Nitrogen-doped carbon / cobalt-based wave-absorbing agent as well as preparation method and application thereof

By loading ZIF-67 on nitrogen-doped carbon nanosheets and pyrolyzed to prepare nitrogen-doped carbon/cobalt-based absorbents, the problems of narrow bandwidth and weak loss ability of the absorbent material are solved, and high reflection loss and wide bandwidth are achieved The electromagnetic wave absorption performance significantly improves the performance of wave absorbing materials.

CN119081649AActive Publication Date: 2024-12-06NORTHWESTERN POLYTECHNICAL UNIV +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411201387.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

Existing wave absorbing materials have problems with narrow effective absorption bandwidth and weak electromagnetic wave loss capability, and it is difficult to achieve high reflection loss and wide bandwidth electromagnetic wave absorption at lower thicknesses.

Method used

By loading ZIF-67 on nitrogen-doped carbon nanosheets and performing pyrolysis between 700°C and 900°C under a protective atmosphere, a nitrogen-doped carbon/cobalt-based absorbent was prepared to form a heterogeneous interface to strengthen the multiple loss mechanism , coordinated magnetic loss and dielectric loss capabilities to achieve high reflection loss and wide bandwidth absorption performance.

Benefits of technology

High reflection loss and wide effective absorption bandwidth are achieved at lower fill amounts. The minimum reflection loss of nitrogen-doped carbon/cobalt-based absorbent reaches -58.34dB, and the effective absorption bandwidth can reach 7.52GHz, far More than most of the reported composite wave absorbing materials, demonstrating the advantages of electromagnetic synergies in electromagnetic wave attenuation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081649A_ABST
    Figure CN119081649A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of wave-absorbing materials, in particular to a nitrogen-doped carbon / cobalt-based wave-absorbing agent and a preparation method and application thereof. The specific preparation method comprises the following steps: by taking a nitrogen-doped carbon nanosheet as a matrix and 2-methylimidazole as an organic ligand, carrying out a co-precipitation reaction with a Co source in a solvent system, so that the formed ZIF-67 is loaded on the nitrogen-doped carbon nanosheet, and then pyrolyzing at 700-900 DEG C in a protective atmosphere to obtain the nitrogen-doped carbon / cobalt-based wave-absorbing agent. The cubic ZIF-67 loaded carbon nanosheet stable structure is prepared, so that the pyrolyzed Co / NCS composite material has a heterogeneous interface, and a multiple loss mechanism is strengthened. The wave-absorbing agent can be used for preparing an electromagnetic wave absorbing material, and higher reflection loss and wider effective absorption bandwidth are realized under the condition of lower filling amount. The problems that an existing wave-absorbing material is narrow in effective absorption bandwidth and weak in electromagnetic wave loss capacity are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of absorbing materials, and in particular to a nitrogen-doped carbon / cobalt-based absorbing agent and a preparation method and application thereof. Background Art

[0002] In today's era of rapid development of information technology, the deployment of 5G networks, the application of unmanned driving technology and the popularization of smart homes have greatly improved people's quality of life. However, while the development of information technology has brought great convenience to people's lives, it has also caused an explosive increase in electromagnetic radiation in space due to the use of a large number of electronic products, which has gradually become a problem that cannot be ignored.

[0003] At present, there are two effective solutions to the problem of electromagnetic wave protection: developing new wireless communication technology and preparing electromagnetic shielding / absorbing materials. According to the existing electromagnetic theory, it is still extremely difficult to achieve point-to-point directional propagation of electromagnetic waves, while the preparation research of electromagnetic shielding / absorbing materials has made great progress. Electromagnetic wave absorbing materials can effectively convert the incident electromagnetic wave energy into other forms of energy to achieve effective absorption of electromagnetic waves. The research goal of this material is to reduce the adverse effects of electromagnetic radiation on human health and electronic equipment, while enhancing the anti-interference performance of electronic equipment. The mechanism of absorbing materials mainly includes various forms such as conductivity loss, dielectric loss and magnetic loss. They are very effective in absorbing electromagnetic waves and can consume electromagnetic wave energy internally. Electromagnetic absorbing materials have been widely used in electromagnetic noise suppression in complex circuits, stable transmission of wireless communication base stations or satellite communication terminal signals, electromagnetic interference protection of high-end electronic instruments, and even in key areas such as anti-radar detection systems for military confrontation. As the application environment of electromagnetic absorbing materials becomes more and more complex, the various properties of absorbing materials are also facing higher requirements. How to achieve higher reflection loss and wider effective absorption bandwidth at a lower thickness has become a research hotspot in the field of electromagnetic wave absorbing materials.

[0004] Carbon materials have the advantages of low density, large dielectric loss, high conductivity, good processing performance, and corrosion resistance, and have received extensive attention and application in the field of electromagnetic wave absorption materials. In terms of morphology, carbon nanomaterials, such as one-dimensional carbon nanotubes, two-dimensional graphene, and three-dimensional porous carbon nanomaterials, have good dielectric properties and high magnetic loss tangent due to their large surface area, abundant dangling bonds, and macroscopic quantum tunneling effects, showing great potential in electromagnetic protection. However, most carbon nanomaterials have excessive surface electron mobility and large dielectric constants, which lead to mismatch between carbon nanomaterials and free space impedance, and thus lead to poor absorption performance of electromagnetic waves. Therefore, in the field of electromagnetic wave absorption materials, the electronic symmetry of nanocarbon is mainly destroyed by introducing heteroatoms such as N, S, B, etc., and a large number of structural defects are formed, thereby increasing its dielectric loss. However, its high dielectric constant leads to characteristic impedance mismatch, which hinders its widespread application.

[0005] In recent years, the development of microwave-absorbing materials by pyrolyzing MOF materials using MOF materials as precursors has become a research hotspot. ZIF-67 is an example of a widely used MOF material. It is characterized by the use of cobalt as a metal node and 2-methylimidazole as an organic ligand. It inherits the general properties of MOF materials, such as a designable pore structure and a high specific surface area, and also exhibits unique properties similar to zeolites, such as chemical stability and thermal stability. However, ZIF-67 has the disadvantages of poor magnetic and electrical conductivity and unclear microwave absorption performance.

[0006] For example, prior art 1 is based on Co 2+ 、Ni 2+ As the metal source, trimer acid was used as the ligand to prepare CoNi-MOF. By heat treating CoNi-MOF, CoNi@C microsphere composite materials with adjustable porous and hollow morphologies were obtained. The minimum reflection loss of this sample at 10.7GHz can reach -44.8dB. The effective absorption bandwidth of this method is relatively narrow, and the minimum reflection loss is low, resulting in poor microwave absorption performance.

[0007] Prior art 2 is to pyrolyze the Co-based MOF precursor ZIF-67 in an Ar atmosphere to obtain a Co / C porous composite material, whose dielectric loss and magnetic loss capabilities are effectively improved, and the reflection loss reaches -35.3dB when the thickness is 4mm. The matching thickness of this method is large, and the reflection loss is low, resulting in poor microwave absorption performance.

[0008] Prior art 1: Liu Z, Duan Y, Deng B, et al. Synthesis of ultralight N-richporous graphene nanosheets derived from fluid catalytic cracking slurry and their electromagnetic wave absorption properties [J]. Industrial & Engineering Chemistry Research, 2020, 59(17): 8243-8251.

[0009] Existing technology 2: LüY, Wang Y, Li H, et al.MOF-Derived Porous Co / CNanocomposites with Excellent Electromagnetic Wave Absorption Properties[J].ACS Applied Materials&Interfaces, 2015,7(24):13604-13611. Summary of the invention

[0010] In order to solve the problems of narrow effective absorption bandwidth and weak electromagnetic wave loss capacity of existing absorbing materials, the purpose of the present invention is to provide a nitrogen-doped carbon / cobalt-based absorbing agent and a preparation method and application thereof.

[0011] To achieve the above objectives, the technical solution of the present invention is as follows.

[0012] A first aspect of the present invention provides a method for preparing a nitrogen-doped carbon / cobalt-based absorber, comprising the following steps:

[0013] Using nitrogen-doped carbon nanosheets as a matrix and 2-methylimidazole as an organic ligand, a co-precipitation reaction is carried out with a Co source in a solvent system to load the formed ZIF-67 on the nitrogen-doped carbon nanosheets, and then pyrolyzed at 700°C to 900°C under a protective atmosphere to obtain a nitrogen-doped carbon / cobalt-based absorber.

[0014] The present invention mainly loads ZIF-67 on nitrogen-doped carbon nanosheets by heating coprecipitation method, prepares a stable structure of carbon nanosheets loaded with cubic ZIF-67, so that the Co / NCS composite material after pyrolysis has a heterogeneous interface and strengthens multiple loss mechanisms. When the magnetic loss capacity and the dielectric loss capacity are fully coordinated, the absorbing material achieves higher reflection loss and wider effective absorption bandwidth at a lower filling amount. The method of the present invention can not only provide a new design idea for the research of lightweight broadband absorbing materials, but also provide necessary innovative technical support and theoretical support for the development of long-distance detection technology, which has important academic significance and practical value.

[0015] Preferably, the pyrolysis temperature is 800°C; the pyrolysis time is 3h to 5h. Subsequent experiments show that the pyrolysis temperature is 700°C to 900°C, and pyrolysis at 800°C can obtain a wider effective absorption bandwidth of 7.52GHz at a thinner thickness of 2.83mm. And the minimum reflection loss RL at a matching thickness of 2.63mm min It reached -58.34dB, far exceeding most reported composite absorbing materials, confirming the advantages of the composite materials prepared at this temperature and the electromagnetic synergistic effect in electromagnetic wave attenuation.

[0016] Preferably, the Co source is Co(NO3)2·6H2O or CoCl2·6H2O; the mass ratio of nitrogen-doped carbon nanosheets, 2-methylimidazole and Co source is 50:500-600:300-360.

[0017] Preferably, the nitrogen-doped carbon nanosheets are prepared by the following method:

[0018] With inorganic salt as template, a carbon source, a nitrogen source, an inorganic salt and water are mixed to prepare a solid mixture; the solid mixture is calcined under a protective atmosphere, then etched in hydrochloric acid, and washed to remove the inorganic salt to obtain nitrogen-doped carbon nanosheets.

[0019] The present invention introduces an inorganic salt as a template, mixes it with a carbon source and a nitrogen source to prepare a solid intermediate, and then calcines, etches, and washes to prepare porous nitrogen-doped carbon nanosheets. The present invention prepares porous nitrogen-doped carbon nanosheets by freeze drying and high-temperature pyrolysis. The porous structure can increase the multiple reflections of electromagnetic waves inside the material and provide more attachment sites for magnetic Co particles.

[0020] Further preferably, the carbon source is citric acid, the nitrogen source is urea, and the inorganic salt is potassium carbonate; the molar ratio of the carbon source, the nitrogen source, and the inorganic salt is 0.01-0.015:0.02-0.021:0.05-0.07.

[0021] More preferably, the calcination temperature is 600° C. to 800° C. and the calcination time is 1 h to 3 h.

[0022] More preferably, the concentration of hydrochloric acid used for etching is 0.8M-1M.

[0023] Preferably, the protective atmosphere is an argon atmosphere.

[0024] Preferably, the coprecipitation reaction temperature is 65° C. to 70° C., and the coprecipitation reaction time is 0.5 h to 2 h. At this temperature, it is helpful to load ZIF-67 on the porous carbon nanosheets by the heating coprecipitation method to obtain a precursor.

[0025] Preferably, the solvent is methanol; the usage ratio of nitrogen-doped carbon nanosheets to methanol is 50 mg: 90 mL to 100 mL.

[0026] The second aspect of the present invention provides a nitrogen-doped carbon / cobalt-based absorber prepared by the preparation method described in the first aspect.

[0027] The third aspect of the present invention provides a use of the nitrogen-doped carbon / cobalt-based absorber described in the second aspect in the preparation of an electromagnetic wave absorbing material.

[0028] Preferably, the specific application method is: mixing the nitrogen-doped carbon / cobalt-based absorber with a polymer matrix to prepare an electromagnetic wave absorbing coating material; wherein the polymer matrix is ​​polyurethane or epoxy resin.

[0029] Preferably, the mass percentage of the nitrogen-doped carbon / cobalt-based absorber in the electromagnetic wave absorbing material is 5% to 20%.

[0030] Beneficial effects of the present invention:

[0031] 1. The present invention mainly uses nitrogen-doped carbon nanosheets as a matrix, loads ZIF-67 by heating coprecipitation method, and prepares a stable structure of carbon nanosheets loaded with cubic ZIF-67, so that the Co / NCS composite material after pyrolysis has a heterogeneous interface and strengthens multiple loss mechanisms. Under the condition that the magnetic loss capacity and the dielectric loss capacity are fully coordinated, the absorbing material achieves higher reflection loss and wider effective absorption bandwidth at a lower filling amount, solving the problems of narrow effective absorption bandwidth and weak electromagnetic wave loss capacity of existing absorbing materials.

[0032] 2. The minimum reflection loss of the nitrogen-doped carbon / cobalt-based absorber prepared by the present invention reaches -58.34dB. At a matching thickness of 2.83mm, its effective absorption bandwidth can reach 7.52GHz, and it can absorb 90% of the electromagnetic waves in the frequency range of 10 to 18GHz. This shows that the effective absorption bandwidth of the electromagnetic wave absorption performance of the nitrogen-doped carbon / cobalt-based absorber prepared by the present invention at a thin thickness far exceeds that of most reported composite absorbers, further confirming the advantages of the nitrogen-doped carbon / cobalt-based absorber and the electromagnetic synergistic effect in electromagnetic wave attenuation. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The SEM images and TEM images of samples Co / NCS-700, Co / NCS-800 and Co / NCS-900 prepared in Examples 1 to 3. Among them, (a1) is the SEM image of Co / NCS-700; (b1) is the SEM image of Co / NCS-800; (c1) is the SEM image of Co / NCS-900; (a2) is the TEM image of Co / NCS-700; (b2) is the TEM image of Co / NCS-800; (c2) is the TEM image of Co / NCS-900.

[0034] Figure 2 The EDS graph of the sample Co / NCS-800 prepared in Example 2. (d1) to (d4) are the EDS graphs of Co / NCS-800.

[0035] Figure 3 HETEM image (e) and SAED image (f) of the sample Co / NCS-800 prepared in Example 2.

[0036] Figure 4 Raman spectra (a) and XRD spectra (b) of samples Co / NCS-700, Co / NCS-800 and Co / NCS-900 prepared in Examples 1 to 3.

[0037] Figure 5 (a) The adsorption-desorption curves and (b) pore size distribution diagrams of samples Co / NCS-700, Co / NCS-800 and Co / NCS-900 prepared in Examples 1 to 3.

[0038] Figure 6 (a) is the hysteresis loop diagram of samples Co / NCS-700, Co / NCS-800 and Co / NCS-900 prepared in Examples 1 to 3 at room temperature and (b) is the partially enlarged hysteresis loop diagram at room temperature.

[0039] Figure 7The electromagnetic parameter diagrams of samples Co / NCS-700, Co / NCS-800 and Co / NCS-900 prepared in Examples 1 to 3. Among them, (a) is the real part of the dielectric constant; (b) is the imaginary part of the dielectric constant; (c) is the dielectric loss tangent; (d) is the real part of the magnetic permeability; (e) is the imaginary part of the magnetic permeability; (f) is the magnetic permeability loss tangent.

[0040] Figure 8 The reflection loss diagrams of samples Co / NCS-700, Co / NCS-800 and Co / NCS-900 prepared in Examples 1 to 3. (a) is the reflection loss diagram of Co / NCS-700; (b) is the reflection loss diagram of Co / NCS-800; (c) is the reflection loss diagram of Co / NCS-900. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0042] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.

[0043] In the field of electromagnetic wave absorbing materials, the introduction of heteroatoms such as N, S, B, etc. will destroy the electronic symmetry of nanocarbon, resulting in the formation of a large number of electric dipoles, which attenuate electromagnetic energy through dipole polarization loss. At the same time, the large number of structural defects in doped carbon can serve as polarization centers of dipoles, thereby increasing its dielectric loss.

[0044] Compared with other heteroatoms, the size of N atoms is close to that of C atoms, avoiding obvious lattice mismatch. Since carbon atoms have a more negative electronegativity, nitrogen-doped carbon atoms can exhibit different electronic conductivity, depending on the content and type of nitrogen in the carbon atoms. So far, reports on various nitrogen-doped carbon materials have accounted for more than 90%, and related research on nitrogen-doped carbon-based high-efficiency electron beam absorbers is also constantly innovating. Researchers have adjusted the structure of nitrogen-doped carbon nanomaterials through different synthesis methods, such as chemical vapor deposition CVD technology, high-temperature carbonization, and in-situ nitrogen doping to optimize their microwave absorption performance. Among them, nitrogen-doped porous carbon nanosheets have shown some excellent performance in the field of microwave absorption, but the characteristic impedance mismatch caused by their high dielectric constant has hindered their wide application.

[0045] Due to the low magnetic permeability and strong magnetization of magnetic materials, the relative complex magnetic permeability can be improved, resulting in strong magnetic loss and improved impedance matching. Therefore, composites with magnetic metals, alloys and oxides have become the development direction of carbon materials.

[0046] In recent years, the development of microwave-absorbing materials by pyrolyzing MOF materials using MOF materials as precursors has become a research hotspot. ZIF-67 is an example of a widely used MOF material. It is characterized by the use of cobalt as a metal node and 2-methylimidazole as an organic ligand. It inherits the general properties of MOF materials, such as a designable pore structure and a high specific surface area, and also exhibits unique properties similar to zeolites, such as chemical stability and thermal stability. In the ZIF-67 material, Co metal exists in the form of ions, while carbon elements exist in the organic skeleton. Therefore, ZIF-67 itself has poor magnetic and conductive properties, and its microwave-absorbing performance is not obvious.

[0047] At present, by high-temperature pyrolysis of ZIF-67 materials, metal ions can be converted into magnetic metal Co atoms, which enhances magnetic loss, and the organic framework is reduced to carbon or nitrogen-doped carbon, which can provide dielectric loss, thereby obtaining a magneto-electric synergistic Co / C composite material. This composite material combines the advantages of metal Co and carbon materials, and its structure and composition are easy to control, becoming a research hotspot in the field of absorbing materials.

[0048] In the prior art, various ZIF-67 composite materials synthesized ingeniously show their broad prospects and effective competitiveness as lightweight microwave absorbing materials. The high specific surface area and ordered pore structure of ZIF-67 help to improve its performance in electromagnetic wave absorption, because these characteristics can increase the interaction between electromagnetic waves and materials, thereby improving the absorption efficiency. In addition, the cobalt metal center in ZIF-67 gives it a certain magnetism, which makes ZIF-67 contribute to electromagnetic wave absorption in terms of magnetic loss, especially when absorbing low-frequency electromagnetic waves. By combining ZIF-67 with other absorbing materials, the absorbing performance and stability of the material can be effectively improved, providing new ideas and methods for the design and preparation of electromagnetic wave absorbing materials. However, the prior art generally has the problem of relatively narrow effective absorbing bandwidth, large matching thickness, and low minimum reflection loss, resulting in poor microwave absorption performance.

[0049] For example: Prior art 1: Liu et al. 2+ 、Ni 2+As the metal source, trimer acid was used as the ligand to develop CoNi-MOF. By heat treating CoNi-MOF, a CoNi@C microsphere composite material with adjustable porous and hollow morphology was obtained. The minimum reflection loss of this sample at 10.7GHz can reach -44.8dB. Prior art 2: Lü et al. pyrolyzed the Co-based MOF precursor ZIF-67 in an Ar atmosphere to obtain a Co / C porous composite material, whose dielectric loss and magnetic loss capabilities were effectively improved, and the reflection loss reached -35.3dB when the thickness was 4mm.

[0050] Based on this, in order to solve the problems of narrow effective absorption bandwidth and weak electromagnetic wave loss capacity of existing absorbing materials, the present invention prepares a transition metal Co / NCS composite material obtained by high-temperature pyrolysis of ZIF-67 loaded with nitrogen-doped carbon nanosheets as a matrix.

[0051] The present invention combines nitrogen-doped carbon nanosheets with ZIF-67 through reasonable components, structural design and pyrolysis temperature regulation, and prepares a structural and functional integrated absorbing material with light weight, broadband and strong absorption after high-temperature pyrolysis, which is very likely to become a major breakthrough in the field of broadband electromagnetic wave absorption. Using nitrogen-doped carbon nanosheets as the matrix, ZIF-67 is loaded by heating coprecipitation method, and a series of nitrogen-doped and heterogeneous nanostructured transition metal / carbon composite materials are prepared after pyrolysis at different temperatures. The development of these studies provides a model system and rich experience for in-depth understanding of the regulation of components and microstructures of transition metal-doped hierarchical carbon composite materials.

[0052] The following is an analysis of the construction of the nitrogen-doped carbon / cobalt-based absorber of the present invention and the study of the band-broadening mechanism through specific examples. The methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are all commercially available unless otherwise specified.

[0053] In the following embodiments, NCS is a nitrogen-doped carbon nanosheet. NCS-600, NCS-700, and NCS-800 are a series of nitrogen-doped carbon nanosheets prepared at different pyrolysis temperatures; Co / NCS-700, Co / NCS-800, and Co / NCS-900 are a series of nitrogen-doped carbon / cobalt-based absorbing materials prepared at different pyrolysis temperatures, i.e., Co / NCS composite materials.

[0054] Example 1

[0055] A method for preparing a nitrogen-doped carbon / cobalt-based absorber comprises the following steps:

[0056] (1) Preparation of nitrogen-doped carbon nanosheets:

[0057] 0.012 mol of citric acid monohydrate, 0.0208 mol of urea and 0.06 mol of potassium carbonate were dissolved in 70 mL of deionized water and stirred for 30 min. The resulting solution was freeze-dried at -80 °C for 24 h. The dried white solid was transferred to a tube furnace and heated at 5 °C / min under an Ar atmosphere. -1 The temperature was raised to 700 °C and kept at this temperature for 2 h, and then naturally cooled to room temperature.

[0058] After the heat preservation, the obtained black powder was etched with 1M HCl and washed several times with deionized water to remove K2CO3 in the product. Finally, the obtained solution was vacuum filtered to obtain a solid, which was dried at 80°C overnight to obtain nitrogen-doped carbon nanosheets, which were recorded as NCS-700.

[0059] (2) Preparation of Co / NCS composites:

[0060] First, in a 250 mL round-bottom flask, 50 mg NCS-700 and 600 mg 2-methylimidazole were dispersed in 50 mL methanol and ultrasonically treated, which was marked as solution A. After that, 360 mg Co(NO3)2·6H2O was dispersed in 50 mL methanol and ultrasonically treated, which was marked as solution B. Solution B was added dropwise to solution A, and the color of the mixture changed from gray to purple. The mixed solution was then stirred at a constant temperature of 70 ° C for 1 h. The purple precipitate NCS / ZIF-67 was collected and dried at 60 ° C. Finally, the obtained purple powder was kept at 700 ° C for 4 hours under Ar protection at a heating rate of 5 ° C / min to obtain a black powder product, which is a Co / NCS composite material, recorded as Co / NCS-700.

[0061] Example 2

[0062] A method for preparing a nitrogen-doped carbon / cobalt-based absorber comprises the following steps:

[0063] (1) Preparation of nitrogen-doped carbon nanosheets:

[0064] 0.012 mol of citric acid monohydrate, 0.0208 mol of urea and 0.06 mol of potassium carbonate were dissolved in 70 mL of deionized water and stirred for 30 min. The resulting solution was freeze-dried at -80 °C for 24 h. The dried white solid was transferred to a tube furnace and heated at 5 °C / min under an Ar atmosphere. -1The temperature was raised to 700°C at a rate of 100 °C and kept at this temperature for 2 h, and then naturally cooled to room temperature. After the insulation, the obtained black powder was etched with 1M HCl and washed several times with deionized water to remove K2CO3 in the product. Finally, the obtained solution was vacuum filtered to obtain a solid, which was dried at 80°C overnight to obtain nitrogen-doped carbon nanosheets, recorded as NCS-700.

[0065] (2) Preparation of Co / NCS composites:

[0066] First, in a 250 mL round-bottom flask, 50 mg NCS-700 and 600 mg 2-methylimidazole were dispersed in 50 mL methanol and ultrasonically treated, which was marked as solution A. After that, 360 mg Co(NO3)2·6H2O was dispersed in 50 mL methanol and ultrasonically treated, which was marked as solution B. Solution B was added dropwise to solution A, and the color of the mixture changed from gray to purple. The mixed solution was then stirred at a constant temperature of 70 ° C for 1 h. The purple precipitate NCS / ZIF-67 was collected and dried at 60 ° C. Finally, the obtained purple powder was kept at 800 ° C for 4 hours under Ar protection at a heating rate of 5 ° C / min to obtain a black powder product, which is a Co / NCS composite material, recorded as Co / NCS-800.

[0067] Example 3

[0068] A method for preparing a nitrogen-doped carbon / cobalt-based absorber comprises the following steps:

[0069] (1) Preparation of nitrogen-doped carbon nanosheets:

[0070] 0.012 mol of citric acid monohydrate, 0.0208 mol of urea and 0.06 mol of potassium carbonate were dissolved in 70 mL of deionized water and stirred for 30 min. The resulting solution was freeze-dried at -80 °C for 24 h. The dried white solid was transferred to a tube furnace and heated at 5 °C / min under an Ar atmosphere. -1 The temperature was raised to 700°C at a rate of 100 °C and kept at this temperature for 2 h, and then naturally cooled to room temperature. After the insulation, the obtained black powder was etched with 1M HCl and washed several times with deionized water to remove K2CO3 in the product. Finally, the obtained solution was vacuum filtered to obtain a solid, which was dried at 80°C overnight to obtain nitrogen-doped carbon nanosheets, recorded as NCS-700.

[0071] (2) Preparation of Co / NCS composites:

[0072] First, in a 250 mL round-bottom flask, 50 mg NCS-700 and 600 mg 2-methylimidazole were dispersed in 50 mL methanol and ultrasonically treated, which was marked as solution A. After that, 360 mg Co(NO3)2·6H2O was dispersed in 50 mL methanol and ultrasonically treated, which was marked as solution B. Solution B was added dropwise to solution A, and the color of the mixture changed from gray to purple. The mixed solution was then stirred at a constant temperature of 70 ° C for 1 h. The purple precipitate NCS / ZIF-67 was collected and dried at 60 ° C. Finally, the obtained purple powder was kept at 900 ° C for 4 hours under Ar protection at a heating rate of 5 ° C / min to obtain a black powder product, which is a Co / NCS composite material, marked as Co / NCS-900.

[0073] Example 4

[0074] A method for preparing a nitrogen-doped carbon / cobalt-based absorber comprises the following steps:

[0075] (1) Preparation of nitrogen-doped carbon nanosheets:

[0076] 0.01 mol of citric acid monohydrate, 0.02 mol of urea and 0.05 mol of potassium carbonate were dissolved in 70 mL of deionized water and stirred for 30 min. The resulting solution was freeze-dried at -80 °C for 20 h. The dried white solid was transferred to a tube furnace and heated at 5 °C / min under an Ar atmosphere. -1 The temperature was raised to 600°C at a rate of 100°C and kept at this temperature for 1 hour, and then naturally cooled to room temperature. After the insulation, the obtained black powder was etched with 1M HCl and washed several times with deionized water to remove K2CO3 in the product. Finally, the obtained solution was vacuum filtered to obtain a solid, which was dried at 80°C overnight to obtain nitrogen-doped carbon nanosheets, recorded as NCS-600.

[0077] (2) Preparation of Co / NCS composites:

[0078] First, in a 250 mL round-bottom flask, 50 mg NCS-600 and 500 mg 2-methylimidazole were dispersed in 45 mL methanol and ultrasonically treated, which was marked as solution A. After that, 300 mg Co(NO3)2·6H2O was dispersed in 45 mL methanol and ultrasonically treated, which was marked as solution B. Solution B was added dropwise to solution A, and the color of the mixture changed from gray to purple. The mixed solution was then stirred at a constant temperature of 65 °C for 0.5 h. The purple precipitate NCS / ZIF-67 was collected and dried at 60 °C. Finally, the obtained purple powder was kept at 800 °C for 3 hours under Ar protection at a heating rate of 5 °C / min to obtain a black powder product, which was the Co / NCS composite material. The SEM and TEM images showed that the Co particles were obviously loaded on the porous carbon nanosheets, and the nitrogen-doped carbon / cobalt-based absorbing material was prepared.

[0079] Example 5

[0080] A method for preparing a nitrogen-doped carbon / cobalt-based absorber comprises the following steps:

[0081] (1) Preparation of nitrogen-doped carbon nanosheets:

[0082] 0.015 mol of citric acid monohydrate, 0.021 mol of urea and 0.07 mol of potassium carbonate were dissolved in 70 mL of deionized water and stirred for 30 min. The resulting solution was freeze-dried at -80 °C for 24 h. The dried white solid was transferred to a tube furnace and heated at 5 °C / min under an Ar atmosphere. -1 The temperature was raised to 800°C at a rate of 100 °C and kept at this temperature for 3 h, and then naturally cooled to room temperature. After the insulation, the obtained black powder was etched with 1M HCl and washed several times with deionized water to remove K2CO3 in the product. Finally, the obtained solution was vacuum filtered to obtain a solid, which was dried at 80°C overnight to obtain nitrogen-doped carbon nanosheets, recorded as NCS-800.

[0083] (2) Preparation of Co / NCS composites:

[0084] First, in a 250 mL round-bottom flask, 50 mg NCS-800 and 550 mg 2-methylimidazole were dispersed in 50 mL methanol and ultrasonically treated, which was marked as solution A. After that, 330 mg Co(NO3)2·6H2O was dispersed in 45 mL methanol and ultrasonically treated, which was marked as solution B. Solution B was added dropwise to solution A, and the color of the mixture changed from gray to purple. The mixed solution was then stirred at a constant temperature of 70 ° C for 2 h. The purple precipitate NCS / ZIF-67 was collected and dried at 60 ° C. Finally, the obtained purple powder was kept at 800 ° C for 5 hours under Ar protection at a heating rate of 5 ° C / min to obtain a black powder product, which was the Co / NCS composite material. The SEM and TEM images showed that the Co particles were obviously loaded on the porous carbon nanosheets, and the nitrogen-doped carbon / cobalt-based absorbing material was prepared.

[0085] In order to explore the performance differences of Co / NCS composite materials obtained by pyrolyzing NCS / ZIF-67 at different temperatures, a series of Co / NCS composite materials were prepared using pyrolysis temperatures of 700°C, 800°C, and 900°C in Examples 1 to 3, respectively. The samples prepared at different pyrolysis temperatures were named Co / NCS-700, Co / NCS-800, and Co / NCS-900. The Co / NCS composite materials prepared in Examples 1 to 3 were subjected to X-ray diffraction analysis, vibrating sample magnetometer VSM, and electromagnetic wave absorption performance tests and characterizations.

[0086] Test 1: SEM analysis and TEM analysis.

[0087] The sample Co / NCS-700 prepared in Example 1, the sample Co / NCS-800 prepared in Example 2, and the sample Co / NCS-900 prepared in Example 3 were subjected to SEM analysis and TEM analysis, respectively. Figure 1 SEM analysis is scanning electron microscope analysis; TEM analysis is transmission electron microscope analysis. SEM images are scanning electron microscope images; TEM images are transmission electron microscope images.

[0088] Figure 1 The SEM images and TEM images of samples Co / NCS-700, Co / NCS-800 and Co / NCS-900 prepared in Examples 1 to 3. Among them, (a1) is the SEM image of Co / NCS-700; (b1) is the SEM image of Co / NCS-800; (c1) is the SEM image of Co / NCS-900; (a2) is the TEM image of Co / NCS-700; (b2) is the TEM image of Co / NCS-800; (c2) is the TEM image of Co / NCS-900.

[0089] Depend on Figure 1 The results show that the Co particles are obviously loaded on the porous carbon nanosheets, and the size of the magnetic particles decreases and the surface roughness increases with the increase of pyrolysis temperature.

[0090] Test 2: EDS analysis, HETEM analysis and SAED analysis.

[0091] The sample Co / NCS-800 prepared in Example 2 was subjected to EDS analysis, HETEM analysis and SAED analysis, and the results are shown in Figure 2 and Figure 3 EDS analysis is energy spectrum analysis; HETEM analysis is high-resolution transmission electron microscopy analysis; SAED analysis is selected area electron diffraction analysis. EDS graph is energy spectrum graph; HETEM graph is high-resolution transmission electron microscopy graph; SAED graph is selected area electron diffraction graph.

[0092] Figure 2 The EDS graph of the sample Co / NCS-800 prepared in Example 2. (d1) to (d4) are the EDS graphs of Co / NCS-800. Figure 3 HETEM image (e) and SAED image (f) of the sample Co / NCS-800 prepared in Example 2.

[0093] Depend on Figure 2 and Figure 3 The results show that diffraction rings of Co(111) and C(002) crystal planes can be seen in the selected area electron diffraction pattern, which is consistent with its high-resolution transmission electron microscopy information, indicating that the C, Co, and N elements are evenly distributed in the material.

[0094] Test 3: Raman spectroscopy and XRD analysis.

[0095] Raman spectroscopy and XRD analysis were performed on samples Co / NCS-700, Co / NCS-800 and Co / NCS-900 prepared in Examples 1 to 3, respectively. Figure 4 XRD analysis is X-ray diffraction analysis. XRD pattern is X-ray diffraction pattern.

[0096] Figure 4 Raman spectra (a) and XRD patterns (b) of samples Co / NCS-700, Co / NCS-800 and Co / NCS-900 prepared in Examples 1 to 3.

[0097] Depend on Figure 4 The results show that with the increase of pyrolysis temperature, the ID / IG value of the sample increases, proving that the defects in the material increase, and the characteristic peak of Co is enhanced, indicating that the crystallinity of Co particles increases with the increase of pyrolysis temperature.

[0098] Test 4: Adsorption-desorption curves and pore size analysis.

[0099] The adsorption-desorption curves and pore size analysis were performed on the samples Co / NCS-700, Co / NCS-800 and Co / NCS-900 prepared in Examples 1 to 3, respectively. Figure 5 .

[0100] Figure 5 (a) The adsorption-desorption curves and (b) pore size distribution diagrams of samples Co / NCS-700, Co / NCS-800 and Co / NCS-900 prepared in Examples 1 to 3.

[0101] Depend on Figure 5 The results show that the Co / NCS-800 sample has the largest specific surface area, and its pore size is concentrated in the range of 2nm to 4nm.

[0102] Test 5: Hysteresis loop analysis.

[0103] Hysteresis loop analysis was performed on samples Co / NCS-700, Co / NCS-800 and Co / NCS-900 prepared in Examples 1 to 3, and the results are shown in Figure 6 .

[0104] Figure 6 (a) is the hysteresis loop diagram of samples Co / NCS-700, Co / NCS-800 and Co / NCS-900 prepared in Examples 1 to 3 at room temperature and (b) is the partially enlarged hysteresis loop diagram at room temperature.

[0105] Depend on Figure 6 The results show that the Co / NCS-800 sample has a lower coercivity, which is beneficial to magnetic storage and electromagnetic wave attenuation.

[0106] Test 6: Electromagnetic parameter analysis.

[0107] Electromagnetic parameter analysis was performed on samples Co / NCS-700, Co / NCS-800 and Co / NCS-900 prepared in Examples 1 to 3, and the results are shown in Figure 7 .

[0108] Figure 7 The electromagnetic parameter diagrams of samples Co / NCS-700, Co / NCS-800 and Co / NCS-900 prepared in Examples 1 to 3. Among them, (a) is the real part of the dielectric constant; (b) is the imaginary part of the dielectric constant; (c) is the dielectric loss tangent; (d) is the real part of the magnetic permeability; (e) is the imaginary part of the magnetic permeability; (f) is the magnetic permeability loss tangent.

[0109] Depend on Figure 7The results show that the Co / NCS-800 sample has better dielectric loss performance and the best magnetic loss performance.

[0110] Test 7: Wave absorbing performance analysis.

[0111] The wave absorption performance of samples Co / NCS-700, Co / NCS-800 and Co / NCS-900 prepared in Examples 1 to 3 was analyzed respectively. The electromagnetic parameters of each sample were input into MATLAB, and the fitting thickness was between 1-5 mm and the frequency range was between 2-18 GHz. The reflectivity graphs of the three samples can be obtained by calculation. The results are shown in Figure 8 .

[0112] Figure 8 The reflection loss diagrams of samples Co / NCS-700, Co / NCS-800 and Co / NCS-900 prepared in Examples 1 to 3. (a) is the reflection loss diagram of Co / NCS-700; (b) is the reflection loss diagram of Co / NCS-800; (c) is the reflection loss diagram of Co / NCS-900.

[0113] Depend on Figure 8 The results show that the minimum reflection loss RL of the sample Co / NCS-800 of Example 2 when the matching thickness is 2.63 mm is min The effective absorption bandwidth reaches -58.34dB, and the effective absorption bandwidth reaches 7.52GHz when the matching thickness is 2.83mm, indicating that the sample Co / NCS-800 can absorb 90% of the electromagnetic waves in the frequency range of 10 to 18GHz. Compared with the reported composite absorbing materials, the effective absorption bandwidth of the electromagnetic wave absorption performance of the sample Co / NCS-800 of Example 2 at a thinner thickness of 2.83mm far exceeds that of most of the reported composite absorbing materials, further confirming the advantages of the composite materials and electromagnetic synergistic effects of the embodiments of the present invention in electromagnetic wave attenuation.

[0114] In summary, the above embodiment of the present invention prepares a magnetoelectric composite material by loading ZIF-67 on nitrogen-doped carbon nanosheets through high-temperature pyrolysis, so that the absorbing material can achieve broadband strong absorption in a thin layer and low filling amount state.

[0115] The above embodiments of the present invention use Co 2+The coordinated MOFs structure was used to prepare Co / NCS composites obtained by pyrolysis of nitrogen-doped carbon nanosheets loaded with ZIF-67 for electromagnetic wave absorption applications. The multiple heterogeneous interfaces formed by nitrogen-doped carbon nanosheets and Co magnetic particles further strengthen the interface polarization, defect polarization, and dipole polarization mechanisms to achieve multiple losses. In addition, the Co magnetic particles present in the Co / NCS composites obtained by high-temperature pyrolysis of nitrogen-doped carbon nanosheets loaded with ZIF-67 can induce magnetic losses, which synergize with the dielectric loss of the carbon matrix to jointly promote the loss of electromagnetic waves. These are only preliminary results and require more systematic research. The use of nitrogen-doped carbon nanosheets and MOFs with diverse structures to prepare magnetic transition metal / nitrogen-doped carbon composites is expected to obtain efficient wave absorbing materials.

[0116] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a nitrogen-doped carbon / cobalt-based absorber, characterized in that: The following steps are involved: Using nitrogen-doped carbon nanosheets as a matrix and 2-methylimidazole as an organic ligand, a co-precipitation reaction is carried out with a Co source in a solvent system to load the formed ZIF-67 on the nitrogen-doped carbon nanosheets, and then pyrolyzed at 700°C to 900°C under a protective atmosphere to obtain a nitrogen-doped carbon / cobalt-based absorber.

2. The method for preparing the nitrogen-doped carbon / cobalt-based absorber according to claim 1, characterized in that: The pyrolysis temperature is preferably 800° C. and the pyrolysis time is 3 h to 5 h.

3. The method for preparing the nitrogen-doped carbon / cobalt-based absorber according to claim 1, characterized in that: The Co source is Co(NO3)2·6H2O or CoCl2·6H2O; The mass ratio of nitrogen-doped carbon nanosheets, 2-methylimidazole and Co source is 50:500-600:300-360.

4. The method for preparing the nitrogen-doped carbon / cobalt-based absorber according to claim 1, characterized in that: The nitrogen-doped carbon nanosheets are prepared by the following method: With inorganic salt as template, a carbon source, a nitrogen source, an inorganic salt and water are mixed to prepare a solid mixture; the solid mixture is calcined under a protective atmosphere, then etched in hydrochloric acid, and washed to remove the inorganic salt to obtain nitrogen-doped carbon nanosheets.

5. The method for preparing the nitrogen-doped carbon / cobalt-based absorber according to claim 4, characterized in that: The carbon source is citric acid; the nitrogen source is urea; and the inorganic salt is potassium carbonate; The molar ratio of the carbon source, the nitrogen source and the inorganic salt is 0.01-0.015: 0.02-0.021: 0.05-0.

07.

6. The method for preparing the nitrogen-doped carbon / cobalt-based absorber according to claim 4, characterized in that: The calcination temperature is 600°C to 800°C; the calcination time is 1h to 3h.

7. The method for preparing the nitrogen-doped carbon / cobalt-based absorber according to claim 1, characterized in that: The temperature of the coprecipitation reaction is 65° C. to 70° C.; the time of the coprecipitation reaction is 0.5 h to 2 h.

8. The method for preparing the nitrogen-doped carbon / cobalt-based absorber according to claim 1, characterized in that: The solvent is methanol; the usage ratio of nitrogen-doped carbon nanosheets to methanol is 50 mg: 90 mL to 100 mL.

9. A nitrogen-doped carbon / cobalt-based absorber prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the nitrogen-doped carbon / cobalt-based absorber according to claim 9 in the preparation of electromagnetic wave absorbing materials.

Citation Information

Patent Citations

  • Method for preparing nitrogen-doped porous carbon by taking cottonseed hull as raw material and application

    CN108455597A

  • Preparation method and application of sulfur-nitrogen co-doped three-dimensional porous carbon nanosheet

    CN111825074A

  • Preparation method of CoNi / NC wave-absorbing material

    CN115332821A

  • Graphene-loaded core-shell structure nanoparticle material and preparation method thereof

    CN115400777A

  • Preparation method of graphene-loaded nitrogen-doped carbon nanocage-coated cobalt phosphide wave-absorbing material