Converter smelting method with low carbon emission
By adding carbon materials three times during the converter smelting process, and using kinetic and thermodynamic conditions to improve the carburization rate, the problem of large carbon emissions in traditional converter smelting is solved, and the effects of high scrap steel ratio and low carbon emissions are achieved.
Patent Information
- Application Number
- CN202411198925.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-29
AI Technical Summary
In traditional long-term blast furnace + converter production, more than 70% of carbon emissions come from the pre-iron process. In the prior art, ferrosilicon is used as a heat replenishing agent, and it is difficult to effectively reduce carbon emissions.
The method of adding carbon materials three times is adopted. After the dephosphorization furnace smelting, the first carbon material, the second carbon material and the third carbon material are added respectively before the decarbonization furnace smelting, and the kinetics and Thermodynamic conditions increase carburization rate and reduce carbon emissions.
The scrap steel ratio has been improved, and carbon emissions have been significantly reduced, and a low-carbon emission converter smelting method has been realized, with high carburization rate and good heat replenishment effect.
Smart Images

Figure CN119061228A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of converter smelting, and specifically relates to a converter smelting method with low carbon emissions. Background Art
[0002] In the traditional "blast furnace + converter" long process, more than 70% of carbon emissions come from the pre-iron process. Therefore, increasing the scrap steel ratio and reducing the molten iron ratio in steelmaking production is one of the main measures to reduce carbon emissions.
[0003] In the prior art, in order to increase the scrap steel ratio, ferrosilicon is usually added as a heat supplement in converter smelting. However, the carbon emission factor of ferrosilicon is high, and there is still room for reducing carbon emissions. Summary of the invention
[0004] In order to solve the current technical problem of high carbon emissions from converter smelting, the present application provides a converter smelting method with low carbon emissions.
[0005] In a first aspect of the present application, a low-carbon emission converter smelting method is provided, comprising the following steps:
[0006] placing molten iron and first scrap steel in a dephosphorization furnace for smelting and then tapping the steel, and adding a first carbon material during the tapping process to obtain a first molten steel;
[0007] The first molten steel is added to a decarburization furnace containing second scrap steel and a second carbon material for smelting, and a third carbon material is added to the decarburization furnace during the smelting process to complete converter smelting;
[0008] The added mass of the first carbon material is 10-25 kg / t, the added mass of the second carbon material is 5-22 kg / t, and the added mass of the third carbon material is 15-30 kg / t.
[0009] In some embodiments, the added masses of the second carbon material, the first carbon material, and the third carbon material increase in sequence.
[0010] In some embodiments, when the carbon mass fraction of the molten steel in the decarburization furnace is lower than 0.9% and / or the temperature of the molten steel in the decarburization furnace is not lower than 1550° C., the third carbon material is added into the decarburization furnace.
[0011] In some implementations, the temperature of the tapped molten steel is 1470° C. to 1550° C., and the carbon mass fraction of the tapped molten steel is 0.7% to 1.5%.
[0012] In some embodiments, the temperature of the molten iron is 1300-1500° C., and the mass fraction of carbon in the molten iron is 3.5%-5.0%.
[0013] In some embodiments, during the steel tapping process, 2-5 kg / t of heat preservation agent is added to the surface of the first molten steel for heat preservation.
[0014] In some embodiments, during the steel tapping process, the bottom blowing gas is stirred for 1 to 3 min to promote carburization.
[0015] In some embodiments, the second scrap steel and the second carbon material are added to the decarburization furnace in the following manner: first, one third to one half of the second scrap steel is added to the decarburization furnace, then the second carbon material is added to the decarburization furnace, and finally, the remaining second scrap steel is added to the decarburization furnace.
[0016] In some embodiments, the added mass of the first scrap steel is 170-285 kg / t steel, and the added mass of the second scrap steel is 130-225 kg / t steel.
[0017] In some embodiments, during the dephosphorization furnace smelting process, the top blowing oxygen amount is 28-35 Nm 3 / t, bottom blowing strength is 0.15~0.25Nm 3 / t / min.
[0018] According to the low-carbon emission converter smelting method provided in the embodiment of the present application, the following steps are included: placing molten iron and a first scrap steel in a dephosphorization furnace for smelting and then tapping the steel, adding a first carbon material during the tapping process to obtain a first molten steel; adding the first molten steel to a decarburization furnace containing a second scrap steel and a second carbon material for smelting, adding a third carbon material to the decarburization furnace during the smelting process to complete converter smelting; wherein the added mass of the first carbon material is 10 to 25 kg / t, the added mass of the second carbon material is 5 to 22 kg / t, and the added mass of the third carbon material is 15 to 30 kg / t.
[0019] The first carbon material is added during the process of steel tapping after the dephosphorization furnace smelting. The good kinetic conditions of the steel tapping process can be used to promote the dissolution of the carbon material into the steel and improve the carburizing rate. The second carbon material is added before the first steel is added to the decarburizing furnace. In this way, the first steel can be fully stirred and mixed when poured into the decarburizing furnace, further improving the carburizing rate. The third carbon material is added during the decarburizing furnace smelting process. The carbon mass fraction in the steel is low at this stage, and there is a very large concentration difference between the carbon material and the steel, which is conducive to improving the carburizing rate. In addition, the temperature of the steel is high after a certain carbon oxidation process at this stage, and high temperature is more conducive to the dissolution of the carbon material into the steel and improving the carburizing rate.
[0020] That is to say, the present application adopts three additions of carbon materials, namely, during the steel-making process of the dephosphorization furnace, before the decarburization furnace is added with iron, and in the later stage of smelting in the decarburization furnace. The steel-making process of the dephosphorization furnace and before the decarburization furnace is added with iron mainly provide the kinetic conditions for carburization, while in the later stage of smelting in the decarburization furnace, it mainly provides the thermodynamic conditions for carburization, promotes the carburization rate, makes the carbon element react with oxygen to release heat and melt the scrap steel, thereby increasing the scrap steel ratio and reducing carbon emissions. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A process step diagram of a low-carbon emission converter smelting method of the present application is shown. DETAILED DESCRIPTION
[0022] In order to make the technical personnel in the technical field to which the present application belongs to understand the present application more clearly, the technical scheme in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.
[0023] The present application provides a converter smelting method with low carbon emissions, which has a high carburizing rate, good heat supplement effect, increased scrap steel ratio, and reduced carbon emissions.
[0024] See also Figure 1 The low-carbon emission converter smelting method provided in the embodiment of the present application comprises the following steps:
[0025] Step 1: placing molten iron and first scrap steel in a dephosphorization furnace for smelting and then tapping the steel, and adding a first carbon material during the tapping process to obtain a first molten steel.
[0026] Step 2: adding the first molten steel into a decarburization furnace containing second scrap steel and a second carbon material for smelting, adding a third carbon material into the decarburization furnace during the smelting process, and completing converter smelting.
[0027] The converter smelting method of the present application is to first use a dephosphorization furnace to dephosphorize molten iron, and then use a decarburization furnace for decarburization smelting. In this double converter smelting process, the low temperature of the molten steel in the early stage is conducive to dephosphorization, and carbon oxidation and heating mainly occur in the later stage. For the double smelting process, carbon material is added three times. During oxygen blowing smelting, the carbon material can be oxidized to release heat and supplement heat, thereby increasing the scrap steel ratio. Among them: the first carbon material is added during the process of steel tapping after the dephosphorization furnace smelting, and the good kinetic conditions of the steel tapping process can be used to promote the dissolution of the carbon material into the steel, thereby increasing the carburization rate; the second carbon material is added before the first steel liquid is added to the decarburization furnace, so that the first steel liquid can be fully stirred and mixed when poured into the decarburization furnace, further increasing the carburization rate. The third carbon material is added during the smelting process in the decarburization furnace. The carbon mass fraction in the molten steel is low at this stage, and there is a very large concentration difference between the carbon material and the molten steel, which is conducive to improving the carburizing rate. In addition, the temperature of the molten steel is high after a certain carbon oxidation process at this stage, and high temperature is more conducive to the dissolution of the carbon material into the molten steel, thereby improving the carburizing rate.
[0028] The first carbon material, the second carbon material and the third carbon material can be the same carbon material, such as coke, carburizing agent, biomass carbon, biomass particles, graphite, etc., with a carbon content of 50% to 99%. In other embodiments, the first carbon material, the second carbon material and the third carbon material can be different.
[0029] The added masses of the second carbon material, the first carbon material and the third carbon material increase in sequence. The added mass of the second carbon material is small because the second carbon material is added before the decarburization furnace is added with iron. Although the kinetic conditions are good, the carbon material has been added once to the molten steel, and the temperature of the molten steel is relatively low after the iron is added. The added mass of the third carbon material is the largest because the carbon content in the molten steel is relatively low in the later stage of smelting in the decarburization furnace, and the temperature of the molten steel is relatively high, providing good thermodynamic conditions for carburizing. The added mass of the first carbon material is in the middle because the kinetic conditions of the steel-out process are good and there is a certain temperature rise.
[0030] For the dephosphorization smelting and steel-making process in step one, in some embodiments, the added mass of the first carbon material is 10-25 kg / t, for example, 11 kg / t, 13 kg / t, 15 kg / t, 18 kg / t and 19 kg / t, etc. If the added mass of the first carbon material is too high, carbon saturation may occur, which will reduce the carburizing rate to a certain extent; if the added mass of the first carbon material is too low, the carburizing amount will be insufficient to a certain extent.
[0031] The reason why carbon material is not added before dephosphorization smelting is that the carbon content in the molten iron is very high, 4.0-5.0%, which is in a saturated state and cannot be carburized. In addition, the temperature of the molten iron is relatively low, 1300°C-1400°C, so carbon material is added during the steel tapping process. In some embodiments, the temperature of the molten steel is 1470°C-1550°C, and the carbon mass fraction of the molten steel is 0.7%-1.5%. At this time, the temperature of the molten steel is relatively high, and the high temperature is conducive to ensuring the activation energy of the carburizing reaction, and the carbon content is reduced to a certain level. There is a concentration difference between the carbon material and the molten steel, which has certain thermodynamic conditions for dissolving carbon.
[0032] In some embodiments, the mass of the first scrap steel added is 170-285 kg / t steel, for example 180 kg / t steel, 190 kg / t steel, 200 kg / t steel and 210 kg / t steel, etc. The heat source of the first scrap steel is mainly molten iron. When the mass of the first scrap steel added is too low, there may be excess heat to a certain extent. When the mass of the first scrap steel added is too high, there may be insufficient heat to a certain extent, and the final temperature of the decarburization furnace is low.
[0033] Steel tapping is to discharge molten steel into a ladle. During the steel tapping process, a heat preservation agent is added to the surface of the first molten steel, that is, a heat preservation agent is added to the ladle. The heat preservation agent can be calcium oxide, which can not only keep the heat but also prevent the carbon material from burning during the transportation of the ladle. It can also pre-melt the lime and reduce the lime consumption of the decarburization furnace. In some embodiments, the added mass of the heat preservation agent is 2 to 5 kg / t steel, such as 3 kg / t steel, 4 kg / t steel, etc. If the added mass of the heat preservation agent is too high, the heat preservation agent itself is a cold material, and adding too much will cool the semi-steel liquid to a certain extent. If the added mass of the heat preservation agent is too low, it will not cover the semi-steel liquid enough to a certain extent, so that the semi-steel liquid is exposed to the air, resulting in cooling and oxidation.
[0034] In some embodiments, during the steel tapping process, the bottom blowing gas is stirred for 1 to 3 min to promote carburization, that is, the bottom blowing gas such as argon is stirred on the ladle to stir the molten steel, improve the dynamic conditions of the molten steel, and promote carburization.
[0035] In some embodiments, during the dephosphorization furnace smelting process, the top blowing oxygen amount is 28-35Nm 3 / t, for example 30Nm 3 / t、31Nm 3 / t、32Nm 3 / t、33Nm 3 / t and 34Nm 3 / t, etc. In some embodiments, when the top blowing oxygen amount is too low, the tapping temperature may be less than 1470°C, and the carbon mass fraction of the tapping steel liquid may be greater than 1.5%. Low temperature and high carbon content may lead to low carburizing rate to a certain extent; when the oxygen blowing amount is higher than 35Nm3 / t, the temperature of the tapping steel liquid may be less than 1550℃, and the carbon mass fraction of the tapping steel liquid may be greater than 0.7%. At this time, it is close to the converter end point, which is easy to affect the converter end point control.
[0036] In some embodiments, during the dephosphorization furnace smelting process, the bottom blowing intensity is 0.15-0.25Nm 3 / t / min, for example 0.18Nm 3 / t / min, 0.19Nm 3 / t / min, 0.20Nm 3 / t / min, 0.21Nm 3 / t / min, 0.22Nm 3 / t / min, 0.23Nm 3 / t / min and 0.24Nm 3 / t / min, etc., to ensure the kinetic conditions of scrap steel melting. Bottom blowing intensity is less than 0.15Nm 3 / t / min, the stirring kinetic energy is reduced to a certain extent, and the scrap steel melts slowly; the bottom blowing intensity is greater than 0.25Nm 3 / t / min, to a certain extent, the stirring kinetic energy is too large, which can easily lead to splashing.
[0037] For the iron addition and decarburization smelting in step 2, in some embodiments, the added mass of the second carbon material is 5-22kg / t steel, such as 6kg / t steel, 7kg / t steel, 8kg / t steel, 9kg / t steel, 10kg / t steel, 11kg / t steel, 12kg / t steel, 13kg / t steel and 14kg / t steel, etc. If the added mass of the second carbon material is too small, the carburization amount will be insufficient to a certain extent, reducing the final temperature of the converter. If the added mass of the second carbon material is too much, carbon saturation may occur, which will reduce the carburization rate to a certain extent.
[0038] In some embodiments, the mass of the second scrap steel added is 130-225 kg / t steel, such as 132 kg / t steel, 138 kg / t steel, 142 kg / t steel, 145 kg / t steel, 150 kg / t steel, 156 kg / t steel, 159 kg / t steel, 163 kg / t steel, 168 kg / t steel, 175 kg / t steel and 178 kg / t steel, etc. The heat consumed by the second scrap steel heating and melting mainly comes from the residual carbon in the molten steel after dephosphorization smelting, the first carbon material, the second carbon material and the carburization amount of the third carbon material. If the mass of the second scrap steel added is too small, the scrap steel ratio will be reduced to a certain extent. If the mass of the second scrap steel added is too large, the carburization amount needs to be increased, which will extend the smelting time to a certain extent.
[0039] In some embodiments, the added mass of the third carbon material is 15-30 kg / t steel, such as 16 kg / t steel, 18 kg / t steel, 19 kg / t steel, 22 kg / t steel, 23 kg / t steel and 24 kg / t steel. If the added mass of the third carbon material is too small, the carburizing amount will be insufficient to a certain extent, and the end point temperature of the converter will be reduced. If the added mass of the third carbon material is too large, the oxygen blowing time may be increased in order to hit the end point carbon, thereby reducing production efficiency.
[0040] In some embodiments, when the carbon mass fraction of the molten steel in the decarburization furnace is lower than 0.9%, and / or the temperature of the molten steel in the decarburization furnace is not lower than 1550° C., the third carbon material is added to the decarburization furnace. This is because the low carbon content of the molten steel and / or the addition of carburizing material at high temperature are beneficial to improving the carburization rate.
[0041] Since the carbon material has a small density and is relatively light, in some embodiments, the second scrap steel and the second carbon material are added to the decarburization furnace as follows: first, one-third to one-half of the second scrap steel is added to the decarburization furnace, then the second carbon material is added to the decarburization furnace, and finally, the remaining second scrap steel is added to the decarburization furnace. On the one hand, the scrap steel bottom can lower the temperature in the decarburization furnace, and the scrap steel added last can press the carbon material between the two layers of scrap steel, thereby increasing the carburization rate of the carbon material.
[0042] In some embodiments, the particle sizes of the first carbon material, the second carbon material, and the third carbon material may all be 3-10 mm.
[0043] The low-carbon emission converter smelting method provided by the present application will be further described below in conjunction with specific embodiments:
[0044] Example 1 to Example 5
[0045] Embodiments 1 to 5 provide a converter smelting method, wherein the smelted steel is IF steel, and the smelting furnace includes a dephosphorization furnace and a decarburization furnace, and the nominal capacities of the dephosphorization furnace and the decarburization furnace are shown in Table 1. The converter smelting method comprises the following steps:
[0046] Dephosphorization furnace smelting steps: first scrap steel and molten iron are loaded into the dephosphorization furnace, wherein the temperature of the molten iron and the mass fraction of carbon in the molten iron can be seen in Table 2, and then slag-making agent is added for top and bottom double blowing smelting. After smelting, steel is tapped into the ladle, and the first carbon material is added during the tapping process, and the mass of the first carbon material added can be seen in Table 3. During the tapping process, lime is added to the ladle for heat preservation, and the mass of the lime added can be seen in Table 3, and argon is blown from the bottom for 1 to 3 minutes for weak stirring.
[0047] Decarburization furnace smelting steps: add one-half of the second scrap steel to the decarburization furnace, then add the second carbon material, then add the remaining one-half of the second scrap steel, and then add the molten steel in the ladle in the previous step to the decarburization furnace, smelt with top and bottom double blowing, smelt until the mass fraction of carbon in the molten steel is as shown in Table 4, and the temperature of the molten steel is as shown in Table 4, add the third carbon material to the decarburization furnace through the silo, and the added mass of the third carbon material is as shown in Table 4. Then continue smelting until the end of smelting.
[0048] Table 1 Nominal capacity of dephosphorization furnace and decarburization furnace Serial number Dephosphorization furnace tonnage / t Decarburization furnace tonnage / t Example 1 120 120 Example 2 210 210 Example 3 300 300 Example 4 300 300 Example 5 300 300
[0049] Table 2 Dephosphorization furnace control parameters
[0050] Table 3 Dephosphorization furnace control parameters Serial number Smelting end point C / % Smelting end point T / ℃ Amount of first carbon material added / t Addition amount of calcium oxide / t Example 1 0.7 1550 1.3 0.37 Example 2 1 1520 3.2 0.82 Example 3 1.2 1510 5.9 1.1 Example 4 1.1 1500 6.2 1.2 Example 5 0.9 1517 7.5 1.0
[0051] Table 4 Control parameters of decarburization furnace
[0052] Comparative Example 1
[0053] Comparative Example 1 is a common single converter production, and the smelted steel type is IF steel. The converter is first charged with scrap steel accounting for 15% of the total charge, and then with molten iron accounting for 85% of the total charge. Top and bottom double blowing is used for smelting. No heat supplementary agent ferrosilicon is added during the smelting process. The LCA carbon (Life Cycle Assessment) emission of IF steel is 2.6tCO2 / t material.
[0054] Comparative Example 2
[0055] Comparative Example 2 is a double converter production. The dephosphorization furnace adds scrap steel at a ratio of 10% and molten iron to produce semi-steel. The decarburization furnace adds scrap steel at a ratio of 20% and semi-steel. 17kg / t of ferrosilicon heat supplement is added to the decarburization furnace. The LCA carbon emission of IF steel is 2.38tCO2 / t material.
[0056] Table 5
[0057] Table 6
[0058] In Table 6, the carbon increase of the molten steel refers to the increase in the mass fraction of carbon in the molten steel before and after carbon addition, wherein the carbon increase of the first carbon material and the second carbon material are both sampled before carbon addition, and the carbon content is detected by sampling 5 minutes after carbon addition. The third carbon material is sampled before carbon addition, and the carbon content is detected by sampling 1-2 minutes after carbon addition. The carburization rate in Table 6 refers to the ratio of the difference between the mass of added carbon and the mass of carbon entering the molten steel to the mass of added carbon.
[0059] It can be seen from the data in Table 5 that the carburizing rate of the converter smelting method provided in the embodiment of the present application is 80.97%-83.25%, the carburizing rate is high, and the heat supplement effect is good, thereby increasing the scrap steel ratio, and the scrap steel ratio is 31.7%~50.7%. The high scrap steel ratio reduces carbon emissions.
[0060] The converter smelting method provided in the embodiment of the present application adopts the addition of carbon materials when the dephosphorization furnace is tapping steel, before the decarburization furnace is adding iron, and in the later stage of smelting in the decarburization furnace. The dephosphorization furnace is in the stage of tapping steel and before the decarburization furnace is adding iron, which mainly provides the kinetic conditions for carburization. The decarburization furnace mainly provides the thermodynamic conditions for carburization in the later stage of smelting, which promotes the carburization rate, makes the carbon element react with oxygen to release heat and melt the scrap steel, thereby increasing the scrap steel ratio and reducing carbon emissions.
[0061] In the present application, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.
[0062] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise" and "counterclockwise" indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0063] In this application, unless otherwise clearly specified and limited, the terms "connection", "fixation", etc. should be understood in a broad sense. For example, "fixation" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0064] In addition, the descriptions of "first", "second", etc. in this application are only for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include one or more features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0065] Although the embodiments of the present application have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the claims and their equivalents.
Claims
1. A low-carbon emission converter smelting method, characterized in that: The steps include: placing molten iron and first scrap steel in a dephosphorization furnace for smelting and then tapping the steel, and adding a first carbon material during the tapping process to obtain a first molten steel; The first molten steel is added to a decarburization furnace containing second scrap steel and a second carbon material for smelting, and a third carbon material is added to the decarburization furnace during the smelting process to complete converter smelting; The added mass of the first carbon material is 10-25 kg / t, the added mass of the second carbon material is 5-22 kg / t, and the added mass of the third carbon material is 15-30 kg / t.
2. The low-carbon emission converter smelting method according to claim 1, characterized in that: The added masses of the second carbon material, the first carbon material, and the third carbon material increase in sequence.
3. The low-carbon emission converter smelting method according to claim 1, characterized in that: When the carbon mass fraction of the molten steel in the decarburization furnace is lower than 0.9% and / or the temperature of the molten steel in the decarburization furnace is not lower than 1550° C., the third carbon material is added into the decarburization furnace.
4. The low-carbon emission converter smelting method according to any one of claims 1 to 3, characterized in that: The temperature of the tapped molten steel is 1470° C. to 1550° C., and the carbon mass fraction of the tapped molten steel is 0.7% to 1.5%.
5. The low-carbon emission converter smelting method according to any one of claims 1 to 3, characterized in that: The temperature of the molten iron is 1300° C. to 1500° C., and the mass fraction of carbon in the molten iron is 3.5% to 5.0%.
6. The low-carbon emission converter smelting method according to any one of claims 1 to 3, characterized in that: During the steel tapping process, 2-5 kg / t of heat preservation agent is added to the surface of the first molten steel for heat preservation.
7. The low-carbon emission converter smelting method according to claim 6, characterized in that: During the steel tapping process, the bottom blowing gas is stirred for 1 to 3 minutes to promote carburization.
8. The low-carbon emission converter smelting method according to any one of claims 1 to 3, characterized in that: The second scrap steel and the second carbon material are added into the decarburization furnace as follows: firstly add one third to one half of the second scrap steel into the decarburization furnace, then add the second carbon material into the decarburization furnace, and finally add the remaining second scrap steel into the decarburization furnace.
9. The low-carbon emission converter smelting method according to claim 8, characterized in that: The added mass of the first scrap steel is 170-285 kg / t steel, and the added mass of the second scrap steel is 130-225 kg / t steel.
10. The low-carbon emission converter smelting method according to claim 1, characterized in that: During the dephosphorization furnace smelting process, the top blowing oxygen amount is 28-35Nm 3 / t, bottom blowing strength is 0.15~0.25Nm 3 / t / min.
Citation Information
Patent Citations
Duplex steelmaking technique of revolving furnace
CN101294230A
Low-molten-iron-consumption blowing method of converter
CN112111622A
Converter steelmaking method
CN114774614A
Method for improving smelting heat balance of converter by adjusting coke adding time of converter temperature raising agent
CN115522011A
Converter smelting method based on electrode heating of waste steel
CN117821689A