bottom of the first semi-steel liquid; wherein the carbon material includes one or more of biomass particles and coal powder, the mass fraction of C in the carbon material is 50% to 99%, and the amount of the carbon material added is 5Kg / t·steel to 15Kg / t·steel.
[0022] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0023] The present application provides a smelting method of molten steel with high scrap ratio and low nitrogen. By adopting the converter double process to smelt molten steel, the scrap ratio of smelting is increased, and the smelting cycle can be controlled at the same time; by injecting coal powder at the bottom to increase carbon and supplement heat, the heat is increased and the denitrification effect is enhanced; by using CO2 as a carrier gas, twice the volume of CO is produced, the stirring is strengthened, and a better denitrification effect is obtained, and the kinetic conditions are better, and the O content at the converter end and the slag T.Fe are reduced. The method provided by the present application can increase the scrap ratio to 35% to 75%, and the mass fraction of N in the obtained molten steel is ≤0.0018%, which reduces the nitrogen content of the molten steel on the basis of ensuring a high scrap ratio during smelting. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0025] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0026] Figure 1 A schematic flow chart of a method for smelting low-nitrogen molten steel with a high scrap steel ratio provided in an embodiment of the present application. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0028] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0029] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.
[0030] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0031] Creative ideas of this application:
[0032] The technical difficulties of smelting in the prior art are as follows: (1) At present, the large scrap steel ratio process is mainly achieved by preheating the scrap steel and adding silicon and carbonaceous heat supplements. After the scrap steel is preheated, although increasing the scrap steel temperature can increase the scrap steel ratio, the amount of molten iron is reduced, making it difficult to control the nitrogen element. Similarly, adding a silicon heat supplement can increase the heat, but the overall carbon-oxygen reaction becomes weaker and the nitrogen content is difficult to control. The thermal efficiency of adding a carbonaceous heat supplement is low, and the generated CO bubbles cannot play a role in the molten steel in the molten pool. (2) The bottom blowing CO2 process is used to reduce nitrogen, mainly using CO2 and molten iron C to react to generate twice the volume of CO. Due to the large scrap steel ratio causing the total source of carbon to be reduced, the denitrification capacity under the condition of a large scrap steel ratio is also deteriorated. (3) RH denitrification after the converter, the RH denitrification capacity has a limit. When the nitrogen content at the converter end is high, the nitrogen content at the RH end increases.
[0033] In the present application, a converter double process is used to smelt molten steel. 250Kg / t·steel to 450Kg / t·steel scrap is added to the first converter, and CO2 is used as a carrier gas to spray pulverized coal at the bottom of the converter during the smelting process to obtain semi-steel. Coal powder, carbon powder and other carbon materials are added to the bottom of the semi-steel ladle, and the semi-steel is carbonized by the strong impact and stirring effect of the molten steel during the steelmaking process. The carbonized semi-steel enters the second converter, and 100Kg / t·steel to 300Kg / t·steel scrap is added to the second converter. CO2 is used as a carrier gas to spray pulverized coal at the bottom, and the amount of pulverized coal blown in is dynamically increased as the carbon content of the molten steel decreases. By adopting this process, coal powder is sprayed at the bottom to increase carbon and supplement heat, so as to achieve the effect of heat increase and enhanced denitrification; the injection amount of carbonaceous raw materials is adjusted according to the carbon content of the process molten steel, so as to improve the utilization rate of carbonaceous raw materials and the carburizing speed; CO2 is used as a carrier gas to produce twice the volume of CO, which strengthens the stirring and obtains a better denitrification effect, and the oxygen content of the molten steel at the end of the converter and the T.Fe in the slag are reduced. The method provided in this application can increase the scrap steel ratio to 35% to 75%, and the mass fraction of N in the obtained molten steel is ≤0.0018%, which reduces the nitrogen content of the molten steel on the basis of ensuring a high scrap steel ratio during smelting.
[0034] Figure 1 A schematic flow chart of a method for smelting low-nitrogen molten steel with a high scrap steel ratio provided in an embodiment of the present application.
[0035] See also Figure 1 The present application provides a method for smelting molten steel with a high scrap steel ratio and low nitrogen content, the method comprising:
[0036] By adopting the converter duplex process to smelt molten steel, the scrap ratio is increased to 35% to 75%, and the smelting cycle can be controlled. Exemplarily, the method can increase the scrap ratio to 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, etc.
[0037] S1, performing a first converter smelting on molten iron and first scrap steel to obtain a first semi-steel molten steel;
[0038] In some embodiments, the amount of the first scrap steel added is 250 Kg / t·steel to 450 Kg / t·steel.
[0039] By adopting the converter double process to smelt molten steel, the scrap steel ratio of smelting can be increased, and the smelting cycle can be controlled. Exemplarily, the amount of the first scrap steel added can be 250Kg / t·steel, 280Kg / t·steel, 300Kg / t·steel, 320Kg / t·steel, 350Kg / t·steel, 380Kg / t·steel, 420Kg / t·steel, 450Kg / t·steel, etc.
[0040] In some embodiments, the first converter smelting time is t1, t1 is 10min to 15min; wherein,
[0041] When the first converter smelting time is less than 5 minutes, pure CO2 is blown from the converter bottom;
[0042] When the smelting time of the first converter is 5min~t1, CO2 is used as a carrier gas to inject pulverized coal at the bottom of the converter.
[0043] In some embodiments, the flow rate of CO2 is 2500Nm2 relative to a converter with a tonnage of 300t. 3 / h~4500Nm 3 / h, the flow rate of the coal powder is 200Kg / min~400Kg / min.
[0044] The flow rates of CO2 and pulverized coal can be reasonably adjusted according to the different tonnages of the converter. The carbon content of the converter is increased by blowing pulverized coal at the bottom, and the bottom blowing absorption rate is high. At this time, the carbon content of the semi-steel is high, and the carbon increase rate is limited, so the amount of pulverized coal cannot be too high; if the amount of pulverized coal is too small, there will be no carbon increase effect. For example, the t1 can be 10min, 11min, 12min, 13min, 14min, 15min, etc.; the flow rate of CO2 can be 2500Nm 3 / h、3000Nm 3 / h、3500Nm 3 / h、4000Nm 3 / h、4500Nm 3 / h, etc.; the flow rate of the coal powder can be 200Kg / min, 250Kg / min, 300Kg / min, 350Kg / min, 400Kg / min, etc.
[0045] S2, carburizing the first semi-steel molten steel to obtain a second semi-steel molten steel; and
[0046] In some embodiments, the mass fraction of C in the second semi-steel liquid is 1.5% to 2.5%; and the tapping temperature of the second semi-steel liquid is 1350°C to 1450°C.
[0047] The carbon content in the second semi-steel liquid is increased by carburization to improve the denitrification effect. For example, the mass fraction of carbon in the second semi-steel liquid can be 1.5%, 1.6%, 1.8%, 2.0%, 2.1%, 2.2%, 2.4%, 2.5%, etc.; the tapping temperature of the second semi-steel liquid can be 1350°C, 1370°C, 1390°C, 1400°C, 1420°C, 1440°C, 1450°C, etc.
[0048] In some embodiments, the carbon increase is performed by adding a carbon material to the bottom of the first semi-steel liquid; wherein the carbon material includes one or more of biomass particles and coal powder, the mass fraction of C in the carbon material is 50% to 99%, and the amount of the carbon material added is 5Kg / t·steel to 15Kg / t·steel.
[0049] Add coal powder, carbon powder and other carbon materials at the bottom of the half ladle, and use the strong impact and stirring of molten steel to increase the carbon of the half steel during the steel tapping process. Use the good kinetic conditions of steel tapping to increase the carbon, and the carbonaceous raw materials are at the bottom of the ladle. Exemplarily, the amount of the carbon material added can be 5Kg / t·steel, 7Kg / t·steel, 9Kg / t·steel, 11Kg / t·steel, 12Kg / t·steel, 14Kg / t·steel, 15Kg / t·steel, etc.
[0050] S3, subjecting the second semi-steel molten steel and the second scrap steel to a second converter smelting, and using CO2 as a carrier gas to inject pulverized coal to reduce the nitrogen content of the molten steel, to obtain converter molten steel.
[0051] In some embodiments, the added amount of the second scrap steel is 100 Kg / t·steel to 300 Kg / t·steel.
[0052] By adopting the converter double process to smelt molten steel, the scrap steel ratio of smelting can be increased, and the smelting cycle can be controlled. Exemplarily, the amount of the second scrap steel added can be 100Kg / t·steel, 130Kg / t·steel, 150Kg / t·steel, 180Kg / t·steel, 200Kg / t·steel, 220Kg / t·steel, 250Kg / t·steel, 300Kg / t·steel, etc.
[0053] In some embodiments, the second converter smelting time is t2, and t2 is 13min to 20min; wherein,
[0054] When the smelting time of the second converter is less than 12 minutes, CO2 is used as carrier gas to inject pulverized coal at the bottom of the converter;
[0055] When the smelting time of the second converter is 12min~t2, pure argon gas is blown from the bottom of the converter.
[0056] In some embodiments, relative to a converter with a tonnage of 300 t, the flow rate of CO2 is (3500+t2×500)Nm 3 / h, the flow rate of the coal powder is (300+t2×50)kg / min, and the flow rate of the argon gas is 1000Nm 3 / h~3000Nm 3 / h.
[0057] The flow rates of CO2 and pulverized coal can be reasonably adjusted according to the different tonnages of converters. Bottom blowing pulverized coal increases C, and the bottom blowing absorption rate is high. According to the characteristics of the molten pool decarburization reaction, as the carbon content of the molten steel decreases, the amount of pulverized coal blown in is dynamically increased, and the carbon absorption rate is further improved. At the end, switch to argon gas, stop increasing carbon, and smelt to the final carbon content. At the end, switch to argon gas to prevent the injection of CO2 from causing an increase in the final oxygen content. Exemplarily, t2 can be 13min, 14min, 15min, 16min, 17min, 18min, 19min, 20min, etc.; the flow rate of CO2 can be 10000Nm 3 / h、10200Nm 3 / h、10500Nm 3 / h、10800Nm 3 / h、11000Nm 3 / h, etc.; the flow rate of coal powder can be 950kg / min, 960kg / min, 980kg / min, 1000kg / min, 1020kg / min, 1050kg / min, etc.; the flow rate of argon gas can be 1000Nm 3 / h、1200Nm 3 / h、1500Nm 3 / h、1800Nm 3 / h、2000Nm 3 / h、2500Nm 3 / h、3000Nm 3 / h, etc.
[0058] In some embodiments, in the converter steel liquid, the mass fraction of C is 0.02% to 0.06%, the mass fraction of N is ≤0.0018%, and the mass fraction of O is 0.03% to 0.05%; and the tapping temperature of the converter steel liquid is 1550°C to 1700°C.
[0059] By injecting pulverized coal at the bottom to increase carbon and heat, the heat can be increased and the denitrification effect can be enhanced; by using CO2 as a carrier gas, twice the volume of CO is produced, stirring is strengthened, and a better denitrification effect is obtained, and the kinetic conditions are better, and the O content at the end of the converter and the T.Fe of the slag are reduced. The method provided in this application can increase the scrap steel ratio to 35% to 75%, and the mass fraction of N in the obtained molten steel is ≤0.0018%, which reduces the nitrogen content of the molten steel on the basis of ensuring a high scrap steel ratio during smelting. Exemplarily, the mass fraction of C can be 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, etc.; the mass fraction of N can be 0.0010%, 0.0012%, 0.0013%, 0.0014%, 0.0015%, 0.0017%, 0.0018%, etc.; the mass fraction of O can be 0.03%, 0.035%, 0.04%, 0.045%, 0.05%, etc.; the tapping temperature of the converter steel liquid can be 1550°C, 1580°C, 1600°C, 1620°C, 1650°C, 1680°C, 1700°C, etc.
[0060] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.
[0061] Example 1
[0062] In the 300t converter, 105t of scrap steel was loaded into the first converter, and the smelting time was 10min. During the 0min to 5min of smelting, pure CO2 was blown from the bottom. During the 5min to 10min, CO2 was used to inject pulverized coal, and the CO2 flow rate was 3000Nm 3 / h, coal powder flow rate is 210kg / min, carbon content of molten steel is 2.0%, temperature is 1406℃, and steel tapping begins. Biomass particles, coal powder and other carbon-containing materials are added to the bottom of the half-steel ladle, and the added amount is 11Kg / t steel. During the smelting process of the second converter, 66t of scrap steel is added, and the blowing time is 13min. During the smelting 0min~12min, CO2 is used to inject coal powder, and the CO2 flow rate is 10000Nm 3 / h, the coal powder flow rate is 950kg / min; from 12min to 13min, bottom blowing pure argon is used, and the argon flow rate is 3000Nm 3 / h, the carbon content of the molten steel is 0.036%, the temperature is 1646℃, and the steel is tapped from the converter. The final nitrogen content is 13ppm, the carbon content is 0.036%, the oxygen content is 0.039%, and the slag T.Fe is 14%.
[0063] Example 2
[0064] In a 150t converter, 42t of scrap steel was loaded into the first converter, and the smelting time was 12min. During the 0min to 5min of smelting, pure CO2 was blown from the bottom. During the 5min to 12min, CO2 was used to inject pulverized coal, and the CO2 flow rate was 1750Nm 3 / h, coal powder flow rate is 140kg / min, carbon content of molten steel is 1.8%, temperature is 1390℃, and steelmaking begins. Biomass particles, coal powder and other carbon-containing materials are added to the bottom of the half-ladle, and the amount added is 6Kg / t steel. During the smelting process of the second converter, 26t of scrap steel is added, and the blowing time is 14min. During the smelting 0min~12min, CO2 is used to inject coal powder, and the CO2 flow rate is 5250Nm 3 / h, the coal powder flow rate is 500kg / min; from 12min to 14min, bottom blowing pure argon is used, and the argon flow rate is 1500Nm 3 / h, the carbon content of the molten steel is 0.04%, the temperature is 1640℃, and the steel is tapped from the converter. The final nitrogen content is 12ppm, the carbon content is 0.04%, the oxygen content is 0.035%, and the slag T.Fe is 13%.
[0065] Example 3
[0066] In the 210t converter, 86t of scrap steel was loaded into the first converter, and the smelting time was 13min. During the 0min to 5min of smelting, pure CO2 was blown from the bottom. During the 5min to 13min, CO2 was used to inject pulverized coal, and the CO2 flow rate was 2940Nm 3 / h, coal powder flow rate is 224kg / min, carbon content of molten steel is 1.9%, temperature is 1387℃, and steel tapping begins. Biomass particles, coal powder and other carbon-containing materials are added to the bottom of the half-steel ladle, and the added amount is 9Kg / t steel. During the smelting process of the second converter, 53t of scrap steel is added, and the blowing time is 15min. During the smelting time of 0min to 12min, CO2 is used to inject coal powder, and the CO2 flow rate is 7700Nm 3 / h, the coal powder flow rate is 735kg / min; from 12min to 15min, bottom blowing pure argon is used, and the argon flow rate is 2100Nm 3 / h, the carbon content of the molten steel is 0.038%, the temperature is 1660℃, and the steel is tapped from the converter. The final nitrogen content is 11ppm, the carbon content is 0.038%, the oxygen content is 0.038%, and the slag T.Fe is 15%.
[0067] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for smelting molten steel with high scrap ratio and low nitrogen content, characterized in that: The method comprises: Performing a first converter smelting on the molten iron and the first scrap steel to obtain a first semi-steel liquid; Carburizing the first semi-steel molten steel to obtain a second semi-steel molten steel; and The second semi-steel molten steel and the second scrap steel are subjected to a second converter smelting, and pulverized coal is injected using CO2 as a carrier gas to reduce the nitrogen content of the molten steel, thereby obtaining a converter molten steel.
2. The method according to claim 1, characterized in that The amount of the first scrap steel added is 250 kg / t·steel to 450 kg / t·steel.
3. The method according to claim 1, characterized in that The added amount of the second scrap steel is 100Kg / t·steel to 300Kg / t·steel.
4. The method according to claim 1, characterized in that: The first converter smelting time is t1, t1 is 10min to 15min; wherein, When the first converter smelting time is less than 5 minutes, pure CO2 is blown from the converter bottom; When the smelting time of the first converter is 5min~t1, CO2 is used as a carrier gas to spray pulverized coal at the bottom of the converter.
5. The method according to claim 4, characterized in that For a 300t converter, the CO2 flow rate is 2500Nm 3 / h~4500Nm 3 / h, the flow rate of the coal powder is 200Kg / min~400Kg / min.
6. The method according to claim 1, characterized in that The second converter smelting time is t2, t2 is 13min~20min; wherein, When the smelting time of the second converter is less than 12 minutes, CO2 is used as carrier gas to inject pulverized coal at the bottom of the converter; When the smelting time of the second converter is 12min~t2, pure argon gas is blown from the bottom of the converter.
7. The method according to claim 6, characterized in that For a converter with a tonnage of 300t, the flow rate of CO2 is (3500+t2×500)Nm 3 / h, the flow rate of the coal powder is (300+t2×50)kg / min, and the flow rate of the argon gas is 1000Nm 3 / h~3000Nm 3 / h.
8. The method according to claim 1, characterized in that The mass fraction of C in the second semi-steel liquid is 1.5% to 2.5%; and the tapping temperature of the second semi-steel liquid is 1350° C. to 1450° C.
9. The method according to claim 1, characterized in that: In the converter steel liquid, the mass fraction of C is 0.02% to 0.06%, the mass fraction of N is ≤0.0018%, and the mass fraction of O is 0.03% to 0.05%; and the tapping temperature of the converter steel liquid is 1550° C. to 1700° C.
10. The method according to claim 1, characterized in that The carbon increase is carried out by adding carbon material to the bottom of the first semi-steel liquid; wherein, the carbon material includes one or more of biomass particles and coal powder, the mass fraction of C in the carbon material is 50% to 99%, and the amount of the carbon material added is 5Kg / t·steel to 15Kg / t·steel.
Citation Information
Patent Citations
Multifunctional oxygen lance system for converter steelmaking and steelmaking method
CN111676343A
System and method for injecting pulverized coal at mouth of converter to increase gas recovery amount
CN111690787A
Converter steelmaking method
CN113957196A
High-scrap-ratio efficient low-carbon steelmaking method
CN117887920A
Smelting method of low-nitrogen steel
CN118272599A
Cited By
Method for controlling nitrogen content of vanadium-containing molten iron under high scrap ratio smelting condition
CN122326865A
Method for improving denitrification effect of converter under high scrap ratio blowing condition
CN122542749A