Multi-metal composite borate compound and multi-metal composite borate crystal as well as preparation method and application of multi-metal composite borate compound and multi-metal composite borate crystal
Synthesis of polymetal composite borate compound K7PbLu2B15O30 through solid phase reaction method and spontaneous crystallization method, solving the problems of slow growth speed and high cost in the prior art, and achieving rapid growth of large-sized crystals, suitable for blue-green band laser frequency conversion. Improves the optical quality and application of nonlinear optical materials.
Patent Information
- Application Number
- CN202310637439.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing blue-green band laser frequency conversion nonlinear optical materials, such as KTP, BBO and LBO, have slow growth rates and high costs, making it difficult to obtain large-sized crystals, and lack trivalent rare earths containing closed-shell electronic configurations and semi-full 4f orbits. Cationic and lonely electron cation materials limit the optical quality and application of the material.
The polymetal composite borate compound K7PbLu2B15O30 was synthesized by solid phase reaction method and spontaneous crystallization method. The powder was ground through solid phase reaction method and heated up multiple times. The crystals were grown in combination with spontaneous crystallization method to achieve rapid growth and low-cost large-size crystals. preparation.
K7PbLu2B15O30 crystal with nonlinear optical effect was obtained, which is suitable for laser frequency conversion of blue and green light bands, with fast growth speed and low cost. It is suitable for the preparation of nonlinear optical devices and realizes the frequency conversion function.
Smart Images

Figure CN119061477A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of growth of nonlinear optical crystals, and more specifically to a multi-metal composite borate compound and a multi-metal composite borate crystal, and a preparation method and application thereof. Background Art
[0002] Crystals with nonlinear optical effects are called nonlinear optical crystals. Nonlinear optical crystal effects refer to frequency doubling, sum frequency, difference frequency, parametric amplification and other effects. Only crystals without a symmetry center can have nonlinear optical effects. Using the nonlinear optical effects of crystals, nonlinear optical devices such as second harmonic generators, up-frequency converters, down-frequency converters, and optical parametric oscillators can be made. The laser generated by the laser can be frequency-converted through nonlinear optical devices to obtain more useful wavelengths of laser, making the laser more widely used. The all-solid-state blue-green laser system can be realized by generating near-infrared lasers from solid lasers and then performing frequency conversion through nonlinear optical crystals. It has great application prospects in the field of laser technology.
[0003] Currently, the nonlinear optical materials used for blue-green band laser frequency conversion mainly include KTP (KTiOPO4), BBO (β-Ba2B2O4) and LBO (LiB3O5) crystals. These materials have shortcomings in growth. For example, since KTP and LBO are non-isotropic melting compounds, and BBO has a phase change at the melting point, they all need to use the flux method to grow, which has a slow growth rate, is difficult to obtain large-size crystals, and has a high cost, which affects the large-scale application and promotion of all-solid-state lasers. At present, most nonlinear optical crystals are synthesized based on anionic groups in theory. With the emergence of more and more nonlinear optical crystal materials, studies have found that in addition to the contribution of anionic groups to the optical properties of materials, trivalent rare earth cations (Re=Y, Gd, Lu, etc.) with closed-shell electronic configuration and half-filled 4f orbitals and cations with lone pair electrons (Am=Sn, Pb, Te, etc.) also have certain effects on them. They can enhance the anisotropy and second harmonic generation properties of the materials and can greatly improve the optical quality of crystal materials. However, there are currently no reports on nonlinear optical materials containing these two types of elements.
[0004] Based on this, finding new nonlinear optical crystal materials with large size has become one of the difficulties and frontier directions in the current research field of nonlinear optical materials. Summary of the invention
[0005] Based on the above problems, the first object of the present invention is to provide a multi-metal composite borate compound.
[0006] The second object of the present invention is to provide a method for preparing the multi-metal composite borate compound as described above.
[0007] The third object of the present invention is to provide a multi-metal composite borate crystal. The chemical formula of the multi-metal composite borate crystal is K7PbLu2B 15 O 30 It is a new type of large-size nonlinear optical crystal material that can be used in blue-green band laser frequency conversion devices.
[0008] The fourth object of the present invention is to provide a method for preparing the above-mentioned multi-metal composite borate crystals. The method has the advantages of fast growth rate, low cost, and easy acquisition of larger-sized crystals.
[0009] The fifth object of the present invention is to provide an application of the multi-metal composite borate crystal as described above in the preparation of a nonlinear optical device. The nonlinear optical device is prepared by orienting a nonlinear optical crystal blank, cutting it according to a desired angle, thickness and cross-sectional size, and then polishing it to be used as a nonlinear optical device.
[0010] The sixth object of the present invention is to provide a nonlinear optical device comprising the above-mentioned multimetallic composite borate crystal, wherein the device can generate at least one output radiation having a frequency different from the incident electromagnetic radiation after at least one incident electromagnetic radiation passes through at least one piece of the multimetallic composite borate nonlinear optical crystal.
[0011] In order to achieve the above first object, the present invention adopts the following technical scheme:
[0012] The present invention discloses a multi-metal composite borate compound, wherein the chemical formula of the multi-metal composite borate compound is K7PbLu2B 15 O 30 .
[0013] In order to achieve the above second purpose, the present invention adopts the following technical solutions:
[0014] The present invention discloses a method for preparing the above-mentioned multi-metal composite borate compound, wherein the multi-metal composite borate compound is synthesized by a solid phase reaction method, and the preparation method comprises the following steps:
[0015] A potassium-containing compound, a lead-containing compound, a lutetium-containing compound, and a boron-containing compound are prepared in a molar ratio of 3.5:1:1:15, mixed and ground, the ground powder is put into a crucible, heated once, kept warm for 24-48 hours, then cooled, taken out after cooling to room temperature, and ground again, then the ground powder is put into a crucible, heated twice, kept warm for 48-96 hours, and then cooled to room temperature at a rate of 50-70°C / h to obtain the product.
[0016] Furthermore, the heating process of the primary heating is to heat the temperature to 450-550° C. at a heating rate of 50-70° C. / h.
[0017] Furthermore, the secondary heating process is to heat the temperature to 830° C. at a heating rate of 50-70° C. / h.
[0018] Further, the potassium-containing compound includes but is not limited to one or more of potassium oxide, potassium nitrate and potassium carbonate; preferably potassium carbonate;
[0019] The lead-containing compound is selected from lead oxides;
[0020] The lutetium-containing compound is selected from lutetium oxides;
[0021] The boron-containing compound includes but is not limited to H3BO3 or B2O3; preferably H3BO3.
[0022] Furthermore, the crucible is made of platinum.
[0023] In order to achieve the third object, the present invention adopts the following technical solutions:
[0024] The invention discloses a multi-metal composite borate nonlinear optical crystal, the chemical formula of which is K7PbLu2B 15 O 30 , belongs to the trigonal crystal system, the space group is R32, and its unit cell parameters are: α=β=90°, γ=120°, Z=2.
[0025] Further, the size of the crystal is (8-11) mm×(7-9) mm×(4-6) mm. For example, the size of the crystal can be 11 mm×9 mm×6 mm, 11 mm×8 mm×6 mm, 11 mm×8 mm×5 mm, 10 mm×9 mm×6 mm, 10 mm×8 mm×6 mm, 10 mm×8 mm×5 mm, 10 mm×8 mm×5 mm, 9 mm×6 mm×5 mm, 9 mm×7 mm×6 mm, 8 mm×7 mm×5 mm, or any other size.
[0026] In order to achieve the fourth objective, the present invention adopts the following technical solutions:
[0027] The present invention discloses a method for preparing the above-mentioned multi-metal composite borate nonlinear optical crystal, wherein the multi-metal composite borate nonlinear optical crystal is grown by a spontaneous crystallization method, and the preparation method comprises the following steps:
[0028] (1) mixing a potassium-containing compound, a lead-containing compound, a lutetium-containing compound, and a boron-containing compound in a molar ratio of 6:1:1:15, and placing the mixed materials into a crucible; placing the crucible containing the materials in a crystal furnace, and heating the materials until they are melted to obtain a high-temperature solution;
[0029] (2) using a seed crystal trial method to find the saturation temperature of crystal growth, introducing the fixed seed crystals onto the surface of the high-temperature melt or into the high-temperature melt at 5-15° C. above the saturation temperature, maintaining the temperature for 500-700 minutes, and then cooling to the saturation temperature;
[0030] (3) Using the saturation temperature as the starting temperature for cooling, cooling at a rate of 0.3-1°C / day, and rotating the crystal and / or the crucible at a rate of 10-100 rpm to grow the crystal; after the crystal grows to a desired size, lifting the crystal from the liquid surface, annealing at a rate of 5-20°C / h to room temperature, and obtaining the multi-metal composite borate nonlinear optical crystal.
[0031] Further, the potassium-containing compound includes but is not limited to one or more of potassium oxide, potassium nitrate and potassium carbonate; preferably potassium fluoride;
[0032] The lead-containing compound is selected from lead fluoride;
[0033] The lutetium-containing compound is selected from lutetium oxides;
[0034] The boron-containing compound includes but is not limited to H3BO3 or B2O3; preferably H3BO3.
[0035] Furthermore, the heating conditions of step (1) are to increase the temperature to 980-1000° C. at a rate of 5-15° C. / h and keep the temperature for 72-96 hours.
[0036] Furthermore, the saturation temperature of the crystal growth is 958-964°C.
[0037] Furthermore, the seed crystal can be fixed to the lower end of the seed crystal rod using a platinum wire, and the technician can adjust the position of the seed crystal and the crystal grown thereon by rotating or pulling the seed crystal rod.
[0038] Furthermore, the crucible is made of platinum.
[0039] In order to achieve the fifth object, the present invention adopts the following technical solutions:
[0040] The present invention discloses an application of the multi-metal composite borate nonlinear optical crystal as described above or the multi-metal composite borate nonlinear optical crystal prepared by the preparation method as described above in the preparation of nonlinear optical devices.
[0041] According to the crystallographic data of the crystal, the crystal blank is oriented, the crystal is cut according to the required angle, thickness and cross-sectional size, and the light-transmitting surface of the crystal is polished, and it can be used as a nonlinear optical device. The optical processing method of the above nonlinear optical crystal is familiar to those skilled in the art. The crystal provided by the present invention has no special requirements on the optical processing accuracy.
[0042] In order to achieve the sixth object, the present invention adopts the following technical solutions:
[0043] The present invention discloses a nonlinear optical device comprising the multi-metal composite borate crystal as described above.
[0044] Furthermore, in the device, it is possible to generate at least one beam of output radiation having a frequency different from that of the incident electromagnetic radiation after at least one beam of incident electromagnetic radiation passes through at least one piece of the multi-metal composite borate nonlinear optical crystal; illustratively, the nonlinear optical crystal of the present invention is made into a self-frequency doubling mechanism device and placed in an optical resonant cavity composed of a total reflection mirror and an output mirror, and after being excited by an optical pump source, the crystal generates a green frequency-doubled laser output.
[0045] Furthermore, the device includes a frequency multiplication generator, an up-frequency converter, a down-frequency converter, an optical parametric oscillator or an optical parametric amplifier.
[0046] The beneficial effects of the present invention are as follows:
[0047] The present invention provides a multi-metal composite borate compound and a multi-metal composite borate crystal and a preparation method and application thereof. The chemical formula of the crystal is K7PbLu2B 15 O 30 , does not have a symmetry center, belongs to the trigonal crystal system, the space group is R32, and its unit cell parameters are: α=β=90°, γ=120°, Z=2. The multimetal composite borate nonlinear optical crystal prepared by the preparation method of the present invention is a single crystal. The multimetal composite borate nonlinear optical crystal has a suitable nonlinear optical effect, can achieve type I phase matching, is non-deliquescent, and is suitable for the needs of laser frequency conversion in the blue-green light band; the crystal can be used to make nonlinear optical devices. The present invention also provides a preparation method for the nonlinear optical crystal, which has the advantages of fast growth rate, low cost, and easy acquisition of larger-sized crystals. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 K7PbLu2B 15 O 30 Powder X-ray diffraction (PXRD) patterns of the compounds.
[0049] Figure 2 K7PbLu2B15 O 30 Powder X-ray diffraction (PXRD) patterns of nonlinear optical crystals.
[0050] Figure 3 K7PbLu2B 15 O 30 Schematic diagram of the structure of a nonlinear optical crystal.
[0051] Figure 4 K7PbLu2B 15 O 30 Differential thermal analysis of nonlinear optical crystals.
[0052] Figure 5 The present invention shows that K7PbLu2B 15 O 30 The working principle diagram of a typical nonlinear optical device made of crystal, where 1 is the laser, 2 is the incident laser beam, and 3 is the K7PbLu2B after crystal post-processing and optical processing. 15 O 30 Single crystal, 4 is the generated outgoing laser beam, and 5 is the filter.
[0053] Figure 6 K7PbLu2B 15 O 30 Powder frequency doubling test diagram of nonlinear optical crystal. DETAILED DESCRIPTION
[0054] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments and drawings. It should be understood by those skilled in the art that the content described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0055] Example 1
[0056] In this example, the solid phase reaction method was used to prepare powdered K7PbLu2B 15 O 30 Compound.
[0057] The feeding amounts of each raw material are: K2CO3: 0.07 mol; PbO: 0.02 mol; Lu2O3: 0.02 mol; H3BO3: 0.3 mol.
[0058] The specific steps are:
[0059] Weigh each raw material according to the above dosage, put the raw materials into a mortar, mix and grind, then put into a platinum crucible, heat to 500°C at a heating rate of 60°C / h, keep warm for 24 hours, cool down, take out after cooling to room temperature, grind evenly and re-fire, heat to 830°C at a heating rate of 60°C / h, keep warm for 48 hours, cool to room temperature at a rate of 60°C / h, grind, and obtain the product K7PbLu2B 15 O 30 Compound.
[0060] Example 2
[0061] In this example, K7PbLu2B was prepared by spontaneous crystallization. 15 O 30 Crystals;
[0062] KF, PbF2, Lu2O3, and H3BO3 are prepared in a molar ratio of 6:1:1:15, mixed, and loaded into a crucible, and the crucible containing the materials is placed in a crystal furnace, heated to fully melt the materials and mix them evenly to obtain a high-temperature solution;
[0063] The crucible containing the high-temperature solution was placed in a vertical single crystal growth furnace. The opening at the top of the furnace was sealed with insulation material. A small hole for the seed crystal rod to enter and exit was left at the top of the furnace corresponding to the center of the crucible. The temperature was raised to 1000°C at a rate of 10°C / h and kept constant for 72 hours to fully homogenize the high-temperature melt. The saturation temperature of crystal growth was found to be 960°C by the seed crystal trial method. The high-temperature melt was cooled to 970°C (10°C above the saturation temperature). K7PbLu2B cut along the c-axis was placed in the furnace. 15 O 30 The seed crystal is fixed to the lower end of the seed crystal rod with a platinum wire, and the seed crystal is introduced into the crucible from the small hole on the top of the furnace so that it contacts the melt surface. The rotation speed of the seed crystal rod is 30rpm, the temperature is kept constant for 600 minutes, and the temperature is quickly reduced to 960℃;
[0064] The temperature was lowered at a rate of 0.3°C / day. After 10 days, the crystal growth was completed. The crystal was lifted out of the melt surface and annealed at a rate of 10°C / h to room temperature to obtain K7PbLu2B with a size of 10 mm×8 mm×5 mm. 15 O 30 Single crystal.
[0065] Example 3
[0066] In this example, K7PbLu2B was prepared by spontaneous crystallization. 15 O 30 Crystals;
[0067] KF, PbF2, Lu2O3 and H3BO3 are prepared in a molar ratio of 6:1:1:15, mixed and loaded into a crucible, and the crucible containing the materials is placed in a crystal furnace and heated to fully melt and mix the materials evenly to obtain a high-temperature solution;
[0068] The crucible containing the high-temperature solution was placed in a vertical single crystal growth furnace. The opening at the top of the furnace was sealed with insulation material. A small hole for the seed crystal rod to enter and exit was left at the top of the furnace corresponding to the center of the crucible. The temperature was raised to 1000°C at a rate of 10°C / h and kept constant for 72 hours to make the high-temperature melt fully homogenized. The saturation temperature of crystal growth was found to be 958°C by the seed crystal trial method. The high-temperature melt was cooled to 966°C (8°C above the saturation temperature). K7PbLu2B cut along the c-axis was placed in the furnace. 15 O 30 The seed crystal is fixed to the lower end of the seed crystal rod with a platinum wire, and the seed crystal is introduced into the crucible from the small hole on the top of the furnace so that it contacts the melt surface. The rotation speed of the seed crystal rod is 30 rpm, the temperature is kept constant for 600 minutes, and the temperature is quickly reduced to 958 ° C;
[0069] The temperature was lowered at a rate of 0.5°C / day. After 7 days, the crystal growth was completed. The crystal was lifted out of the melt surface and annealed at a rate of 10°C / h to room temperature to obtain K7PbLu2B with a size of 9mm×6mm×5mm. 15 O 30 Single crystal.
[0070] Example 4
[0071] In this example, K7PbLu2B was prepared by spontaneous crystallization. 15 O 30 Crystals;
[0072] KF, PbF2, Lu2O3 and H3BO3 are prepared in a molar ratio of 6:1:1:15, mixed and loaded into a crucible, and the crucible containing the materials is placed in a crystal furnace and heated to fully melt and mix the materials evenly to obtain a high-temperature solution;
[0073] The crucible containing the high-temperature solution was placed in a vertical single crystal growth furnace. The opening at the top of the furnace was sealed with insulation material. A small hole for the seed crystal rod to enter and exit was left at the top of the furnace corresponding to the center of the crucible. The temperature was raised to 1000°C at a rate of 10°C / h and kept constant for 72h to make the high-temperature melt fully homogenized. The saturation temperature of crystal growth was found to be 962°C by the seed crystal trial method. The high-temperature melt was cooled to 974°C (12°C above the saturation temperature). K7PbLu2B cut along the c-axis was placed in the furnace. 15 O 30 The seed crystal is fixed to the lower end of the seed crystal rod with a platinum wire, and the seed crystal is introduced into the crucible from the small hole on the top of the furnace so that it contacts the melt surface. The rotation speed of the seed crystal rod is 30 rpm, the temperature is kept constant for 600 minutes, and the temperature is quickly reduced to 962 ° C;
[0074] The temperature was lowered at a rate of 0.5°C / day. After 8 days, the crystal growth was completed. The crystal was lifted out of the melt surface and annealed at a rate of 10°C / h to room temperature to obtain K7PbLu2B with a size of 9mm×7mm×6mm. 15 O 30 Single crystal.
[0075] Example 5
[0076] In this example, K7PbLu2B was prepared by spontaneous crystallization. 15 O 30 Crystals;
[0077] KF, PbF2, Lu2O3 and H3BO3 are prepared in a molar ratio of 6:1:1:15, mixed and loaded into a crucible, and the crucible containing the materials is placed in a crystal furnace and heated to fully melt and mix the materials evenly to obtain a high-temperature solution;
[0078] The crucible containing the high-temperature solution was placed in a vertical single crystal growth furnace. The opening at the top of the furnace was sealed with insulation material. A small hole for the seed crystal rod to enter and exit was left at the top of the furnace corresponding to the center of the crucible. The temperature was raised to 1000°C at a rate of 10°C / h and kept constant for 72h to make the high-temperature melt fully homogenized. The saturation temperature of crystal growth was found to be 964°C by the seed crystal trial method. The high-temperature melt was cooled to 978°C (14°C above the saturation temperature). K7PbLu2B cut along the c-axis was placed in the furnace. 15 O 30 The seed crystal is fixed to the lower end of the seed crystal rod with a platinum wire, and the seed crystal is introduced into the crucible from the small hole on the top of the furnace so that it contacts the melt surface. The rotation speed of the seed crystal rod is 30 rpm, the temperature is kept constant for 600 minutes, and the temperature is quickly reduced to 964 ° C;
[0079] The temperature was lowered at a rate of 0.8°C / day. After 6 days, the crystal growth was completed. The crystal was lifted out of the melt surface and annealed at a rate of 10°C / h to room temperature to obtain K7PbLu2B with a size of 8mm×7mm×5mm. 15 O 30 Single crystal.
[0080] After testing, the K7PbLu2B prepared in Examples 2-5 15 O 30 The nonlinear optical crystal belongs to the trigonal system, the space group is R32, and its unit cell parameters are: α=β=90°, γ=120°, Z=2.
[0081] Figure 3 The K7PbLu2B prepared in Examples 2-5 is shown 15 O 30Schematic diagram of the structure of a nonlinear optical crystal, from which we can understand its microscopic components.
[0082] Figure 4 The K7PbLu2B prepared in Examples 2-5 is shown 15 O 30 The differential thermal analysis diagram of the nonlinear optical crystal shows that it has good thermal stability.
[0083] Comparative Example 1
[0084] Example 2 was repeated, with the only difference being that the heating rate in "heating to 1000°C at a rate of 10°C / h and maintaining the temperature for 72h" was changed to 20°C / h, and the other conditions remained unchanged. The experiment found that if the heating rate was too fast, the raw materials would erupt out of the crucible, and thus large-sized single crystals could not be obtained.
[0085] Comparative Example 2
[0086] Example 2 was repeated, with the only difference being that the heating temperature in "raising the temperature to 1000°C at a rate of 10°C / h and maintaining the temperature for 72h" was changed to 900°C, and the other conditions remained unchanged. The experiment found that the raw materials could not be completely melted and large-sized single crystals could not be prepared.
[0087] Comparative Example 3
[0088] Example 2 was repeated, except that "cooling at a rate of 0.3°C / day, and crystal growth ended after 10 days" was changed to cooling at a rate of 1.2°C / day, and other conditions remained unchanged. It was found that cracks occurred inside the obtained crystal.
[0089] Example 6
[0090] The K7PbLu2B prepared in Example 2-5 15 O 30 A typical nonlinear optical device prepared by single crystal, its working principle diagram is as follows Figure 5 As shown, 1 is the laser, 2 is the incident laser beam, and 3 is the K7PbLu2B after crystal post-processing and optical processing. 15 O 30 Single crystal, 4 is the generated outgoing laser beam, and 5 is the filter.
[0091] Combine the following Figure 5 The nonlinear optical device is described in detail: the incident laser beam 2 is emitted by laser 1 and enters K7PbLu2B 15 O 30The single crystal 3, the generated outgoing laser beam 4 passes through the filter 5, thereby obtaining the required laser beam. The nonlinear optical device can be a frequency doubling generator, an up-frequency converter, a down-frequency converter, an optical parametric oscillator, etc. The laser 1 can use a neodymium-doped yttrium aluminum garnet (Nd:YAG) laser or other lasers. For the frequency doubling device using the Nd:YAG laser as the light source, the incident laser beam 2 is an infrared light with a wavelength of 1064nm, which passes through the K7PbLu2B 15 O 30 The single crystal generates green double frequency light with a wavelength of 532nm. The outgoing laser beam 4 contains infrared light with a wavelength of 1064nm and green light of 532nm. The function of the filter 5 is to filter out the infrared light component and only allow the green double frequency light to pass.
[0092] K7Pb 15 O 30 The single crystal is not easy to break, easy to cut, polish and store, and does not deliquesce. The crystal is made into a frequency doubling device with a cross-sectional size of 7mm×7mm and a light-transmitting thickness of 5mm. Figure 5 The device shown is assembled at room temperature, using a Q-switched Nd:YAG laser as the light source, an incident infrared light with a wavelength of 1064nm, an output green laser with a wavelength of 532nm, and a laser signal intensity of 770.3mJ, which is approximately 1.1 times that of KDP (purchased from Aladdin, analytical grade 99.5%).
[0093] The prepared K7PbLu2B 15 O 30 Powder frequency doubling test of nonlinear optical crystals:
[0094] Sample preparation: K7PbLu2B 15 O 30 The nonlinear optical crystal and KDP (purchased from Aladdin, analytically pure 99.5%) were ground and sieved to prepare samples with different particle sizes.
[0095] Then, the powder frequency doubling test was performed on samples with different particle sizes. Figure 5 The device shown in the figure was assembled and tested at room temperature using a Q-tuned Nd:YAG laser with a wavelength of 1064 nm as the fundamental frequency light. The test results are shown in Figure 6 , its application effect in outputting 532nm green laser is close to that of KDP.
[0096] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A multi-metal composite borate compound, characterized in that: The chemical formula of the multi-metal composite borate compound is K7PbLu2B 15 O 30 .
2. The method for preparing the multi-metal composite borate compound according to claim 1, characterized in that: The multi-metal composite borate compound is synthesized by a solid phase reaction method, and the preparation method thereof comprises the following steps: A potassium-containing compound, a lead-containing compound, a lutetium-containing compound, and a boron-containing compound are prepared in a molar ratio of 3.5:1:1:15, mixed and ground, the ground powder is put into a crucible, heated once, kept warm for 24-48 hours, then cooled, taken out after cooling to room temperature, and ground again, then the ground powder is put into a crucible, heated twice, kept warm for 48-96 hours, and then cooled to room temperature at a rate of 50-70°C / h to obtain the product.
3. The preparation method according to claim 2, characterized in that: The heating process of the primary heating is to heat the temperature to 450-550°C at a heating rate of 50-70°C / h; Preferably, the secondary heating process is to heat the temperature to 830° C. at a heating rate of 50-70° C. / h.
4. The preparation method according to claim 2, characterized in that: The potassium-containing compound is selected from one or more of potassium oxide, potassium nitrate and potassium carbonate; preferably potassium carbonate; The lead-containing compound is selected from lead oxides; The lutetium-containing compound is selected from lutetium oxides; The boron-containing compound is selected from H3BO3 or B2O3; preferably H3BO3.
5. A multi-metal composite borate nonlinear optical crystal, characterized in that: The chemical formula of the crystal is K7PbLu2B 15 O 30 , belongs to the trigonal crystal system, the space group is R32, and its unit cell parameters are: α=β=90°, γ=120°, Z=2.
6. The method for preparing a multi-metal composite borate nonlinear optical crystal according to claim 5, characterized in that: The multi-metal composite borate nonlinear optical crystal is grown by a spontaneous crystallization method, and the preparation method thereof comprises the following steps: (1) mixing a potassium-containing compound, a lead-containing compound, a lutetium-containing compound, and a boron-containing compound in a molar ratio of 6:1:1:15, placing the mixture into a crucible, placing the crucible containing the materials in a crystal furnace, and heating the materials until they are melted to obtain a high-temperature solution; (2) using a seed crystal trial method to find the saturation temperature of crystal growth, introducing the fixed seed crystals onto the surface of the high-temperature melt or into the high-temperature melt at 5-15° C. above the saturation temperature, maintaining the temperature for 500-700 minutes, and then cooling to the saturation temperature; (3) Using the saturation temperature as the starting temperature for cooling, cooling at a rate of 0.3-1°C / day, and rotating the crystal and / or the crucible at a rate of 10-100 rpm to grow the crystal; after the crystal grows to a desired size, lifting the crystal from the liquid surface, annealing at a rate of 5-20°C / h to room temperature, and obtaining the multi-metal composite borate nonlinear optical crystal.
7. The preparation method according to claim 6, characterized in that: The potassium-containing compound is selected from one or more of potassium oxides, potassium halides and potassium carbonates; preferably potassium fluoride; The lead-containing compound is selected from lead fluoride; The lutetium-containing compound is selected from lutetium oxides; The boron-containing compound is selected from H3BO3 or B2O3; preferably H3BO3.
8. The preparation method according to claim 6, characterized in that: The heating conditions of step (1) are to increase the temperature to 980-1000° C. at a rate of 5-15° C. / h and keep the temperature for 72-96 hours.
9. Use of the multi-metal composite borate nonlinear optical crystal according to claim 5 or the multi-metal composite borate nonlinear optical crystal prepared by the preparation method according to any one of claims 6 to 8 in preparing nonlinear optical devices.
10. A nonlinear optical device, characterized in that: The nonlinear optical device comprises the multimetal composite borate nonlinear optical crystal as claimed in claim 5 or the multimetal composite borate nonlinear optical crystal prepared by the preparation method as claimed in any one of claims 6 to 8.
Citation Information
Patent Citations
Series of composite metal rare-earth borates, series of composite metal rare-earth borate nonlinear optical crystals as well as preparation method and application of the nonlinear optical crystals
CN107699948A
Potassium lutetium borate nonlinear optical crystal as well as preparation method and application thereof
CN109763169A