Method for improving quality of vanadium oxide low-temperature catalytic growth graphene
By optimizing vanadium oxide films and using H2 etching, the method addresses substrate contamination and amorphous film issues, achieving high-quality graphene at lower temperatures and enabling reliable graphene devices.
Patent Information
- Application Number
- CN202411188598.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-28
AI Technical Summary
Existing methods for graphene growth using metal catalysts contaminate semiconductor substrates, leading to reliability and performance issues, while amorphous vanadium oxide films hinder high-quality graphene production.
Optimize the vanadium oxide thin film substrate and gas flow rate during graphene growth, using H2 etching to improve graphene quality, and employ a low-temperature in-situ growth process involving oxidation of V2O5 to achieve a uniform, continuous, and crystalline catalyst layer.
The method results in high-quality, uniform large-area graphene films with reduced defects, enabling reliable graphene devices and lower growth temperatures, and opens possibilities for non-metallic catalysts in graphene growth.
Smart Images

Figure HDA0005014353540000011 
Figure HDA0005014353540000012 
Figure HDA0005014353540000013
Abstract
Description
Technical Field
[0001] The present invention is a technology for improving the quality of low-temperature catalytic growth of graphene by vanadium oxide with phase change properties, specifically involving a sputtering-oxidation method for preparing a vanadium oxide film and a low-temperature in-situ patterned growth of graphene, belonging to the fields of material preparation technology and semiconductor optoelectronic integration. Background Art
[0002] There are many methods for synthesizing graphene, among which chemical vapor deposition is one of the most promising graphene growth methods, which can produce large-area and relatively high-quality graphene films. In most direct growth methods, the use of metal catalysts as the main method to improve the quality of graphene can easily lead to contamination of mainstream semiconductor substrates, which will affect the reliability and performance of the device. Therefore, the development of a process for low-temperature transfer-free growth of graphene using non-metal catalysts is of great significance to improving the preparation technology of graphene devices and promoting the widespread application of graphene devices. The metal-insulator phase transition characteristics (MIT) of vanadium oxide can be used to catalyze the growth of graphene under low temperature conditions. After the growth of graphene is completed, vanadium oxide can be removed as a sacrificial layer through a corrosion process, or it can be retained as an insulating layer. At room temperature, vanadium oxide will not cause short circuits in graphene devices like metal catalysts, effectively solving the damage to graphene caused by subsequent transfer and photolithography steps, which is of great significance to promoting the widespread application of directly grown graphene.
[0003] Currently, the vanadium oxides used to catalyze the growth of graphene are sputtered V 2 O 5 Thin film, V 2 O 5 As the target material, magnetron sputtering equipment is used to deposit Si / SiO 2 A thin film is deposited on the substrate. This method is simple to operate and the film is dense, but the sputtered film is amorphous or polycrystalline, without obvious preferred orientation. The good surface morphology and lattice structure of the catalytic layer directly affect the growth of graphene, so the preparation of a high-quality catalytic layer is crucial to the growth of graphene.
[0004] The vertical cold-wall PECVD furnace can achieve low-temperature (below 400°C) growth of graphene, and its growth time can be greatly shortened compared to the tube furnace. During the growth process, Ar is used to provide plasma and dilute the gas concentration in the chamber. 4 To provide carbon source, H 2 The role of is mainly reflected in two aspects: on the one hand, it promotes the cracking of carbon source, and on the other hand, it improves the uniformity and quality of graphene. Summary of the invention
[0005] The purpose of the present invention is to optimize the quality of the vanadium oxide thin film substrate and the gas flow rate during the growth process, thereby improving the quality of graphene. 2 O 5 The film is used as the graphene catalyst layer, and after the graphene is grown, ten times the flow rate of H 2 , using H ions to etch graphene growth defects and impurities, further improving the quality of graphene, and ultimately obtaining a uniform large-area graphene film. The above-mentioned improved technology is used to grow graphene in situ at low temperature, specifically including the following steps:
[0006] (1) Cleaning Si / SiO 2 Substrate sheet, to remove dust and grease adsorbed on the surface;
[0007] (2) Photolithography and development of the substrate using a mask to reveal the desired pattern;
[0008] (3) using a magnetron sputtering device to deposit metal V. The thickness of the deposited metal V is adjusted according to the needs and the performance of the sputtering device to ensure that the film is dense. Usually, the thickness of the deposited metal V is 3-10 nm, preferably 5 nm.
[0009] (4) peeling off to obtain a patterned sputtered metal thin layer;
[0010] (5) Place in a rapid annealing furnace and pass O 2 , at 300℃min -1 Heat to 400°C, hold for 10-20 min, preferably 15 min (the specific oxidation time is related to the thickness of V sputtering, for 5 nm thick V the corresponding holding time is 15 min), then heat at 300°C min -1 The temperature is lowered to below 100℃ and taken out. The surface is V 2 O 5 film;
[0011] (6) Then place it in a vertical cold-wall PECVD to grow graphene at 200°C min -1 The temperature was heated to 300 °C at a rate of 100 °C and a pressure of 10 mbar. Ar:H 2 and CH 4 , where Ar:H 2 :CH 4 Flow ratio = 960:20:5, H 2 The flow rate was 20 sccm; plasma was ignited at the same time (80 W, 15 kHz), grown for 5 min, and then CH 4 , H 2 The flow rate was increased to 200 sccm. 2The plasma was then turned off and heated at 300 °C min -1 Cool down to 100℃ at a rate of 2 , turn off Ar;
[0012] (7) After the growth is completed, wait for the machine to cool down to below 100° C., open the chamber, take out the sample, and obtain patterned graphene.
[0013] Advantages of the present invention
[0014] The present invention focuses on V prepared by oxidation of V 2 O 5 As a catalyst layer, instead of using directly sputtered V 2 O 5 , and the addition of large H after graphene growth 2 The flow annealing step has the following advantages:
[0015] 1) Oxidation of V to prepare V 2 O 5 The film is uniform and continuous, the surface roughness is small, and the crystal plane has an obvious preferred orientation in the (001) direction, which improves the V 2 O 5 The single crystal degree of the film, good surface morphology and lattice structure are crucial to the growth of high-quality graphene;
[0016] 2) After the growth is completed, 2 Annealing under flow, H ions react with dangling bonds or defects in graphene to repair or eliminate these defects, further optimizing the quality of graphene and obtaining a uniform and large-area graphene film;
[0017] 3) Two improved methods were used to achieve the preparation of graphene at a lower temperature (300°C), which is 100°C lower than the previous 400°C growth process;
[0018] 4) Based on the present invention, a new method is provided for optimizing the catalytic growth of graphene by vanadium oxide and phase change materials, which provides more possibilities for other non-metallic materials to be used as catalysts. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 :Cleaning Si / SiO 2 Substrate, SiO 2 Layer thickness 300 nm;
[0020] Figure 2 :The first photolithography development of the substrate;
[0021] Figure 3 :Wet etching of SiO in the pattern area 2The photoresist used as a mask is then removed;
[0022] Figure 4 : Second photolithography development of substrate;
[0023] Figure 5 : After sputtering the metal V film, the photoresist used as a mask is removed;
[0024] Figure 6 :Oxidation of V to V in a rapid annealing furnace 2 O 5 , about four times thicker;
[0025] Figure 7 : Graphene growth in PECVD;
[0026] Figure 8 :The third photolithography development of the substrate;
[0027] Fig. 9 : After sputtering the metal electrode, the photoresist used as a mask is removed;
[0028] in, For Si substrate, SiO 2 Substrate, Photoresist For metal V, V 2 O 5 , For graphene, It is a Ti / Au electrode.
[0029] Fig.10 : Comparison of Raman spectra of graphene before and after using the content of the present invention. DETAILED DESCRIPTION
[0030] The present invention is further described in detail below with reference to the accompanying drawings and examples, but the present invention is not limited to the following embodiments.
[0031] Example 1
[0032] V prepared by oxidation 2 O 5 Thin film catalytic growth of graphene to produce graphene-V 2 O 5 -Si(GVS) photodetector, the process steps are as follows:
[0033] (I) Preparation of Graphical V 2 O 5 film
[0034] (1) Clean Si / SiO with acetone, anhydrous ethanol, and deionized water in sequence 2Substrate sheet. See attached Figure 1 ;
[0035] (2) Use the first photolithography plate to photolithograph a 1.3×1.3 mm window on the substrate. Figure 2 ;
[0036] (3) Using photoresist as a mask, a 300nm thick SiO 2 Use wet etching to remove and expose the Si substrate;
[0037] (4) Use a stripping solution to remove the photoresist and clean the substrate. Figure 3 ;
[0038] (5) Use the second photolithography plate to etch a 1.5×1.5 mm window on the substrate. The window is located above the second photolithography window and is in the same position as the square. Figure 4 ;
[0039] (6) Place the magnetron sputtering device (Denton Vacuum Discovery) in a vacuum chamber and deposit a 5 nm layer of V on the surface. The sputtering power is 300W;
[0040] (7) Take out the sample, remove the photoresist with a stripping solution, and clean the substrate. Figure 5 ;
[0041] (8) Place in a rapid annealing furnace (RTP) and pass O 2 , at 300℃min -1 Raise the temperature to 400℃, hold for 15min, then increase the temperature to 300℃min -1 After cooling to 100℃, a layer of V with a thickness of about 20nm was obtained. 2 O 5 .
[0042] See attached Figure 6 ;
[0043] (ii) In the graphical V 2 O 5 Graphene is grown on the substrate and electrodes are sputtered
[0044] (9) placing the substrate in a PECVD furnace (Aixtron Black Magic) to grow graphene on the substrate using plasma chemical vapor deposition;
[0045] (10) The chamber was evacuated to 0.2 mbar, and Ar with a flow rate of 1000 sccm was introduced to clean the chamber. The cycle was repeated twice, each time for 1 min.
[0046] (11) After cleaning, turn off Ar and introduce H at a flow rate of 1000 sccm.2 , while controlling the chamber pressure to 10 mbar, and then heating at 200 °C min -1 The temperature was raised to 350°C at a rate of 100 °C and stabilized for 10 seconds;
[0047] (12) 960 sccm Ar, 20 sccm H 2 and 5 sccm CH 4 Introduced into the chamber, plasma (80 W, 15 kHz) was ignited at the same time, and the plasma and mixed gas were maintained for 5 min to grow graphene;
[0048] (13) Closing CH after growth 4 , H 2 The flow rate was increased to 200 sccm and maintained for 12 min after stabilization. 2 Flow etches surface defects and impurities;
[0049] (14) Turn off the plasma and heat at 300℃min -1 After cooling to 275℃, turn off H 2 , introduce 1000 sccm of Ar to continue natural cooling;
[0050] (15) When the temperature is lower than 100°C, end the program, open the furnace cover and take out the sample. Figure 7 ;
[0051] (16) Use the third photolithography plate to overlay the electrode pattern. Figure 8 ;
[0052] (17) Ti / Au (15 / 300nm) electrodes were prepared on the positive side and the negative side of the sample.
[0053] (18) Use a stripping solution to remove the photoresist, clean the sample, and obtain graphene-V 2 O 5 -Si (GVS) photodetector. See attached Fig. 9 .
[0054] (iii) Conducting Raman spectroscopy tests on the graphene grown before and after improvement to characterize the quality of the graphene.
[0055] Raman spectroscopy is a detection method that can quickly evaluate the quality of graphene. The D, G and 2D peaks of graphene Raman spectrum are located at 1337cm -1 、1597cm -1 and 2661cm -1 At the peak intensity ratio of D peak to G peak (I D / I G) is usually used to judge the degree of defects in graphene. The lower the value, the fewer defects in graphene. The peak intensity ratio of the 2D peak to the G peak (I 2D / I G ) can roughly determine the number of graphene layers.
[0056] The black and red curves in the figure are the Raman spectra of graphene grown before and after improvement, see the attached Fig.10 To ensure the rigor of the experiment, except for the two points described in the content of the invention, the other experimental conditions are kept consistent. 2 O 5 After the graphene film is grown, its I D / I G is 0.90. Due to the large half-peak width of the D peak and the G peak, the two peaks will be stuck together, indicating that the quality of graphene is poor and there are many defects. 2 O 5 After the graphene film is grown and passed through a large flow of H 2 The etching of D / I G It is 0.71, the D peak decreases, and the characteristic peak becomes sharp, indicating that the quality of graphene is significantly improved.
Claims
1. A method for improving the quality of graphene grown by low temperature catalysis of vanadium oxide, characterized in that: The V2O5 film oxidized from V is used as the graphene catalyst layer. After the graphene is grown, a large flow of H2 is introduced to etch the growth defects and impurities of the graphene using H ions, thereby further improving the quality of the graphene and finally obtaining a uniform large-area graphene film. The main process steps include the following: (1) Clean the Si / SiO2 substrate to remove dust and grease adsorbed on the surface; (2) Photolithography and development of the substrate using a mask to reveal the desired pattern; (3) Depositing metal V using magnetron sputtering equipment; (4) peeling off to obtain a patterned sputtered metal thin layer; (5) Place in a rapid annealing furnace, introduce O2, and heat at 300℃min -1 Heat to 400℃, hold for 10-20min, preferably 15min, then heat at 300℃min -1 Cool down to below 100℃ and take it out. At this time, the surface is a V2O5 film. (6) Then place it in a vertical cold-wall PECVD to grow graphene at 200°C min -1 The temperature was raised to 300°C at a rate of 1000 °C and a pressure of 10 mbar. Ar:H2 and CH4 were introduced, with a flow ratio of Ar:H2:CH4 of 960:20:5 and a H2 flow rate of 20 sccm. The plasma was ignited at the same time and grown for 5 min. Then CH4 was turned off and the H2 flow rate was increased to 200 sccm. The high H2 flow rate was maintained for 12 min. The plasma was then turned off and the growth was continued at 300°C min. -1 Cool down to 100℃ at a cooling rate of , turn off H2, turn off Ar; (7) After the growth is completed, wait for the machine to cool down to below 100° C., open the chamber, take out the sample, and obtain patterned graphene.
2. The method according to claim 1, characterized in that The V2O5 thin film catalyst layer is no longer prepared by sputtering with V2O5 as the target, but by a two-step sputtering-oxidation method using V as the target. The thin film prepared by this method is uniform and continuous, with low surface roughness, and the crystal plane has an obvious preferential orientation in the (001) direction, which improves the single crystallinity of the V2O5 thin film. Good surface morphology and lattice structure are crucial to the growth of high-quality graphene.
3. The method according to claim 1, characterized in that After growing graphene, introducing a large flow of H2 can effectively etch impurities and defects on the graphene surface, further optimizing the quality of graphene and obtaining a uniform and large-area graphene film.
4. The method according to claim 1, characterized in that Graphene is grown at a lower temperature of 300°C.
5. The method according to claim 1, characterized in that The peak intensity ratio of D peak to G peak is I D / I G It is 0.71.
Citation Information
Patent Citations
Method for preparing single-layer graphene
CN102134067A
Catalyst with vanadium oxide / graphene compound material and preparation method thereof
CN102836703A
Method for preparing graphene on silicon base without metal catalyst
CN106868469A
Vanadium dioxide-graphene composite film structure, and preparation method and application thereof
CN110627055A
Preparation method of hole transport layer and crystalline silicon solar cell
CN113410335A