Solvent-free polyurethane resin for ball leather as well as preparation method and application of solvent-free polyurethane resin
By using solvent-free polyurethane resin composed of polyester polyol PDS-EO and polyisocyanate, the problems of poor flatness and low hot melt strength during the processing process are solved, and high fineness and strength of bubble cells are achieved The polyurethane foam layer meets the application needs of thick ball leather.
Patent Information
- Application Number
- CN202411399087.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, 2-5mm thick solvent-free polyurethane ball leather is prone to problems such as poor flatness, difficulty in laying the fabric base and low hot melt strength during processing, resulting in less application.
Using solvent-free polyurethane resin composed of polyester polyol PDS-EO, polyisocyanate and sealing agent, through specific group distribution ratios and process conditions, polyurethane foam with high cell fineness, peel strength and hot melt strength is formed. layer.
It has achieved the effect of good flatness, high cloth-based bonding tolerance and high hot welding strength of 2-5mm thick solvent-free polyurethane ball leather, which meets the processing requirements of thick ball leather.
Smart Images

Figure BDA0005074686360000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional polyurethane resins, and specifically relates to a solvent-free polyurethane resin for ball leather and a preparation method thereof, and application of the solvent-free polyurethane resin in preparing ball leather. Background Art
[0002] In the production of traditional ball leather, the bonding layer resin used to bond the ball surface and the inner elastic substrate is mainly solvent-based polyurethane resin. However, it is difficult to completely remove the organic solvent during the processing, so the finished ball leather often has a certain amount of solvent left. Therefore, it is an inevitable trend for solvent-free polyurethane ball leather to replace solvent-based polyurethane ball leather.
[0003] Ball leather is usually made of multiple layers of material, among which the middle foam layer is generally required to have a certain thickness and high elasticity, so that the ball can immediately return to its original shape after being kicked or deformed by impact, to ensure the best flight or movement trajectory of the ball. The common middle foam layer of the ball is a polyolefin polymer material, which has the disadvantage of low melting temperature. When hot cutting, the polyurethane surface layer has not yet melted, but the middle foam layer has melted, resulting in hot cutting failure, and the surface layer and the foam layer are separated. With the continuous development and update of synthetic leather technology, its physical properties have approached or even exceeded those of natural leather. The application of polyurethane foam materials in ball leather is increasing, but 2-5mm thick solvent-free polyurethane ball leather products are extremely rare.
[0004] The melting temperatures of the polyurethane foam layer and the polyurethane surface layer are close, so there is generally no problem of hot cutting delamination. However, solvent-free polyurethane foam ball leather is prone to problems such as poor flatness, difficulty in bonding the cloth base, and low hot melt strength during processing.
[0005] It is precisely because of the above-mentioned technical difficulties that 2-5mm thick solvent-free polyurethane ball leather products are rarely seen. Summary of the invention
[0006] In view of this, the primary purpose of the present invention is to provide a solvent-free polyurethane resin for ball leather, which can solve the problems of poor flatness, difficult cloth base bonding and low hot melt strength of 2-5mm thick solvent-free polyurethane ball leather, and the formed polyurethane foam layer has the advantages of fine pores, high peel strength and hot cutting welding strength.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] The present invention first provides a solvent-free polyurethane resin for ball leather, wherein the solvent-free polyurethane resin for ball leather comprises component A and component B;
[0009] In parts by mass, the component A comprises 85-95 parts of polyester polyol PDS-EO, 5-15 parts of polyol and 0.3-0.5 parts of crosslinking agent; the component B comprises 40-80 parts of polyisocyanate, 50-100 parts of polyester polyol PDS-EO and 3-8 parts of blocking agent;
[0010] The polyester polyol PDS-EO is prepared by polycondensation reaction of long carbon chain polyacid, long carbon chain polyol, small molecule diol, trimethylolpropane, polyethylene glycol monomethyl ether and a catalyst.
[0011] In a further embodiment, the hydroxyl value of the polyester polyol PDS-EO is 28-56 mgKOH / g.
[0012] In a further embodiment, the raw materials for preparing the polyester polyol PDS-EO are, by weight, 88-145 parts of long-chain polyacids, 55-105 parts of long-chain polyols, 5-15 parts of small-molecule diols, 2-3 parts of trimethylolpropane, 6-21 parts of polyethylene glycol monomethyl ether and 0.01-0.03 parts of catalysts.
[0013] In a further embodiment, the long-chain polyacid is one of dimer acid, 1,10-decanedioic acid, and 1,8-octanedioic acid; and / or the long-chain polyol is one of 1,10-decanediol and 1,2-octanediol; and / or the small molecule diol is ethylene glycol.
[0014] In a further embodiment, the added amounts of trimethylolpropane and polyethylene glycol monomethyl ether are kept the same.
[0015] In a further embodiment, the polyethylene glycol monomethyl ether is a monohydroxy compound with a number average molecular weight of 400-1200.
[0016] In a further embodiment, in the component A, the polyol is any one of ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 2-methyl-1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, neopentyl glycol, and diethylene glycol, or a combination of two or more thereof;
[0017] And / or, the cross-linking agent is at least one of glycerol and trimethylolpropane.
[0018] In a further embodiment, the component A further comprises any one or a combination of two or more of a pore leveling agent, a catalyst, and water.
[0019] In a further embodiment, the content of the pore leveling agent in the component A is 0.3 to 1.5 parts; and / or, the content of the catalyst in the component A is 0.01 to 2 parts; and / or, the content of water in the component A is 0.8 to 1.5 parts.
[0020] In a further embodiment, in the component B, the polyisocyanate is at least one of 4,4'-diphenylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate.
[0021] And / or, the blocking agent is at least one of methyl ethyl ketone oxime, 3,5-dimethylpyrazole, diethyl malonate, acetanilide, and 1,2,4-triazole.
[0022] In a further embodiment, the component B also includes an antioxidant.
[0023] In a further embodiment, the content of the antioxidant in the component B is 0.1 to 0.3 parts.
[0024] In a further embodiment, the mass ratio of component A to component B is 100:90 to 100:170.
[0025] The present invention further provides a method for preparing the solvent-free polyurethane resin for ball leather as described above, comprising the following steps:
[0026] The polyester polyol PDS-EO, polyol, crosslinking agent and other optional auxiliary agents are mixed and reacted to obtain component A;
[0027] The polyisocyanate, polyester polyol PDS-EO, blocking agent and other optional additives are reacted until the NCO content is tested to be qualified to obtain component B;
[0028] The components A and B are fully mixed, and cured at 130-140° C. to obtain a solvent-free polyurethane resin for ball leather.
[0029] In a further embodiment, in the step of obtaining component A, the temperature of the mixing reaction is 50-70°C.
[0030] In a further embodiment, in the step of obtaining component B, the reaction temperature is 70-90°C.
[0031] The present invention further provides a solvent-free polyurethane ball leather, which contains the solvent-free polyurethane resin for ball leather as described above or the solvent-free polyurethane resin for ball leather prepared by the preparation method described above.
[0032] In a further embodiment, the preparation of the solvent-free polyurethane ball leather comprises the following steps:
[0033] Component A and component B are coated on the polyurethane surface layer according to the proportion, pre-reacted at 80-100°C for 50-70s, and bonded to the base fabric; then, the reaction is performed at 130-140°C to cure and form, so as to obtain solvent-free polyurethane ball leather.
[0034] Beneficial effects of the present invention:
[0035] The present invention adds polyester polyol PDS-EO to component A and component B. The polyester polyol PDS-EO has the characteristics of long carbon chain and easy emulsification. On the one hand, the side chain of the polyester polyol PDS-EO contains hydrophilic polyethylene glycol (PEO) chain forging, so that water in the foaming system can be more evenly emulsified and dispersed in the polyurethane resin, thereby obtaining more delicate and uniform pores, which is beneficial to improving the flatness of leather making and the regularity of hot-cut melting cross-section; on the other hand, the polyester polyol PDS-EO has a long carbon chain main chain, and has a lower ester group density and better hydrophobicity than ordinary adipic acid series polyester polyols, wherein the low ester group density and low cohesive force can obtain better open porosity, which can effectively prevent the shrinkage of polyurethane foam, and the better hydrophobicity is beneficial to the improvement of hydrolysis resistance; in addition, the long carbon chain polyester polyol shows strong crystallinity, so that the leather is easy to hot-cut, and the peeling strength and hot-cut welding strength are high.
[0036] At the same time, the present invention adds a sealing agent to the B component, so that the reaction degree of the solvent-free polyurethane resin can be controlled, which solves the problem of "surface drying" during the lamination of thick polyurethane foam of 2-5 mm, and is beneficial to the lamination operation tolerance of the cloth base; after the cloth is pasted, the sealed isocyanate is unblocked and placed in a 130-140° C. oven to continue the aging reaction with the excess polyol to obtain a ball leather with better mechanical properties. DETAILED DESCRIPTION
[0037] Embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.
[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0039] The first aspect of the present invention provides a solvent-free polyurethane resin for ball leather, wherein the solvent-free polyurethane resin for ball leather comprises component A and component B;
[0040] In parts by mass, the component A comprises 85-95 parts of polyester polyol PDS-EO, 5-15 parts of polyol and 0.3-0.5 parts of crosslinking agent; the component B comprises 40-80 parts of polyisocyanate, 50-100 parts of polyester polyol PDS-EO and 3-8 parts of blocking agent;
[0041] The polyester polyol PDS-EO is prepared by polycondensation reaction of long carbon chain polyacid, long carbon chain polyol, small molecule diol, trimethylolpropane, polyethylene glycol monomethyl ether and a catalyst.
[0042] The invention adds polyester polyol PDS-EO with long carbon chain and easy emulsification into components A and B, and adds a sealing agent into component B, so that the polyurethane foam layer formed by subsequent leather making has the advantages of good flatness, fine pores, high peeling strength and hot cutting welding strength.
[0043] The polyester polyol PDS-EO described herein is formed by subjecting a long carbon chain polyacid, a long carbon chain polyol, a small molecule diol, trimethylolpropane, polyethylene glycol monomethyl ether and a catalyst to polycondensation reaction, and then removing the small molecule diol. In the present invention, its hydroxyl value is 28-56 mgKOH / g, for example, it can be 28 mgKOH / g, 30 mgKOH / g, 32 mgKOH / g, 35 mgKOH / g, 40 mgKOH / g, 48 mgKOH / g, 50 mgKOH / g, 56 mgKOH / g, etc.
[0044] The long-chain polyacid described herein refers to an organic acid having 8 or more carbon atoms in the molecular formula, and specific examples include dimer acid, 1,10-decanedioic acid, and 1,8-octanedioic acid, but are not limited thereto.
[0045] The long carbon chain polyol described herein refers to an organic alcohol having 8 or more carbon atoms in the molecular formula, and specific examples thereof include 1,10-decanediol and 1,2-octanediol, but are not limited thereto.
[0046] The small molecule diol described in this article is mainly used to reduce the acid value of the system in the early stage of the reaction, and can be removed in the later stage. Therefore, diols with small molecular weight that are more common in the field should be selected as much as possible to facilitate later removal; preferably, the small molecule diol is ethylene glycol.
[0047] The main function of trimethylolpropane and polyethylene glycol monomethyl ether herein is to introduce trifunctionality and monofunctionality structure into the structure of polyester polyol, and introduce hydrophilic group at the same time. In some specific implementation cases of the present invention, the addition amount of trimethylolpropane and polyethylene glycol monomethyl ether keeps the same amount of substance. The polyethylene glycol monomethyl ether is a monohydroxy compound with a number average molecular weight of 400-1200.
[0048] The catalyst described herein is a relatively conventional catalyst in the art that can promote the efficiency of polycondensation reaction, and a specific example is tetraisopropyl titanate, but it is not limited thereto.
[0049] In the present invention, the raw materials for preparing the polyester polyol PDS-EO are calculated by weight as follows: 88-145 parts of long carbon chain polyacid, 55-105 parts of long carbon chain polyol, 5-15 parts of small molecule diol, 2-3 parts of trimethylolpropane, 6-21 parts of polyethylene glycol monomethyl ether and 0.01-0.03 parts of catalyst. The specific amount of each raw material can be adjusted or optimized according to actual needs.
[0050] In some specific implementation cases of the present invention, the polyester polyol PDS-EO is prepared according to the following method:
[0051] Taking a long carbon chain polyacid, a long carbon chain polyol, a small molecule diol, trimethylolpropane and polyethylene glycol monomethyl ether, and carrying out a dehydration polycondensation reaction under a protective atmosphere;
[0052] When the detected acid value is ≤20 mgKOH / g, a catalyst is added to continue the reaction, and then the temperature is gradually raised to 240°C and the vacuum degree is ≥0.095 MPa. After removing the small molecular diol, a polyester polyol PDS-EO with a hydroxyl value of 28-56 mgKOH / g is obtained.
[0053] It is understandable that the protective atmosphere is an inert or inactive gas commonly used in the art, and specific examples include nitrogen or a rare gas (such as helium, argon, etc.).
[0054] Furthermore, the component A and the component B described herein are respectively the polyol component and the isocyanate component in the two-component polyurethane foaming material.
[0055] Among them, according to needs, in addition to polyester polyol, polyol and cross-linking agent, component A also includes other functional additives, such as pore leveling agent, catalyst, any one or a combination of two or more in water, which can be selected according to needs.
[0056] In some specific implementation cases of the present invention, the component A is composed of 85-95 parts of polyester polyol PDS-EO, 5-15 parts of polyol, 0.3-0.5 parts of crosslinking agent, 0.3-1.5 parts of pore leveling agent, 0.01-2 parts of catalyst and 0.8-1.5 parts of water by weight. However, it can be understood that the functional additives contained in the component A can be selected or added according to the actual performance requirements, and are not limited to the above composition.
[0057] Among them, the polyol is mainly used for chain growth. It can react with the functional groups on the polymer chain to extend the molecular chain and increase the molecular weight. Conventional components in this field can be used. Specific examples include but are not limited to one of ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 2-methyl-1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, neopentyl glycol, and diethylene glycol.
[0058] The cross-linking agent is mainly used to promote the cross-linking of component A and component B, and specific examples include but are not limited to one of glycerol and trimethylolpropane.
[0059] The pore leveling agent, catalyst, etc. can all be conventional types in the art. For example, the pore leveling agent can be one of Silbyk TP 3796, Silbyk 9100, Silbyk 9103, Silbyk 9115, and Silbyk 9120; the catalyst can be a delayed-type environmentally friendly metal catalyst, such as one of BiCAT 8106, BiCAT 8108, BiCAT 8124, BiCAT 3228, Borchi Kat 22, Borchi Kat 24, BiCAT 4130, and BiCAT 4232.
[0060] Similarly, in addition to some essential ingredients, component B may also contain some functional additives, such as antioxidants, according to performance requirements. In some specific implementation cases of the present invention, component B is composed of 40-80 parts of polyisocyanate, 50-100 parts of polyester polyol PDS-EO, 3-8 parts of blocking agent and 0.1-0.3 parts of antioxidant in parts by mass.
[0061] The polyisocyanate is the main raw material for preparing polyurethane resin in the art, usually diisocyanate, and specific examples thereof include 4,4'-diphenylmethane diisocyanate (MDI-100), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), 4,4'-dicyclohexylmethane diisocyanate (HDI), 12 MDI), but not limited thereto.
[0062] The blocking agent is at least one of methyl ethyl ketone oxime, 3,5-dimethylpyrazole, diethyl malonate, acetanilide, and 1,2,4-triazole. By adding the blocking agent, the polyisocyanate is blocked, and after the pre-reaction, part of the blocked isocyanate is not unblocked, so that the reaction degree is reliable, and the laminating process of the base cloth is wide and easy to operate; when the curing reaction continues, the blocked isocyanate is completely unblocked, and the solvent-free polyurethane resin can fully cure and react, thereby solving the problem of difficult lamination and obtaining ball leather with excellent performance.
[0063] The antioxidant may be any conventional antioxidant in the art, such as 245, 1010, 1035, 1076, 1098 or 3114, but is not limited thereto.
[0064] Furthermore, the ratio of component A to component B can be adjusted as needed. In the implementation case of the present invention, the mass ratio of component A to component B is 100:90 to 100:170.
[0065] The second aspect of the present invention provides a method for preparing the solvent-free polyurethane resin for ball leather as described above, comprising the following steps:
[0066] The polyester polyol PDS-EO, polyol, crosslinking agent and other optional auxiliary agents are mixed and reacted to obtain component A;
[0067] The polyisocyanate, polyester polyol PDS-EO and blocking agent are reacted until the NCO content is tested to be qualified to obtain component B;
[0068] The components A and B are fully mixed, and cured at 130-140° C. to obtain a solvent-free polyurethane resin for ball leather.
[0069] Preferably, in the step of obtaining component A, the temperature of the mixing reaction is 50-70°C.
[0070] Preferably, in the step of obtaining component B, the reaction temperature is 70-90°C.
[0071] The third aspect of the present invention provides a solvent-free polyurethane ball leather, which contains the solvent-free polyurethane resin for ball leather as described above or the solvent-free polyurethane resin for ball leather prepared by the preparation method described above.
[0072] It is understandable that the ball leather also includes a polyurethane surface layer, a cloth base, etc., which are not particularly limited and can be any conventional type in the art.
[0073] In some specific implementation cases of the present invention, the preparation of the solvent-free polyurethane ball leather comprises the following steps:
[0074] Component A and component B are coated on the polyurethane surface layer according to the proportion, pre-reacted at 80-100°C for 50-70s, and bonded to the base fabric; then, the reaction is performed at 130-140°C to cure and form, so as to obtain solvent-free polyurethane ball leather.
[0075] The solvent-free polyurethane ball leather obtained by the present invention has good flatness. For example, in some specific embodiments of the present invention, the product needs to be 3.0 mm in size, with a thickness between 3.0 and 3.1 mm, and a density of the solvent-free polyurethane foam layer of 240 to 260 kg / cm 3 The peel strength between the foam layer and the cloth base can reach more than 60N / 3cm, and the hot cutting welding tensile force can reach more than 100N / 2.54cm, which can meet the downstream 4-piece ball making processing requirements.
[0076] The present invention is described below by means of specific examples. It should be noted that the following specific examples are only for illustrative purposes and do not limit the scope of the present invention in any way. In addition, unless otherwise specified, methods without specific conditions or steps are conventional methods, and the reagents and materials used can be obtained from commercial channels.
[0077] The raw materials used in the following examples are:
[0078] HMDI, MDI, and IPDI are isocyanates produced by Yantai Wanhua Company; antioxidants such as 1076 are produced by Double Bond Chemical Co., Ltd. in Taiwan Province of China; catalysts such as MB-20 are produced by Air Products and Chemicals, Inc. of the United States; tetraisopropyl titanate is a catalyst produced by Osjia Materials Technology Co., Ltd.; Silbyk 9100 and other pore leveling agents are produced by BYK; the surface layer resin LT-95 is a polyurethane resin produced by Hefei Amway Polyurethane New Materials Co., Ltd.; dimer acid, sebacic acid, ethylene glycol, 1,4-butanediol, propylene glycol, trimethylolpropane, methyl ethyl ketone oxime, etc. are commercially available products.
[0079] Example 1
[0080] 1. This embodiment first provides a method for preparing an easily emulsifiable long-chain polyester polyol, and the specific steps are as follows:
[0081] A four-necked flask equipped with a magnetic stirrer, a constant pressure burette, a thermometer, a N2 inlet tube and an air-cooled condenser was installed in a mantle-type resistance heater, and dimer acid (145 g), 1,2-octanediol (55 g), ethylene glycol (5 g), trimethylolpropane (2 g) and polyethylene glycol monomethyl ether (molecular weight 400, 6 g) were added into the four-necked flask; then, the temperature was gradually increased under nitrogen protection to carry out a dehydration polycondensation reaction, and the top temperature of the condenser was controlled to be lower than 100°C during the heating process; when the detected acid value was not greater than 20 mgKOH / g, a catalyst tetraisopropyl titanate (0.01 g) was added and the reaction was continued for 30 minutes, and then the temperature was gradually increased to 240°C, and the vacuum degree was ≥0.095 MPa, and after the ethylene glycol was removed, an easily emulsifiable long carbon chain polyester polyol PDS-EO with a hydroxyl value of 56 mgKOH / g was obtained.
[0082] 2. This embodiment further provides a method for preparing a solvent-free polyurethane resin based on the polyester polyol prepared above. The specific steps are as follows:
[0083] Preparation of component A:
[0084] PDS-EO (95 g) was added into a reactor, followed by ethylene glycol (5 g), trimethylolpropane (0.3 g), pore leveler Silbyk TP 3796 (0.3 g), catalyst BiCAT 8106 (0.01 g) and water (0.8 g). The mixture was stirred and reacted at 50°C for 4 h to obtain component A.
[0085] Preparation of component B:
[0086] MDI-100 (60 g) and antioxidant 245 (0.3 g) were put into a reactor and stirred to mix evenly, followed by adding PDS-EO (50 g), heating to 70° C. and stirring to react for 3 h; then adding blocking agent methyl ethyl ketone oxime (8 g), stirring to react at 70° C. for 4 h until the NCO content was tested to be qualified, and component B was obtained.
[0087] Preparation of solvent-free polyurethane resin:
[0088] Component A and component B are placed in a low-pressure casting machine at a mass ratio of 100:90 and fully mixed, and reacted at 130° C. for 8 minutes to obtain a solvent-free polyurethane resin.
[0089] 3. This embodiment further provides a ball leather prepared based on the above solvent-free polyurethane resin, which is specifically prepared as follows:
[0090] The surface resin slurry LT-95 was coated on the release paper, and the polyurethane surface layer was obtained after drying at 130°C for 2 minutes;
[0091] The solvent-free A component and B component are fully mixed in a mass ratio of 100:90 through a low-pressure casting machine and coated on the surface layer. Pre-react at 90°C for 70s, at which time part of the blocked isocyanate is not unblocked, the degree of reaction is controllable, and the bonding process of the base fabric is wide and easy to operate; then continue to react at 130°C for 7min, at which time the isocyanate is completely unblocked and the solvent-free polyurethane resin is fully cured; after molding, roll it up and peel off the release paper to obtain the solvent-free polyurethane ball leather.
[0092] Example 2
[0093] 1. This embodiment first provides a method for preparing an easily emulsifiable long-chain polyester polyol, and the specific steps are as follows:
[0094] A four-necked flask equipped with a magnetic stirrer, a constant pressure burette, a thermometer, a N2 inlet tube and an air-cooled condenser was installed in a mantle-type resistance heater, and sebacic acid (95 g), 1,10-decanediol (100 g), ethylene glycol (11 g), trimethylolpropane (3 g) and polyethylene glycol monomethyl ether (molecular weight of 800, 18 g) were added to the flask; then, the temperature was gradually increased under nitrogen protection to carry out a dehydration polycondensation reaction, and the top temperature of the condenser was controlled to be lower than 100°C during the heating process; when the acid value was detected to be no more than 20 mgKOH / g, a catalyst tetraisopropyl titanate (0.02 g) was added and the reaction was continued for 30 minutes, and then the temperature was gradually increased to 240°C, and the vacuum degree was ≥0.095 MPa, and after removing the ethylene glycol reaction, an easily emulsifiable long carbon chain polyester polyol PDS-EO with a hydroxyl value of 37 mgKOH / g was obtained.
[0095] 2. This embodiment further provides a method for preparing a solvent-free polyurethane resin based on the polyester polyol prepared above. The specific steps are as follows:
[0096] Preparation of component A:
[0097] PDS-EO (90 g) was added into the reactor, followed by 1,4-butanediol (10 g), propylene glycol (0.5 g), pore leveling agent Silbyk 9100 (0.5 g), catalyst BiCAT 8108 (0.03 g) and water (1.0 g). The mixture was stirred and reacted at 60°C for 3 h to obtain component A.
[0098] Preparation of component B:
[0099] MDI-100 (80 g) and antioxidant 1035 (0.2 g) were put into a reactor and stirred to mix evenly, followed by adding PDS-EO (90 g), heating to 80° C. and stirring to react for 2 h; then adding blocking agent 3,5-dimethylpyrazole (5 g), stirring to react at 80° C. for 3 h until the NCO content was tested to be qualified, and component B was obtained.
[0100] Preparation of solvent-free polyurethane resin:
[0101] Component A and component B are placed in a low-pressure casting machine at a mass ratio of 100:120, mixed thoroughly, and reacted at 135° C. for 7 minutes to obtain a solvent-free polyurethane resin for ball leather.
[0102] 3. This embodiment further provides a ball leather prepared based on the above solvent-free polyurethane resin, which is specifically prepared as follows:
[0103] The surface layer resin slurry LT-95 was coated on the release paper, and the surface layer was obtained after drying at 130°C for 2 minutes;
[0104] The solvent-free A component and B component are mixed and coated on the surface layer in a mass ratio of 100:120 through a low-pressure casting machine, and pre-reacted at 80°C for 60s. At this time, part of the blocked isocyanate is not unblocked, the degree of reaction is controllable, and the bonding process of the base fabric is wide and easy to operate; then continue to react at 135°C for 6min, at this time the isocyanate is completely unblocked, and the solvent-free polyurethane resin is fully cured and reacted; after molding, the roll is rolled up and the release paper is peeled off to obtain the solvent-free polyurethane ball leather.
[0105] Example 3
[0106] 1. This embodiment first provides a method for preparing an easily emulsifiable long-chain polyester polyol, and the specific steps are as follows:
[0107] A four-necked flask equipped with a magnetic stirrer, a constant pressure burette, a thermometer, a N2 inlet tube and an air-cooled condenser is installed in a mantle-type resistance heater, and 1,8-octanedioic acid (88 g), 1,10-decanediol (105 g), ethylene glycol (15 g), trimethylolpropane (2.3 g) and polyethylene glycol monomethyl ether (molecular weight of 1200, 21 g) are added to the flask; then, the temperature is gradually increased under nitrogen protection to carry out a dehydration polycondensation reaction, and the top temperature of the condenser is controlled to be lower than 100°C during the heating process; when the acid value is detected to be no more than 20 mgKOH / g, a catalyst tetraisopropyl titanate (0.03 g) is added, and the reaction is continued for 30 minutes, and then the temperature is gradually increased to 240°C, and the vacuum degree is ≥0.095 MPa. After removing the ethylene glycol, a long carbon chain easily emulsifiable polyester polyol (PDS-EO) with a hydroxyl value of 28 mgKOH / g is obtained.
[0108] 2. This embodiment further provides a method for preparing a solvent-free polyurethane resin based on the polyester polyol prepared above. The specific steps are as follows:
[0109] Preparation of component A:
[0110] PDS-EO (85 g) was added into a reactor, followed by DEG (15 g), propylene glycol (0.4 g), pore leveling agent Silbyk 9115 (1.5 g), catalyst BiCAT 3228 (2 g) and water (1.5 g). The mixture was stirred at 70°C for 2 h to obtain component A.
[0111] Preparation of component B:
[0112] IPDI (40 g) and antioxidant 1076 (0.1 g) were put into a reactor and stirred to mix evenly, followed by adding PDS-EO (100 g), heating to 90° C. and stirring to react for 4 h; then adding blocking agent 1,2,4-triazole (3 g), stirring to react at 90° C. for 5 h until the NCO content was qualified, and obtaining component B.
[0113] Preparation of solvent-free polyurethane resin:
[0114] Component A and component B are placed in a low-pressure casting machine at a mass ratio of 100:170, mixed thoroughly, and reacted at 140° C. for 5 minutes to obtain a solvent-free polyurethane resin.
[0115] 3. This embodiment further provides a ball leather prepared based on the above solvent-free polyurethane resin, which is specifically prepared as follows:
[0116] The surface layer resin slurry LT-95 was coated on the release paper, and the surface layer was obtained after drying at 130°C for 2 minutes;
[0117] The solvent-free A component and B component are mixed and coated on the surface layer in a mass ratio of 100:170 through a low-pressure casting machine, and pre-reacted at 100°C for 50s. At this time, part of the blocked isocyanate is not unblocked, the degree of reaction is controllable, and the bonding process of the base fabric is wide and easy to operate; then continue to react at 140°C for 10min, at this time the isocyanate is completely unblocked, and the solvent-free polyurethane resin is fully cured and reacted; after molding, the roll is rolled up and the release paper is peeled off to obtain the solvent-free polyurethane ball leather.
[0118] Comparative Example 1
[0119] 1. This comparative example first provides a method for preparing a polyester polyol, which is implemented in the same manner as in Example 1, except that trimethylolpropane and polyethylene glycol monomethyl ether are not added in the preparation of the polyester polyol.
[0120] The preparation steps of polyester polyol in this comparative example are as follows:
[0121] A four-necked flask equipped with a magnetic stirrer, a constant pressure burette, a thermometer, a N2 inlet tube and an air-cooled condenser is installed in a mantle-type resistance heater, and sebacic acid (95 g), 1,10-decanediol (100 g) and ethylene glycol (11 g) are added to the flask; then, the temperature is gradually increased under nitrogen protection to carry out a dehydration polycondensation reaction, and the top temperature of the condenser is controlled to be lower than 100°C during the heating process; when the acid value is detected to be no more than 20 mgKOH / g, a catalyst tetraisopropyl titanate (0.02 g) is added, and the reaction is continued for 30 minutes, and then the temperature is gradually increased to 240°C, and the vacuum degree is ≥0.095 MPa, and after removing the ethylene glycol reaction, a polyester polyol with a hydroxyl value of 37 mgKOH / g is obtained.
[0122] 2. The preparation of the solvent-free polyurethane resin in this comparative example adopts the same implementation as in Example 1, except that the PDS-EO in components A and B are replaced with an equal mass of polyester polyol prepared in Comparative Example 1. Other process conditions are the same as in Example 1.
[0123] 3. The solvent-free polyurethane ball leather in this comparative example is prepared in the same manner as in Example 1, except that the solvent-free polyurethane resin is the solvent-free polyurethane resin prepared in this comparative example 1. Other process conditions are the same as in Example 1.
[0124] Comparative Example 2
[0125] 1. The preparation of the solvent-free polyurethane resin provided in this comparative example adopts the same implementation as in Example 1, except that the PDS-EO in components A and B is replaced with an equal mass of commercially available polyester polyol PBA-2000 (polybutylene adipate polyol with a hydroxyl value of 56 mgKOH / g). The other process conditions are the same as in Example 1.
[0126] 2. The solvent-free polyurethane ball leather in this comparative example is prepared in the same manner as in Example 1, except that the solvent-free polyurethane resin is the solvent-free polyurethane resin prepared in this comparative example 2. Other process conditions are the same as in Example 1.
[0127] Comparative Example 3
[0128] 1. This comparative example first provides a method for preparing a polyester polyol, which is implemented in the same manner as in Example 1, except that in the preparation of the polyester polyol, dimer acid and 1,2-octanediol are replaced by adipic acid and butanediol of equal mass, respectively. Other process conditions are the same as in Example 1.
[0129] The preparation steps of polyester polyol in this comparative example are as follows:
[0130] A four-necked flask equipped with a magnetic stirrer, a constant pressure burette, a thermometer, a N2 inlet tube and an air-cooled condenser is installed in a mantle-type resistance heater, and adipic acid (145 g), butanediol (55 g), ethylene glycol (5 g), trimethylolpropane (2 g) and polyethylene glycol monomethyl ether (molecular weight 400, 6 g) are added to the four-necked flask; then, the temperature is gradually increased under nitrogen protection to carry out a dehydration polycondensation reaction, and the top temperature of the condenser is controlled to be lower than 100° C. during the heating process; when the acid value is detected to be no more than 20 mgKOH / g, a catalyst tetraisopropyl titanate (0.01 g) is added and the reaction is continued for 30 minutes, and then the temperature is gradually increased to 240° C., and the vacuum degree is ≥0.095 MPa, and after removing the ethylene glycol reaction, a polyester polyol with a hydroxyl value of 56 mgKOH / g is obtained.
[0131] 2. The preparation of the solvent-free polyurethane resin in this comparative example adopts the same implementation as in Example 1, except that the PDS-EO in components A and B are replaced with an equal mass of the polyester polyol prepared in this comparative example 1. The other process conditions are the same as in Example 1.
[0132] 3. The solvent-free polyurethane ball leather in this comparative example is prepared in the same manner as in Example 1, except that the solvent-free polyurethane resin is the solvent-free polyurethane resin prepared in Comparative Example 3. Other process conditions are the same as in Example 1.
[0133] Comparative Example 4
[0134] 1. The polyester polyol provided in this comparative example is the same as that in Example 1.
[0135] 2. This comparative example further provides a preparation method for a solvent-free polyurethane resin based on the polyester polyol prepared above. The specific steps are as follows:
[0136] Preparation of component A: same as in Example 1.
[0137] The preparation of component B is carried out in the same manner as in Example 1, except that the blocking agent methyl ethyl ketone oxime is not added. Other process conditions are the same as in Example 1.
[0138] 3. The solvent-free polyurethane ball leather in this comparative example is prepared in the same manner as in Example 1, except that the solvent-free polyurethane resin is the solvent-free polyurethane resin prepared in Comparative Example 4. Other process conditions are the same as in Example 1.
[0139] Performance Testing
[0140] The thickness, peel strength, and hot-cut welding tensile force of the solvent-free polyurethane ball leathers prepared in Examples 1-3 and Comparative Examples 1-4 were tested for performance, and the results are shown in the following table:
[0141]
[0142] Note: The peel strength test is carried out in accordance with GB / T 8949-2008 5.9;
[0143] The weld tensile strength test was conducted by welding the finished leather using a JS-00033 high frequency heat sealing machine (Shenzhen Jinsheng Machinery Equipment Co., Ltd.) according to the welding process (pressure 30 psi, current 0.25-0.26 A, welding time 6 s, cooling time 6 s), and referring to GB / T8949-2008 5.9 for testing.
[0144] As can be seen from the above table, the leather products prepared by the present invention have good flatness, the thickness of each point of the entire width is maintained between 3.0-3.1 mm, the thickness uniformity is good, and the density of the solvent-free polyurethane foam layer is 240-260 kg / cm 3 The peel strength between the foam layer and the cloth base is over 60N / 3cm, and the hot cutting welding tensile force is over 100N / 2.54cm, which can meet the downstream 4-piece ball making processing requirements.
[0145] Among them, compared with Example 1, the thickness uniformity of Comparative Example 1 across the entire width is worse than that of Example 1, and has large fluctuations. This is because the polyester polyol in Comparative Example 1 does not contain a hydrophilic group, has a poor emulsification effect on water, and causes uneven foaming.
[0146] Compared with Example 1, the thickness of Comparative Example 2 is thinner overall, which is due to the high ester group density and strong cohesive force of the polybutylene adipate polyol used, insufficient foaming open-cell properties, and foam shrinkage.
[0147] Compared with Example 1, in Comparative Example 3, hydrophilic groups were introduced into the polyester polyol, and the thickness uniformity was improved. However, due to the strong rigidity of the polyester polyol itself, the open porosity was insufficient and the overall thickness was insufficient.
[0148] Compared with Example 1, since no sealing agent is introduced into component B of Comparative Example 4, the lamination operation space is narrow, and the peel strength and welding tensile force are low, that is, the foaming layer has a "surface drying" problem, which leads to loose lamination.
[0149] Based on the above embodiments and performance test results, it can be seen that the solvent-free polyurethane resin for ball leather provided in the present invention has excellent performance, can be used to prepare thick solvent-free polyurethane ball leather with a thickness of about 3 mm, and the finished leather has good flatness, fine pores in the foaming layer, controllable degree of reaction, high lamination tolerance for the cloth base and easy operation, and high peel strength and welding tensile strength.
[0150] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0151] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A solvent-free polyurethane resin for ball leather, characterized in that: The solvent-free polyurethane resin for ball leather comprises component A and component B; In parts by mass, the component A comprises 85-95 parts of polyester polyol PDS-EO, 5-15 parts of polyol and 0.3-0.5 parts of crosslinking agent; the component B comprises 40-80 parts of polyisocyanate, 50-100 parts of polyester polyol PDS-EO and 3-8 parts of blocking agent; The polyester polyol PDS-EO is prepared by polycondensation reaction of long carbon chain polyacid, long carbon chain polyol, small molecule diol, trimethylolpropane, polyethylene glycol monomethyl ether and a catalyst.
2. The solvent-free polyurethane resin for ball leather according to claim 1, characterized in that The hydroxyl value of the polyester polyol PDS-EO is 28-56 mgKOH / g.
3. The solvent-free polyurethane resin for ball leather according to claim 1, characterized in that The raw materials for preparing the polyester polyol PDS-EO are, by weight: 88-145 parts of long carbon chain polyacid, 55-105 parts of long carbon chain polyol, 5-15 parts of small molecule diol, 2-3 parts of trimethylolpropane, 6-21 parts of polyethylene glycol monomethyl ether and 0.01-0.03 parts of catalyst; Preferably, the long carbon chain polyacid is one of dimer acid, 1,10-decanedioic acid, and 1,8-octanedioic acid; and / or, the long carbon chain polyol is one of 1,10-decanediol and 1,2-octanediol; and / or, the small molecule diol is ethylene glycol; Preferably, the amount of trimethylolpropane and polyethylene glycol monomethyl ether added is kept the same; Preferably, the polyethylene glycol monomethyl ether is a monohydroxy compound with a number average molecular weight of 400-1200.
4. The solvent-free polyurethane resin for ball leather according to claim 1, characterized in that In the component A, the polyol is any one of ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 2-methyl-1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, neopentyl glycol, and diethylene glycol, or a combination of two or more thereof; And / or, the cross-linking agent is at least one of glycerol and trimethylolpropane.
5. The solvent-free polyurethane resin for ball leather according to claim 1, characterized in that The component A also includes any one or a combination of two or more of a pore leveling agent, a catalyst, and water; Preferably, the content of the pore leveling agent in the component A is 0.3 to 1.5 parts; and / or, the content of the catalyst in the component A is 0.01 to 2 parts; and / or, the content of water in the component A is 0.8 to 1.5 parts.
6. The solvent-free polyurethane resin for ball leather according to claim 1, characterized in that In the B component, the polyisocyanate is at least one of 4,4'-diphenylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate; And / or, the blocking agent is at least one of methyl ethyl ketone oxime, 3,5-dimethylpyrazole, diethyl malonate, acetanilide, and 1,2,4-triazole.
7. The solvent-free polyurethane resin for ball leather according to claim 1, characterized in that: The B component also includes an antioxidant; Preferably, the content of the antioxidant in the component B is 0.1 to 0.3 parts.
8. The solvent-free polyurethane resin for ball leather according to claim 1, characterized in that The mass ratio of the component A to the component B is 100:90 to 100:
170.
9. A method for preparing a solvent-free polyurethane resin for ball leather according to any one of claims 1 to 8, characterized in that: The following steps are involved: The polyester polyol PDS-EO, polyol, crosslinking agent and other optional auxiliary agents are mixed and reacted to obtain component A; The polyisocyanate, polyester polyol PDS-EO, blocking agent and other optional additives are reacted until the NCO content is tested to be qualified to obtain component B; The components A and B are fully mixed, and cured at 130-140° C. to obtain a solvent-free polyurethane resin for ball leather; Preferably, in the step of obtaining component A, the temperature of the mixing reaction is 50-70°C; Preferably, in the step of obtaining component B, the reaction temperature is 70-90°C.
10. A solvent-free polyurethane ball leather, characterized in that: A solvent-free polyurethane resin for ball leather comprising any one of claims 1 to 8 or a solvent-free polyurethane resin for ball leather prepared by the preparation method according to claim 9; Preferably, the preparation of the solvent-free polyurethane ball leather comprises the following steps: Component A and component B are coated on the polyurethane surface layer according to the proportion, pre-reacted at 80-100°C for 50-70s, and bonded to the base fabric; then, the reaction is performed at 130-140°C to cure and form, so as to obtain solvent-free polyurethane ball leather.