Preparation process of sodium ion battery positive electrode material
Through a two-step calcination process and the preparation process of the positive electrode material of the molten sodium ion battery accelerated by acid solution, the problems of uneven composition and incomplete reaction caused by calcination in high-temperature stages are solved, and the electrochemical performance and cycle stability of the material are improved.
Patent Information
- Application Number
- CN202411086307.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-12-06
AI Technical Summary
The direct calcination of existing sodium ion battery positive electrode materials in the high temperature section leads to uneven composition and incomplete reactions, resulting in unstable crystal structures, affecting electrochemical performance.
A two-step calcination process is adopted, first performing the first calcination in the low-temperature section, then heating to the high-temperature section for solid phase reaction, and acid liquid is added when mixing to accelerate the melting of raw materials to ensure uniformity of the material mixing and completeness of the reaction.
The crystal phases of the generated cathode material are more uniform, avoiding local overreaction or incompleteness, and improving electrochemical performance and cycling stability.
Smart Images

Figure BDA0004985275570000051
Abstract
Description
Technical Field
[0001] The present invention relates to the field of sodium ion batteries, and in particular to a process for preparing a positive electrode material for a sodium ion battery. Background Art
[0002] Sodium-ion battery is a rechargeable battery that mainly relies on the movement of sodium ions between the positive and negative electrodes to work, similar to lithium-ion batteries. The concept of sodium-ion battery started in the 1980s, almost at the same time as lithium-ion batteries. The working principle of sodium-ion battery is similar to that of lithium-ion battery. When charging, Na + The electrons are released from the positive electrode material, embedded in the negative electrode material through the electrolyte, and transferred to the negative electrode through the external circuit to maintain charge balance; the opposite is true during discharge. The key factor restricting the performance of sodium-ion batteries lies in the positive electrode material. Among them, layered oxides are used as positive electrode materials. In the existing preparation process, the raw materials are often directly mixed evenly, and then solidified in the high temperature section. However, calcination directly in the high temperature section often makes its composition uneven, the reaction is incomplete, and it is easy to cause local excess generation of unstable crystalline structures, thereby affecting the performance of the positive electrode active material. Summary of the invention
[0003] The purpose of the present invention is to solve at least one of the technical problems existing in the prior art and to provide a process for preparing a positive electrode material for a sodium ion battery.
[0004] The technical solution of the present invention is as follows:
[0005] A process for preparing a positive electrode material for a sodium ion battery comprises the following steps:
[0006] Add pyrolusite, iron source and sodium carbonate according to different amounts of substances, continue to add acid solution, then grind, and carry out solid phase reaction to obtain positive electrode active material, wherein the solid phase reaction is specifically: first calcination at 200-500°C, then heating to 800-1000°C for second calcination, cooling, and obtaining.
[0007] As a preferred embodiment of the present invention, the first calcination time is 3-5 hours, and the second calcination time is 6-10 hours.
[0008] As a preferred embodiment of the present invention, the grinding specifically comprises grinding the pyrolusite, the iron source and the sodium carbonate to 40-60 nm.
[0009] As a preferred embodiment of the present invention, the acid solution is acetic acid.
[0010] As a preferred embodiment of the present invention, the concentration of acetic acid is 5-12 wt %.
[0011] As a preferred embodiment of the present invention, the heating rate of the first calcination is 3-5°C / min; the heating rate of the second calcination is 1-3°C / min.
[0012] As a preferred embodiment of the present invention, the particle size of the pyrolusite and the iron source is controlled at 100-200 meshes.
[0013] The beneficial effects of the present invention are:
[0014] (1) In the preparation process of a positive electrode material for a sodium ion battery of the present invention, the raw materials are first calcined in a low temperature section and then enter a high temperature section for solid phase reaction, so that the crystal phase of the generated material is more uniform, avoiding the conventional method of directly using a high temperature section curing reaction to cause excessive or incomplete local reaction, resulting in non-uniform crystal phase of the product, thereby affecting the electrochemical performance of the positive electrode active material.
[0015] (2) The present invention provides a process for preparing a positive electrode material for a sodium ion battery. By adding acid during mixing, the surfaces of iron and manganese are dissolved in the acid solution, which can accelerate the melting of the raw materials, making the fused materials more evenly mixed, and more conducive to the subsequent high-temperature solid-phase reaction, that is, the reaction is more complete, and the crystal structure of the generated product is more uniform. DETAILED DESCRIPTION
[0016] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. If no specific techniques or conditions are specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used that do not specify the manufacturer are all conventional products that can be obtained commercially.
[0017] Example 1 (P2)
[0018] A process for preparing a positive electrode material for a sodium ion battery comprises the following steps:
[0019] Pyrolusite, an iron source and sodium carbonate were added in a molar ratio of manganese ion, iron ion and sodium ion of 0.9:0.1:0.7, and acetic acid was added, and then ground to 50 nm, and a solid phase reaction was carried out to obtain a positive electrode active material, wherein the solid phase reaction was specifically: a first calcination at 350°C, and then the temperature was raised to 950°C for a second calcination, and cooled to obtain the iron source using iron carbonate.
[0020] The first calcination time is 4 hours, and the second calcination time is 8 hours.
[0021] The concentration of the acetic acid is 5 wt %.
[0022] The heating rate of the first calcination is 4°C / min; the heating rate of the second calcination is 2°C / min.
[0023] The particle size of the pyrolusite and the iron source is controlled at 100 meshes.
[0024] Example 2
[0025] A process for preparing a positive electrode material for a sodium ion battery comprises the following steps:
[0026] Pyrolusite, an iron source and sodium carbonate were added in a molar ratio of manganese ion, iron ion and sodium ion of 0.9:0.1:0.7, and acetic acid was added, and then ground to 50 nm, and a solid phase reaction was carried out to obtain a positive electrode active material, wherein the solid phase reaction was specifically: a first calcination at 350°C, and then the temperature was raised to 950°C for a second calcination, and cooled to obtain the iron source using iron carbonate.
[0027] The first calcination time is 4 hours, and the second calcination time is 8 hours.
[0028] The concentration of the acetic acid is 8 wt %.
[0029] The heating rate of the first calcination is 4°C / min; the heating rate of the second calcination is 2°C / min.
[0030] The particle size of the pyrolusite and the iron source is controlled at 100 meshes.
[0031] Example 3
[0032] A process for preparing a positive electrode material for a sodium ion battery comprises the following steps:
[0033] Pyrolusite, an iron source and sodium carbonate were added in a molar ratio of manganese ion, iron ion and sodium ion of 0.9:0.1:0.7, and acetic acid was added, and then ground to 50 nm, and a solid phase reaction was carried out to obtain a positive electrode active material, wherein the solid phase reaction was specifically: a first calcination at 350°C, and then the temperature was raised to 950°C for a second calcination, and cooled to obtain the iron source using iron carbonate.
[0034] The first calcination time is 4 hours, and the second calcination time is 8 hours.
[0035] The concentration of the acetic acid was 12 wt %.
[0036] The heating rate of the first calcination is 4°C / min; the heating rate of the second calcination is 2°C / min.
[0037] The particle size of the pyrolusite and the iron source is controlled at 100 meshes.
[0038] Example 4 (without addition of acid solution)
[0039] This example is a variation of Example 2, specifically, no acetic acid is added.
[0040] Example 5 (O3)
[0041] This example is a variation of Example 2, specifically, pyrolusite, an iron source, and sodium carbonate are added in a molar ratio of manganese ions, iron ions, and sodium ions of 0.9:0.1:1.
[0042] Example 6 (O3+P2)
[0043] This example is a variation of Example 2, specifically, pyrolusite, an iron source, and sodium carbonate are added in a molar ratio of manganese ions, iron ions, and sodium ions of 0.9:0.1:0.9.
[0044] Example 7
[0045] This example is a variation of Example 6, specifically, chromium trioxide is further added in the solid phase reaction. Specifically, pyrolusite, iron source, sodium carbonate, and chromium trioxide are added according to the molar ratio of manganese ion, iron ion, sodium ion, and chromium ion of 0.9:0.1:0.9:0.01.
[0046] Comparative Example 1
[0047] A process for preparing a positive electrode material for a sodium ion battery comprises the following steps:
[0048] Pyrolusite, an iron source and sodium carbonate were added in a molar ratio of manganese ion, iron ion and sodium ion of 0.9:0.1:0.7, and a solid phase reaction was carried out to obtain a positive electrode active material, wherein the solid phase reaction was specifically as follows: heating to 950°C at a heating rate of 2°C / min, calcining for 10 hours, and cooling to obtain the positive electrode active material.
[0049] The particle size of the pyrolusite and the iron source is controlled at 100 meshes.
[0050] The first discharge gram capacity and 1000 cycles of the sodium ion battery (finished battery) made of the positive electrode active material of the above embodiment were tested. The test results are shown in Table 1.
[0051] Table 1 Performance test results of embodiments and comparative examples
[0052]
[0053] As can be seen from the above table, the performance of Example 4 is better than that of Comparative Example 1. The main reasons may be as follows: the embodiment first calcines the raw materials in the low temperature section, and then enters the high temperature section for solid phase reaction, so that the crystal phase of the generated material is more uniform, avoiding the traditional method of directly using the high temperature section curing reaction to cause excessive or incomplete local reaction, making the product crystal phase non-uniform, thereby affecting the electrochemical performance of the positive electrode active material; wherein the performance of Examples 1-3 is further optimized than that of Example 4, which may be due to the fact that the embodiment can accelerate the melting between the raw materials by adding an acidic environment in the low temperature section, so that the fused materials are mixed more evenly, which is more conducive to the subsequent high temperature solid phase reaction, and the crystal phase structure of the generated product is more uniform. While Examples 5 (O3) and 6 (mixture) adjust the ratio of the raw materials to obtain active materials with different crystal phase structures from Example 2 (P2), thereby affecting the electrochemical performance, that is, the O3 crystal has an ultra-high discharge electrochemical capacity. And O3 is easy to transform to O2, resulting in capacity loss in electrochemistry, causing electrochemical deterioration, but the cycle performance is better. Therefore, by adjusting the amount of raw materials added, a mixture of P2 and O3 structures can be obtained (Example 5), and a mixed structure with excellent comprehensive performance is obtained; in Example 7, by adding chromium trioxide, the structure of the active material obtained is more stable, thereby improving the electrochemical properties of the material.
[0054] The above-mentioned embodiments only express the preferred implementation modes of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, various other corresponding changes and deformations can be made according to the technical solutions and concepts described above, and all these changes and deformations should fall within the scope of protection of the claims of the present invention.
Claims
1. A process for preparing a positive electrode material for a sodium ion battery, characterized in that: The following steps are involved: Add pyrolusite, iron source and sodium carbonate according to different amounts of substances, continue to add acid solution, then grind, and carry out solid phase reaction to obtain positive electrode active material, wherein the solid phase reaction is specifically: first calcination at 200-500°C, then heating to 800-1000°C for second calcination, cooling, and obtaining.
2. The process for preparing a sodium ion battery positive electrode material according to claim 1, characterized in that: The first calcination time is 3-5 hours, and the second calcination time is 6-10 hours.
3. The process for preparing a positive electrode material for a sodium ion battery according to claim 1, characterized in that: The grinding specifically comprises grinding pyrolusite, iron source and sodium carbonate to 40-60 nm.
4. The process for preparing a positive electrode material for a sodium ion battery according to claim 1, characterized in that: The acid solution is acetic acid.
5. The process for preparing a positive electrode material for a sodium ion battery according to claim 4, characterized in that: The concentration of the acetic acid is 5-12 wt %.
6. The process for preparing a sodium ion battery positive electrode material according to claim 1, characterized in that: The heating rate of the first calcination is 3-5°C / min; the heating rate of the second calcination is 1-3°C / min.
7. The process for preparing a positive electrode material for a sodium ion battery according to claim 1, characterized in that: The particle sizes of the pyrolusite and the iron source are controlled at 100-200 meshes.