Battery pole piece, phosphate / carbon composite electrode material as well as application and preparation method of phosphate / carbon composite electrode material

Through the porous structure of the phosphate/carbon composite electrode material, the problem of poor circulation and rate performance of potassium ion batteries is solved, and high conductivity and stability is achieved, which is suitable for the negative electrode material of potassium ion batteries.

CN119069668AActive Publication Date: 2024-12-03NANCHANG HANGKONG UNIVERSITY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411101207.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-12-03
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

Developing potassium ion batteries with high theoretical capacity, high conductivity and high cycling stability remains a research problem, especially due to the difficulty of migration, embedding and deintercalation of potassium ions, resulting in poor cycling performance and poor rate performance.

Method used

Using phosphate/carbon composite electrode material, the porous composite structure of carbon material and phosphate can be improved to improve ion transport performance and electrochemical performance, including the hydrothermal heat of nitrogen-doped porous carbon nanosheets and phosphate particles using graphite-like phases. Reaction preparation to form a composite material with a high specific surface area.

Benefits of technology

It significantly improves the circulation and rate performance of potassium ion batteries, alleviates the problem of volume expansion, improves electrochemical performance and stability, and is suitable for the negative electrode material of potassium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069668A_ABST
    Figure CN119069668A_ABST
Patent Text Reader

Abstract

The invention discloses a battery pole piece, a phosphate / carbon composite electrode material and application and a preparation method thereof, and belongs to the field of new energy materials. The phosphate / carbon composite electrode material is porous, and also comprises an integrated structure which takes a carbon material as a matrix and takes a phosphoric acid material as an attachment. Wherein the carbon material is a graphite-like phase nitrogen-doped porous carbon nanosheet, the phosphoric acid material is phosphate, and the phosphate is anchored to the carbon nanosheet in the form of particles. The phosphate / carbon composite electrode material has the advantages of good conductivity, high specific capacity, good rate capability, good cycle performance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of new energy materials, and relates to novel carbon nitride-derived porous carbon nanosheets and phosphate composite electrode materials, and specifically to a battery electrode, a phosphate / carbon composite electrode material, and its application and preparation method. Background Art

[0002] Lithium-ion batteries are widely used in electric vehicles and electronic products due to their excellent high energy density and cycle performance. However, the extremely uneven geographical distribution and limited supply of lithium mineral resources pose significant challenges to the further development of lithium-ion battery technology. Given the abundance of potassium and sodium in the earth's crust, potassium-ion batteries and sodium-ion batteries have shown promise as potential alternatives to lithium-ion batteries.

[0003] In comparison, potassium-ion batteries exhibit several advantages.

[0004] First, due to the physical and chemical properties of alkaline metal lithium itself, lithium-ion batteries have approached the limit of their theoretical energy density.

[0005] Secondly, the redox potential of potassium is lower than that of sodium and similar to that of lithium, which enables potassium-ion batteries to provide energy density comparable to that of lithium-ion batteries.

[0006] In addition, potassium ions have significantly lower Lewis acidity than lithium ions and sodium ions. This promotes faster ion migration, further strengthening the performance advantages of potassium ion batteries. Therefore, potassium ion batteries are expected to become an effective solution to large-scale energy storage problems and address energy sustainability.

[0007] However, developing a potassium-ion battery with high theoretical capacity, high conductivity and high cycle stability remains a research problem and faces many challenges. Summary of the invention

[0008] The examples of the present application provide a battery electrode sheet, a phosphate / carbon composite electrode material, and its application and preparation method, which can.

[0009] The solution of this application example is implemented through the following contents.

[0010] In a first aspect, the present application discloses a phosphate / carbon composite electrode material.

[0011] The electrode material is porous and comprises a composite integral structure of a carbon material and a phosphoric acid material; the carbon material is a matrix, and the phosphoric acid material is an attachment on the matrix; The carbon material is a nitrogen-doped porous carbon nanosheet in a graphite-like phase, the phosphoric acid material is a phosphate, and the phosphate is anchored to the carbon nanosheet in the form of particles.

[0012] Optionally, the carbon material is a derivative formed by denitrification of graphite-like carbon nitride (g-C3N4); or, the particles are in the form of nanowires; or, the specific surface area of ​​the phosphate / carbon composite electrode material is 260 m² / g; or, the phosphate is antimony phosphate. Nanosized particles help improve ion transport performance such as shortening the transport distance, thereby having a positive effect on capacitance and rate.

[0013] In a second aspect, the present application discloses a battery electrode sheet containing a phosphate / carbon composite electrode material.

[0014] In a third aspect, the present application discloses an application of a phosphate / carbon composite electrode material in a potassium ion battery, wherein the phosphate / carbon composite electrode material is used as a negative electrode material of the potassium ion battery.

[0015] Optionally, the method comprises: thermally denitrifying a precursor powder obtained by heat-treating and pulverizing urea using zinc powder, dezincifying the precursor powder using acid solution, washing the precursor powder with water until the precursor powder is neutral, and drying the precursor powder to obtain carbon nanosheets; and Carbon nanosheets, metal chloride, phosphate and ethylene glycol are subjected to a hydrothermal reaction to generate a precipitate, and the precipitate is heat-treated.

[0016] Optionally, the method for heat treating urea includes: heating urea at a preset temperature system, the temperature system being: 2-10°C·min -1 The temperature is raised to 500°C to 600°C at a rate of 100°C and kept at this temperature for 3 to 10 hours. Preferably, the heating rate is, for example, 3°C·min -1 、4℃·min -1 、5℃·min -1 、6℃·min -1 、7℃·min -1 、8℃·min -1 , or 9℃·min -1 The heating temperature can be 510 to 590°C, 520 to 550°C, 520 to 560°C, 540 to 580°C. The heat preservation time can be controlled at 3 to 4 hours, 5 to 9 hours, 3 to 8 hours, 5 to 7 hours.

[0017] Optionally, the heat treatment of urea is carried out by placing the urea in a combustion boat and heating it in a muffle furnace. Optionally, the pulverization operation is carried out by grinding in an agate mortar.

[0018] Optionally, the method of thermally denitrifying the precursor powder using zinc powder includes: mixing the precursor powder with zinc powder and pressing the tablets, and then calcining them in an inert atmosphere.

[0019] Optionally, the mixing method is grinding, and the tableting pressure is 5 to 20 MPa. For example, the pressure can be 5 to 18 MPa, 11 to 19 MPa, 10 to 16 MPa, 8 to 12 MPa, or 13 to 17 MPa.

[0020] Optionally, the temperature regime of the calcination process is: 5-10°C·min -1 The temperature is raised to 700°C to 850°C at a rate of 100°C and kept at this temperature for 2 to 6 hours. Preferably, the heating rate is, for example, 6°C·min -1 、7℃·min -1 、8℃·min -1 The heating temperature can be 720 to 840°C, 710 to 800°C, 750 to 820°C, 760°C to 810°C. The heat preservation time can be controlled at 2 to 5 hours, 3 to 4 hours, 5 to 6 hours.

[0021] Optionally, the metal chloride is used at a concentration of 0.02-0.05 mol L -1 Preferably, the concentration may be 0.02 to 0.03 mol L -1 , 0.04 to 0.05 mol L -1 or 0.03 to 0.04 mol L -1 、.

[0022] Optionally, phosphate is used at a concentration of 0.05-0.1 mol L -1 Preferably, the concentration may be 0.05 to 0.07 mol L -1 , 0.06 to 0.08 mol L -1 , or 0.07 to 0.09 mol L -1 , 0.09 to 0.1 mol L -1 、.

[0023] Optionally, a hydrothermal reactor with a volume of 100 mL is used during the hydrothermal reaction, the amount of carbon nanosheets used is 60-150 g, and the amount of ethylene glycol used is 60 mL. The amount of carbon nanosheets used can also be 60-70 g, or 65-90 g, or 80-100 g, or 90-110 g, or 120-140 g.

[0024] Optionally, the carbon nanosheets, metal chloride, phosphate and ethylene glycol are dispersed by ultrasonic wave in a water bath heated at a temperature of 50° C. to 70° C. to form a dispersion, and the dispersion is used for a hydrothermal reaction.

[0025] Optionally, the temperature of the hydrothermal reaction is 160°C to 200°C, and the reaction time is 2 to 24 hours. Preferably, the temperature of the hydrothermal reaction is 160 to 180 degrees, or 170°C to 180°C, and the reaction time is 5 to 10 hours.

[0026] Optionally, the precipitate is heat treated by annealing.

[0027] Optionally, the annealing process atmosphere is nitrogen or argon.

[0028] Optionally, the annealing temperature is 500-600°C, and the annealing time is 4-10 hours. Preferably, the annealing temperature is 510-580°C, or 520-560 degrees, or 530-590 degrees; accordingly, the annealing time can be 5-9 hours, 6-8 hours, 7 to 10 hours, or 4 to 8 hours.

[0029] Optionally, the method for preparing a battery electrode sheet includes: Providing a phosphate / carbon composite electrode material, or a phosphate / carbon composite electrode material obtained by implementing a method for preparing a phosphate / carbon composite electrode material; and A slurry of phosphate / carbon composite electrode material mixed with CMC2200, conductive carbon black and NMP solvent is coated on copper foil, wherein CMC2200 is sodium carboxymethyl cellulose, which serves as a binder or thickener.

[0030] Optionally, the mass ratio of the phosphate / carbon composite electrode material to CMC2200 and the conductive carbon black is 7:1.5:1.5, or 7:2:1, or 8:1:1.

[0031] The phosphate / carbon composite electrode material described in the present application has the advantages of high conductivity and high specific capacity, and the raw materials are cheap and readily available, the preparation process is simple, and the operation is highly controllable. The potassium ion battery manufactured using the composite electrode material can exhibit excellent cycle and rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application.

[0033] Figure 1 XRD pattern of the SbPO4 / NC composite material prepared in Example 1 of the present application; Figure 2 This is a SEM image of the SbPO4 / NC composite material prepared in Example 1 of the present application; Figure 3The SbPO4 / NC composite material prepared in Example 1 of the present application is used as a negative electrode material for a potassium ion battery. The voltage range is 0.01-3.0 V and the current density is 200 mA g -1 Cyclic performance test diagram under conditions of .

[0034] Figure 4 This is a rate performance test diagram of the SbPO4 / NC composite material prepared in Example 1 of the present application as a negative electrode material for a potassium ion battery. DETAILED DESCRIPTION

[0035] Due to the high cost of lithium-ion batteries and the reality that performance is difficult to improve, a phosphate / carbon composite electrode material that can be used to manufacture potassium-ion batteries is proposed in this application. The composite material is a metal phosphate-based material and is used as a negative electrode material for potassium-ion batteries.

[0036] From a microstructural perspective, phosphate / carbon composite electrode materials have a porous structure, which allows rapid migration of charges and ions, thereby alleviating to a certain extent the volume expansion problem caused by the secondary batteries manufactured based on them during the cycle process.

[0037] Especially considering that the radius of potassium ions is large (relative to lithium-ion batteries), the migration, embedding and de-embedding of potassium ions are relatively difficult. The expansion coefficient is large during charging and discharging, and the negative electrode is easily pulverized, resulting in poor cycle performance. In addition, potassium ions have slow kinetics and a small diffusion coefficient, resulting in poor rate performance. The composite material of phosphate and carbon material of the present application can solve the above problems well.

[0038] Moreover, the composite electrode material can also enable the negative electrode material prepared based on it to have better electrochemical properties, thereby being more suitable for potassium ion batteries.

[0039] Specifically, the carbon matrix in the composite electrode material contains macropores and mesopores.

[0040] The pore diameter of the macropore is 100-200 nm, such as 100 nm, 160 nm, 170 nm, 180 nm, 190 nm or 200 nm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0041] The pore size of the mesopores is 5-15 nm, such as 5 nm, 8 nm, 10 nm, 12 nm or 15 nm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0042] In addition, the phosphate in the composite electrode material is a particulate matter. Preferably, the particulate matter is a nanowire structure. For example, the phosphate nanowire is a short rod with a diameter of 10-50nm and a length of 0.2-1μm. Exemplarily, the nanowire diameter is 10nm, 20nm, 30nm, 40nm or 50nm, and the nanowire length is 0.2μm, 0.4μm, 0.6μm, 0.8μm or 1μm, but it is not limited to the listed values. Other unlisted values ​​within the numerical range, or any values ​​defined between the two are also applicable.

[0043] In this application, one advantage of using phosphates (such as K3PO4) is that: It is a good ion conductor and can significantly improve the conductivity of materials.

[0044] In addition, metal phosphate K3PO4 is a product of SbPO4 after recycling, so it is low-cost. Moreover, metal phosphate K3PO4 is non-toxic, so it is eco-friendly, and it also has the advantages of high abundance and high crystallinity. All these make metal phosphate a new type of energy storage electrode material, and can also improve the cycle stability of potassium ion batteries made based on such materials during operation.

[0045] Furthermore, phosphates also have an open framework structure in which the large and stable PO4 3- Anions can cause a much smaller volume change than the alloy negative electrode during battery operation, avoiding more side reactions and thus improving cycle stability.

[0046] Antimony phosphate, which has faster ion transport capability and higher structural durability, has great application potential in alkali metal ion batteries. In addition, the antimony ions in antimony phosphate crystals have lone pairs of electrons, so it has better conductivity. More importantly, phosphate is also an ion conductor, which can effectively reduce the diffusion barrier of sodium ions and promote reaction kinetics.

[0047] In summary, metal phosphates have a special structure, lower operating voltage, are environmentally friendly and have a higher theoretical capacity.

[0048] In particular, in the present application, carbon materials are also compounded with metal phosphates, so as to suppress the large volume change and low conductivity of the negative electrode materials manufactured based on the above materials during the actual potassium storage process, thereby improving the capacity attenuation problem of the corresponding potassium ion battery during the charging and discharging cycle.

[0049] Combined with the porous structure of the carbon matrix and the nanowire structure of the phosphate, the phosphate / carbon composite material has a higher specific surface area, thus having more reactive sites. At the same time, it also provides an ideal path for ion migration, thereby providing a higher ion mobility (0.1×10 -10 ~5×10 -10 cm 2 s -1 ). For example, the specific surface area of ​​the composite material is 120-300m 2 g -1 , for example, including 120m 2 g -1 、130m 2 g -1 、160m 2 g -1 、180m 2 g -1 or 300m 2 g -1 The above range is not limited to the listed values, and other values ​​not listed within the above range are also applicable.

[0050] In particular, the carbon material in the composite electrode is a nitrogen-doped porous carbon nanosheet in a graphite-like phase.

[0051] In particular, the carbon material is a derivative formed by denitrification of graphite-like carbon nitride (g-C3N4). The nitrogen-doped porous carbon derived from g-C3N4 contains a high pyrrolic N content of up to 7.81 at%. Since pyrrolic N has a strong electrostatic repulsion, it has a certain influence on the expansion of the carbon interlayer spacing, which will affect the subsequent potassium storage performance.

[0052] In addition, N doping can adjust the structure of the carbon layer and optimize its physical and chemical properties such as electronic conductivity and surface hydrophilicity, thereby promoting K + The strong porous carbon matrix will effectively alleviate the poor conductivity and volume expansion problems of antimony phosphate, thereby providing better cycle performance.

[0053] Based on the convenience of implementation by those skilled in the art, the present disclosure also provides a method for preparing phosphate / carbon composite electrode materials.

[0054] Furthermore, the method comprises: Step S1, thermally denitrify the precursor powder obtained by heat-treating and crushing urea using zinc powder, then dezincify with acid solution, wash with water to neutrality, and dry to obtain carbon nanosheets.

[0055] Step S2: using carbon nanosheets, metal chloride, phosphate and ethylene glycol to perform hydrothermal reaction to generate a precipitate, and heat-treating the precipitate.

[0056] A more specific example is as follows: (1) Urea was placed in a combustion boat, heated in a muffle furnace, cooled, and ground into powder using an agate mortar to obtain a g-C3N4 precursor for further use.

[0057] (2) Synthesis of porous carbon nanosheets: The sample described in step (1) is mixed with zinc powder and placed in a tube furnace for high-temperature denitrification treatment to obtain a black solid. The zinc powder is removed with hydrochloric acid, washed with deionized water until neutral, and dried to obtain a carbon nanosheet.

[0058] (3) After mixing the carbon nanosheets described in step (2) with metal chloride, phosphate and ethylene glycol, the mixture is transferred to a hydrothermal reactor for hydrothermal reaction. The precipitate is collected and processed, and heat-treated to obtain a phosphate / carbon composite electrode material.

[0059] Furthermore, the composite electrode material, CMC2200 and conductive carbon black in step (3) are mixed in a mass ratio of 7:1.5:1.5 (or 7:2:1, or 8:1:1, etc.), and the obtained slurry is coated on the copper foil to obtain the negative electrode. The negative electrode is cut into pieces, assembled into a battery, and the electrochemical performance is tested.

[0060] In particular, due to the ideal capacity performance, the above materials can also be considered for the manufacture of supercapacitors.

[0061] The following are several specific examples of the application of the composite material in batteries, wherein the battery is, for example, a button battery, and its typical structure includes, for example, a positive electrode shell, a positive electrode sheet, a separator, a negative electrode sheet, a gasket, a spring sheet, and a negative electrode shell.

[0062] If the specific conditions in the examples are not specified, the experiments were carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased from the market.

[0063] Example 1 1. Place urea in a combustion boat and heat it in a muffle furnace at 5°C min -1 After heating to 550 °C for 5 h, it was cooled and ground into powder using an agate mortar to obtain the g-C3N4 precursor for further use; 2. Put the sample from step (1) and zinc powder in a mortar at a mass ratio of 1:2, grind for 1 hour and mix, then press the tablets at a pressure of 10 MPa. Then put the pressed tablets into a tube furnace and heat them at 5 °C min under argon protection. -1 The temperature was raised to 750°C and kept for 2 hours to obtain a black solid. The excess zinc powder was removed with hydrochloric acid, washed with deionized water until neutral, and dried to obtain a carbon nanosheet. The nitrogen content of the carbon nanosheet was 17.92%, of which pyridine nitrogen accounted for 53.03%; 3. Mix the carbon nanosheets (90 mg) from step (2) with 0.025 mol L -1 SbCl3, 0.075 mol L -1 NH4H2PO 4、 After mixing with 60 mL of ethylene glycol, the mixture was transferred to a hydrothermal reactor and heated to 180 °C for 12 h. The precipitate was collected and treated. The treated precipitate was then placed in argon and annealed at 550 °C for 6 h to obtain a phosphate / carbon composite electrode material.

[0064] (4) The composite electrode material of step (3), CMC2200 and conductive carbon black are mixed in NMP solvent at a ratio of 7:1.5:1.5 to obtain a slurry, which is then coated on a copper foil to obtain a negative electrode; (5) Cut the negative electrode from step (4) into pieces, assemble the battery, and test the electrochemical performance.

[0065] Figure 1 The XRD diagram of the SbPO4 / NC composite material prepared in Example 1, the horizontal axis is the diffraction angle (2Theta), and the vertical axis is the diffraction peak intensity (Intensity); Figure 2 This is a SEM image of the SbPO4 / NC composite material prepared in Example 1; Figure 3 The SbPO4 / NC composite material prepared in Example 1 is used as the negative electrode material of potassium ion battery. -1 The cycle performance test diagram under the conditions of , the horizontal axis is the cycle number (Cycle Number), the left vertical axis is the specific capacitance (Specific Capacity), and the right vertical axis is the Coulomb efficiency (Coulombicefficiency).

[0066] Figure 4 This is a rate performance test graph of the SbPO4 / NC composite material prepared in Example 1 as a negative electrode material for a potassium ion battery, where the horizontal axis is the cycle number and the vertical axis is the specific capacitance.

[0067] Example 2 1. Place urea in a combustion boat and heat it in a muffle furnace at 10°C min -1 After heating to 550 °C for 3 h, it was cooled and ground into powder using an agate mortar to obtain the g-C3N4 precursor for further use; 2. Put the sample from step (1) and zinc powder in a mortar at a mass ratio of 1:1, grind for 1 hour and mix, then press the tablets at a pressure of 10 MPa. Then put the pressed tablets into a tube furnace and heat them at 5 °C min under argon protection.-1 The temperature was raised to 750°C and kept for 2 hours to obtain a black solid. The excess zinc powder was removed with hydrochloric acid, washed with deionized water until neutral, and dried to obtain a carbon nanosheet. The nitrogen content of the carbon nanosheet was 18.79%, of which pyridine nitrogen accounted for 41.70%; 3. Mix the carbon nanosheets (90 mg) from step (2) with 0.025 mol L -1 SbCl3, 0.075 mol L -1 After NH4H2PO4 and 60 mL of ethylene glycol are mixed, they are transferred to a hydrothermal reactor and heated to 180°C for 12 h. The precipitate is collected and treated. The treated precipitate is then placed in argon gas and annealed at 550°C for 6 h to obtain a phosphate / carbon composite electrode material.

[0068] (4) The composite electrode material of step (3) is mixed with CMC2200 and conductive carbon black in a ratio of 7:1.5:1.5 in NMP solvent to obtain a slurry, which is then coated on a copper foil to obtain a negative electrode; (5) Cut the negative electrode from step (4) into pieces, assemble the battery, and test the electrochemical performance.

[0069] Example 3 1. Place urea in a combustion boat and heat it in a muffle furnace at 5 °C min -1 After heating to 550 °C for 5 h, it was cooled and ground into powder using an agate mortar to obtain the g-C3N4 precursor for further use; 2. Put the sample from step (1) and zinc powder in a mortar at a mass ratio of 1:3, grind for 1 hour and mix, then press the tablets at a pressure of 10 MPa. Then put the pressed tablets into a tube furnace and heat them at 5 °C min under argon protection. -1 The temperature was raised to 700°C and kept for 2 hours to obtain a black solid. The excess zinc powder was removed with hydrochloric acid, washed with deionized water until neutral, and dried to obtain a carbon nanosheet. The nitrogen content of the carbon nanosheet was 20.52%, of which pyridine nitrogen accounted for 52.74%; 3. Mix the carbon nanosheets (90 mg) from step (2) with 0.025 mol L -1 SbCl3, 0.075 mol L -1 After NH4H2PO4 and 60 mL of ethylene glycol are mixed, they are transferred to a hydrothermal reactor and heated to 180°C for 12 h. The precipitate is collected and treated. The treated precipitate is then placed in argon gas and annealed at 550°C for 6 h to obtain a phosphate / carbon composite electrode material.

[0070] (4) The composite electrode material of step (3) is mixed with CMC2200 and conductive carbon black in a ratio of 7:1.5:1.5 in NMP solvent to obtain a slurry, which is then coated on a copper foil to obtain a negative electrode; (5) Cut the negative electrode from step (4) into pieces, assemble the battery, and test the electrochemical performance.

[0071] Example 4 1. Place urea in a combustion boat and heat it in a muffle furnace at 5 °C min -1 After heating to 550 °C for 5 h, it was cooled and ground into powder using an agate mortar to obtain the g-C3N4 precursor for further use; 2. Put the sample from step (1) and zinc powder in a mortar at a mass ratio of 1:2, grind for 1 hour and mix, then press the tablets at a pressure of 10 MPa. Then put the pressed tablets into a tube furnace and heat them at 5 °C min under argon protection. -1 The temperature was raised to 750°C and kept for 2 hours to obtain a black solid. The excess zinc powder was removed with hydrochloric acid, washed with deionized water until neutral, and dried to obtain a carbon nanosheet. The nitrogen content of the carbon nanosheet was 17.92%, of which pyridine nitrogen accounted for 53.03%; 3. Mix the carbon nanosheets (90 mg) from step (2) with 0.025 mol L -1 BiCl3, 0.075 mol L -1 After NH4H2PO4 and 60 mL of ethylene glycol are mixed, they are transferred to a hydrothermal reactor and heated to 180°C for 12 h. The precipitate is collected and treated. The treated precipitate is then placed in argon gas and annealed at 550°C for 6 h to obtain a phosphate / carbon composite electrode material.

[0072] (4) The composite electrode material of step (3) is mixed with CMC2200 and conductive carbon black in a ratio of 7:1.5:1.5 in NMP solvent to obtain a slurry, which is then coated on a copper foil to obtain a negative electrode; (5) Cut the negative electrode from step (4) into pieces, assemble the battery, and test the electrochemical performance.

[0073] Example 5 1. Place urea in a combustion boat and heat it in a muffle furnace at 5°C min -1 After heating to 550 °C for 5 h, it was cooled and ground into powder using an agate mortar to obtain the g-C3N4 precursor for further use; 2. Put the sample from step (1) and zinc powder in a mortar at a mass ratio of 1:2, grind for 1 hour and mix, then press the tablets at a pressure of 10 MPa. Then put the pressed tablets into a tube furnace and heat them at 5 °C min under argon protection. -1 The temperature was raised to 750°C and kept for 2 hours to obtain a black solid. The excess zinc powder was removed with hydrochloric acid, washed with deionized water until neutral, and dried to obtain a carbon nanosheet. The nitrogen content of the carbon nanosheet was 17.92%, of which pyridine nitrogen accounted for 53.03%; 3. Mix the carbon nanosheets (90 mg) from step (2) with 0.025 mol L -1SbCl3, 0.075 mol L -1 After mixing NaH2PO4 and 60 mL of ethylene glycol, transfer them to a hydrothermal reactor, heat them to 180°C and keep them warm for 20 hours, collect and treat the precipitate, and then place the treated precipitate in argon gas and anneal at 550°C for 6 hours to obtain a phosphate / carbon composite electrode material.

[0074] (4) The composite electrode material of step (3) is mixed with CMC2200 and conductive carbon black in a ratio of 7:1.5:1.5 in NMP solvent to obtain a slurry, which is then coated on a copper foil to obtain a negative electrode; (5) Cut the negative electrode from step (4) into pieces, assemble the battery, and test the electrochemical performance.

[0075] Example 6 1. Place urea in a combustion boat and heat it in a muffle furnace at 5°C min -1 After heating to 550 °C for 5 h, it was cooled and ground into powder using an agate mortar to obtain the g-C3N4 precursor for further use; 2. Put the sample from step (1) and zinc powder in a mortar at a mass ratio of 1:2, grind for 1 hour and mix, then press the tablets at a pressure of 10 MPa. Then put the pressed tablets into a tube furnace and heat them at 5 °C min under argon protection. -1 The temperature was raised to 750°C and kept for 2 hours to obtain a black solid. The excess zinc powder was removed with hydrochloric acid, washed with deionized water until neutral, and dried to obtain a carbon nanosheet. The nitrogen content of the carbon nanosheet was 17.92%, of which pyridine nitrogen accounted for 53.03%; 3. Mix the carbon nanosheets (90 mg) from step (2) with 0.025 mol L -1 SbCl3, 0.075 mol L -1 After NH4H2PO4 and 60 mL of ethylene glycol are mixed, they are transferred to a hydrothermal reactor and heated to 180°C for 12 h. The precipitate is collected and treated. The treated precipitate is then placed in argon gas and annealed at 600°C for 10 h to obtain a phosphate / carbon composite electrode material.

[0076] (4) The composite electrode material of step (3) is mixed with CMC2200 and conductive carbon black in a ratio of 7:1.5:1.5 in NMP solvent to obtain a slurry, which is then coated on a copper foil to obtain a negative electrode; (5) Cut the negative electrode from step (4) into pieces, assemble the battery, and test the electrochemical performance.

[0077] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.

[0078] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.

Claims

1. A phosphate / carbon composite electrode material, characterized in that: The electrode material is porous and comprises a composite integral structure of a carbon material and a phosphoric acid material, wherein the carbon material is a matrix and the phosphoric acid material is an attachment on the matrix; The carbon material is a nitrogen-doped porous carbon nanosheet in a graphite-like phase, and the phosphoric acid material is a phosphate, and the phosphate is anchored to the carbon nanosheet in the form of particles.

2. The phosphate / carbon composite electrode material according to claim 1, characterized in that: The carbon material is a derivative formed by denitrification of graphite-like carbon nitride (g-C3N4); Alternatively, the particles are in the form of nanowires; Alternatively, the specific surface area of ​​the phosphate / carbon composite electrode material is 260 m² / g; Alternatively, the phosphate is antimony phosphate.

3. A battery pole piece, characterized in that: Contains the phosphate / carbon composite electrode material according to claim 1 or 2.

4. Use of the phosphate / carbon composite electrode material as claimed in claim 1 or 2 in a potassium ion battery, characterized in that: The phosphate / carbon composite electrode material is used as the negative electrode material of the potassium ion battery.

5. A method for preparing a phosphate / carbon composite electrode material, characterized in that: The method comprises: Thermally denitrifying the precursor powder obtained by heat-treating and pulverizing urea using zinc powder, dezincifying the precursor powder using acid solution, washing the precursor powder with water until the precursor powder is neutral, and drying the precursor powder to obtain carbon nanosheets; and Carbon nanosheets, metal chloride, phosphate and ethylene glycol are subjected to a hydrothermal reaction to generate a precipitate, and the precipitate is heat-treated.

6. The method for preparing a phosphate / carbon composite electrode material according to claim 5, characterized in that: The method for heat treating urea comprises: heating urea at a preset temperature system, wherein the temperature system is: 2-10°C·min -1 The temperature is raised to 500° C. to 600° C. at a speed of 100° C., and kept at this temperature for 3 to 10 hours; Optionally, the heat treatment of urea is carried out by placing the urea in a combustion boat and heating it in a muffle furnace. Optionally, the pulverization operation is carried out by grinding in an agate mortar. Alternatively, the method of thermally denitrifying a precursor powder using zinc powder comprises: mixing the precursor powder with zinc powder and pressing the tablets, and then calcining in an inert atmosphere; Optionally, the mixing method is grinding, and the tableting pressure is 5 to 20 MPa; Optionally, the temperature regime of the calcination process is: 5-10°C·min -1 The temperature is raised to 700°C to 850°C at a rate of 100°C and maintained at this temperature for 2 to 6 hours.

7. The method for preparing a phosphate / carbon composite electrode material according to claim 5, characterized in that: The concentration of metal chloride is 0.02~0.05mol L -1 Provided in the form of SbCl3 or BiCl3; Optionally, phosphate is used at a concentration of 0.05-0.1 mol L -1 Provided in the form of NH4H2PO4 or NaH2PO4; Optionally, a hydrothermal reaction kettle with a volume of 100 mL is used during the hydrothermal reaction, the amount of carbon nanosheets used is 60-150 g, and the amount of ethylene glycol used is 60 mL; Optionally, the carbon nanosheets, metal chloride, phosphate and ethylene glycol are dispersed by ultrasonic wave in a water bath heated at a temperature of 50° C. to 70° C. to form a dispersion, and the dispersion is used for a hydrothermal reaction; Optionally, the temperature of the hydrothermal reaction is 160° C. to 200° C., and the reaction time is 2 hours to 24 hours.

8. The method for preparing a phosphate / carbon composite electrode material according to claim 5, characterized in that: The heat treatment method for the precipitate is annealing; Optionally, the annealing atmosphere is nitrogen or argon; Optionally, the annealing temperature is 500-600° C., and the annealing time is 4-10 hours.

9. A method for preparing a battery electrode, characterized in that: include: Providing a phosphate / carbon composite electrode material as claimed in claim 1 or 2, or a phosphate / carbon composite electrode material obtained by implementing the method for preparing a phosphate / carbon composite electrode material as claimed in any one of claims 5 to 8; as well as The slurry of the phosphate / carbon composite electrode material mixed with CMC2200, conductive carbon black and NMP solvent is coated on a copper foil.

10. The method for preparing a battery pole piece according to claim 9, characterized in that: The mass ratio of the phosphate / carbon composite electrode material to CMC2200 and the conductive carbon black is 7:1.5:1.5, or 7:2:1, or 8:1:1.

Citation Information

Patent Citations

  • Carbon nitride material, preparation method of carbon nitride material, gas-sensitive sensor and preparation method of gas-sensitive sensor

    CN104671244A

  • Preparation of cuprous oxide modified antimony phosphate composite photocatalyst

    CN108452818A

  • A preparation of antimony phosphate modified graphene carbon nitride composite photocatalyst

    CN108479830A

  • Transition metal doped two-dimensional carbon nanosheet as well as preparation method and application thereof

    CN112952119A

  • Preparation method of SbPO4 / nitrogen-doped carbon composite material

    CN113479860A