All-solid-state secondary battery
The all-solid-state secondary battery structure with lithium-containing sulfide-based materials and an inactive member addresses safety and stability issues by preventing polysulfide reactions and electrolyte defects, ensuring stable ion and electron transport paths.
Patent Information
- Application Number
- CN202410720921.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-02-26
- Filing Date
- 2024-06-05
- Publication Date
- 2024-12-06
AI Technical Summary
Lithium secondary batteries face issues with safety due to flammable organic solvents, volume changes causing transport path disconnection, and defects in the solid electrolyte layer leading to short circuits, while all-solid-state batteries need to prevent polysulfide side reactions and electrolyte layer defects.
An all-solid-state secondary battery structure with a positive electrode layer, negative electrode layer, and solid electrolyte layer, incorporating lithium-containing sulfide-based materials and a first inactive member to prevent polysulfide reactions, maintain ion and electron transport paths, and suppress electrolyte layer defects.
Enhances safety by preventing short circuits and improving cycle characteristics through stable ion and electron transport paths, and suppressing polysulfide reactions and electrolyte defects.
Smart Images

Figure CN119092790A_ABST
Abstract
Description
[0001] This application is based on and claims the priority of Korean Patent Application No. 10-2023-0072378 filed in the Korean Intellectual Property Office on June 5, 2023, Korean Patent Application No. 10-2023-0113180 filed in the Korean Intellectual Property Office on August 28, 2023, and Korean Patent Application No. 10-2024-0027556 filed in the Korean Intellectual Property Office on February 26, 2024, and the disclosures of the three Korean patent applications are incorporated herein by reference in their entirety. Technical Field
[0002] One or more embodiments relate to an all-solid-state secondary battery. Background Art
[0003] Recently, with the rapid popularization of electronic devices (such as mobile phones, laptop computers and electric vehicles) using batteries, the demand for secondary batteries with high energy density and high capacity has increased rapidly. In addition, research and development for improving the performance of lithium secondary batteries has been actively carried out. A lithium secondary battery is a battery including an electrolyte and a positive electrode and a negative electrode each containing an active material capable of embedding and de-embedding lithium ions. If lithium ions are embedded in / de-embedded from the positive electrode and the negative electrode, the lithium secondary battery generates electrical energy through oxidation and reduction reactions.
[0004] Recently, due to the needs of industry, batteries with high energy density and safety have been actively developed. For example, lithium batteries are commercialized not only in the fields of information-related devices and communication devices, but also in the field of vehicles. In the field of vehicles, vehicles are related to life, so safety is particularly important.
[0005] Lithium batteries use an electrolyte solution including a flammable organic solvent as an electrolyte, and therefore short circuits occur, leading to the possibility of overheating and fire.
[0006] All-solid-state batteries using solid electrolytes instead of electrolyte solutions have been proposed.
[0007] All-solid-state batteries do not use flammable organic solvents, so even if a short circuit occurs, the possibility of fire or explosion can be greatly reduced. Compared with lithium batteries that use electrolytes, this all-solid-state battery can significantly improve safety. Summary of the invention
[0008] Secondary batteries use sulfur materials (e.g., S) as positive electrode active materials to increase capacity. During the charge / discharge process of the secondary battery, polysulfides are generated from the sulfur materials, and the generated polysulfides move to the negative electrode and react with the negative electrode. Due to this side reaction, the life characteristics of the secondary battery are deteriorated. A secondary battery capable of suppressing the side reaction between polysulfides and lithium metal is needed.
[0009] In a secondary battery including a sulfur-based material (e.g., S), the volume of the sulfur-based material increases during the initial discharge, so that the volume decreases again during the charging process, during which the volume of the sulfur-based material increases, the transport path of ions and / or electrons in the electrode is disconnected. This disconnection of the transport path of ions and / or electrons leads to the degradation of the secondary battery. A secondary battery capable of suppressing this disconnection of the transport path of ions and / or electrons is needed.
[0010] During the manufacturing process and / or charging / discharging process of the secondary battery, a defect occurs in the solid electrolyte layer, and due to this defect, a crack appears and grows in the solid electrolyte layer. When lithium grows through this crack, a short circuit occurs. A secondary battery is needed that can suppress the occurrence of this defect during the manufacturing process and / or charging / discharging process of the secondary battery.
[0011] One or more embodiments include a secondary battery having a new structure that prevents side reactions between an electrolyte layer and lithium metal during charge / discharge, suppresses disconnection of a transport path for ions and / or electrons, prevents side reactions caused by polysulfides during charge / discharge, and suppresses defects in the secondary battery during manufacturing and / or charge / discharge.
[0012] Additional aspects will be set forth in part in the description which follows and, in part, will be obvious from the description, or may be learned by practice of the disclosed presented embodiments.
[0013] According to one or more embodiments, an all-solid-state secondary battery includes: a positive electrode layer; a negative electrode layer; a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer; and a first inactive member disposed on one side of the positive electrode layer, wherein the positive electrode layer includes a positive electrode current collector and a positive electrode active material layer disposed on one side or both sides of the positive electrode current collector, the positive electrode active material layer includes a lithium-containing sulfide-based positive electrode active material, the lithium-containing sulfide-based positive electrode active material includes Li2S, a Li2S-containing composite, or a combination thereof, the negative electrode layer includes a negative electrode current collector and a first negative electrode active material layer disposed on one side of the negative electrode current collector, a ratio (B / A) of an initial charge capacity (B) of the first negative electrode active material layer to an initial charge capacity (A) of the positive electrode active material layer is in the range of about 0.005 to about 0.45, and the initial charge capacity of the positive electrode active material layer is charged from a first open circuit voltage to a voltage for Li / Li+ The initial charge capacity of the first negative electrode active material layer is determined by charging from the second open circuit voltage to the maximum charge voltage of Li / Li + A voltage of about 0.01V is determined.
[0014] According to one or more embodiments, an all-solid-state secondary battery includes: a positive electrode layer; a negative electrode layer; a solid electrolyte layer, arranged between the positive electrode layer and the negative electrode layer, wherein the positive electrode layer includes a positive electrode collector and a positive electrode active material layer arranged on one side or both sides of the positive electrode collector, and the negative electrode layer includes a negative electrode collector and a first negative electrode active material layer arranged on one side of the negative electrode collector, wherein the positive electrode active material layer includes a lithium-containing sulfide-based positive electrode active material, the lithium-containing sulfide-based positive electrode active material includes a Li2S-containing complex, and the Li2S-containing complex includes: a complex of Li2S and a lithium salt; a complex of Li2S, a lithium salt and a conductive material; a complex of Li2S and a metal halide; a complex of Li2S, a metal halide and a conductive material; a complex of Li2S, a lithium salt and a metal halide; a complex of Li2S, a lithium salt, a metal halide and a conductive material; a complex of Li2S, a lithium salt and a metal halide; a complex of Li2S, a lithium salt, a metal halide and a conductive material; or a combination thereof.
[0015] An all-solid-state secondary battery includes: a positive electrode layer; a negative electrode layer; a solid electrolyte layer, arranged between the positive electrode layer and the negative electrode layer; and a first inactive component arranged on the side of the positive electrode layer, wherein the positive electrode layer includes a positive electrode collector and a positive electrode active material layer arranged on one side or both sides of the positive electrode collector, the positive electrode active material layer includes a lithium-containing sulfide-based positive electrode active material, the lithium-containing sulfide-based positive electrode active material includes a Li2S-containing complex, and the negative electrode layer includes a negative electrode collector and a first negative electrode active material layer arranged on one side of the negative electrode collector. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The above and other aspects, features and advantages of certain disclosed embodiments will be more apparent from the following description in conjunction with the accompanying drawings, in which:
[0017] Figure 1 is a cross-sectional view of an all-solid-state secondary battery according to an embodiment.
[0018] Figure 2 is a cross-sectional view of an all-solid-state secondary battery according to an embodiment.
[0019] Figure 3 is a cross-sectional view of a dual-cell all-solid-state secondary battery according to an embodiment;
[0020] Figure 4 is a schematic diagram of a positive electrode layer of an all-solid-state secondary battery according to an embodiment;
[0021] Figure 5is a schematic diagram partially showing the interior of an all-solid-state secondary battery according to an embodiment;
[0022] Figure 6 is a cross-sectional view of an all-solid-state secondary battery according to an embodiment;
[0023] Figure 7 is a cross-sectional view of an all-solid-state secondary battery according to an embodiment;
[0024] Figure 8 is a cross-sectional view of a dual-cell all-solid-state secondary battery according to an embodiment; and
[0025] Fig. 9 is a cross-sectional view of a stack of stacked dual-cell all-solid-state secondary batteries according to an embodiment. DETAILED DESCRIPTION
[0026] Reference will now be made in detail to embodiments, examples of which are shown in the accompanying drawings, wherein the same reference numerals always refer to the same elements. In this regard, the embodiments provided may have different forms and should not be construed as being limited to the descriptions set forth herein. In addition, the embodiments are described below only by reference to the drawings to explain aspects of this specification. As used herein, the term "and / or" includes any and all combinations of one or more of the related listed items. If a statement such as "at least one (kind / person) of ... " is after a column of elements, the entire column of elements is modified without modifying the individual elements of the column.
[0027] Various embodiments are shown in the accompanying drawings. However, the inventive concept may be implemented in different forms and should not be construed as being limited to the embodiments set forth herein. On the contrary, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the inventive concept to those skilled in the art. The same reference numerals represent the same elements.
[0028] It will be understood that if an element is described as being "on" another element, it can be directly disposed on the other element, or another element may be present between them. In addition, if an element is described as being "directly on" another element, another element may not be present between them.
[0029] It will be understood that although the terms "first", "second", and "third" may be used herein to describe various elements, components, regions, layers, and / or parts, these elements, components, regions, layers, and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer, or part from another element, component, region, layer, or part. Therefore, without departing from the teachings of this specification, the first element, component, region, layer, or part described below may be referred to as a second element, component, region, layer, or part.
[0030] The terms used herein are only used for the purpose of describing specific embodiments and are not intended to limit the inventive concept. As used herein, unless the content clearly indicates otherwise, the singular forms "one", "one (kind / person)" and "the (described)" are also intended to include the plural forms comprising "at least one (kind / person)". "At least one (kind / person)" should not be interpreted as being limited to the singular. As used herein, the term "and / or" includes any combination and all combinations of one or more of the related listed items. When the terms "include", "comprising" and / or its variations are used in a specific embodiment, it is indicated that there are stated features, regions, integers, steps, operations, elements and / or components, but it is not excluded that there are or add one or more other features, regions, integers, steps, operations, elements, components and / or their groups.
[0031] Spatially relative terms such as "under," "below," "below," "above," and "on" may be used herein to easily describe the relationship of one element or feature to another. It will be understood that, in addition to the orientations shown in the figures, the spatially relative terms are also intended to cover different orientations of the device in use or operation. For example, if the device in the accompanying drawings is turned over, an element described as "under" or "below" other elements or features will then be located "above" or "on" the other elements or features. Thus, the example term "under" may cover both above and below orientations. The device may be otherwise oriented (rotated 90 degrees or in other orientations), and the spatially relative terms used herein may be interpreted accordingly.
[0032] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those commonly understood by those skilled in the art to which the present disclosure belongs. In addition, it will also be understood that terms (such as those defined in commonly used dictionaries) should be interpreted as having a meaning consistent with their meaning in the context of the relevant art and the present disclosure, and will not be interpreted in an idealized or overly formal sense unless explicitly defined as such herein.
[0033] Embodiments are described herein with reference to cross-sectional views as schematic diagrams of idealized embodiments. As such, variations in the illustrated shapes due to, for example, manufacturing techniques and / or tolerances are expected. Therefore, the embodiments described herein should not be construed as being limited to the specific shape regions shown herein, but may include shape deviations, for example, caused by manufacturing. For example, a region shown or described as flat may typically be rough and / or have nonlinear features. In addition, sharply drawn angles may be rounded. Therefore, the regions shown in the drawings are schematic in nature, and their shapes are not intended to illustrate the actual shape of the region, and are not intended to limit the scope of the claims.
[0034] "Group" refers to a Group of the Periodic Table of the Elements according to the International Union of Pure and Applied Chemistry ("IUPAC") Group I to Group XVIII classification system.
[0035] Unless otherwise defined herein, particle diameter can be average particle diameter. For example, particle diameter refers to average particle diameter (D50), which refers to the diameter of particles with a cumulative volume of 50 volume % in particle size distribution. Average particle diameter (D50) can be measured by methods well known to those skilled in the art (for example, by using a particle size analyzer (PSA), a transmission electron microscope (TEM) image or a scanning electron microscope (SEM) image). By other methods, it is possible to measure by using a measuring device utilizing dynamic light scattering, perform data analysis to count the number of particles in each size range, and then the value of average particle diameter (D50) can be easily obtained therefrom by calculation. In other embodiments, average particle diameter (D50) can be measured by using a laser diffraction method. During measurement by laser diffraction, more specifically, the particles to be measured can be dispersed in a dispersion medium and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT3000), 28 kHz ultrasonic waves can be irradiated thereto at an output power of about 60 W, and then the average particle size (D50) based on 50% particle size distribution can be calculated in the measuring device.
[0036] As used herein, if the particles are spherical, the term "particle size" refers to the average diameter, and if the particles are non-spherical, the term "particle size" refers to the average major axis length. "Average particle size" refers to, for example, D50 which is the median particle size.
[0037] D50 is a particle size corresponding to 50% cumulative volume if the particle size distribution measured by the laser diffraction method is calculated starting from particles having a smaller particle size.
[0038] D90 is a particle size corresponding to 90% cumulative volume if the particle size distribution measured by the laser diffraction method is calculated starting from particles having a smaller particle size.
[0039] D10 is a particle size corresponding to 10% cumulative volume if the particle size distribution measured by the laser diffraction method is calculated starting from particles having a smaller particle size.
[0040] The term "metal" as used herein includes all metals and metalloids (such as silicon and germanium) in the elemental or ionic state.
[0041] As used herein, the term "alloy" refers to a mixture of two or more metals.
[0042] As used herein, the term "electrode active material" refers to an electrode material that can undergo lithiation and delithiation.
[0043] As used herein, the term "positive electrode active material" refers to a positive electrode material that can undergo lithiation and delithiation.
[0044] As used herein, the term "negative electrode active material" refers to a negative electrode material that can undergo lithiation and delithiation.
[0045] As used herein, the term "lithiation" and variations thereof refer to the process of adding lithium to an electrode active material.
[0046] As used herein, the term "delithiation" and variations thereof refer to the process of removing lithium from an electrode active material.
[0047] As used herein, the term "charging" and variations thereof refer to the process of providing electrochemical energy to a battery.
[0048] As used herein, the term "discharge" and variations thereof refer to the process of removing electrochemical energy from a battery.
[0049] As used herein, the terms "positive electrode" and "positive electrode" refer to the electrode that undergoes electrochemical reduction and lithiation during the discharge process.
[0050] As used herein, the terms "negative electrode" and "negative electrode" refer to an electrode that undergoes electrochemical oxidation and delithiation during the discharge process.
[0051] Although specific embodiments have been described, the applicant or other persons skilled in the art may think of substitutions, modifications, variations, improvements, and substantial equivalents that are not currently foreseeable or may not be foreseeable. In some embodiments, the appended claims submitted and as they may be amended are intended to cover all such substitutions, modifications, variations, improvements, and substantial equivalents.
[0052] Hereinafter, an all-solid-state secondary battery according to an embodiment will be described in more detail.
[0053] [All-solid-state secondary battery]
[0054] The all-solid-state secondary battery according to the embodiment may include a positive electrode layer, a negative electrode layer, a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, and a first inactive member disposed on the side of the positive electrode layer. The positive electrode layer may include a positive electrode current collector and a positive electrode active material layer disposed on one side or both sides of the positive electrode current collector. The positive electrode active material layer may include a lithium-containing sulfide-based positive electrode active material. The lithium-containing sulfide-based positive electrode active material may include Li2S, a Li2S-containing composite, or a combination thereof. The negative electrode layer may include a negative electrode current collector and a first negative electrode active material layer disposed on one side of the negative electrode current collector. The ratio (B / A) of the initial charge capacity (B) of the first negative electrode active material layer to the initial charge capacity (A) of the positive electrode active material layer may be in the range of about 0.005 to about 0.45. The initial charge capacity of the positive electrode active material layer may be charged from a first open circuit voltage (OCV) to a voltage for Li / Li + Maximum charge voltage (e.g., maximum charge voltage vs. Li / Li + ) is determined. The initial charge capacity of the first negative electrode active material layer is determined by charging from the second OCV to the Li / Li + A voltage of about 0.01V is determined.
[0055] The all-solid-state secondary battery may include a lithium-containing sulfide-based positive electrode active material instead of lithium metal as a lithium source. In some embodiments, the lithium source (such as lithium metal) may be omitted from the negative electrode layer. Since the volume of the negative electrode layer is reduced, the energy density of the all-solid-state secondary battery is increased.
[0056] The all-solid-state secondary battery may include a lithium-containing sulfide-based positive electrode active material as a positive electrode active material. In some embodiments, the disconnection of the transport path of ions and / or electrons caused by the increase in volume of the lithium-free sulfide-based positive electrode active material (e.g., sulfur (S)) during the initial discharge can be prevented. The disconnection of the transport path of ions and / or electrons can be prevented, thereby improving the cycle characteristics of the all-solid-state secondary battery.
[0057] The all-solid-state secondary battery may include a first negative electrode active material layer having an initial charge capacity in the range of about 0.005 to about 0.45 relative to the initial charge capacity of the positive electrode active material layer. Since the first negative electrode active material layer has a small initial charge capacity in this range, the negative electrode layer can effectively compensate for the volume change of the positive electrode layer during charge / discharge. In some embodiments, the total volume change of the all-solid-state secondary battery can be suppressed during charge / discharge. Since the deterioration caused by the occurrence of cracks and the like caused by rapid volume changes during charge / discharge of the all-solid-state secondary battery can be prevented, the short circuit of the all-solid-state secondary battery is prevented and the cycle characteristics are improved.
[0058] Since the all-solid-state secondary battery can include a solid electrolyte layer, polysulfides generated in the lithium-containing sulfide-based positive electrode active material during charge / discharge can be prevented from moving to the negative electrode layer. In some embodiments, side reactions between polysulfides and the negative electrode active material can be suppressed.
[0059] The first inactive member may be disposed on the side of the positive electrode layer, thereby suppressing cracks in the solid electrolyte layer that occur during the pressing and / or charging / discharging of the all-solid-state secondary battery. In some embodiments, cracks in the solid electrolyte layer may be suppressed during the manufacture and / or charging / discharging of the all-solid-state secondary battery, thereby suppressing a short circuit of the all-solid-state secondary battery. In some embodiments, a short circuit of the all-solid-state secondary battery may be prevented, and the life characteristics of the all-solid-state secondary battery may be improved.
[0060] Reference Figures 1 to 9 , the all-solid-state secondary battery 1 may include a positive electrode layer 10, a negative electrode layer 20, and a solid electrolyte layer 30 disposed between the positive electrode layer 10 and the negative electrode layer 20. The positive electrode layer 10 may include a positive electrode collector 11 and a positive electrode active material layer 12 disposed on one side or both sides of the positive electrode collector 11. The positive electrode active material layer 12 may include a sulfide-based positive electrode active material. The sulfide-based positive electrode active material may include Li2S, a composite containing Li2S, or a combination thereof. The all-solid-state secondary battery 1 may include a first inactive member 40 disposed on a side of the positive electrode layer 10. The negative electrode layer 20 includes a negative electrode collector 21 and a first negative electrode active material layer 22 disposed on one side of the negative electrode collector 21. The ratio (B / A) of the initial charge capacity (B) of the first negative electrode active material layer 22 to the initial charge capacity (A) of the positive electrode active material layer 12 may be in the range of about 0.005 to about 0.45. The initial charge capacity of the positive electrode active material layer 12 can be increased by charging from the first OCV to the Li / Li + The initial charge capacity of the first negative electrode active material layer can be determined by charging from the second OCV to the maximum charge voltage of Li / Li + The ratio (B / A) of the initial charge capacity (B) of the first negative active material layer 22 to the initial charge capacity (A) of the positive active material layer 12 may be, for example, in the range of about 0.01 to about 0.4, about 0.01 to about 0.3, or about 0.01 to about 0.1.
[0061] [Positive electrode layer]
[0062] [Positive electrode layer: positive electrode active material]
[0063] Reference Figures 1 to 9, the positive electrode active material layer 12 may include, for example, a positive electrode active material and a solid electrolyte. The solid electrolyte included in the positive electrode active material layer 12 may be similar to or different from the solid electrolyte included in the solid electrolyte layer 30. The solid electrolyte may be defined as in the part of the solid electrolyte layer 30.
[0064] The positive electrode active material may include a lithium-containing sulfide-based positive electrode active material. The lithium-containing sulfide-based positive electrode active material may be, for example, an electrode material in which lithium is added to a sulfur-based positive electrode active material. The sulfur-based positive electrode active material may include, for example, a sulfur-based material, a composite containing a sulfur-based material, or a combination thereof. The sulfur-based material may be, for example, inorganic sulfur, Li2Sn (where n>1), a disulfide compound, an organic sulfur compound, a carbon-sulfur polymer, or a combination thereof. The composite containing a sulfur-based material may be a composite including inorganic sulfur, Li2Sn (where n>1), a disulfide compound, an organic sulfur compound, a carbon-sulfur polymer, or a combination thereof. The composite of the sulfur-containing material may include, for example, a composite of a sulfur-containing material and carbon, a composite of a sulfur-containing material, carbon and a solid electrolyte, a composite of a sulfur-containing material, carbon and a lithium salt, a composite of a sulfur-containing material and a lithium salt, a composite of a sulfur-containing material and a solid electrolyte, a composite of a sulfur-containing material and a metal carbide, a composite of a sulfur-containing material, carbon and a metal carbide, a composite of a sulfur-containing material and a metal nitride, a composite of a sulfur-containing material, carbon and a metal nitride, or a combination thereof. Since the lithium-containing sulfide-based positive active material can provide a higher discharge capacity per unit weight than the oxide-based positive active material, the energy density per unit weight of the all-solid-state secondary battery including the lithium-containing sulfide-based positive active material can be increased.
[0065] The lithium-containing sulfide positive electrode active material may include, for example, Li2S, a composite containing Li2S, or a combination thereof. Since the lithium-containing sulfide positive electrode active material may include Li2S with high capacity, a composite containing Li2S, or a combination thereof, if an all-solid-state secondary battery is manufactured, the use of lithium metal may be omitted. Since lithium metal may have high reactivity and high ductility, lithium metal may reduce the mass production rate during the manufacture of the battery. In some embodiments, the mass production rate of the all-solid-state secondary battery may be improved. Since lithium metal may be omitted from the negative electrode layer, the volume of the negative electrode layer may be reduced, thereby improving the energy density per unit volume of the all-solid-state secondary battery, and constructing an all-solid-state secondary battery with a simpler structure.
[0066] The lithium-containing sulfide positive electrode active material (e.g., Li2S) may undergo delithiation, for example, during the initial charge, so that its volume may be reduced, and the lithium-containing sulfide positive electrode active material may undergo lithiation again during the subsequent discharge, so that its volume may increase. In some embodiments, since the volume of the lithium-containing sulfide positive electrode active material may change in a state where the transmission path of ions and / or electrons is maintained due to the conductive material, etc. disposed around the lithium-containing sulfide positive electrode active material, the possibility of disconnection of the transmission path of ions and / or electrons may be low. In other embodiments, the sulfur-based positive electrode active material (e.g., S) may undergo lithiation, for example, during the initial discharge, so that its volume increases, and the sulfur-based positive electrode active material may undergo delithiation again during the subsequent charge, so that its volume may be reduced. In some embodiments, the initial transmission path of ions and / or electrons caused by the conductive material, etc. disposed around the sulfur-based positive electrode active material may collapse due to the initial volume increase of the sulfur-based positive electrode active material, so the possibility of disconnection of the transmission path of ions and / or electrons may be high.
[0067] The particle size of the lithium-containing sulfide positive electrode active material can be, for example, about 1 nm to about 50 μm, about 10 nm to about 50 μm, about 50 nm to about 40 μm, about 100 nm to about 30 μm, about 500 nm to about 30 μm, or about 1 μm to about 20 μm. Since the lithium-containing sulfide positive electrode active material can have a particle size within this range, the cycle characteristics of the all-solid-state secondary battery including the sulfide positive electrode active material can be further improved. The Li2S-containing composite can be, for example, a composite of Li2S and a conductive material. The conductive material can be, for example, an ion conductive material, an electronic conductive material, or a combination thereof.
[0068] The electronically conductive material may have, for example, 1.0×10 3 S / m, 1.0×10 4 S / m or 1.0×10 5S / m or greater electronic conductivity. The electronic conductive material may be, for example, in the form of a granular electronic conductive material, a plate-like electronic conductive material, a rod-like electronic conductive material, or a combination thereof, but is not necessarily limited thereto. The electronic conductive material may include, for example, carbon, metal powder, a metal compound, etc. If carbon is included as an electronic conductive material, the carbon may have a high electronic conductivity and may be light, so that an all-solid-state secondary battery with a high energy density per unit mass can be achieved. The electronic conductive material may have holes. Since the electronic conductive material may have holes, Li2S may be included in the holes, thereby increasing the contact area between Li2S and the electronic conductive material and increasing the specific surface area of Li2S. The pore volume may be, for example, in the range of about 0.1cc / g to about 20.0cc / g, about 0.5cc / g to about 10cc / g, or about 0.5cc / g to about 5cc / g. The average pore size may be, for example, in the range of about 1nm to about 100nm, about 1nm to about 50nm, or about 1nm to about 20nm. If the average pore size is 15 nm or less, the Brunauer, Emmett and Teller (BET) specific surface area of the electronic conductive material having pores can be about 200 m 2 / g to about 4,500m 2 / g, and if the average pore size is greater than about 15 nm, the Brunauer, Emmett and Teller (BET) specific surface area of the electronic conductive material having pores may be about 100 m 2 / g to about 2,500m 2 The BET specific surface area, pore size, pore volume and average pore size can be obtained using, for example, a nitrogen adsorption method (such as ASTM D6556, ASTM D4567 and / or ISO9277:2022).
[0069] The ion-conducting material may have, for example, 1.0×10 -5 S / m, 1.0×10 -4 S / m or 1.0×10 -3 S / m or greater ionic conductivity. The ionic conductive material may have holes. Since the ionic conductive material may have holes, Li2S may be included in the holes, thereby increasing the contact area between Li2S and the ionic conductive material and increasing the specific surface area of Li2S. The ionic conductive material may be, for example, in the form of a granular ionic conductive material, a plate-like ionic conductive material, a rod-like ionic conductive material, or a combination thereof, but is not necessarily limited thereto. The ionic conductive material may be, for example, a sulfide-based solid electrolyte or an oxide-based solid electrolyte. If a sulfide-based solid electrolyte is included as an ionic conductive material, the sulfide-based solid electrolyte may have a high ionic conductivity and may be formed into various forms, thereby realizing an all-solid-state secondary battery with a large capacity.
[0070] The composite containing Li2S may include, for example, a composite of Li2S and a conductive material, a composite of Li2S, a solid electrolyte and a conductive material, a composite of Li2S and a solid electrolyte, a composite of Li2S, a lithium salt and a conductive material, a composite of Li2S and a lithium salt, a composite of Li2S and a metal carbide, a composite of Li2S, a metal carbide and a conductive material, a composite of Li2S and a metal nitride, a composite of Li2S, a metal nitride and a conductive material, or a combination thereof. The composite containing Li2S may be distinguished from a simple mixture of Li2S, a conductive material, a solid electrolyte, a lithium salt, a metal carbide and a metal nitride. A simple mixture of Li2S, a conductive material, a solid electrolyte, a lithium salt, a metal carbide and a metal nitride may provide a high interface resistance because a dense interface between Li2S and these components is not maintained, and thus the life characteristics of the all-solid-state secondary battery may be degraded.
[0071] The composite containing Li2S may include, for example, a composite of Li2S and a lithium salt, a composite of Li2S, a lithium salt and a conductive material, a composite of Li2S and a metal halide, a composite of Li2S, a metal halide and a conductive material, a composite of Li2S, a lithium salt and a metal halide, a composite of Li2S, a lithium salt, a metal halide and a conductive material, or a combination thereof. The composite containing Li2S may be distinguished from a simple mixture of Li2S, a lithium salt, a metal halide and a conductive material. A simple mixture of Li2S, a metal halide, a lithium salt and a conductive material may provide a high interface resistance because a dense interface between Li2S and these other components is not maintained, thereby deteriorating the life characteristics of an all-solid-state secondary battery. The composite containing Li2S may include Li2S. Since L2S may have a high theoretical capacity, a secondary battery with a high energy density may be provided. However, in order to overcome disadvantages such as low ionic conductivity and / or low electronic conductivity, L2S may form a composite with a lithium salt, a metal halide, a conductive material, and the like. Relative to the total weight of the Li2S-containing composite, the content of Li2S in the Li2S-containing composite can be, for example, in the range of about 10wt% to about 80wt%, about 20wt% to about 80wt%, about 30wt% to about 80wt%, or about 40wt% to about 80wt%. If the content of Li2S in the Li2S-containing composite is excessively increased, it will not be easy to improve the ionic conductivity and / or electronic conductivity of the Li2S-containing composite. If the content of Li2S in the Li2S-containing composite is too low, the energy density of the all-solid-state secondary battery will be reduced.
[0072] The composite of Li2S and the conductive material may include a conductive material. The conductive material may include, for example, a carbon-based material. As the carbon-based material, for example, any material may be used as long as the material may be a material including carbon atoms and may be used as a conductive material in the art. The carbon-based material may be, for example, a crystalline carbon-based material, an amorphous carbon-based material, or a combination thereof. The carbon-based material may be, for example, a sintered material of a carbon precursor. The carbon-based material may include, for example, a carbon nanostructure.
[0073] The carbon nanostructure may be, for example, a one-dimensional carbon nanostructure, a two-dimensional carbon nanostructure, a three-dimensional carbon nanostructure, or a combination thereof. The carbon nanostructure may be, for example, a carbon nanotube (CNT), a carbon nanofiber (CNF), a carbon nanobelt, a carbon nanorod, a graphene, or a combination thereof. The carbon-based material may be, for example, a porous carbon-based material or a nonporous carbon-based material. The porous carbon-based material may include, for example, periodic and regular two-dimensional or three-dimensional pores. The porous carbon-based material may include, for example, carbon black (CB) (such as Ketjen black (KB), acetylene black (AB), superconducting acetylene black (Denka black), thermal black (thermal black) or channel black (channel black)), graphite, activated carbon, or a combination thereof. The form of the carbon-based material may be, for example, a particle form, a sheet form, or a plate form, etc., but one or more embodiments are not limited thereto. Any material may be used as long as the material is used as a carbon-based material in the art. The method for preparing a composite of Li2S and a carbon-based material may be a dry method, a wet method, or a combination thereof, but is not limited thereto. In the art, methods for preparing a composite of Li2S and a carbon-based material may include, for example, a grinding method, a heat treatment method, a deposition method, etc., but one or more embodiments are not limited thereto. Any method may be used as long as the method can be used in the art.
[0074] The composite of Li2S, solid electrolyte and conductive material may include conductive material and solid electrolyte. The conductive material may include, for example, carbon-based materials. Carbon-based materials may be defined as the above-mentioned carbon-based materials used in the composite of Li2S and conductive material. As a solid electrolyte, for example, any material used as an ion conductive material in the art may be used. The solid electrolyte may be, for example, an inorganic solid electrolyte. The solid electrolyte may be, for example, a crystalline solid electrolyte, an amorphous solid electrolyte, or a combination thereof. The solid electrolyte may be, for example, a sulfide-based solid electrolyte, an oxide-based solid electrolyte, or a combination thereof. The sulfide-based solid electrolyte may include, for example, Li, S and P, and may optionally further include a halogen element. The sulfide-based solid electrolyte may be selected from the sulfide-based solid electrolyte used in the solid electrolyte layer 30. For example, the sulfide-based solid electrolyte may have a carbon content of 1×10 -5S / m or more. The oxide-based solid electrolyte may include, for example, Li, O, and a transition metal element, and may optionally further include other elements. The oxide-based solid electrolyte may be, for example, a solid electrolyte having an ionic conductivity of 1×10 -5 The oxide-based solid electrolyte may be selected from oxide-based solid electrolytes used in the solid electrolyte layer 30 .
[0075] The solid electrolyte may be defined as the above-mentioned solid electrolyte used in a composite of Li2S, a conductive material, and a solid electrolyte.
[0076] The composite of Li2S, lithium salt and conductive material may include Li2S, lithium salt and conductive material. The conductive material may include, for example, carbon-based materials. The carbon-based material may be defined as the above-mentioned carbon-based material used in the composite of Li2S and conductive material. The lithium salt may be a compound that does not include sulfur (S). The lithium salt may be, for example, a binary compound or a ternary compound. For example, the lithium salt may be a binary compound including lithium and an element selected from Groups XIII to XVII of the periodic table. The binary compound may include, for example, at least one selected from LiF, LiCl, LiBr, LiI, LiH, Li2O, Li2Se, Li2Te, Li3N, Li3P, Li3As, Li3Sb, Li3Al2 and Li3B. For example, the lithium salt may be a ternary compound including lithium and two elements selected from Groups XIII to XVII of the periodic table. The ternary compound may include, for example, at least one selected from Li3OCl, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiNO3, Li2CO3, LiBH4, Li3BO3, Li3PO4, Li4NCl, Li5NCl2 and Li3BN2. The lithium salt may include at least one lithium halide compound selected from LiF, LiCl, LiBr and LiI. The composite of Li2S, lithium salt and conductive material may be, for example, a composite of Li2S, lithium halide and carbon-based material. The composite of Li2S, lithium salt and carbon-based material may also include lithium halide, thus providing further improved ionic conductivity. The composite of Li2S, lithium salt and carbon-based material may be distinguished from a simple mixture of Li2S, lithium salt and carbon-based material. The simple mixture of Li2S, lithium salt and carbon-based material may provide high interface resistance because it will not maintain a dense interface between Li2S, lithium salt and carbon-based material, thus deteriorating the life characteristics of the all-solid-state secondary battery.
[0077] The composite of Li2S and a lithium salt may include a lithium salt. The lithium salt may be defined as the above-mentioned lithium salt used in the composite of Li2S, a lithium salt and a conductive material.
[0078] The composite of Li2S and metal carbide may include metal carbide. The metal carbide may be, for example, a two-dimensional metal carbide. The two-dimensional metal carbide may be, for example, M n+1 C n T x (wherein M is a transition metal, T is an end group, T is O, OH and / or F, n=1, 2 or 3, and x is the number of end groups). The two-dimensional metal carbide may be, for example, Ti2CT x 、(Ti 0.5 ,Nb 0.5 )2CT x 、Nb2CT x 、V2CT x 、Ti3C2T x ,(V 0.5 ,Cr 0.5 )3C2T x 、Ti3CNT x 、Ta4C3T x 、Nb4C3T x or a combination thereof. The surface of the two-dimensional metal carbide may be terminated with O, OH and / or F, wherein the total number of O, OH and / or F groups at the surface is the number of terminal groups.
[0079] The composite of Li2S, metal carbide and conductive material may include Li2S, metal carbide and conductive material. The conductive material may include, for example, carbon-based materials. Carbon-based materials may be defined as the above-mentioned carbon-based materials used in the composite of Li2S and conductive material. Metal carbide may be defined as the metal carbide used in the above-mentioned composite of Li2S and metal carbide.
[0080] The composite of Li2S and metal nitride may include Li2S and metal nitride. The metal nitride may be, for example, a two-dimensional metal nitride. The two-dimensional metal nitride may be, for example, M n+1 N n T x (wherein M is a transition metal, T is a terminal group, T is O, OH and / or F, n=1, 2 or 3, and x is the number of terminal groups). The surface of the two-dimensional metal nitride can be terminated with O, OH and / or F, wherein the total number of O, OH and / or F groups at the surface is the number of terminal groups.
[0081] The composite of Li2S, metal nitride and conductive material may include Li2S, metal nitride and conductive material. The conductive material may include, for example, a carbon-based material. The carbon-based material may be defined as the above-mentioned carbon-based material used in the composite of Li2S and conductive material. The metal nitride may be defined as the above-mentioned metal nitride used in the composite of Li2S and metal nitride.
[0082] Li2S and lithium salt (Li a X1 b ) can be composed, for example, of Li2S-Li a X1 b Represents, wherein 1≤a≤5, 1≤b≤5, and X1 is I, Br, Cl, F, H, O, Se, Te, N, P, As, Sb, Al, B, OCl, PF6, BF4, SbF6, AsF6, ClO4, AlO2, AlCl4, NO3, CO3, BH4, SO4, BO3, PO4, NCl, NCl2, BN2 or a combination thereof.
[0083] Li2S, lithium salt (Li a X1 b ) and the conductive material (C) can be composed of, for example, Li2S-Li a X1 b -C represents, wherein 1≤a≤5, 1≤b≤5, and X1 is I, Br, Cl, F, H, O, Se, Te, N, P, As, Sb, Al, B, OCl, PF6, BF4, SbF6, AsF6, ClO4, AlO2, AlCl4, NO3, CO3, BH4, SO4, BO3, PO4, NCl, NCl2, BN2 or a combination thereof. The conductive material can be, for example, a carbon-based material.
[0084] Li2S and metal halide (M c X2 d ) can be composed, for example, of Li2S-M c X2 d , wherein 1≤c≤5, 1≤d≤5, M is at least one metal selected from Group II to Group XV of the periodic table, and X2 is I, Br, Cl, F or a combination thereof. The conductive material may be, for example, a carbon-based material.
[0085] Li2S, metal halide (M c X2 d ) and the conductive material (C) can be composed of, for example, Li2S-M c X2 d -C represents, wherein 1≤c≤5, 1≤d≤5, M is at least one metal selected from Group II to Group XV of the periodic table, and X2 is I, Br, Cl, F or a combination thereof. The conductive material may be, for example, a carbon-based material.
[0086] Li2S, lithium salt (Li a X1 b ) and metal halides (M a X2 b) can be composed of Li2S-Li a X1 b -M c X2 d , wherein 1≤a≤5, 1≤b≤5, 1≤c≤5, 1≤d≤5, X1 is I, Br, Cl, F, H, O, Se, Te, N, P, As, Sb, Al, B, OCl, PF6, BF4, SbF6, AsF6, ClO4, AlO2, AlCl4, NO3, CO3, BH4, SO4, BO3, PO4, NCl, NCl2, BN2 or a combination thereof, M is at least one metal selected from Group II to Group XV of the periodic table, and X2 is I, Br, Cl, F or a combination thereof. The conductive material may be, for example, a carbon-based material.
[0087] Li2S, lithium salt (Li a X1 b ), metal halide (M a X2 b ) and the conductive material (C) can be composed of Li2S-Li a X1 b -M c X2 d -C represents, wherein 1≤a≤5, 1≤b≤5, 1≤c≤5, 1≤d≤5, X1 is I, Br, Cl, F, H, O, Se, Te, N, P, As, Sb, Al, B, OCl, PF6, BF4, SbF6, AsF6, ClO4, AlO2, AlCl4, NO3, CO3, BH4, SO4, BO3, PO4, NCl, NCl2, BN2 or a combination thereof, M is at least one metal selected from Group II to Group XV of the periodic table, and X2 is I, Br, Cl, F or a combination thereof. The conductive material can be, for example, a carbon-based material.
[0088] In the Li2S-containing composite, for example, 1≤a≤4, 1≤b≤4, 1≤c≤4, 1≤d≤4, 1≤a≤3, 1≤b≤3, 1≤c≤3, 1≤d≤3, or 1≤a≤2, 1≤b≤2, 1≤c≤2, 1≤d≤2.
[0089] The Li2S-containing composite may include a metal halide, and the metal halide may include at least one metal selected from Al, Mg, Ti, Sn, As, Sb, Nb, Sc, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, and Se. The metal halide may include such a metal, thereby further improving the cycle characteristics of the all-solid-state secondary battery including the Li2S-containing composite.
[0090] The Li2S-containing composite may include a metal halide, for example, the metal halide may include AlF3, AlCl3, AlBr3, AlI3, MgF2, MgCl2, MgBr2, MgI2, TiF4, TiCl4, TiBr4, TiI4, SnF4, SnCl4, SnBr4, SnI4, AsF4, AsCl4, AsBr4, AsI4, SbF4, SbCl4, SbBr4, SbI4, or a combination thereof. The Li2S-containing composite may include such a metal halide, thereby further improving the cycle characteristics of the all-solid-state secondary battery including the Li2S-containing composite.
[0091] The Li2S-containing composite may include, for example, a solid solution of Li2S and a lithium salt; a solid solution of Li2S and a metal halide; a solid solution of Li2S, a lithium salt and a metal halide, or a combination thereof. a X1 b ) and / or Li2S, lithium salt (Li a X1 b The composite of Li2S and a conductive material (C) may include a solid solution of Li2S and a lithium salt. For example, Li2S and a metal halide (M c X2 d ) and / or Li2S, metal halide (M c X2 d ) and the conductive material (C) may include a solid solution of Li2S and a metal halide. For example, Li2S, a lithium salt (Li a X1 b ) and metal halides (M a X2 b ) and / or Li2S, lithium salt (Li a X1 b ), metal halide (M a X2 b ) and a conductive material (C) may include a solid solution of Li2S, a lithium salt and a metal halide.
[0092] The composite containing Li2S may include a solid solution of Li2S and a lithium salt, a solid solution of Li2S and a metal halide, a solid solution of Li2S, a lithium salt and a metal halide, or a combination thereof, so that the ionic conductivity of the composite containing Li2S can be increased. For example, a solid solution of Li2S and a lithium salt, a solid solution of Li2S and a metal halide, a solid solution of Li2S, a lithium salt and a metal halide, or a combination thereof may include lithium ions, metal ions and / or halide ions disposed in Li2S crystallites, so that the ionic conductivity of the solid solution of Li2S, a lithium salt and a metal halide can be improved compared to Li2S. In some embodiments, the ionic conductivity of the composite containing Li2S can be improved, and the internal resistance of the composite containing Li2S can be reduced. The lithium-containing sulfide-based positive active material may include such a composite containing Li2S, thereby further improving the cycle characteristics of the all-solid-state secondary battery including the lithium-containing sulfide-based positive active material. For example, the high rate characteristics of an all-solid-state secondary battery including such a lithium-containing sulfide-based positive electrode active material can be further improved.
[0093] Li2S, a composite of a lithium salt and a conductive material, a composite of Li2S, a metal halide and a conductive material, and a composite of Li2S, a lithium salt, a metal halide and a conductive material may include a conductive material. The conductive material may include, for example, a carbon-based material, a metal-based material, or a combination thereof.
[0094] The carbon-based material may include, for example, a fiber carbon-based material. The metal-based material may include, for example, a fiber metal-based material.
[0095] The composite of Li2S, metal halide and conductive material may include fibrous carbon material and / or fibrous metal material, thereby further improving the electronic conductivity of the composite of Li2S, metal halide and conductive material. The composite of Li2S, metal halide and conductive material may include fibrous carbon material and / or fibrous metal material, so that it is easier to conduct electrons from the surface to the inside of the composite of Li2S, metal halide and conductive material. The internal resistance of the positive active material layer including the composite of Li2S, metal halide and conductive material can be reduced, and the cycle characteristics of the all-solid-state secondary battery including the positive active material layer can be further improved.
[0096] The aspect ratio of the fibrous carbon-based material and / or the fibrous metal-based material may be, for example, 2 or more, 3 or more, 4 or more, 5 or more, 10 or more, or 20 or more. The aspect ratio of the fibrous carbon-based material and / or the fibrous metal-based material may be, for example, in the range of about 2 to about 30, about 3 to about 30, about 4 to about 30, about 5 to about 30, about 10 to about 30, or about 20 to about 30. The aspect ratio of the fibrous carbon-based material and / or the fibrous metal-based material may be, for example, in the range of about 2 to about 30, about 2 to about 20, about 2 to about 10, about 2 to about 8, about 2 to about 5, or about 2 to about 4. The fibrous carbon-based material and / or the fibrous metal-based material may have an aspect ratio within such a range, so that the overall electronic conductivity of the composite of Li2S, lithium salt and conductive material can be improved, and the imbalance of the local electronic conductivity in the composite of Li2S, lithium salt and conductive material can be further alleviated.
[0097] The fiber carbon material may include, for example, a carbon nanostructure. The carbon nanostructure may include, for example, CNF, CNT, carbon nanobelt, carbon nanorod, or a combination thereof. The fiber metal material may include, for example, a metal nanostructure. The metal nanostructure may include, for example, a metal nanofiber (MNF), a metal nanotube (MNT), a metal nanobelt, a metal nanorod, or a combination thereof.
[0098] The carbon nanostructure may include, for example, a primary carbon nanostructure composed of a single carbon nanostructure, a secondary carbon nanostructure in which a plurality of primary carbon nanostructures are aggregated, or a combination thereof.
[0099] The diameter of primary carbon nanostructure can be, for example, about 1nm to about 200nm, about 1nm to about 150nm, about 1nm to about 100nm, about 1nm to about 50nm, about 1nm to about 30nm, or about 1nm to about 20nm. The length of primary carbon nanostructure can be, for example, 10nm to about 2 μm, about 10nm to about 1.5 μm, about 10nm to about 1 μm, about 10nm to about 500nm, about 10nm to about 400nm, about 10nm to about 300nm, about 10nm to about 200nm, or about 10nm to about 100nm. The diameter and length of primary carbon nanostructure can be measured by SEM or TEM images. In other embodiments, the diameter and / or length of primary carbon nanostructure can be measured by laser diffraction.
[0100] Secondary carbon nanostructure can be, for example, a structure formed by clustering the primary carbon nanostructure as a whole or in part to form a bundle or rope-type nanostructure. Secondary carbon nanostructure can include, for example, bundle-type carbon nanostructure, rope-type carbon nanostructure or a combination thereof. The diameter of the secondary carbon nanostructure can be, for example, in the range of about 2nm to about 200nm, about 3nm to about 150nm, about 5nm to about 100nm, about 5nm to about 50nm, about 5nm to about 30nm or about 5nm to about 20nm. The length of the secondary carbon nanostructure can be, for example, in the range of about 20nm to about 2 μm, about 30nm to about 1.5 μm, about 50nm to about 1 μm, about 50nm to about 500nm, about 50nm to about 400nm, about 50nm to about 300nm, about 50nm to about 200nm or about 50nm to 100nm. The diameter and length of the secondary carbon nanostructure can be measured by SEM images or optical microscopes. In other embodiments, the diameter and / or length of the secondary carbon nanostructure can be measured by laser diffraction. The secondary carbon nanostructure may be dispersed in, for example, a solvent or the like to be converted into a primary carbon nanostructure, and then may be used to prepare a composite of Li2S, a metal halide, and a conductive material.
[0101] The particle size of the sulfide positive active material (e.g., the particle size of the composite containing Li2S) can be, for example, 10 μm or less, 8 μm or less, 5 μm or less, 4 μm or less, 2 μm or less, 1.5 μm or less, or 1 μm or less. The particle size of the composite containing Li2S can be, for example, in the range of about 1 μm to about 10 μm, about 2 μm to about 10 μm, about 2 μm to about 8 μm, or about 3 μm to about 8 μm. The particle size of the composite containing Li2S can be, for example, in the range of about 0.1 μm to about 10 μm, about 0.1 μm to about 8 μm, about 0.1 μm to about 5 μm, about 0.1 μm to about 4 μm, about 0.1 μm to about 2 μm, about 0.1 μm to about 1.5 μm, or about 0.1 μm to about 1 μm. The particle size of the particles of the Li2S-containing composite can be within such a range that the volume change of the sulfide-based positive electrode active material during charge / discharge can be suppressed, and the degradation of the sulfide-based positive electrode active material during charge / discharge can be more effectively suppressed. If the particle size of the Li2S-containing composite is excessively increased, the volume change of the Li2S-containing composite during charge and discharge will increase, which will accelerate the degradation of the sulfide-based positive electrode active material. In some embodiments, the cycle characteristics of an all-solid-state secondary battery including such a sulfide-based positive electrode active material will deteriorate. The particle size of the Li2S-containing composite can be measured, for example, using laser diffraction, scanning electron microscopy, and the like. The particle size of the Li2S-containing composite can be, for example, the arithmetic mean of the particle sizes of multiple particles measured by SEM images using software.
[0102] The particle size of the Li2S particles included in the Li2S-containing composite may be, for example, 2 μm or less, 1.5 μm or less, or 1 μm or less. The particle size of the Li2S particles may be, for example, in the range of about 0.1 μm to about 2 μm, about 0.1 μm to about 1.5 μm, or about 0.1 μm to about 1 μm. The particle size of the Li2S particles may be within such a range, so that the volume change of the Li2S-containing composite during charge / discharge may be suppressed, thereby suppressing the degradation of the sulfide-based positive active material including the Li2S-containing composite during charge / discharge. If the particle size of the Li2S particles is excessively increased, the volume change of the Li2S-containing composite during charge and discharge may increase, which may accelerate the degradation of the sulfide-based positive active material including the Li2S-containing composite. In some embodiments, the cycle characteristics of the secondary battery including such a sulfide-based positive active material may deteriorate.
[0103] The ionic conductivity of the Li2S-containing composite at a temperature of about 25°C and a pressure of about 1 atm may be, for example, 1×10 -5 S / cm or more, 2×10 -5 S / cm or more, 4×10 -5 S / cm or more, 6×10 -5 S / cm or more, 8×10 -5 S / cm or more, or 1×10 -4 S / cm or more. The ionic conductivity can be measured by using, for example, electrochemical impedance spectroscopy, direct current (DC) polarization method, etc. The Li2S-containing composite can have an ionic conductivity within such a range, so the internal resistance of the positive electrode active material layer including the Li2S-containing composite can be further reduced. The cycle characteristics of the all-solid-state secondary battery including the positive electrode active material layer can be improved.
[0104] The electronic conductivity of the Li2S-containing composite at a temperature of about 25°C and a pressure of about 1 atm may be, for example, 1×10 -5 S / cm or more, 2×10 -5 S / cm or more, 4×10 -5 S / cm or more, 6×10 -5 S / cm or more, 8×10 -5 S / cm or more, or 1×10 -4S / cm or more. The electronic conductivity can be measured by using, for example, electrochemical impedance spectroscopy, DC polarization, etc. The Li2S-containing composite can have an electronic conductivity within such a range, so the internal resistance of the positive electrode active material layer including the Li2S-containing composite can be further reduced. The cycle characteristics of the all-solid-state secondary battery including the positive electrode active material layer can be improved. For example, relative to 100 parts by weight of a composite of Li2S, a lithium salt, a metal halide and a conductive material, Li2S can be included in an amount of about 40 parts by weight to about 80 parts by weight, a combination of a lithium salt and a metal halide can be included in an amount of about 1 part by weight to about 40 parts by weight, and a conductive material can be included in an amount of about 1 part by weight to about 20 parts by weight. The conductive material can be, for example, a carbon-based material. In the combination of a lithium salt and a metal halide, the molar ratio of the lithium salt to the metal halide can be, for example, in the range of about 3:1 to about 1:3, about 2:1 to about 1:2, or about 1.5:1 to about 1:1.5.
[0105] The content of Li2S included in the composite of Li2S, lithium salt, metal halide and conductive material may be, for example, in the range of about 10 parts by weight to about 80 parts by weight, about 20 parts by weight to about 70 parts by weight, about 30 parts by weight to about 60 parts by weight, or about 40 parts by weight to about 60 parts by weight, relative to 100 parts by weight of the composite of Li2S, lithium salt, metal halide and conductive material. The conductive material may be, for example, a carbon-based material.
[0106] The content of lithium salt and metal halide included in the composite of Li2S, lithium salt, metal halide and conductive material (e.g., the content of the combination of lithium salt and metal halide) may be in the range of about 10 parts by weight to about 40 parts by weight, about 15 parts by weight to about 40 parts by weight, about 20 parts by weight to about 40 parts by weight, or about 25 parts by weight to about 35 parts by weight relative to 100 parts by weight of the composite of Li2S, lithium salt, metal halide and conductive material. The conductive material may be, for example, a carbon-based material. The molar ratio of lithium salt to metal halide may be in the range of about 3:1 to about 1:3.
[0107] The content of the conductive material included in the composite of Li2S, lithium salt, metal halide and conductive material may be, for example, in the range of about 1 to about 20 parts by weight, about 5 to about 20 parts by weight, or about 5 to about 15 parts by weight relative to 100 parts by weight of the composite of Li2S, lithium salt, metal halide and conductive material. The conductive material may be, for example, a carbon-based material.
[0108] The composite of Li2S, lithium salt, metal halide and conductive material can have a composition of Li2S, lithium salt, metal halide and conductive material within such a range, and thus the sulfide-based positive active material including the composite of Li2S, lithium salt, metal halide and conductive material can provide better ionic conductivity and / or electronic conductivity.
[0109] Relative to the total weight of the positive electrode active material layer 12, the content of Li2S included in the positive electrode active material layer 12 may be, for example, in the range of about 30 wt% to about 90 wt%, about 35 wt% to about 90 wt%, about 40 wt% to about 90 wt%, about 45 wt% to about 80 wt%, or about 50 wt% to about 70 wt%.
[0110] The content of the sulfide-based positive active material included in the positive active material layer 12 may be, for example, in the range of about 10 wt % to about 90 wt %, about 10 wt % to about 80 wt %, about 10 wt % to about 70 wt %, about 10 wt % to about 60 wt %, or about 10 wt % to about 50 wt %, relative to the total weight of the positive active material layer 12. In other embodiments, the content of the sulfide-based positive active material included in the positive active material layer 12 may be, for example, in the range of about 10 wt % to about 90 wt %, about 20 wt % to about 90 wt %, about 30 wt % to about 90 wt %, about 40 wt % to about 90 wt %, or about 50 wt % to about 90 wt %, relative to the total weight of the positive active material layer 12.
[0111] The positive electrode active material layer 12 may further include, for example, a sulfide compound different from Li2S. The sulfide compound may be, for example, a compound including a metal element other than Li and a sulfur element. The sulfide compound may be, for example, a compound including a sulfur element and at least one of a metal element selected from Groups I to XIV of the periodic table having an atomic weight of 10 or more. The sulfide compound may be, for example, FeS2, VS2, NaS, MnS, FeS, NiS, CuS, or a combination thereof. The positive electrode active material layer 12 may further include a sulfide compound, so that the cycle characteristics of the all-solid-state secondary battery may be further improved. The content of the sulfide compound included in the positive electrode active material layer 12 and different from Li2S may be 10wt% or less, 5wt% or less, 3wt% or less, or 1wt% or less of the total weight of the positive electrode active material layer 12.
[0112] [Cathode layer: solid electrolyte]
[0113] The positive electrode active material layer 12 may also include, for example, a solid electrolyte. The solid electrolyte may be, for example, a sulfide-based solid electrolyte. The solid electrolyte included in the positive electrode layer 10 may be similar to or different from the solid electrolyte included in the solid electrolyte layer 30. The solid electrolyte may be defined as in the part of the solid electrolyte layer 30.
[0114] The solid electrolyte included in the positive electrode active material layer 12 may have an average particle size (D50) smaller than the average particle size (D50) of the solid electrolyte included in the solid electrolyte layer 30. For example, the average particle size (D50) of the solid electrolyte included in the positive electrode active material layer 12 may be 90% or less, 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, or 20% or less of the average particle size (D50) of the solid electrolyte included in the solid electrolyte layer 30. The average particle size (D50) may be, for example, a median particle size (D50). The median particle size (D50) may be, for example, a particle size corresponding to 50% cumulative volume when the particle size distribution measured by the laser diffraction method is calculated starting from particles having a smaller particle size.
[0115] The content of the solid electrolyte included in the positive active material layer 12 may be in the range of, for example, about 1 wt % to about 40 wt %, about 1 wt % to about 30 wt %, about 1 wt % to about 20 wt %, or about 1 wt % to about 10 wt % of the total weight of the positive active material layer 12 .
[0116] [Positive electrode layer: conductive material]
[0117] The positive electrode active material layer 12 may also include, for example, a conductive material. The conductive material may be, for example, a carbon-based conductive material, a metal-based conductive material, or a combination thereof. The carbon-based conductive material may be, for example, graphite, CB, AB, KB, carbon fiber, or a combination thereof, but is not limited thereto. Any material used as a carbon-based conductive material in the art may be used. The metal-based conductive material may be a metal powder, a metal fiber, or a combination thereof, but is not limited thereto. Any material used as a metal-based conductive material in the art may be used. The content of the conductive material included in the positive electrode active material layer 12 may be in the range of, for example, about 1wt% to about 30wt%, about 1wt% to about 20wt%, or about 1wt% to about 10wt% of the total weight of the positive electrode active material layer 12.
[0118] [Positive electrode layer: binder]
[0119] The positive electrode active material layer 12 may further include, for example, a binder. The binder may be, for example, styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene (PE), etc., but is not limited thereto. Any material used as a binder in the art may be used. The content of the binder included in the positive electrode active material layer 12 may be, for example, about 1wt% to about 10wt% of the total weight of the positive electrode active material layer 12. The binder may be omitted.
[0120] [Cathode layer: other additives]
[0121] The positive electrode active material layer 12 may further include, for example, additives such as a filler, a coating agent, a dispersant, and an ion conduction aid in addition to the above-described positive electrode active material, solid electrolyte, binder, and conductive material.
[0122] As a filler, a coating agent, a dispersant, an ion conductive aid, and the like that may be included in the positive electrode active material layer 12 , known materials generally used in electrodes of all-solid-state secondary batteries may be used.
[0123] [Positive electrode layer: positive electrode current collector]
[0124] The positive electrode collector 11 may be formed in the form of a plate, foil, etc. composed of, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode collector 11 may be omitted. The thickness of the positive electrode collector 11 may be, for example, in the range of about 1 μm to about 100 μm, about 1 μm to about 50 μm, about 5 μm to about 25 μm, or about 10 μm to about 20 μm.
[0125] The positive electrode current collector 11 may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), PE, polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. The base film may be, for example, an insulator. Since the base film may include an insulating thermoplastic polymer, if a short circuit occurs, the base film may soften or liquefy to block the operation of the battery, thereby suppressing the rapid increase in current. The metal layer may include indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), or an alloy thereof. The metal layer may be used as an electrochemical fuse and may be cut off if an overcurrent occurs, thereby performing a short circuit prevention function. The thickness of the metal layer may be adjusted to adjust the limiting current and the maximum current. The metal layer may be electroplated or deposited on the base film. If the thickness of the metal layer is reduced, the limiting current and / or maximum current of the positive current collector 11 can be reduced, so the stability of the lithium battery during short circuit can be improved. A lead tab can be added to the metal layer for external connection. The lead tab can be welded to the metal layer or the metal layer / substrate film stack by ultrasonic welding, laser welding, spot welding, etc. When the substrate film and / or the metal layer melts during welding, the metal layer can be electrically connected to the lead tab. In order to weld the metal layer and the lead tab more firmly, a metal sheet (chip) can be added between the metal layer and the lead tab. The metal sheet can be a flake composed of the same material as the metal of the metal layer. The metal sheet can be, for example, a metal foil or a metal mesh. The metal sheet can be, for example, an aluminum foil, a copper foil, or a SUS foil. The metal sheet can be disposed on the metal layer and then welded to the lead tab, so that the lead tab can be welded to the metal sheet / metal layer stack or the metal sheet / metal layer / substrate film stack. During welding, when the base film, the metal layer and / or the metal sheet melt, the metal layer or the metal layer / metal sheet stack can be electrically connected to the lead tab. The metal sheet and / or the lead tab can be added to a portion of the metal layer. The thickness of the base film can be, for example, in the range of about 1 μm to about 50 μm, about 1.5 μm to about 50 μm, about 1.5 μm to about 40 μm, or about 1 μm to about 30 μm. Since the base film has a thickness in this range, the weight of the electrode assembly can be more effectively reduced. The melting point of the base film can be, for example, in the range of about 100°C to about 300°C, about 100°C to about 250°C, or about 100°C to about 200°C. Since the base film can have a melting point in this range, the base film can be melted in the process of welding the lead tab and easily bonded to the lead tab.In order to improve the adhesion strength between the base film and the metal layer, the base film may be subjected to a surface treatment (such as a corona treatment). The thickness of the metal layer may be, for example, in the range of about 0.01 μm to about 3 μm, about 0.1 μm to about 3 μm, about 0.1 μm to about 2 μm, or about 0.1 μm to about 1 μm. Since the metal layer may have a thickness within this range, the stability of the electrode assembly may be ensured while maintaining conductivity. The thickness of the metal sheet may be, for example, in the range of about 2 μm to about 10 μm, about 2 μm to about 7 μm, or about 4 μm to about 6 μm. Since the metal sheet may have a thickness within this range, the metal layer may be more easily connected to the lead tab. Since the positive electrode current collector 11 may have such a structure, the weight of the positive electrode may be reduced, thereby improving the energy density of the positive electrode and the lithium battery.
[0126] [Positive Electrode Layer: First Inactive Member]
[0127] Reference Figure 1 , the positive electrode layer 10 may include a positive electrode collector 11 and a positive electrode active material layer 12 disposed on one side of the positive electrode collector 11. The first inactive member 40 may be disposed on the side of the positive electrode layer 10. The first inactive member 40 may be disposed on the side of the positive electrode active material layer 12 and the side of the positive electrode collector 11. Figure 2 The first inactive member 40 may be disposed on the side of the positive active material layer 12 and may be disposed between the solid electrolyte layer 30 and the positive current collector 11 opposite to the solid electrolyte layer 30. The first inactive member 40 may not be disposed on the side of the positive current collector 11.
[0128] Since the first inactive member 40 can be provided, cracks in the solid electrolyte layer 30 can be prevented during manufacture and / or charge / discharge of the all-solid-state secondary battery 1, thereby improving the cycle characteristics of the all-solid-state secondary battery 1. In the all-solid-state secondary battery 1 that does not include the first inactive member 40, during manufacture and / or charge / discharge of the all-solid-state secondary battery 1, non-uniform pressure may be applied to the solid electrolyte layer 30 in contact with the positive electrode layer 10, which causes cracks in the solid electrolyte layer 30 and increases the possibility of a short circuit due to growth of lithium metal through the cracks.
[0129] In the all-solid-state secondary battery 1, the thickness T2 of the first inactive member 40 may be greater than or equal to the thickness T1 of the positive electrode active material layer 12. In the all-solid-state secondary battery 1, the thickness T2 of the first inactive member 40 may be substantially equal to the thickness T3 of the positive electrode layer 10. Since the thickness T2 of the first inactive member 40 may be equal to the thickness T3 of the positive electrode layer 10, uniform pressure may be applied to the positive electrode layer 10 and the solid electrolyte layer 30, and the positive electrode layer 10 may be in sufficiently close contact with the solid electrolyte layer 30, so that the interface resistance between the positive electrode layer 10 and the solid electrolyte layer 30 may be reduced. In other embodiments, the solid electrolyte layer 30 may be sufficiently sintered during the press manufacturing process of the all-solid-state secondary battery 1, thereby reducing the internal resistance of the solid electrolyte layer 30 and the all-solid-state secondary battery 1 including the solid electrolyte layer 30.
[0130] The first inactive member 40 may surround the side of the positive electrode layer 10 and may be in contact with the solid electrolyte layer 30. Since the first inactive member 40 may surround the side of the positive electrode layer 10 and may be in contact with the solid electrolyte layer 30, cracks of the solid electrolyte layer 30 caused in the solid electrolyte layer 30 not in contact with the positive electrode layer 10 due to the pressure difference during the pressing process may be effectively suppressed. The first inactive member 40 may surround the side of the positive electrode layer 10 and may be separated from the negative electrode layer 20 (more specifically, the first negative electrode active material layer 22). The first inactive member 40 may surround the side of the positive electrode layer 10, may be in contact with the solid electrolyte layer 30, and may be separated from the negative electrode layer 20. In some embodiments, the possibility of a short circuit due to physical contact between the positive electrode layer 10 and the first negative electrode active material layer 22 may be suppressed, or the possibility of a short circuit due to overcharge of lithium may be suppressed. For example, the first inactive member 40 may be disposed on the side of the positive active material layer 12 and also on the side of the positive current collector 11 at the same time, thereby more effectively suppressing the possibility of a short circuit due to contact between the positive current collector 11 and the negative electrode layer 20 .
[0131] Reference Figures 1 to 5 , the first inactive member 40 (40a or 40b) may extend from one side of the positive electrode layer 10 to the end of the solid electrolyte layer 30. Since the first inactive member 40 may extend to the end of the solid electrolyte layer 30, it is possible to suppress the occurrence of cracks in the end of the solid electrolyte layer 30. The end of the solid electrolyte layer 30 may be the outermost portion in contact with one side of the solid electrolyte layer 30.
[0132] The first inactive member 40 may extend to an outermost portion in contact with one side of the solid electrolyte layer 30 .
[0133] The first inactive member 40 may be separated from the negative electrode layer 20 (e.g., the first negative electrode active material layer 22). The first inactive member 40 extends to the end of the solid electrolyte layer 30 but does not contact the negative electrode layer 20. The first inactive member 40 may fill, for example, a space extending from one side of the positive electrode layer 10 to the end of the solid electrolyte layer 30.
[0134] Reference Figure 1 and Figure 2 , the width W2 of the first inactive member 40 extending from one side of the positive electrode layer 10 to the end of the solid electrolyte layer 30 may be in the range of, for example, about 1% to about 30%, about 1% to about 25%, about 1% to about 20%, about 1% to about 15%, about 1% to about 10%, or about 1% to about 5% of the width W1 between one side of the positive electrode layer 10 and the other side opposite to the one side. Figure 1 and Figure 2 , the width of the first inactive member 40 extending from one side of the positive electrode layer 10 to the end of the solid electrolyte layer 30 may be, for example, in the range of about 1% to about 30%, about 3% to about 30%, about 5% to about 30%, about 5% to about 20%, about 5% to about 15%, or about 5% to about 10% of the width between one side of the positive electrode layer 10 and the other side opposite to the one side. If the width W2 of the first inactive member 40 is too wide, the energy density of the all-solid-state secondary battery 1 may be reduced. If the width W2 of the first inactive member 40 is too narrow, the effect of arranging the first inactive member 40 may be insignificant.
[0135] The area S1 of the positive electrode layer 10 (such as the area S1 of the positive electrode active material layer 12 (for example, the cross-sectional area S1 of the positive electrode layer 10 or the cross-sectional area S1 of the positive electrode active material layer 12 relative to the stacking direction or thickness direction of the all-solid-state secondary battery 1)) can be smaller than the area S3 of the solid electrolyte layer 30 in contact with the positive electrode layer 10 (or the positive electrode active material layer 12) (for example, the cross-sectional area S3 of the solid electrolyte layer 30 relative to the stacking direction or thickness direction of the all-solid-state secondary battery 1). The first inactive member 40 having flame retardancy can be provided to surround the side of the positive electrode layer 10 to compensate for the area difference between the positive electrode layer 10 (or the positive electrode active material layer 12) and the solid electrolyte layer 30. Since the area S2 of the first inactive member 40 having flame retardancy (e.g., the cross-sectional area S2 of the first inactive member 40 with respect to the stacking direction or the thickness direction of the all-solid-state secondary battery 1) can compensate for the difference between the area S1 of the positive electrode layer 10 (or the positive electrode active material layer 12) and the area S3 of the solid electrolyte layer 30, cracks in the solid electrolyte layer 30 caused by the pressure difference during the pressing process can be effectively suppressed. For example, the sum of the area S1 of the positive electrode layer 10 (or the positive electrode active material layer 12) and the area S2 of the first inactive member 40 is equal to the area S3 of the solid electrolyte layer 30.
[0136] The area S1 of the positive electrode layer 10 (or the positive electrode active material layer 12) may be, for example, less than 100%, 99% or less, 98% or less, 97% or less, 96% or less, or 95% or less of the area S3 of the solid electrolyte layer 30. The area S1 of the positive electrode layer 10 (or the positive electrode active material layer 12) may be in the range of, for example, about 50% to less than about 100%, about 50% to about 99%, about 55% to about 98%, about 60% to about 97%, about 70% to about 96%, about 80% to about 95%, or about 85% to about 95% of the area S3 of the solid electrolyte layer 30.
[0137] If the area S1 of the positive electrode layer (or positive electrode active material layer 12) 10 is greater than or equal to the area S3 of the solid electrolyte layer 30, the possibility of a short circuit due to physical contact between the positive electrode layer 10 (or positive electrode active material layer 12) and the first negative electrode active material layer 22 will increase, or the possibility of a short circuit due to overcharge of lithium will increase. The area S1 of the positive electrode layer 10 may be equal to, for example, the area of the positive electrode active material layer 12. The area S1 of the positive electrode layer 10 may be equal to, for example, the area of the positive electrode current collector 11.
[0138] The area S2 of the first inactive member 40 may be, for example, 50% or less, 40% or less, 30% or less, 20% or less, or 10% or less of the area S1 of the positive electrode layer 10 (or the positive electrode active material layer 12). The area S2 of the first inactive member 40 may be, for example, in the range of about 1% to about 50%, about 5% to about 40%, about 5% to about 30%, about 5% to about 20%, or about 5% to about 15% of the area S1 of the positive electrode layer 10 (or the positive electrode active material layer 12).
[0139] The area S1 of the positive electrode layer 10 (or the positive electrode active material layer 12) may be smaller than the area S4 of the negative electrode collector 21 (e.g., the cross-sectional area S4 of the negative electrode collector 21 relative to the stacking direction or thickness direction of the all-solid-state secondary battery 1). The area S1 of the positive electrode layer 10 (or the positive electrode active material layer 12) may be, for example, less than about 100%, 99% or less, 98% or less, 97% or less, 96% or less, or about 95% or less of the area S4 of the negative electrode collector 21. The area S1 of the positive electrode layer 10 (or the positive electrode active material layer 12) may be, for example, about 50% to less than about 100%, about 50% to about 99%, about 55% to about 98%, about 60% to about 97%, about 70% to about 96%, about 80% to about 95%, or about 85% to about 95% of the area S4 of the negative electrode collector 21. The area S4 of the negative electrode current collector 21 may be equal to, for example, the area of the negative electrode layer 20 (e.g., the cross-sectional area of the negative electrode layer 20 relative to the stacking direction or thickness direction of the all-solid-state secondary battery 1). The area S4 of the negative electrode current collector 21 may be equal to, for example, the area of the first negative electrode active material layer 22 (e.g., the cross-sectional area of the first negative electrode active material layer 22 relative to the stacking direction or thickness direction of the all-solid-state secondary battery 1).
[0140] As used herein, "equal" area, length, width, thickness, and / or shape encompasses all cases of having "substantially equal" area, length, width, thickness, and / or shape, except where the area, length, width, thickness, and / or shape are intentionally expressed as being different. "Equal" area, length, width, and / or thickness encompasses ranges where the unintentional difference in area, length, width, and / or thickness between the comparison objects is less than 3%, less than 1%, less than 0.5%, or less than 0.1%.
[0141] The thickness of the first inactive member 40 may be greater than, for example, the thickness of the first negative active material layer 22. The thickness of the first negative active material layer 22 may be, for example, 50% or less, 40% or less, 30% or less, 20% or less, or 10% or less of the thickness of the first inactive member 40. The thickness of the first negative active material layer 22 is in the range of, for example, about 1% to about 50%, about 1% to about 40%, about 1% to about 30%, about 1% to about 20%, or about 1% to about 10% of the thickness of the first inactive member 40.
[0142] The negative electrode layer 20 may include a negative electrode collector 21 and a first negative electrode active material layer 22 disposed on one side of the negative electrode collector 21. For example, the other side of the negative electrode collector 21 opposite to the one side may not have the first negative electrode active material layer 22. For example, the first negative electrode active material layer 22 may be disposed only on one side of the negative electrode collector 21, and the first negative electrode active material layer 22 may not be disposed on the other side.
[0143] The first inactive member 40 may be a gasket. A gasket may be used as the first inactive member 40 to effectively suppress cracks of the solid electrolyte layer 30 due to a pressure difference during a pressing process.
[0144] The first inactive member 40 may have, for example, a single-layer structure. In other embodiments, although not shown in the drawings, the first inactive member 40 may have a multilayer structure. In the first inactive member 40 having a multilayer structure, the corresponding layers may have different compositions. The first inactive member 40 having a multilayer structure may have, for example, a two-layer structure, a three-layer structure, a four-layer structure, or a five-layer structure. The first inactive member 40 having a multilayer structure may include, for example, one or more adhesive layers and one or more supporting layers. For example, the adhesive layer may effectively prevent the positive electrode layer 10 from being separated from the solid electrolyte layer 30 due to the volume change of the positive electrode layer 10 caused during the charging / discharging process of the all-solid-state secondary battery 1. In other embodiments, the adhesive layer may provide an adhesive force between the supporting layer and other layers to improve the film strength of the first inactive member 40. The supporting layer may provide a supporting force to the first inactive member 40, may prevent the non-uniformity of the pressure applied to the solid electrolyte layer 30 during the pressing process or the charging / discharging process, and may prevent the shape deformation of the all-solid-state secondary battery 1 to be manufactured.
[0145] Reference Figure 3, the all-solid-state secondary battery 1 may include a positive electrode layer 10, a negative electrode layer 20 (20a, 20b), and a solid electrolyte layer 30 (30a, 30b) disposed between the positive electrode layer 10 and the negative electrode layer 20. The positive electrode layer 10 may include a positive electrode current collector 11 and each of a first positive electrode active material layer 12a and a second positive electrode active material layer 12b disposed on both sides of the positive electrode current collector 11. The solid electrolyte layer 30 may include a first solid electrolyte layer 30a in contact with the first positive electrode active material layer 12a, respectively, and a second solid electrolyte layer 30b in contact with the second positive electrode active material layer 12b. The negative electrode layer 20 may include a first negative electrode layer 20a in contact with the first solid electrolyte layer 30a, respectively, and a second negative electrode layer 20b in contact with the second solid electrolyte layer 30b. The first inactive member 40 may be disposed between the first solid electrolyte layer 30a and the second solid electrolyte layer 30b opposite to each other to surround the side of the positive electrode layer 10. The first inactive member 40 includes, for example, the 1a inactive member 40a in contact with the first solid electrolyte layer 30a and the 1b inactive member 40b in contact with the second solid electrolyte layer 30b. In some embodiments, the all-solid-state secondary battery 1 may have a dual-battery monomer structure. Since the all-solid-state secondary battery 1 may have such a dual-battery monomer structure, the solid electrolyte layer 30 and the negative electrode layer 20 may be symmetrically arranged relative to each other with respect to the positive electrode layer 10, thereby more effectively suppressing structural deformation caused by the pressure applied during the manufacture of the all-solid-state secondary battery 1, etc. In some embodiments, cracks in the solid electrolyte layer 30 may be suppressed during the manufacturing process and / or charging / discharging process of the all-solid-state secondary battery 1 to prevent short circuits of the all-solid-state secondary battery 1, thereby further improving the cycle characteristics of the all-solid-state secondary battery 1. In other embodiments, since only one positive electrode current collector 11 may be used for multiple positive electrode active material layers 12a, 12b, the energy density of the all-solid-state secondary battery 1 may be increased.
[0146] Reference Figures 1 to 5 , the first inactive member 40 may be, for example, a flame retardant inactive member. The flame retardant inactive member may provide flame retardancy to prevent the possibility of thermal runaway and fire of the all-solid-state secondary battery 1. In some embodiments, the safety of the all-solid-state secondary battery 1 may be further improved. Since the flame retardant inactive member may absorb residual moisture in the all-solid-state secondary battery 1, the degradation of the all-solid-state secondary battery 1 may be prevented to improve the life characteristics of the all-solid-state secondary battery 1.
[0147] The flame retardant inactive member may include, for example, a matrix and a filler. The matrix may include, for example, a substrate and a reinforcing material. The matrix may include, for example, a fiber substrate and a fiber reinforcing material. The matrix may include a substrate and may therefore have elasticity. In some embodiments, the matrix may effectively receive the volume change of the all-solid-state secondary battery 1 during charge / discharge, and may be disposed at any one of various positions. The substrate included in the matrix may include, for example, a first fiber material. The substrate may include a first fiber material, thereby effectively receiving the volume change of the positive electrode layer 10 caused during the charge / discharge process of the all-solid-state secondary battery 1, and effectively suppressing the deformation of the first inactive member 40 caused by the volume change of the positive electrode layer 10. The first fiber material may be, for example, a material having an aspect ratio of 5 or more, 20 or more, or 50 or more. The first fiber material may be, for example, a material having an aspect ratio of about 5 to about 1,000, about 20 to about 1,000, or about 50 to about 1,000. The first fiber material may be, for example, an insulating material. The first fiber material may be an insulating material, thereby effectively preventing a short circuit between the positive electrode layer 10 and the negative electrode layer 20 caused by lithium dendrites, etc., generated during the charge / discharge of the all-solid-state secondary battery 1. The first fiber material may include, for example, at least one selected from pulp fibers, insulating polymer fibers, and ion conductive polymer fibers. The matrix includes a reinforcing material, so the strength of the matrix can be improved. In some embodiments, the matrix can prevent excessive volume changes during the charge / discharge of the all-solid-state secondary battery 1, and can prevent deformation of the all-solid-state secondary battery 1. The reinforcing material included in the matrix may include, for example, a second fiber material. Since the reinforcing material may include the second fiber material, the strength of the matrix may be increased more uniformly. The second fiber material may be, for example, a material having an aspect ratio of 3 or more, 5 or more, or 10 or more. The second fiber material may be, for example, a material having an aspect ratio of about 3 to about 100, about 5 to about 100, or about 10 to about 100. The second fiber material may be, for example, a flame retardant material. The second fiber material may be a flame retardant material, thereby effectively suppressing ignition caused by thermal runaway caused by external impact or the charge / discharge process of the all-solid-state secondary battery 1. The second fiber material may be, for example, glass fiber, metal oxide fiber, ceramic fiber, or the like.
[0148] The flame retardant inactive member may include a filler in addition to the matrix. The filler may be disposed inside the matrix, on the surface of the matrix, or both inside and on the surface. The filler may be, for example, an inorganic material. The filler included in the flame retardant inactive member may be, for example, a hygroscopic agent. The filler may adsorb moisture at a temperature of, for example, less than 100°C to remove moisture remaining in the all-solid-state secondary battery 1, thereby preventing degradation of the all-solid-state secondary battery 1. If the temperature of the all-solid-state secondary battery 1 rises to greater than or equal to 150°C or higher due to thermal runaway caused by an external impact or a charge / discharge process of the all-solid-state secondary battery 1, the filler may release the adsorbed moisture to effectively suppress the ignition of the all-solid-state secondary battery 1. For example, the filler may be, for example, a flame retardant. The filler may be, for example, a metal hydroxide having hygroscopicity. The metal hydroxide included in the filler may be, for example, Mg(OH)2, Fe(OH)3, Sb(OH)3, Sn(OH)4, Ti(OH)3, Zr(OH)4, Al(OH)3, or a combination thereof. Relative to about 100 parts by weight of the first inactive component 40 having flame retardancy, the content of the filler included in the flame retardant inactive component can be in the range of, for example, about 10 parts by weight to about 80 parts by weight, about 20 parts by weight to about 80 parts by weight, about 30 parts by weight to about 80 parts by weight, about 40 parts by weight to about 80 parts by weight, about 50 parts by weight to about 80 parts by weight, about 60 parts by weight to about 80 parts by weight, or about 65 parts by weight to about 80 parts by weight.
[0149] The flame retardant inactive member may also include, for example, a binder. The binder may include, for example, a curable polymer or a non-curable polymer. The curable polymer is a polymer that is cured by heat and / or pressure. The curable polymer may be, for example, solid at room temperature. The first inactive member 40 having flame retardancy may include, for example, a thermosetting film and / or a cured product thereof. The thermosetting polymer may be, for example, TSA-66 manufactured by TORAY INDUSTRIES, INC.
[0150] In addition to the above-mentioned base material, reinforcing material, filler and binder, the flame retardant inactive component may additionally include other materials. The flame retardant inactive component may also include at least one selected from, for example, paper, insulating polymer, ion conductive polymer, insulating inorganic material, oxide solid electrolyte and sulfide solid electrolyte. The insulating polymer may be, for example, an olefin polymer (such as PP or PE.
[0151] The density of the base material or reinforcing material included in the flame retardant inactive member may be in the range of, for example, about 10% to about 300%, about 10% to about 150%, about 10% to about 140%, about 10% to about 130%, or about 10% to about 120% of the density of the positive active material included in the positive active material layer 12.
[0152] The first inactive member 40 may be a member that does not include an electrochemically active substance (e.g., an electrode active substance). The electrode active substance may be a material that absorbs / desorbs lithium. The first inactive member 40 may be a member composed of a material used in the art, and is a material other than the electrode active substance.
[0153] [Negative electrode layer]
[0154] [Negative electrode layer: negative electrode active material]
[0155] Reference Figures 1 to 5 , the negative electrode layer 20 may include a first negative electrode active material layer 22. The first negative electrode active material layer 22 may include, for example, a negative electrode active material and a binder.
[0156] The negative electrode active material included in the first negative electrode active material layer 22 may be, for example, a negative electrode material that may form an alloy or a compound with lithium.
[0157] The negative electrode active material included in the first negative electrode active material layer 22 may have, for example, a particle form. The negative electrode active material having a particle form may have, for example, an average particle size of 4 μm or less, 3 μm or less, 2 μm or less, 1 μm or less, 500 nm or less, 300 nm or less, or 100 nm or less. The negative electrode active material having a particle form may have, for example, an average particle size of about 10 nm to about 4 μm, about 10 nm to about 3 μm, about 10 nm to about 2 μm, about 10 nm to about 1 μm, about 10 nm to about 500 nm, about 10 nm to about 300 nm, or about 10 nm to about 100 nm. Since the negative electrode active material may have an average particle size within such a range, reversible absorption and / or desorption of lithium may be more easily performed during charge / discharge. The average particle size of the negative electrode active material may be, for example, a median diameter (D50) measured using a laser-type particle size distribution analyzer.
[0158] The negative electrode active material included in the first negative electrode active material layer 22 may include, for example, at least one selected from a carbon-based negative electrode active material and a metal or metalloid negative electrode active material.
[0159] The carbon-based negative active material may include, for example, amorphous carbon, crystalline carbon, porous carbon, or a combination thereof.
[0160] Specifically, the carbon-based negative electrode active material may be amorphous carbon. Amorphous carbon may be, for example, CB, AB, furnace black (FB), KB, graphene, etc., but is not necessarily limited thereto. Any material classified as amorphous carbon in the art may be used. Amorphous carbon may be carbon that has no crystallinity or has very low crystallinity, and is distinguished from crystalline carbon or graphite-based carbon.
[0161] The carbon-based negative electrode active material may be, for example, porous carbon. The pore volume of the porous carbon may be, for example, in the range of about 0.1 cc / g to about 10.0 cc / g, about 0.5 cc / g to about 5 cc / g, or about 0.1 cc / g to about 1 cc / g. The average pore size of the porous carbon may be, for example, in the range of about 1 nm to about 50 nm, about 1 nm to about 30 nm, or about 1 nm to about 10 nm. The BET specific surface area of the porous carbon may be, for example, about 100 m 2 / g to about 3,000m 2 The BET specific surface area of porous carbon can be measured, for example, according to ISO 9277:2022.
[0162] The metal or metalloid negative electrode active material may include at least one selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn) and zinc (Zn), but one or more embodiments are not necessarily limited thereto. Any material used as a metal negative electrode active material or a metalloid negative electrode active material that forms an alloy or compound with lithium can be used in the art. For example, since nickel (Ni) may not form an alloy with lithium, nickel (Ni) may not be a metal negative electrode active material.
[0163] Among such negative electrode active materials, the first negative electrode active material layer 22 may include one negative electrode active material or a mixture of multiple different negative electrode active materials. For example, the first negative electrode active material layer 22 may include only amorphous carbon or at least one selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn) and zinc (Zn). In other embodiments, the first negative electrode active material layer 22 may include amorphous carbon and a mixture of at least one selected from the group consisting of gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn) and zinc (Zn). The mixing ratio of the mixture of amorphous carbon and gold or the like may be, for example, in the range of about 99:1 to about 1:99, about 10:1 to about 1:2, about 5:1 to about 1:1, or about 4:1 to about 2:1 based on a weight ratio, but is not necessarily limited to such a range, and is selected according to the desired characteristics of the all-solid-state secondary battery 1. Since the negative electrode active material may have such a composition, the cycle characteristics of the all-solid-state secondary battery 1 may be further improved.
[0164] The negative electrode active material included in the first negative electrode active material layer 22 may include, for example, a mixture of first particles composed of amorphous carbon and second particles composed of a metal or a metalloid. The metal or metalloid may include, for example, gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), etc. In other embodiments, the metalloid is a semiconductor. The content of the second particles may be in the range of about 1 wt% to about 99 wt%, about 1 wt% to about 60 wt%, about 8 wt% to about 60 wt%, about 10 wt% to about 50 wt%, about 15 wt% to about 40 wt%, or about 20 wt% to about 30 wt% with respect to the total weight of the mixture. For example, since the second particles may have a content within such a range, the cycle characteristics of the all-solid-state secondary battery 1 can be further improved.
[0165] In other embodiments, the first negative electrode active material layer 22 may include a composite negative electrode active material. The composite negative electrode active material may include, for example, a carbonaceous carrier and a metal-based negative electrode active material supported on the carbonaceous carrier. The composite negative electrode active material may have such a structure that the localization of the metal-based negative electrode active material in the first negative electrode active material layer 22 can be prevented and its uniform distribution can be obtained. In some embodiments, the cycle characteristics of the all-solid-state secondary battery 1 including the first negative electrode active material layer 22 can be further improved.
[0166] The metal-based negative electrode active material supported on the carbonaceous carrier may include, for example, a metal, a metal oxide, a composite of a metal and a metal oxide, or a combination thereof. Examples of the metal may include gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), aluminum (Al), bismuth (Bi), tin (Sn), tellurium (Te), zinc (Zn), etc. Examples of the metal oxide may include gold oxide (Au), platinum oxide (Pt), palladium oxide (Pd), silicon oxide (Si), silver oxide (Ag), aluminum oxide (Al), bismuth oxide (Bi), tin oxide (Sn), tellurium oxide (Te), zinc oxide (Zn), etc. The metal oxide may include, for example, Au x O y (where 0 < x ≤ 2 and 0 < y ≤ 3), Pt x O y (where 0 < x ≤ 1 and 0 < y ≤ 2), Pd x O y (where 0 < x ≤ 1 and 0 < y ≤ 1), Si x O y (where 0 < x ≤ 1 and 0 < y ≤ 2), Ag x O y (where 0 < x ≤ 2 and 0 < y ≤ 1), Al x O y(where 0 < x ≤ 2 and 0 < y ≤ 3), Bi x O y (where 0 < x ≤ 2 and 0 < y ≤ 3), Sn x O y (where 0 < x ≤ 1 and 0 < y ≤ 2), Te x O y (where 0 < x ≤ 1 and 0 < y ≤ 3), Zn x O y (where 0 < x ≤ 1 and 0 < y ≤ 1) or combinations thereof. The composite of the metal and the metal oxide may include, for example, a composite of Au and Au x O y (where 0 < x ≤ 2 and 0 < y ≤ 3), a composite of Pt and Pt x O y (where 0 < x ≤ 1 and 0 < y ≤ 2), a composite of Pd and Pd x O y (where 0 < x ≤ 1 and 0 < y ≤ 1), a composite of Si and Si x O y (where 0 < x ≤ 1 and 0 < y ≤ 2), a composite of Ag and Ag x O y (where 0 < x ≤ 2 and 0 < y ≤ 1), a composite of Al and Al x O y (where 0 < x ≤ 2 and 0 < y ≤ 3), a composite of Bi and Bi x O y (where 0 < x ≤ 2 and 0 < y ≤ 3), a composite of Sn and Sn x O y (where 0 < x ≤ 1 and 0 < y ≤ 2), a composite of Te and Te x O y (where 0 < x ≤ 1 and 0 < y ≤ 3), a composite of Zn and Zn x O y (where 0 < x ≤ 1 and 0 < y ≤ 1) or combinations thereof.
[0167] The carbonaceous support may include, for example, amorphous carbon. Examples of amorphous carbon may include CB, AB, furnace black (FB), KB, graphene, activated carbon, CNF, CNT, etc., but one or more embodiments are not necessarily limited thereto. Any material may be used as long as the material is classified as amorphous carbon in the art. Amorphous carbon may be carbon that does not have crystallinity or has very low crystallinity and may be distinguished from crystalline carbon or graphite-like carbon. The carbonaceous material may be, for example, a carbonaceous negative electrode active material.
[0168] The composite negative electrode active material may have, for example, a particle form. The particle size of the composite negative electrode active material in particle form may be, for example, in the range of about 10 nm to about 4 μm, about 10 nm to about 1 μm, about 10 nm to about 500 nm, about 10 nm to about 200 nm, or about 10 nm to about 100 nm. Since the composite negative electrode active material may have a particle size within this range, the reversible absorption and / or desorption of lithium may become easier during charge / discharge. The metal negative electrode active material loaded on the carbon-based carrier may have, for example, a particle form. The particle size of the metal negative electrode active material may be, for example, in the range of about 1 nm to about 200 nm, about 1 nm to about 150 nm, about 5 nm to about 100 nm, or about 10 nm to about 50 nm. The carbon-based carrier may have, for example, a particle form. The particle size of the carbon-based carrier may be, for example, in the range of about 10 nm to about 2 μm, about 10 nm to about 1 μm, about 10 nm to about 500 nm, about 10 nm to about 200 nm, or about 10 nm to about 100 nm. Since the carbon-based carrier has a particle size within this range, the carbon-based carrier can be more uniformly arranged in the first negative electrode active material layer 22. The carbon-based carrier may include, for example, nanoparticles having a particle size of 500 nm or less. The particle size of the composite negative electrode active material, the particle size of the metal-based negative electrode active material, and the particle size of the carbon-based carrier may all be, for example, an average particle size. The average particle size may be, for example, a median diameter (D50) measured by using a laser-type particle size distribution instrument. In other embodiments, the average particle size may be automatically determined from, for example, an electron microscope image using software or manually determined according to a manual.
[0169] [Negative electrode layer: binder]
[0170] The binder included in the first negative electrode active material layer 22 may be, for example, SBR, polytetrafluoroethylene, polyvinylidene fluoride, PE, vinylidene fluoride / hexafluoropropylene copolymer, polyacrylonitrile, polymethyl methacrylate, etc., but is not necessarily limited thereto. Any material used as a binder in the art may be used. The binder may include a single binder or a plurality of different binders.
[0171] The first negative active material layer 22 may include a binder and thus be stabilized on the negative current collector 21. In other embodiments, although the volume and / or relative position of the first negative active material layer 22 changes during charge / discharge, cracks in the first negative active material layer 22 may be suppressed. For example, if the first negative active material layer 22 does not include a binder, the first negative active material layer 22 may be easily separated from the negative current collector 21. If the first negative active material layer 22 is separated from the negative current collector 21, the negative current collector 21 may contact the solid electrolyte layer 30 at the exposed portion of the negative current collector 21, thereby increasing the possibility of a short circuit. For example, a slurry in which a material constituting the first negative active material layer 22 is dispersed may be applied to the negative current collector 21 and dried to manufacture the first negative active material layer 22. A binder may be included in the first negative active material layer 22 so that the negative active material is stably dispersed in the slurry. For example, if the slurry is applied on the negative electrode collector 21 by a screen printing method, clogging of the screen (eg, clogging due to aggregation of the negative electrode active material) may be suppressed.
[0172] [Negative electrode layer: other additives]
[0173] The first negative active material layer 22 may further include additives used in conventional all-solid-state secondary batteries (such as a filler, a coating agent, a dispersant, and an ion conductive aid).
[0174] [Negative electrode layer: solid electrolyte]
[0175] The first negative electrode active material layer 22 may further include a solid electrolyte. The solid electrolyte may be, for example, a material selected from the solid electrolyte included in the solid electrolyte layer 30. The solid electrolyte included in the first negative electrode active material layer 22 may serve as a reaction point where lithium metal begins to form in the first negative electrode active material layer 22, or may serve as a space for storing the formed lithium metal or as a path for transferring lithium ions. The solid electrolyte may be omitted.
[0176] In the first negative electrode active material layer 22, the content of the solid electrolyte may be high, for example, in a region adjacent to the solid electrolyte layer 30, and may be low in a region adjacent to the negative electrode current collector 21. In the first negative electrode active material layer 22, the solid electrolyte may have, for example, a concentration gradient in which the concentration decreases from a region adjacent to the solid electrolyte layer 30 to a region adjacent to the negative electrode current collector 21.
[0177] [Negative electrode layer: first negative electrode active material layer]
[0178] The ratio (B / A) of the initial charge capacity (B) of the first negative electrode active material layer 22 to the initial charge capacity (A) of the positive electrode active material layer 12 may be in the range of about 0.005 to about 0.45. The initial charge capacity of the positive electrode active material layer 12 may be charged from the first OCV to the Li / Li + The initial charge capacity of the first negative electrode active material layer 22 can be determined by charging from the second OCV to the maximum charge voltage for Li / Li + A voltage of about 0.01V is determined.
[0179] The maximum charge voltage may be determined according to the type of positive active material. The maximum charge voltage may be, for example, about 1.5 V, about 2.0 V, about 2.5 V, about 3.0 V, about 3.5 V, about 4.0 V, about 4.2 V, or about 4.3 V. For example, the maximum charge voltage of Li2S or a composite containing Li2S may be about 1.5 V, about 2.0 V, about 2.5 V, about 3.0 V, about 3.5 V, about 4.0 V, about 4.2 V, or about 4.3 V. + For example, the maximum charge voltage of Li2S or a composite containing Li2S may be about 2.5 V for Li / Li + The ratio (B / A) of the initial charge capacity (B) of the first negative active material layer 22 to the initial charge capacity (A) of the positive active material layer 12 may be, for example, in the range of about 0.01 to about 0.3, about 0.01 to about 0.2, or about 0.05 to about 0.1.
[0180] The initial charge capacity (mAh) of the positive electrode active material layer 12 can be obtained by multiplying the charge specific capacity (mAh / g) of the positive electrode active material layer 12 by the mass (g) of the positive electrode active material of the positive electrode active material layer 12. If multiple types of positive electrode active materials are used, a value can be calculated by multiplying the charge specific capacity by the mass for each positive electrode active material, and the sum of these values can be the initial charge capacity of the positive electrode active material layer 12. The initial charge capacity of the first negative electrode active material layer 22 can also be calculated in the same manner. The initial charge capacity of the first negative electrode active material layer 22 can be obtained by multiplying the charge specific capacity (mAh / g) of the first negative electrode active material layer 22 by the mass (g) of the negative electrode active material of the first negative electrode active material layer 22. If multiple types of negative electrode active materials are used, a value can be calculated by multiplying the charge specific capacity by the mass for each negative electrode active material, and the sum of these values can be the initial charge capacity of the first negative electrode active material layer 22. The charge capacity of each of the positive electrode active material and the negative electrode active material can be measured using an all-solid-state half-cell using lithium metal as a counter electrode. The initial charge capacity of each of the positive electrode active material layer 12 and the first negative electrode active material layer 22 can be measured using an all-solid-state half-cell at, for example, about 0.1 mA / cm2 For the positive electrode, the charge current can be directly measured at a constant current density of . For the positive electrode, the charge current can be directly measured at a constant current density of . + )) is measured at an operating voltage of about 0.01 V for the negative electrode (e.g., lithium metal). For example, an all-solid-state half-cell including a positive electrode active material layer may be measured at about 0.1 mA / cm 2 The all-solid-state half-cell battery including the first negative active material layer can be charged from the first OCV to about 3.0V at a constant current of about 0.1 mA / cm 2 The current density during constant current charging can be, for example, about 0.2 mA / cm 2 or about 0.5mA / cm 2 The all-solid-state half-cell including the positive active material layer can be charged, for example, from the first OCV to about 2.5 V, about 3.0 V, about 3.5 V, or about 4.0 V. The maximum charge voltage of the positive active material layer can be determined according to the maximum voltage of the battery that satisfies the safety conditions according to JIS C 8712:2015 of the Japanese Standards Association.
[0181] If the initial charge capacity of the first negative electrode active material layer 22 is too low, the first negative electrode active material layer 22 becomes very thin, and thus lithium dendrites formed between the first negative electrode active material layer 22 and the negative electrode current collector 21 during repeated charge / discharge processes collapse the first negative electrode active material layer 22, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery 1. If the charge capacity of the first negative electrode active material layer 22 is excessively increased, the energy density of the all-solid-state secondary battery 1 is reduced, and the internal resistance of the all-solid-state secondary battery 1 due to the first negative electrode active material layer 22 is increased, making it difficult to improve the cycle characteristics of the all-solid-state secondary battery 1.
[0182] The thickness of the first negative electrode active material layer 22 may be, for example, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 5% or less of the thickness of the positive electrode active material layer 12. The thickness of the first negative electrode active material layer 22 may be in the range of, for example, about 1% to about 50%, about 1% to about 40%, about 1% to about 30%, about 1% to about 20%, about 1% to about 10%, or about 1% to about 5% of the thickness of the positive electrode active material layer 12. The thickness of the first negative electrode active material layer 22 may be in the range of, for example, about 1 μm to about 20 μm, about 2 μm to about 15 μm, or about 3 μm to about 10 μm. If the first negative electrode active material layer 22 is too thin, lithium dendrites formed between the first negative electrode active material layer 22 and the negative electrode current collector 21 may collapse the first negative electrode active material layer 22, which makes it difficult to improve the cycle characteristics of the all-solid-state secondary battery 1. If the thickness of the first negative electrode active material layer 22 is excessively increased, the energy density of the all-solid-state secondary battery 1 is reduced, and the internal resistance of the all-solid-state secondary battery 1 caused by the first negative electrode active material layer 22 is increased, which makes it difficult to improve the cycle characteristics of the all-solid-state secondary battery 1. For example, if the thickness of the first negative electrode active material layer 22 is reduced, the initial charge capacity of the first negative electrode active material layer 22 is also reduced.
[0183] [Negative electrode layer: second negative electrode active material layer]
[0184] Although not shown in the drawings, the all-solid-state secondary battery 1 may further include, for example, a second negative electrode active material layer, which is disposed between the negative electrode current collector 21 and the first negative electrode active material layer 22 after the all-solid-state secondary battery 1 is charged. The second negative electrode active material layer may be a metal layer including lithium or a lithium alloy. The metal layer may include lithium or a lithium alloy. In some embodiments, since the second negative electrode active material layer may be a metal layer including lithium, the second negative electrode active material layer may be used as, for example, a lithium storage member. The lithium alloy may be, for example, a Li-Al alloy, a Li-Sn alloy, a Li-In alloy, a Li-Ag alloy, a Li-Au alloy, a Li-Zn alloy, a Li-Ge alloy, a Li-Si alloy, etc., but is not limited thereto. Any material used as a lithium alloy in the art may be used. The second negative electrode active material layer may be composed of one or lithium selected from such an alloy, or may be composed of a plurality of types of alloys. The second negative electrode active material layer may be, for example, a plated layer. For example, during the charging process of the all-solid-state secondary battery 1 , the second negative electrode active material layer may be precipitated between the first negative electrode active material layer 22 and the negative electrode collector 21 .
[0185] The thickness of the second negative electrode active material layer may be, for example, in the range of about 1 μm to about 500 μm, about 1 μm to about 200 μm, about 1 μm to about 150 μm, about 1 μm to about 100 μm, or about 1 μm to about 50 μm, but is not particularly limited. If the second negative electrode active material layer is too thin, the second negative electrode active material layer is difficult to use as a lithium storage member. If the second negative electrode active material layer is too thick, there is a possibility that the mass and volume of the all-solid-state secondary battery 1 will increase, and the cycle characteristics of the all-solid-state secondary battery 1 will deteriorate instead.
[0186] In other embodiments, in the all-solid-state secondary battery 1, for example, before assembling the all-solid-state secondary battery 1, the second negative electrode active material layer may be disposed between the negative electrode collector 21 and the first negative electrode active material layer 22. If the second negative electrode active material layer is disposed between the negative electrode collector 21 and the first negative electrode active material layer 22 before assembling the all-solid-state secondary battery 1, the second negative electrode active material layer may be a metal layer including lithium and thus serves as a lithium storage member. For example, before assembling the all-solid-state secondary battery 1, a lithium foil may be disposed between the negative electrode collector 21 and the first negative electrode active material layer 22.
[0187] If the second negative electrode active material layer can be precipitated by charging the all-solid-state secondary battery 1 after assembly, the second negative electrode active material layer may not be included during the assembly of the all-solid-state secondary battery 1, so the energy density of the all-solid-state secondary battery 1 can be increased. If the all-solid-state secondary battery 1 is charged, the first negative electrode active material layer 22 may be charged beyond its charge capacity. For example, the first negative electrode active material layer 22 may be overcharged. In the initial stage of charging, lithium may be absorbed in the first negative electrode active material layer 22. The negative electrode active material included in the first negative electrode active material layer 22 may form an alloy or compound with lithium ions moved from the positive electrode layer 10. If the first negative electrode active material layer 22 is charged beyond its capacity (for example, lithium may be precipitated on the rear side of the first negative electrode active material layer 22, for example, between the negative electrode collector 21 and the first negative electrode active material layer 22), a metal layer corresponding to the second negative electrode active material layer may be formed by the precipitated lithium. The second negative electrode active material layer may be a metal layer mainly composed of lithium (for example, metallic lithium). For example, this result can be obtained because the negative electrode active material included in the first negative electrode active material layer 22 can include a material that forms an alloy or a compound with lithium. During discharge, the lithium in the first negative electrode active material layer 22 and the second negative electrode active material layer (e.g., a metal layer) can be ionized to move toward the positive electrode layer 10. In some embodiments, in the all-solid-state secondary battery 1, lithium can be used as a negative electrode active material. In other embodiments, since the first negative electrode active material layer 22 can cover the second negative electrode active material layer, the first negative electrode active material layer 22 can be used as a protective layer for the second negative electrode active material layer (e.g., a metal layer), and at the same time can be used to suppress the precipitation growth of lithium dendrites. In some embodiments, short circuits and capacity reductions of the all-solid-state secondary battery 1 can be suppressed, and in some embodiments, the cycle characteristics of the all-solid-state secondary battery 1 can be improved. In other embodiments, if the second negative electrode active material layer is set by charging the all-solid-state secondary battery 1 after assembly, the negative electrode layer 20 (e.g., the negative electrode current collector 21, the first negative electrode active material layer 22, and the area therebetween) can be a Li-free area that does not include lithium (Li) in the initial state of the all-solid-state secondary battery 1 or in the state after the all-solid-state secondary battery 1 is fully discharged.
[0188] [Negative electrode layer: negative electrode current collector]
[0189] The negative electrode current collector 21 (21a or 21b) may be composed of, for example, a material that does not react with lithium (e.g., does not form an alloy or compound with lithium). The material constituting the negative electrode current collector 21 may be, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co) or nickel (Ni), but is not necessarily limited thereto. Any material used as an electrode current collector in the art may be used. The negative electrode current collector 21 may be composed of an alloy or a coating material of at least one, two or more metals selected from the above metals. The negative electrode current collector 21 may be, for example, in the form of a plate or foil.
[0190] For example, although not shown in the drawings, the all-solid-state secondary battery 1 may also include a thin film containing an element capable of forming an alloy with lithium on one side of the negative electrode current collector 21. The thin film may be disposed between the negative electrode current collector 21 and the first negative electrode active material layer 22. The thin film may include, for example, an element capable of forming an alloy with lithium. The element capable of forming an alloy with lithium may be, for example, gold, silver, zinc, tin, indium, silicon, aluminum, bismuth, etc., but is not necessarily limited thereto. Any element capable of forming an alloy with lithium in the art may be used. The thin film may be composed of an alloy of one or more metals selected from the metals. For example, the thin film may be disposed on one side of the negative electrode current collector 21, thereby further flattening the precipitation form of the second negative electrode active material layer precipitated between the thin film and the first negative electrode active material layer 22, and further improving the cycle characteristics of the all-solid-state secondary battery 1.
[0191] The thickness of the film can be, for example, in the range of about 1 nm to about 800 nm, about 10 nm to about 700 nm, about 50 nm to about 600 nm, or about 100 nm to about 500 nm. If the thickness of the film is less than about 1 nm, the film may be difficult to work. If the film is too thick, the film itself absorbs lithium, so the amount of lithium precipitated at the negative electrode will decrease, resulting in a decrease in the energy density of the all-solid-state secondary battery 1 and causing the cycle characteristics of the all-solid-state secondary battery 1 to deteriorate. The film can be arranged on the negative electrode current collector 21 by, for example, a vacuum deposition method, a sputtering method, an electroplating method, etc., and any method capable of forming a film in the art can be used.
[0192] Although not shown in the drawings, the negative electrode current collector 21 may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may be, for example, a thermoplastic polymer. The polymer may include, for example, PET, PE, PP, PBT, PI, or a combination thereof. The polymer may be an insulating polymer. Since the base film may include an insulating thermoplastic polymer, if a short circuit occurs, the base film may soften or liquefy to block the operation of the battery, thereby suppressing the rapid increase in current. The metal layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The negative electrode current collector 21 may additionally include a metal sheet and / or a lead tab. The base film, metal layer, metal sheet, and lead tab of the negative electrode current collector 21 may be defined as the positive electrode current collector 11 described above. Since the negative electrode current collector 21 may have such a structure, the weight of the negative electrode may be reduced, thereby improving the energy density of the negative electrode and the lithium battery.
[0193] [Negative Electrode Layer: Second Inactive Member]
[0194] Reference Figures 6 to 9 The all-solid-state secondary battery 1 ( 1 a or 1 b ) may further include a second inactive member 50 ( 50 a , 50 b , 50 c ) disposed on the other side of the negative electrode collector 21 ( 21 a and 21 b ).
[0195] The second inactive member 50 may be different from the first inactive member 40 in that the second inactive member 50 may additionally include a conductive material to have conductivity. The second inactive member 50 may be, for example, a conductive flame retardant inactive member.
[0196] The conductive material may include, for example, graphite, CB, AB, KB, superconductive acetylene black, carbon fiber, CNT, graphene, metal fiber, metal powder, etc. The electronic conductivity of the second inactive member 50 at about 25° C. may be, for example, 100 times or more, 1,000 times or more, or 10,000 times or more of the electronic conductivity of the first inactive member 40 at about 25° C.
[0197] The second inactive member 50 may include, for example, a matrix, a filler, and a conductive material. The matrix may include, for example, a base material and a reinforcing material. The second inactive member 50 may also include a filler and a binder. The content of the conductive material included in the second inactive member 50 may be, for example, in the range of about 1 part by weight to about 30 parts by weight, about 1 part by weight to about 20 parts by weight, about 1 part by weight to about 15 parts by weight, about 1 part by weight to about 10 parts by weight, about 5 parts by weight to about 40 parts by weight, about 5 parts by weight to about 30 parts by weight, or about 5 parts by weight to about 35 parts by weight relative to about 100 parts by weight of the second inactive member 50.
[0198] The Young's modulus of the second inactive member 50 may be, for example, less than the Young's modulus of the negative electrode current collector 21. The Young's modulus of the second inactive member 50 may be, for example, 50% or less, 30% or less, 10% or less, or 5% or less of the Young's modulus of the negative electrode current collector 21. The Young's modulus of the second inactive member 50 may be in the range of, for example, about 0.01% to about 50%, about 0.1% to about 30%, about 0.1% to about 10%, or about 1% to about 5% of the Young's modulus of the negative electrode current collector 21. The Young's modulus of the second inactive member 50 may be, for example, 100 MPa or less, 50 MPa or less, 30 MPa or less, 10 MPa or less, or 5 MPa or less. The Young's modulus of the second inactive member 50 may be, for example, in the range of about 0.01 MPa to about 100 MPa, about 0.1 MPa to about 50 MPa, about 0.1 MPa to about 30 MPa, about 0.1 MPa to about 10 MPa, or about 1 MPa to about 5 MPa. The Young's modulus of the second inactive member 50 may be measured by using a DMA (dynamic mechanical analyzer) or a UTM (universal testing machine). The Young's modulus of the second inactive member 50 may be measured according to ASTM D638.
[0199] Since the second inactive member 50 (50a and 50b) may have electrical conductivity, the second inactive member 50 may be used as the negative electrode current collector 21. In other embodiments, since the second inactive member 50 (50a and 50b) may have a Young's modulus smaller than that of the negative electrode current collector 21, the second inactive member 50 may effectively receive the volume change of the negative electrode layer 20 during the charge / discharge of the all-solid-state secondary battery 1. In some embodiments, the second inactive member 50 (50a and 50b) may effectively relieve the internal stress caused by the volume change of the all-solid-state secondary battery 1 during the charge / discharge of the all-solid-state secondary battery 1, thereby improving the cycle characteristics of the all-solid-state secondary battery 1.
[0200] The thickness of the second inactive member 50 may be greater than, for example, the thickness of the first negative active material layer 22. Since the second inactive member 50 may be thicker than the first negative active material layer 22, the second inactive member 50 may more effectively receive the volume change of the negative electrode layer 20 during charge / discharge. The thickness of the first negative active material layer 22 may be, for example, 50% or less, 40% or less, 30% or less, 20% or less, or 10% or less of the thickness of the second inactive member 50. The thickness of the first negative active material layer 22 may be, for example, in the range of about 1% to about 50%, about 1% to about 40%, about 1% to about 30%, about 1% to about 20%, or about 1% to about 10% of the thickness of the second inactive member 50. The thickness of the second inactive member 50 may be, for example, in the range of about 1 μm to about 300 μm, about 10 μm to about 300 μm, about 50 μm to about 300 μm, or about 100 μm to about 200 μm. If the second inactive member 50 is too thin, it may be difficult to provide the expected effect, and if the second inactive member 50 is too thick, the energy density of the all-solid-state secondary battery 1 may be reduced. The form of the second inactive member 50 is not particularly limited, and can be selected according to the form of the all-solid-state secondary battery 1. The second inactive member 50 may have, for example, a sheet form, a rod form, or a washer form.
[0201] The second inactive member 50 may be provided, for example, on one side or both sides of the all-solid-state secondary battery 1. The second inactive member 50 may be provided, for example, between a plurality of stacked all-solid-state secondary batteries 1. For example, the second inactive member 50 may be provided between a plurality of stacked all-solid-state secondary batteries 1, on the uppermost surface, and / or on the lowermost surface.
[0202] The ratio of the volume of the all-solid-state secondary battery 1 before charging to the volume of the all-solid-state secondary battery 1 after charging (e.g., volume expansion rate) can be, for example, 15% or less, 10% or less, or 5% or less. The volume of the all-solid-state secondary battery 1 before charging can be measured by measuring the thickness of the all-solid-state battery at 25°C before the formation step. In addition, the volume of the all-solid-state secondary battery 1 after charging can be measured at 25°C in the formation step by measuring the thickness of the all-solid-state battery after completing the first charging step.
[0203] The volume increase of the negative electrode layer 20 during charging of the all-solid-state secondary battery 1 can be offset by the volume reduction of the positive electrode layer 10 , and the second inactive member 50 can receive the volume change of the negative electrode layer 20 , which reduces the volume change of the all-solid-state secondary battery 1 before and after charging.
[0204] The energy density per unit volume of the all-solid-state secondary battery 1 can be, for example, in the range of about 500Wh / L to about 900Wh / L, about 500Wh / L to about 800Wh / L, or about 500Wh / L to about 700Wh / L. The energy density per unit weight of the all-solid-state secondary battery 1 can be, for example, in the range of about 350Wh / g to about 600Wh / g, about 350Wh / g to about 580Wh / g, about 350Wh / g to about 570Wh / g, or about 350Wh / g to 550Wh / g. Since the all-solid-state secondary battery 1 can have an energy density within this range, an increased energy density can be provided compared to a conventional secondary battery.
[0205] [Solid electrolyte layer]
[0206] [Solid electrolyte layer: solid electrolyte]
[0207] Reference Figures 1 to 5 The solid electrolyte layer 30 (30a, 30b) may include a solid electrolyte disposed between the positive electrode layer 10 and the negative electrode layer 20. The electrolyte may include, for example, a solid electrolyte, a gel electrolyte, or a combination thereof.
[0208] The solid electrolyte may include, for example, a sulfide-based solid electrolyte, an oxide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof.
[0209] The solid electrolyte may be, for example, a sulfide solid electrolyte. The sulfide solid electrolyte may be, for example, selected from Li2S-P2S5, Li2S-P2S5-LiX (wherein X is a halogen element), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (wherein m and n are positive numbers, and Z is at least one selected from Ge, Zn and Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q (wherein p and q are positive numbers, and M is at least one selected from P, Si, Ge, B, Al, Ga, and In), Li 7-x PS 6-x C (where 0≤x≤2), Li 7-x PS 6-x Br x(where 0≤x≤2) and Li 7-x PS 6-x I x (wherein, 0≤x≤2) at least one. The sulfide solid electrolyte can be prepared by treating raw materials such as Li2S or P2S5 through a melt quenching method, a mechanical grinding method, etc. In other embodiments, after such treatment, a heat treatment can be performed. The solid electrolyte can be in an amorphous state, a crystalline state, or a mixed state thereof. In other embodiments, the solid electrolyte can be, for example, a material including at least sulfur (S), phosphorus (P), and lithium (Li) as constituent elements among the above-mentioned sulfide solid electrolyte materials. For example, the solid electrolyte can be a material including Li2S-P2S5. If Li2S-P2S5 is included as a sulfide solid electrolyte material forming a solid electrolyte, the mixed molar ratio of Li2S to P2S5 (e.g., Li2S:P2S5) can be in the range of about 20:80 to about 90:10, about 25:75 to about 90:10, about 30:70 to about 70:30, or about 40:60 to about 60:40.
[0210] The sulfide-based solid electrolyte may include, for example, an argyrodite-type solid electrolyte represented by Formula 1 below.
[0211] <Formula 1>
[0212] Li + 12-n-x A n+ X 2- 6-x Y - x
[0213] In Formula 1, A is P, As, Ge, Ga, Sb, Si, Sn, Al, In, Ti, V, Nb or Ta, X is S, Se or Te, Y is Cl, Br, I, F, CN, OCN, SCN or N3, 1≤n≤5, 0≤x≤2. The sulfide-based solid electrolyte may be, for example, a sulfide-based solid electrolyte selected from Li 7-x PS 6-x Cl x (where 0≤x≤2), Li 7-x PS 6-x Br x (where 0≤x≤2) and Li 7-x PS 6-x I x (wherein 0≤x≤2). The sulfide-based solid electrolyte may be, for example, an argyrodite-type compound including at least one selected from Li6PS5Cl, Li6PS5Br, and Li6PS5I.
[0214] The density of the argyrodite-type solid electrolyte can be in the range of about 1.5 g / cc to about 2.0 g / cc. The argyrodite-type solid electrolyte can have a density of about 1.5 g / cc or more, thereby reducing the internal resistance of the all-solid-state secondary battery 1 and effectively suppressing the penetration of Li into the solid electrolyte layer 30.
[0215] The oxide-based solid electrolyte can be, for example, Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (where 0 < x < 2 and 0 ≤ y < 3), BaTiO3, Pb(Zr,Ti)O3 (PZT), Pb 1-x La x Zr 1-y Ti y O3 (PLZT) (where 0 ≤ x < 1 and 0 ≤ y < 1), Pb(Mg3Nb 2 / 3 )O3 - PbTiO3 (PMN - PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3 (where 0 < x < 2 and 0 < y < 3), Li x Al y Ti z (PO4)3 (where 0 < x < 2, 0 < y < 1, and 0 < z < 3), Li 1+x+y (Al,Ga) x (Ti,Ge) 2-x Si y P 3-y O 12 (where 0 ≤ x ≤ 1 and 0 ≤ y ≤ 1), Li x La y TiO3 (where 0 < x < 2 and 0 < y < 3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O - Al2O3 - SiO2 - P2O5 - TiO2 - GeO2, Li 3+x La3M2O 12 (where M = Te, Nb or Zr 0 ≤ x ≤ 10) or a combination thereof. The oxide-based solid electrolyte can be prepared, for example, by a sintering method or the like.
[0216] The oxide-based solid electrolyte can be, for example, selected from Li7La3Zr2O12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 A garnet-type solid electrolyte of (M-doped LLZO) (where M = Ga, W, Nb, Ta or Al, 0 < a < 2, and 0 ≤ x ≤ 10).
[0217] For example, a polymer solid electrolyte can include a mixture of a lithium salt and a polymer or can include a polymer having ion-conductive functional groups. A polymer solid electrolyte can be, for example, a polymer electrolyte that is in a solid state at a temperature of about 25 °C and a pressure of about 1 atm. A polymer solid electrolyte can not include, for example, a liquid. A polymer solid electrolyte can be a polymer, and the polymer can include, for example, polyethylene oxide (PEO), PVDF, poly(vinylidene fluoride - hexafluoropropylene) (PVDF-HFP), poly(styrene-b-ethylene oxide) (PS-PEO) block copolymer, poly(styrene-butadiene), poly(styrene-isoprene-styrene), poly(styrene-b-divinylbenzene) block copolymer, poly(styrene-ethylene oxide-styrene) block copolymer, polystyrene sulfonate (PSS), polyvinyl fluoride (PVF), poly(methyl methacrylate) (PMMA), polyethylene glycol (PEG), polyacrylonitrile (PAN), polytetrafluoroethylene (PTFE), poly(ethylenedioxythiophene) (PEDOT), polypyrrole (PPY), polyaniline, polyacetylene, Nafion TM 、 Gore TM 、Aciplex TM 、 Sulfonated poly(ether ether ketone) (SPEEK), sulfonated poly(arylene ether ketone ketone sulfone) (SPAEKKS), sulfonated poly(arylene ether ketone) (SPAEK), poly[bis(benzimidazole benzoisoquinolinone)] (SPBIBI), lithium 9,10-diphenylanthracene-2-sulfonate (DPASLi + ) or a combination thereof, but one or more embodiments are not limited thereto. Any material can be used as long as the material can be used for a polymer electrolyte in the art. As a lithium salt, any material can be used as long as the material can be used as a lithium salt in the art. The lithium salt can include, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, or LiN(C x F 2x+1 SO2)(C y F 2y+1SO2) (wherein, x and y are both natural numbers of 1 to 20), LiCl, LiI or a mixture thereof. The polymer included in the polymer solid electrolyte may be, for example, a compound including 10 or more, 20 or more, 50 or more or 100 or more repeating units. The weight average molecular weight of the polymer included in the polymer solid electrolyte may be, for example, 1,000 Daltons or more, 10,000 Daltons or more, 100,000 Daltons or more or 1,000,000 Daltons or more.
[0218] The gel electrolyte may include, for example, a polymer gel electrolyte. The gel electrolyte may have a gel state without including, for example, a polymer.
[0219] The polymer gel electrolyte may include, for example, a liquid electrolyte and a polymer, or may include an organic solvent and a polymer having an ion conductive functional group. The polymer gel electrolyte may be, for example, a polymer electrolyte in a gel state at a temperature of about 25° C. and a pressure of about 1 atm. The polymer gel electrolyte may have, for example, a gel state without including a liquid. The liquid electrolyte used for the polymer gel electrolyte may include, for example, an ionic liquid, a mixture of a lithium salt and an organic solvent, a mixture of a lithium salt and an organic solvent, a mixture of an ionic liquid and an organic solvent, or a mixture of a lithium salt and an ionic liquid. The polymer used for the polymer gel electrolyte may be selected from polymers used for solid polymer electrolytes. The organic solvent may be selected from organic solvents used for liquid electrolytes. The lithium salt may be selected from lithium salts used for polymer solid electrolytes. The ionic liquid may refer to a salt that is liquid at room temperature or a room temperature molten salt having a melting point at room temperature or lower and is composed only of ions. The ionic liquid may include, for example, at least one selected from compounds including: a) a cation selected from ammonium cations, pyrrolidinyl cations, pyridinyl cations, pyrimidinyl cations, imidazolyl cations, piperidinyl cations, pyrazolyl cations, oxazolyl cations, pyridazinyl cations, phosphonium cations, sulfonium cations, triazolyl cations and mixtures thereof; and b) a cation selected from BF4 - PF6 - 、AsF6 - 、SbF6 - 、AlCl4 - 、HSO4 - 、ClO4 - 、CH3SO3 - CF3CO2 - , Cl - Br - ,I - 、SO4 - CF3SO3 -、(FSO2)2N - 、(C2F5SO2)2N - 、(C2F5SO2)(CF3SO2)N - and (CF3SO2)2N - At least one anion in the electrolyte. The polymer solid electrolyte can be immersed in a liquid electrolyte in, for example, a secondary battery to form a polymer gel electrolyte. The polymer gel electrolyte may also include inorganic particles. The polymer included in the polymer gel electrolyte may be, for example, a compound including 10 or more, 20 or more, 50 or more, or 100 or more repeating units. The weight average molecular weight of the polymer included in the polymer gel electrolyte may be, for example, 500 Daltons or more, 1,000 Daltons or more, 10,000 Daltons or more, 100,000 Daltons or more, or 1,000,000 Daltons or more.
[0220] The solid electrolyte layer 30 may be impermeable to lithium polysulfide. In some embodiments, a side reaction between lithium polysulfide and the negative electrode layer 20 that occurs during charge / discharge of the sulfide-based positive electrode active material may be prevented. In some embodiments, the cycle characteristics of the all-solid-state secondary battery 1 including the solid electrolyte layer 30 may be improved.
[0221] [Solid electrolyte layer: Binder]
[0222] The solid electrolyte layer 30 may include, for example, a binder. The binder included in the solid electrolyte layer 30 may be, for example, SBR, polytetrafluoroethylene, polyvinylidene fluoride, PE, etc., but is not limited thereto. Any material used as a binder in the art may be used. The binder of the solid electrolyte layer 30 may be the same as or different from the binder included in the positive electrode active material layer 12 and the first negative electrode active material layer 22. The binder may be omitted.
[0223] Relative to the total weight of the solid electrolyte layer 30, the content of the binder included in the solid electrolyte layer 30 may be in the range of about 0.1 wt % to about 10 wt %, about 0.1 wt % to about 5 wt %, about 0.1 wt % to about 3 wt %, about 0.1 wt % to about 1 wt %, about 0 wt % to about 0.5 wt % or about 0 wt % to about 0.1 wt %.
[0224] The present inventive concept will be described in more detail through the following examples and comparative examples. However, the examples are only for illustrative purposes, and the scope of the present inventive concept is not limited by the examples.
[0225] Preparation Example 1: Li2S-LiI-AlI3-CNF Composite
[0226] (Phase 1)
[0227] LiI and AlI 3 were mixed in a molar ratio of 1:1 to prepare a first mixture.
[0228] Li2S and the first mixture were mixed in a weight ratio of 40:20 to prepare a second mixture. The second mixture was mechanically ground using a ball mill to prepare a Li2S-LiI-AlI3 composite. The grinding conditions included a temperature of 25°C, a speed of 600 rpm, and a grinding time of 10 hours. The grinding energy applied to the sample during grinding was 28G.
[0229] (Phase 2)
[0230] The Li2S-LiI-AlI3 composite and CNF were mixed in a weight ratio of 60:10 to prepare a third mixture. The third mixture was mechanically ground using a ball mill to prepare Li2S-LiI-AlI3-CNF The grinding conditions included a temperature of 25° C., a speed of 600 rpm, and a grinding time of 10 hours. The grinding energy applied to the sample during grinding was 28 G. Li2S-LiI-AlI3-CNF composite as sulfide-based cathode active material .
[0231] Reference preparation example 1: mixture of Li2S, LiI, AlI3 and CNF
[0232] LiI and AlI 3 were mixed in a molar ratio of 1:1 to prepare a first mixture.
[0233] Li2S was mixed with the first mixture at a weight ratio of 40:20, and a mixture of Li2S, LiI, and AlI3 was additionally mixed with CNF at a weight ratio of 60:10 to be used as a sulfide-based positive active material.
[0234] Example 1: Mono-cell all-solid-state secondary battery, sulfide-based positive electrode active material (Li2S- CNF composite) and a first inactive member having flame retardancy
[0235] (Preparation of negative electrode layer)
[0236] A 10 μm thick SUS foil was prepared as the negative electrode current collector. In other embodiments, CB having a primary particle size of about 30 nm and silver (Ag) particles having an average particle size of about 60 nm were prepared as the negative electrode active material.
[0237] 4 g of a mixed powder in which CB and silver (Ag) particles were mixed in a weight ratio of 3: 1 was introduced into a container, and 4 g of an N-methyl-2-pyrrolidone (NMP) solution including 7 wt % of a PVDF binder (#9300, manufactured by Kureha Corporation) was added thereto to prepare a mixed solution. Next, while NMP was added little by little to the mixed solution, the mixed solution was stirred to prepare a slurry. The prepared slurry was applied to a SUS sheet using a rod coater and dried in air at a temperature of 80°C for 10 minutes. Thus, the obtained stack was vacuum dried at a temperature of 40°C for 10 hours. The dried stack was passed through a cold roller press at 5 tonf / cm 2 The stack was pressed at a pressure of 500 and a speed of 5 m / sec to make the surface of the first negative electrode active material layer of the stack flat. The negative electrode layer was prepared by this process. The thickness of the first negative electrode active material layer included in the negative electrode layer was about 15 μm. The area of the first negative electrode active material layer was the same as the area of the negative electrode current collector. The initial charge capacity of the negative electrode layer was measured by using the above-mentioned half-cell monomer. The initial charge capacity of the first negative electrode active material layer was 2.3 mAh.
[0238] (Preparation of positive electrode layer)
[0239] Li2S-CNF composite was prepared as a positive electrode active material. In addition to changing the vapor-grown carbon fiber (VGCF) to CNF, the Li2S-CNF composite was prepared according to the method disclosed in Electrochimica Acta, 230 (2017), pp. 279-284. Li6PS5Cl (D50 = 3.0 μm, crystallized) as a argyrodite-type crystal was prepared as a solid electrolyte. KB was prepared as a conductive agent. These materials were mixed so that the weight ratio of the positive electrode active material, the solid electrolyte and the conductive agent was 40:50:10 to prepare a positive electrode mixture. The positive electrode mixture was obtained by dry mixing using a ball mill. The positive electrode mixture obtained by ball milling forms an ion conductive and electronic conductive network.
[0240] The positive electrode mixture was placed on one side of a positive electrode current collector consisting of aluminum foil or SUS having one side coated with carbon, and the plate was pressed at a pressure of 200 MPa for 10 minutes to prepare a positive electrode layer. The thickness of the positive electrode layer was about 120 μm. The thickness of the positive electrode active material layer was about 100 μm, and the thickness of the aluminum foil coated with carbon was about 20 μm. The area of the positive electrode active material layer was the same as that of the positive electrode current collector.
[0241] The initial charge capacity of the positive electrode was measured by using the above half-cell unit. The initial charge capacity of the positive electrode active material layer was 25 mAh.
[0242] In Example 1, the ratio (B / A) of the initial charge capacity (B) of the first negative active material layer to the initial charge capacity (A) of the positive active material layer is 0.09. The initial charge capacity of the positive active material layer is calculated by charging from the first OCV to 2.8 V vs. Li / Li + The initial charge capacity of the first negative electrode active material layer is determined by charging from the second OCV to 0.01Vvs.Li / Li + In each of Examples 2 to 8 and Comparative Example 1, the ratio (B / A) of the initial charge capacity (B) of the first negative electrode active material layer to the initial charge capacity (A) of the positive electrode active material layer measured under the same conditions as those in Example 1 was 0.07 to 0.09. Since double-sided negative electrodes were used in Examples 7 and 8, half of the initial charge capacity of the positive electrode layer was used to calculate the ratio (B / A).
[0243] (Preparation of Solid Electrolyte Layer)
[0244] A mixture is prepared by adding 1.5 parts by weight of an acrylic binder relative to 98.5 parts by weight of a solid electrolyte to a Li6PS5Cl solid electrolyte (D50=3.0 μm, crystallized) as a argyrodite-type crystal. Octyl acetate is added to the prepared mixture and stirred to prepare a slurry. The prepared slurry is applied to a 15 μm thick non-woven fabric placed on a 75 μm thick PET substrate using a rod coater and dried in air at a temperature of 80°C for 10 minutes to obtain a stack. The obtained stack is vacuum dried at a temperature of 80°C for 2 hours. A solid electrolyte layer is prepared by this process.
[0245] (Flame retardant inactive components)
[0246] A slurry which is a mixture of pulp fiber (cellulose fiber), glass fiber, aluminum hydroxide (Al(OH) 3 ), an acrylic binder, and a solvent is formed into a gasket form, and the solvent is removed to prepare a flame retardant inactive member.
[0247] The weight ratio of pulp fiber (cellulose fiber), glass fiber, aluminum hydroxide (Al(OH) 3) and acrylic binder is 20:8:70:2. The thickness of the flame retardant inactive member is about 120 μm.
[0248] Before the prepared flame-retardant inactive member was disposed on the solid electrolyte layer, vacuum heat treatment was performed thereon at a temperature of 80° C. for 5 hours to remove moisture and the like from the flame-retardant inactive member.
[0249] (Manufacturing of all-solid-state secondary batteries)
[0250] Reference Figure 1, a solid electrolyte layer is arranged on the negative electrode layer so that the first negative electrode active material layer is in contact with the solid electrolyte layer, and a positive electrode layer is arranged on the solid electrolyte layer. A gasket surrounding the positive electrode layer and in contact with the solid electrolyte layer is arranged around the positive electrode layer to prepare a stack. The thickness of the gasket is about 120 μm. A flame retardant inactive member is used as a gasket. The gasket is arranged to contact the side of the positive electrode layer and the solid electrolyte layer. The positive electrode layer is arranged at the central portion of the solid electrolyte layer, and the gasket is arranged to surround the positive electrode layer and extend to the end of the solid electrolyte layer. The area of the positive electrode layer is about 90% of the area of the solid electrolyte layer, and the gasket is arranged in all of the remaining area of 10% of the solid electrolyte layer on which the positive electrode layer is not arranged.
[0251] The prepared stack was plate-pressed at a temperature of 85°C and a pressure of 500MPa for 30 minutes. The solid electrolyte layer was sintered by this pressing process, thereby improving the battery characteristics. The thickness of the sintered solid electrolyte layer was about 45μm. The density of the Li6PS5Cl solid electrolyte was 1.6g / cc, and the Li6PS5Cl solid electrolyte was a silver germanium sulfide crystal and was included in the sintered solid electrolyte layer. The area of the solid electrolyte layer was the same as that of the negative electrode layer.
[0252] The pressed stack is introduced into a bag and vacuum-sealed to manufacture an all-solid-state secondary battery. Portions of the positive and negative current collectors extend to the outside of the sealed all-solid-state secondary battery and serve as positive and negative electrode layer terminals.
[0253] Example 2: Sulfide-based positive electrode active material (Li2S-CNF composite), first inactive member with flame retardancy and a second inactive member having electrical conductivity and flame retardancy
[0254] An all-solid-state secondary battery was manufactured in the same manner as in Example 1, except that a conductive flame-retardant member in the form of a sheet having the same area and shape as the stack was additionally disposed on the negative electrode current collector of the pressed stack before the pressed stack was introduced into a bag and vacuum-sealed to manufacture an all-solid-state secondary battery. A conductive flame-retardant inactive member sheet was prepared by the following method. The conductive flame-retardant inactive member sheet can be used as an elastic sheet.
[0255] (Conductive flame-retardant inactive components)
[0256] The slurry is formed into a sheet form and then dried to prepare a flame retardant inactive member, the slurry being a mixture of pulp fiber (cellulose fiber), glass fiber, aluminum hydroxide (Al(OH)3), acrylic binder, conductive material (superconductive acetylene black) and solvent. The weight ratio of pulp fiber (cellulose fiber), glass fiber, aluminum hydroxide (Al(OH)3), acrylic binder and conductive material is 20:8:50:2:20. The thickness of the flame retardant inactive member is about 120 μm. Before the prepared flame retardant inactive member is disposed on the negative electrode collector, a vacuum heat treatment is performed thereon at a temperature of 80°C for 5 hours to remove moisture, etc. from the flame retardant inactive member.
[0257] Example 3: Sulfide-based positive electrode active material (Li2S-CNF composite) and a first non-flame retardant non-active member
[0258] An all-solid-state secondary battery was manufactured in the same manner as in Example 1, except that the flame-retardant inactive member was changed to a non-flame-retardant inactive member.
[0259] The non-flame retardant inactive member includes pulp fiber and acrylic binder at a weight ratio of 98:2, and does not include glass fiber and Al(OH) 3. The thickness of the non-flame retardant inactive member is about 120 μm.
[0260] Example 4: Sulfide-based positive electrode active material (Li2S-C-Li6PS5Cl composite) and a first non-flammable Active Components
[0261] An all-solid-state secondary battery was manufactured in the same manner as in Example 1, except that the Li2S-C-Li6PS5Cl composite was used instead of the Li2S-CNF composite as the positive electrode active material.
[0262] The Li2S-C-Li6PS5Cl composite was prepared according to the method disclosed in Nano Lett. 2016, 16, 7, pp4521-4527.
[0263] Example 5: Sulfide positive electrode active material (Li2S-CNF composite), first negative electrode active material layer (loaded with Ag), a flame retardant first inactive member, and a flame retardant second inactive member
[0264] An all-solid-state secondary battery was manufactured in the same manner as in Example 2, except that the following silver-carrying particles CB were used as the negative electrode active material instead of the mixture of carbon black and silver particles.
[0265] (Preparation of CB loaded with silver particles)
[0266] The CB was dispersed in a 1.0 M sulfuric acid solution, stirred for 2 hours, and then filtered and dried to prepare an acid-treated CB.
[0267] 10g of acid-treated CB was added to a mixed solvent of 1,500g of distilled water, 1,500g of ethanol and 30g of glycerol and stirred, and then 2g of AgNO3 was added and stirred to prepare a mixed solution. The particle size of CB was 80nm. A reducing agent was added to the mixed solution, and silver ions were reduced and loaded on CB. The CB loaded with silver-containing particles was filtered, cleaned and dried to prepare a composite negative electrode active material. As a result of scanning electron microscopy and X-ray photoelectron spectroscopy (XPS) measurements, it was confirmed that multiple silver-containing particles were loaded on CB particles. The silver-containing particles include silver particles, silver oxide (Ag2O) particles, and composite particles of silver (Ag) and silver oxide (Ag2O). The content of the silver-containing particles included in the composite negative electrode active material is 5wt%. The average particle size of the silver particles is 10nm.
[0268] Example 6: Sulfide-based positive electrode active material (Li2S-C-LiI composite), flame-retardant first inactive member
[0269] An all-solid-state secondary battery was manufactured in the same manner as in Example 1, except that a Li 2 S—C—LiI composite was used instead of a Li 2 S—CNF composite as a positive electrode active material.
[0270] The Li2S-C-LiI composite was prepared according to the method disclosed in Nano Lett. 2016, 16, 7, pp4521-4527, except that Li6PS5Cl was changed to LiI.
[0271] Comparative Example 1: Sulfide-based positive electrode active material and no (no) inactive component
[0272] An all-solid-state secondary battery was manufactured in the same manner as in Example 1, except that a flame-retardant inactive member (eg, gasket) was not used in manufacturing the all-solid-state secondary battery.
[0273] Comparative Example 2: Oxide-based positive electrode active material and first inactive member having flame retardancy
[0274] An all-solid-state secondary battery was manufactured in the same manner as in Example 1, except that a positive electrode including a lithium transition metal oxide was used instead of the positive electrode including a Li 2 S positive electrode active material.
[0275] In Comparative Example 2, the ratio (B / A) of the initial charge capacity (B) of the first negative electrode active material layer to the initial charge capacity (A) of the positive electrode active material layer is 0.09. The initial charge capacity of the positive electrode active material layer is calculated by charging from the first OCV to the maximum charge voltage 4.25 V (vs. Li / Li + The initial charge capacity of the first negative electrode active material layer is determined by charging from the second OCV to 0.01 V (vs. Li / Li + ) is determined by the voltage.
[0276] The positive electrode including the lithium transition metal oxide was prepared by the following method.
[0277] (Preparation of positive electrode layer)
[0278] LiNi coated with Li2O-ZrO2 (LZO) 0.8 Co 0.15 Al 0.05 O2(NCA) was prepared as a positive electrode active material. A positive electrode active material coated with LZO was prepared according to the method disclosed in Korean Patent Publication No. 10-2016-0064942. Li6PS5Cl (D50=0.5μm, crystallized) as a argyrodite-type crystal was prepared as a solid electrolyte. A polytetrafluoroethylene (PTFE) binder (Teflon binder manufactured by DuPont) was prepared as a binder. CNF was prepared as a conductive agent. A mixture of these materials mixed into a xylene solvent so that the weight ratio of the positive electrode active material, the solid electrolyte, the conductive agent and the binder was 84:11.5:3:1.5 was formed into a sheet form, and then dried at a temperature of 40°C for 8 hours to prepare a positive electrode sheet. The positive electrode sheet was arranged on one side of a positive electrode current collector consisting of an aluminum foil having one side coated with carbon, and the plate was pressed for 10 minutes at a pressure of 200MPa to prepare a positive electrode layer. The thickness of the positive electrode layer is about 120μm. The thickness of the positive electrode active material layer was about 100 μm, and the thickness of the carbon-coated aluminum foil was about 20 μm. The area of the positive electrode active material layer was the same as the area of the positive electrode current collector.
[0279] Example 7: A bi-cell all-solid-state secondary battery, sulfide-based positive electrode active material (Li2S-CNF composite) and a first inactive member having flame retardancy
[0280] (Manufacturing of dual-cell all-solid-state secondary batteries)
[0281] A positive electrode layer was prepared in the same manner as in Example 1, except that the positive electrode active material layer was prepared to be provided on both sides of the positive electrode current collector.
[0282] The entire thickness of the positive electrode layer was about 220 μm, the thickness of the positive electrode active material layer was about 100 μm, and the thickness of the carbon-coated aluminum foil was about 20 μm.
[0283] In the same manner as in Example 1, two negative electrode layers, two solid electrolyte layers, and two flame-retardant inactive members were prepared.
[0284] Reference Figure 3, a solid electrolyte layer is disposed on the negative electrode layer so that the first negative electrode active material layer is in contact with the solid electrolyte layer, and the positive electrode layer is disposed on the solid electrolyte layer. The positive electrode layer has a structure in which the positive electrode active material layer is disposed on each of the two sides of the positive electrode current collector. A gasket is disposed around the positive electrode layer to surround the positive electrode layer and to contact the solid electrolyte layer. The thickness of the gasket is about 220 μm. The gasket may have a structure in which, for example, two gaskets having a thickness of 110 μm are stacked or a gasket having a thickness of 220 μm is provided. A flame retardant inactive member is used as a gasket.
[0285] The gasket is arranged to contact the side of the positive electrode layer and the solid electrolyte layer. The positive electrode layer is arranged at the central portion of the solid electrolyte layer, and the gasket is arranged to surround the positive electrode layer and extend to the end of the solid electrolyte layer. The area of the positive electrode layer is about 90% of the area of the solid electrolyte layer, and the gasket is arranged in the entirety of the remaining 10% area of the solid electrolyte layer on which the positive electrode layer is not arranged. The solid electrolyte layer is arranged on the positive electrode layer and the gasket, and the negative electrode layer is arranged on the solid electrolyte layer, thereby preparing a stacked body.
[0286] The prepared stack was plate-pressed at a temperature of 85°C and a pressure of 500MPa for 30 minutes. The solid electrolyte layer was sintered by this pressing process, and the battery characteristics were improved. The thickness of a sintered solid electrolyte layer was about 45μm. The density of the Li6PS5Cl solid electrolyte was 1.6g / cc, and the Li6PS5Cl solid electrolyte was a silver germanium sulfide crystal and was included in the sintered solid electrolyte layer. The area of the solid electrolyte layer was the same as that of the negative electrode layer.
[0287] The pressed stack is introduced into a bag and vacuum-sealed to manufacture an all-solid-state secondary battery. Portions of the positive electrode collector and the negative electrode collector extend to the outside of the sealed battery and serve as positive electrode layer terminals and negative electrode layer terminals.
[0288] Example 8: A dual-cell all-solid-state secondary battery, sulfide-based positive electrode active material (Li2S-CNF composite a first inactive member having flame retardancy and a second inactive member having electrical conductivity and flame retardancy
[0289] An all-solid-state secondary battery was manufactured in the same manner as in Example 7, except that a conductive flame-retardant inactive member in the form of a sheet having the same area and shape as the stack was additionally disposed on one side of the pressed stack and the other side opposite to the one side before the pressed stack was introduced into a bag and vacuum-sealed to manufacture an all-solid-state secondary battery. A conductive flame-retardant inactive member was prepared in the same manner as in Example 2.
[0290] Example 9: Mono-cell all-solid-state secondary battery, sulfide-based positive electrode active material (Li2S- LiI-AlI3-CNF composite) and flame retardant first inactive member
[0291] An all-solid-state secondary battery was manufactured in the same manner as in Example 1, except that the Li 2 S—LiI—AlI 3 —CNF composite prepared in Preparation Example 1 was used as a positive electrode active material instead of the Li 2 S—CNF composite.
[0292] Reference Example 1: Mono-cell all-solid-state secondary battery, sulfide-based positive electrode active material (Li2S-LiI-AlI3-CNF mixture), flame retardant first inactive member
[0293] An all-solid-state secondary battery was manufactured in the same manner as in Example 1, except that a simple mixture of Li2S, LiI, AlI3 and CNF prepared in Reference Preparation Example 1 was used instead of the Li2S-CNF composite as a positive electrode active material.
[0294] Evaluation Example 1: Calculation of Volume Change Rate during Charging of All-Solid State Secondary Batteries
[0295] By having [Al current collector (10 μm) / LiNi 0.8 Co 0.15 Al 0.05 The initial first volume of the first all-solid-state secondary battery of the structure of [O2(NCA) positive electrode active material layer (100μm) / Li6PS5Cl solid electrolyte layer (32μm) / first negative electrode active material layer (7μm) / SUS current collector (10μm)] and the second volume of the first all-solid-state secondary battery after charging in which a lithium metal layer having a thickness of 30μm is precipitated between the first negative electrode active material layer and the SUS current collector by charging, the volume change of the first all-solid-state secondary battery during charging is calculated and shown in the following Table 1. It is assumed that the thickness of the NCA positive electrode active material layer does not change before and after charging.
[0296] The volume change of the second all-solid-state secondary battery during charging is calculated and shown in Table 1 below by the initial first volume of the second all-solid-state secondary battery having a structure of [Al current collector (10μm) / Li2S (60wt%)-carbon (40wt%) positive electrode active material layer (50μm) / Li6PS5Cl solid electrolyte layer (32μm) / first negative electrode active material layer (7μm) / SUS current collector (10μm)] and the second volume of the second all-solid-state secondary battery after charging in which a lithium metal layer having a thickness of 30μm is precipitated between the first negative electrode active material layer and the SUS current collector by charging. Assume that the thickness of Li2S (60wt%)-carbon (40wt%) decreases from 50μm to 35μm, for example, by 15μm after charging. Assume that all lithium included in Li2S moves to the negative electrode. Assume that the positive electrode active material layer of the second all-solid-state secondary battery consists only of Li2S and carbon. Assume that the positive electrode active material layer of the first all-solid-state secondary battery consists of NCA.
[0297] [Table 1]
[0298]
[0299] As shown in Table 1, in the second all-solid-state secondary battery including the positive electrode active material layer including Li2S, the volume of the negative electrode layer increases due to the precipitation of the lithium metal layer, but the volume of the positive electrode active material layer decreases to suppress the increase in the total volume of the second all-solid-state secondary battery. In other embodiments, in the first all-solid-state secondary battery including the positive electrode active material layer including the lithium transition metal oxide, since the volume change of the positive electrode active material layer is not significant, the total volume of the first all-solid-state secondary battery is significantly increased due to the precipitation of the lithium metal layer.
[0300] In some embodiments, it is confirmed that in the second all-solid-state secondary battery, the volume change occurring during the charging / discharging of the second all-solid-state secondary battery is reduced compared to the volume change occurring during the charging / discharging of the first all-solid-state secondary battery, thereby effectively preventing degradation caused by cracks, etc. of the second all-solid-state secondary battery.
[0301] Evaluation Example 2: XRD Analysis and SEM Analysis
[0302] By using CuKα radiation, X-ray diffraction (XRD) spectra were measured for bare Li2S used in Preparation Example 1, crushed Li2S, and the Li2S-LiI-AlI3-CNF composite prepared in Example 1. The measurement results are shown in the following Table 2. The Li2S grain size and lattice constant are derived from the first peak of the (111) crystal plane of Li2S appearing in the XRD spectrum.
[0303] The milled Li2S was prepared by milling under the same conditions except that the 40:20 weight ratio mixture of Li2S and the first mixture (1:1 molar ratio mixture of LiI and AlI3) in the first stage of Preparation Example 1 was changed to 50 parts by weight of Li2S. The second stage was not performed.
[0304] By using PSA using laser and SEM, the particle size of the composite (ie, D50 particle size) and the Li2S particle size of the composite were measured for bare Li2S used in Preparation Example 1, pulverized Li2S, and the Li2S-LiI-AlI3-CNF composite prepared in Preparation Example 1. The measurement results are shown in Table 2 below.
[0305] [Table 2]
[0306]
[0307] As shown in Table 2, the Li2S particle size and Li2S crystallite size in the Li2S-LiI-AlI3-CNF composite of Preparation Example 1 are significantly reduced compared to bare Li2S.
[0308] Although not shown in Table 2, the Li2S lattice constant of the Li2S-LiI-AlI3-CNF composite of Preparation Example 1 is larger than that of bare Li2S.
[0309] Compared with the lattice constant of bare Li2S, the increase in the Li2S lattice constant of the Li2S-LiI-AlI3-CNF composite is determined to be caused by the dissolution of LiI and / or AlI3 in the Li2S crystal. In some embodiments, it is confirmed that Li2S, LiI and / or AlI3 form a solid solution in the Li2S-LiI-AlI3-CNF composite. Although not shown in Table 2, the particle size of the Li2S-LiI-AlI3-CNF composite prepared in Preparation Example 1 is about 5 μm.
[0310] Evaluation Example 3: Charge / Discharge Test
[0311] The charge / discharge characteristics of the all-solid secondary batteries manufactured in Examples 1 to 9 and Comparative Example 1 were evaluated by the following charge / discharge test. The all-solid secondary batteries were introduced into a thermostatic bath having a temperature of 45° C. to perform the charge / discharge test.
[0312] In the first cycle, the all-solid-state secondary battery was charged at a constant current of 0.1C for 12.5 hours until the battery voltage reached a range of 2.5 V to 2.8 V. Subsequently, the all-solid-state secondary battery was discharged at a constant current of 0.1C for 12.5 hours until the battery voltage reached 0.5V.
[0313] In the second cycle, the all-solid-state secondary battery was charged at a constant current of 0.33C for 12.5 hours until the battery voltage reached a range of 2.5 V to 2.8 V. Subsequently, the all-solid-state secondary battery was discharged at a constant current of 0.33C for 12.5 hours until the battery voltage reached 0.5V.
[0314] In the third cycle, the all-solid-state secondary battery was charged at a constant current of 1.0 C for 12.5 hours until the battery voltage reached a range of 2.5 V to 2.8 V. Subsequently, the all-solid-state secondary battery was discharged at a constant current of 1.0 C for 12.5 hours until the battery voltage reached 0.5 V.
[0315] The charge / discharge characteristics of the all-solid-state secondary battery manufactured in Comparative Example 2 were evaluated by the following charge / discharge test. The all-solid-state secondary battery was introduced into a thermostatic bath having a temperature of 45° C. to perform the charge / discharge test.
[0316] In the first cycle, the all-solid-state secondary battery was charged at a constant current of 0.1C for 12.5 hours until the battery voltage reached a range of 3.9 V to 4.25 V. Subsequently, the all-solid-state secondary battery was discharged at a constant current of 0.1C for 12.5 hours until the battery voltage reached 2.5 V.
[0317] In the second cycle, the all-solid-state secondary battery was charged at a constant current of 0.33C for 12.5 hours until the battery voltage reached a range of 3.9 V to 4.25 V. Subsequently, the all-solid-state secondary battery was discharged at a constant current of 0.33C for 12.5 hours until the battery voltage reached 2.5V.
[0318] In the third cycle, the all-solid-state secondary battery was charged at a constant current of 1.0 C for 12.5 hours until the battery voltage reached a range of 3.9 V to 4.25 V. Subsequently, the all-solid-state secondary battery was discharged at a constant current of 1.0 C for 12.5 hours until the battery voltage reached 2.5 V.
[0319] During the charge / discharge process up to the third cycle, whether a short circuit occurred, the initial discharge capacity, and the high rate characteristics are shown in Table 3 below.
[0320] If a short circuit occurs before the first cycle is completed, ○ is used to indicate whether a short circuit occurs. If a short circuit occurs in the second cycle, △ is used to indicate whether a short circuit occurs. If a short circuit does not occur until the third cycle is completed, × is used to indicate whether a short circuit occurs.
[0321] [Table 3]
[0322]
[0323] As shown in Table 3, compared with the all-solid-state secondary battery of Comparative Example 1, the all-solid-state secondary batteries of Examples 1 to 9 exhibited improved cycle characteristics.
[0324] Evaluation Example 4: High-temperature life characteristics test
[0325] The charge / discharge characteristics of the all-solid secondary batteries manufactured in Examples 1 to 9 and Reference Example 1 were evaluated by the following charge / discharge test. The all-solid secondary batteries were introduced into a thermostatic bath having a temperature of 45° C. to perform the charge / discharge test.
[0326] In the first cycle, the all-solid-state secondary battery is 0.6 mA / cm 2 The all-solid-state secondary battery was charged at a constant current of 100 mA / cm for 12.5 hours until the battery voltage reached a range of 2.5 V to 2.8 V. Subsequently, the all-solid-state secondary battery was charged at 0.6 mA / cm 2 The battery was discharged at a constant current for 12.5 hours until the battery voltage reached 0.5V.
[0327] The charge / discharge characteristics of the all-solid-state secondary battery manufactured in Comparative Example 2 were evaluated by the following charge / discharge test. The all-solid-state secondary battery was introduced into a thermostatic bath having a temperature of 45° C. to perform the charge / discharge test.
[0328] In the first cycle, the all-solid-state secondary battery is 0.6 mA / cm 2 The all-solid-state secondary battery was then charged at a constant current of 0.6 mA / cm for 12.5 hours until the battery voltage reached a range of 3.9 V to 4.25 V. 2 The battery was discharged at a constant current for 12.5 hours until the battery voltage reached 2.5V.
[0329] The discharge capacity of the first cycle was taken as the standard capacity. From the second cycle onwards, charging and discharging were performed up to 1100 cycles under the same conditions as the first cycle. The measurement results are shown in Table 4 below.
[0330] As the number of cycles required for the discharge capacity to decrease to 95% of the standard capacity from the second cycle increases, it is considered to have excellent life characteristics.
[0331] In the all-solid-state secondary battery of Comparative Example 1, a short circuit occurred before the first cycle was completed, and thus the lifespan characteristics could not be measured.
[0332] [Table 4]
[0333]
[0334]
[0335] As shown in Table 4, compared with the all-solid-state secondary battery of Comparative Example 2, the lifespan characteristics of the all-solid-state secondary batteries of Examples 1 to 9 are improved.
[0336] Since the all-solid-state secondary battery of Example 6 includes the Li2S-C-LiI composite as the positive electrode active material, its lifespan characteristics are further improved compared with Example 1 including the Li2S-CNF composite and Example 4 including the Li2S-C-Li6PS5Cl composite.
[0337] It was determined that the lifespan characteristics of the all-solid-state secondary batteries of Examples 1 to 6 including Li2S were improved compared to the all-solid-state secondary battery of Comparative Example 2 including an oxide-based positive active material due to reduced volume change during charge / discharge.
[0338] It is determined that since the all-solid-state secondary batteries of Examples 7 and 8 have a dual-cell structure in which components are symmetrically arranged, the volume change during charging / discharging is effectively reduced, and thus the all-solid-state secondary batteries of Examples 7 and 8 have improved life characteristics compared to the all-solid-state secondary batteries of Examples 1 to 4 having a single-cell structure.
[0339] It was confirmed that the all-solid-state secondary batteries of Examples 1, 2, and 4 included the flame-retardant inactive member and thus had improved lifespan characteristics compared to Example 3 including the non-flame-retardant inactive member.
[0340] It was determined that the second inactive member was additionally provided on the negative electrode current collector to effectively relieve the stress of the negative electrode layer on which the volume change was accumulated, so that the all-solid-state secondary battery of Example 8 had improved life characteristics compared with the all-solid-state secondary battery of Example 7. It was determined that, for the same reason, the all-solid-state secondary battery of Example 2 had improved life characteristics compared with Examples 1, 3, and 4. By using carbon loaded with silver particles, the all-solid-state secondary battery of Example 5 was determined to have improved life characteristics compared with Example 2 including a simple mixture of silver particles and carbon particles.
[0341] Although not shown in Table 4, the life characteristics of the all-solid-state secondary battery of Reference Example 1 are deteriorated compared to the all-solid-state secondary battery of Example 9.
[0342] As described above, the all-solid-state secondary battery according to the presented embodiments may be applied to various portable devices or vehicles.
[0343] Although the embodiments have been described in detail with reference to the accompanying drawings, the inventive concept is not limited to the embodiments. It is obvious to those skilled in the art that various changes and modifications are conceivable within the scope of the technical concept described in the claims, and these changes and modifications are understood to naturally belong to the technical scope of the inventive concept.
[0344] According to one aspect, according to an all-solid-state secondary battery having a novel structure, an all-solid-state secondary battery in which a short circuit is suppressed and cycle characteristics are improved can be provided.
[0345] It should be understood that the embodiments described herein should be considered in a descriptive sense only and not for purposes of limitation. The description of features or aspects within each embodiment should generally be considered applicable to other similar features or aspects in other embodiments. Although one or more embodiments have been described with reference to the drawings, it will be understood by those of ordinary skill in the art that various changes in form and detail may be made therein without departing from the spirit and scope of the disclosure as defined by the appended claims.
Claims
1. An all-solid-state secondary battery, comprising: positive electrode layer; Negative electrode layer; A solid electrolyte layer, disposed between the positive electrode layer and the negative electrode layer; as well as A first inactive member is disposed on a side surface of the positive electrode layer, The positive electrode layer includes a positive electrode current collector and a positive electrode active material layer disposed on one side or both sides of the positive electrode current collector. The positive electrode active material layer includes a lithium-containing sulfide-based positive electrode active material, and The lithium-containing sulfide positive electrode active material includes Li2S, a composite containing Li2S, or a combination thereof. The negative electrode layer includes a negative electrode current collector and a first negative electrode active material layer disposed on one side of the negative electrode current collector. The ratio of the initial charge capacity of the first negative electrode active material layer to the initial charge capacity of the positive electrode active material layer is in the range of 0.005 to 0.45, The initial charge capacity of the positive electrode active material layer is charged from the first open circuit voltage to the Li / Li + The maximum charging voltage is determined by The initial charge capacity of the first negative electrode active material layer is charged from the second open circuit voltage to the Li / Li + The voltage of 0.01V is determined.
2. The all-solid-state secondary battery according to claim 1, wherein: The Li2S-containing composite includes: a composite of Li2S and a conductive material; a composite of Li2S, a solid electrolyte and a conductive material; a composite of Li2S and a solid electrolyte; a composite of Li2S, a lithium salt and a conductive material; a composite of Li2S and a lithium salt; a composite of Li2S and a metal carbide; a composite of Li2S, a metal carbide and a conductive material; a composite of Li2S and a metal nitride; a composite of Li2S, a metal nitride and a conductive material; or a combination thereof.
3. The all-solid-state secondary battery according to claim 1, wherein: The Li2S-containing composite includes: a composite of Li2S and a lithium salt; a composite of Li2S, a lithium salt and a conductive material; a composite of Li2S and a metal halide; a composite of Li2S, a metal halide and a conductive material; a composite of Li2S, a lithium salt and a metal halide; a composite of Li2S, a lithium salt, a metal halide and a conductive material; or a combination thereof. Wherein, the composite of Li2S and lithium salt is composed of Li2S-Li a X1 b represents, where 1≤a≤5 and 1≤b≤5, The composite of Li2S, lithium salt and conductive material is composed of Li2S-Li a X1 b -C means, where 1≤a≤5 and 1≤b≤5, The Li2S and metal halide complex is composed of Li2S-M c X2 d represents, where 1≤c≤5 and 1≤d≤5, The composite of Li2S, metal halide and conductive material is composed of Li2S-M c X2 d -C means, where 1≤c≤5 and 1≤d≤5, The complex of Li2S, lithium salt and metal halide is composed of Li2S-Li a X1 b -M c X2 d , means, where 1≤a≤5, 1≤b≤5, 1≤c≤5 and 1≤d≤5, The composite of Li2S, lithium salt, metal halide and conductive material is composed of Li2S-Li a X1 b -M c X2 d -C represents, wherein 1≤a≤5, 1≤b≤5, 1≤c≤5, 1≤d≤5, X1 is I, Br, Cl, F, H, O, Se, Te, N, P, As, Sb, Al, B, OCl, PF6, BF4, SbF6, AsF6, ClO4, AlO2, AlCl4, NO3, CO3, BH4, SO4, BO3, PO4, NCl, NCl2, BN2 or a combination thereof, M is at least one metal selected from Group II to Group XV of the periodic table, and X2 is I, Br, Cl, F or a combination thereof.
4. The all-solid-state secondary battery according to claim 3, wherein: The Li2S-containing composite includes: a solid solution of Li2S and a lithium salt; a solid solution of Li2S and a metal halide; a solid solution of Li2S, a lithium salt and a metal halide; or a combination thereof.
5. The all-solid-state secondary battery according to claim 3, wherein: The lithium salt is a binary compound or a ternary compound, Wherein, the binary compound comprises LiI, LiBr, LiCl, LiF, LiH, Li2O, Li2Se, Li2Te, Li3N, Li3P, Li3As, Li3Sb, Li3Al2, Li3B or a combination thereof, and The ternary compound includes Li3OCl, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiNO3, Li2CO3, LiBH4, Li2SO4, Li3BO3, Li3PO4, Li4NCl, Li5NCl2, Li3BN2 or a combination thereof.
6. The all-solid-state secondary battery according to claim 3, wherein: The metal halide includes at least one metal selected from Al, Mg, Ti, Sn, As, Sb, Nb, Sc, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn and Se, and includes AlF3, AlCl3, AlBr3, AlI3, MgF2, MgCl2, MgBr2, MgI2, TiF4, TiCl4, TiBr4, TiI4, SnF4, SnCl4, SnBr4, SnI4, AsF4, AsCl4, AsBr4, AsI4, SbF4, SbCl4, SbBr4, SbI4 or a combination thereof.
7. The all-solid-state secondary battery according to claim 1, wherein: The Li2S-containing composite comprises a composite of Li2S, a lithium salt, a metal halide and a conductive material, and The Li2S-containing composite includes 40 to 80 parts by weight of Li2S, 1 to 40 parts by weight of a combination of a lithium salt and a metal halide, and 1 to 20 parts by weight of a conductive material, relative to 100 parts by weight of the composite of Li2S, a lithium salt, a metal halide, and a conductive material. wherein the molar ratio of the lithium salt to the metal halide is in the range of 3:1 to 1:3, and The content of Li2S in the positive electrode active material layer is 40 wt% or more.
8. The all-solid-state secondary battery according to claim 1, wherein: The first inactive member surrounds the side of the positive electrode layer and is in contact with the solid electrolyte layer, The first inactive member extends from one side of the positive electrode layer along the surface of the solid electrolyte layer to an end of the solid electrolyte layer, The area of the positive electrode layer is smaller than the area of the solid electrolyte layer in contact with the positive electrode layer, the first inactive member is provided to surround the side of the positive electrode layer and to compensate for the difference between the area of the positive electrode layer and the area of the solid electrolyte layer, The thickness of the first inactive member is greater than the thickness of the first negative electrode active material layer. The thickness of the first negative electrode active material layer is 50% or less of the thickness of the first inactive member, and The negative electrode collector does not have the negative electrode active material layer on the opposite side of the negative electrode collector.
9. The all-solid-state secondary battery according to claim 1, wherein: The first inactive member includes a flame retardant inactive member, and The flame retardant inactive component comprises a matrix and a filler, Wherein, the matrix includes a base material and a reinforcing material, The substrate comprises a first fiber material, The first fiber material is an insulating material and includes at least one selected from pulp fibers, insulating polymer fibers and ion-conductive polymer fibers, The reinforcing material comprises a second fiber material, The second fiber material is a flame retardant material and includes at least one selected from glass fiber and ceramic fiber. The filler is a hygroscopic agent and comprises a metal hydroxide, and The metal hydroxide includes at least one selected from Mg(OH)2, Fe(OH)3, Sb(OH)3, Sn(OH)4, TI(OH)3, Zr(OH)4 and Al(OH)3.
10. The all-solid-state secondary battery according to claim 1, wherein: The first negative electrode active material layer includes a negative electrode active material and a binder, and The negative electrode active material has a particle form and has an average particle size of 4 μm or less.
11. The all-solid-state secondary battery according to claim 10, wherein: The negative electrode active material includes at least one selected from carbon-based negative electrode active materials and metal or metalloid negative electrode active materials. Wherein, the carbon-based negative electrode active material includes amorphous carbon, crystalline carbon, porous carbon or a combination thereof, and The metal or metalloid negative electrode active material includes gold, platinum, palladium, silicon, silver, aluminum, bismuth, tin, zinc or a combination thereof.
12. The all-solid-state secondary battery according to claim 10, wherein: The negative electrode active material includes a mixture of first particles composed of amorphous carbon and second particles composed of metal or metalloid, and Wherein, the content of the second particles is in the range of 1 wt % to 60 wt % relative to the total weight of the mixture.
13. The all-solid-state secondary battery according to claim 1, wherein: The first negative electrode active material layer further includes a solid electrolyte.
14. The all-solid-state secondary battery according to claim 1, wherein: The negative electrode active material includes a carbon carrier and a metal negative electrode active material supported on the carbon carrier. The metal negative electrode active material comprises a metal, a metal oxide, a composite of a metal and a metal oxide, or a combination thereof, and has a particle form and a particle size of 1 nm to 200 nm. The carbon-based carrier is in the form of particles and has a particle size of 10 nm to 2 μm, and The all-solid-state secondary battery further includes a second negative electrode active material layer, which is disposed between the negative electrode current collector and the first negative electrode active material layer after the all-solid-state secondary battery is charged. Wherein, the second negative electrode active material layer is a metal layer, and The metal layer includes lithium or a lithium alloy.
15. The all-solid-state secondary battery according to claim 1, further comprising a second inactive member disposed on an opposite side of the negative electrode current collector, in, The second inactive component includes a conductive flame retardant inactive component.
16. The all-solid-state secondary battery according to claim 15, wherein: The Young's modulus of the second inactive member is smaller than the Young's modulus of the negative electrode current collector, the Young's modulus of the second inactive member is 100 MPa or less, The second inactive member has a thickness greater than that of the first negative electrode active material layer, and The thickness of the first negative electrode active material layer is 50% or less of the thickness of the second inactive member.
17. The all-solid-state secondary battery according to claim 1, wherein: The volume expansion rate of the all-solid-state secondary battery after charging is 15% or less, and The energy density of the all-solid-state secondary battery is in the range of 500Wh / L to 900Wh / L or 350Wh / kg to 600Wh / kg.
18. The all-solid-state secondary battery according to claim 1, wherein: The solid electrolyte layer includes an electrolyte, Wherein, the electrolyte comprises a solid electrolyte, a gel electrolyte or a combination thereof, The solid electrolyte includes a sulfide solid electrolyte, an oxide solid electrolyte, a polymer solid electrolyte or a combination thereof. The gel electrolyte includes a polymer gel electrolyte, and The solid electrolyte layer is impermeable to lithium polysulfide.
19. The all-solid-state secondary battery according to claim 1, wherein the sulfide-based solid electrolyte is at least one selected from the following materials: Li2S-P2S5; Li2S-P2S5-LiX, wherein: X is a halogen element; Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S-P2S5-Z m S n , wherein m and n are positive numbers, and Z is at least one selected from Ge, Zn and Ga; Li2S-GeS2; Li2S-SiS2-Li3PO4; Li2S-SiS2-Li p MO q , wherein p and q are positive numbers, and M is at least one selected from P, Si, Ge, B, Al, Ga and In; Li 7-x PS 6-x Cl x , where 0≤x≤2; Li 7- x PS 6-x Br x , where 0≤x≤2; and Li 7-x PS 6-x I x , where 0≤x≤2, and The sulfide-based solid electrolyte is an argyrodite-type solid electrolyte including at least one selected from Li6PS5Cl, Li6PS5Br and Li6PS5I, and The density of the argyrodite-type solid electrolyte is in the range of 1.5 g / cc to 2.0 g / cc.
20. The all-solid-state secondary battery according to claim 1, wherein: At least one of the positive electrode current collector and the negative electrode current collector includes a base film and a metal layer disposed on one side or both sides of the base film, Wherein, the base film includes a polymer, the polymer includes polyethylene terephthalate, polyethylene, polypropylene, polybutylene terephthalate, polyimide or a combination thereof, and the metal layer includes indium, copper, magnesium, stainless steel, titanium, iron, cobalt, nickel, zinc, aluminum, germanium, lithium or an alloy thereof.