Rechargeable lithium battery

By controlling the volume of the cylindrical tank and electrolyte additives, the problems of metal dissolution and increased resistance of rechargeable lithium batteries at high temperatures are solved, which extends the cycle life and improves the high-temperature characteristics.

CN119092819APending Publication Date: 2024-12-06SAMSUNG SDI CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410424946.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-06-05
Filing Date
2024-04-10
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Rechargeable lithium batteries have problems with metal dissolution, increased resistance and reduced cycle life at high temperatures, especially when the cylindrical tank volume and electrolyte additive content are incorrect.

Method used

By controlling the volume of the cylindrical tank and the type and content of electrolyte additives, metal dissolution and increase resistance are suppressed and cycle life is improved. Specific measures include the use of specific non-aqueous organic solvents, lithium salts and additives in the electrolyte, limiting the content of the second additive to less than 5 wt%, to stabilize the electrode and reduce side reactions.

Benefits of technology

It effectively suppresses metal dissolution and increase resistance, extends the cycle life of rechargeable lithium batteries, and improves high-temperature characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092819A_ABST
    Figure CN119092819A_ABST
Patent Text Reader

Abstract

Some example embodiments of the present disclosure provide a rechargeable lithium battery comprising: a cylindrical can; an electrode assembly accommodated in the cylindrical can; and an electrolyte impregnated in the electrode assembly, wherein the volume of the cylindrical can is controlled and the type (or species) and content of an electrolyte additive are limited. The volume of the cylindrical can and the type (or species) and content of electrolyte additives are described in detail in the specification.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of the present disclosure relate to rechargeable lithium batteries. Background Art

[0002] Rechargeable lithium batteries are rechargeable and have three times or more times higher energy density per unit weight than existing lead batteries, nickel-cadmium batteries, nickel-metal hydride batteries, nickel-zinc batteries, etc., and can be charged at a high speed, so they are commercially manufactured for use in laptop computers, cellular phones, power tools, electric bicycles, etc., and research on improving additional energy density has been actively conducted.

[0003] A rechargeable lithium battery may be manufactured by injecting an electrolyte into a battery cell including a positive electrode including a positive electrode active material capable of intercalating / deintercalating lithium and a negative electrode including a negative electrode active material capable of intercalating / deintercalating lithium.

[0004] One of the recent development directions of rechargeable lithium batteries is to improve high temperature characteristics. In general, rechargeable lithium batteries may have problems such as metal dissolution at high temperatures, increased resistance, and / or reduced cycle life.

[0005] However, if the battery case housing electrode assembly is a cylindrical can, the above problem may become more serious depending on the volume of the cylindrical can. Summary of the invention

[0006] Some example embodiments of the present disclosure reduce metal dissolution at high temperatures, resistance increase, and / or cycle life reduction in a rechargeable lithium battery using a cylindrical can.

[0007] Some example embodiments provide a rechargeable lithium battery, including: a cylindrical can; an electrode assembly contained in the cylindrical can; and an electrolyte impregnated in the electrode assembly, wherein the volume of the cylindrical can is controlled and the type (or kind) and content of the electrolyte additive are limited. The volume of the cylindrical can and the type (or kind) and content of the electrolyte additive will be described in more detail herein below.

[0008] The rechargeable lithium battery of some example embodiments can inhibit or reduce metal dissolution and inhibit or reduce the increase in resistance at high temperatures, and / or ensure or improve the cycle life of the rechargeable lithium battery by controlling the volume of the cylindrical can and limiting the type (or kind) and content of electrolyte additives. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] The accompanying drawings, together with the specification, illustrate embodiments of the presently disclosed subject matter, and, together with the description, serve to explain principles of embodiments of the presently disclosed subject matter.

[0010] Figure 1is a schematic diagram illustrating a rechargeable lithium battery according to some example embodiments of the present disclosure.

[0011] Description of Reference Numerals

[0012] 100: Rechargeable lithium battery

[0013] 112: Negative electrode

[0014] 113: Diaphragm

[0015] 114: Positive electrode

[0016] 120: Battery housing

[0017] 140: Sealing member DETAILED DESCRIPTION

[0018] Hereinafter, a rechargeable lithium battery according to some exemplary embodiments of the present disclosure will be described in more detail with reference to the accompanying drawings. However, these embodiments are examples, and the present disclosure is not limited thereto and is defined by the scope of the appended claims and their equivalents.

[0019] As used herein, "substituted" means that the hydrogen of the compound is replaced by a substituent selected from the following: deuterium, a halogen atom, a hydroxyl group, an amino group, a substituted or unsubstituted C1-C30 amine group, a nitro group, a substituted or unsubstituted C1-C40 silyl group, a C1-C30 alkyl group, a C1-C10 alkylsilyl group, a C6-C30 arylsilyl group, a C3-C30 cycloalkyl group, a C3-C30 heterocycloalkyl group, a C6-C30 aryl group, a C2-C30 heteroaryl group, a C1-C20 alkoxy group, a C1-C10 fluoroalkyl group, a cyano group and / or a combination thereof.

[0020] Some example embodiments provide a rechargeable lithium battery including: a cylindrical can; an electrode assembly accommodated in the cylindrical can; and an electrolyte impregnated in the electrode assembly.

[0021] The rechargeable lithium battery of some example embodiments can inhibit or reduce metal dissolution and inhibit or reduce the increase of resistance at high temperature and / or ensure or improve the cycle life of the rechargeable lithium battery by controlling the volume of the cylindrical can and limiting the type (or kind) and content of the electrolyte additive. Herein, the term "content" and the term "amount" are used synonymously.

[0022] First, the volume of the cylindrical tank is described as follows.

[0023] The cylindrical tank may have a diameter greater than about 15 cm 3 If the volume of the cylindrical tank is significantly less than about 15 cm 3, even if the type (or kind) and content of the electrolyte additive are changed, the amount of metal dissolved at high temperature does not change significantly. If the volume of the cylindrical tank exceeds about 15cm 3 , the amount of metal dissolved varies with the type (or kind) and content of the electrolyte additive. For example, in some embodiments, the cylindrical tank may have a diameter greater than or equal to about 16 cm 3 A volume of greater than or equal to about 1.8 cm, a diameter of greater than or equal to about 6.5 cm, and a height of greater than or equal to about 6.5 cm.

[0024] In some embodiments, the volume of the cylindrical tank may be less than or equal to about 296 cm 3 , the diameter may be less than or equal to about 5.6 cm, and the height may be less than or equal to about 12.0 cm. If the volume of the cylindrical tank exceeds about 296 cm 3 , regardless of the type (or kind) and content of the electrolyte additive, the amount of metal dissolution at high temperature may excessively increase, and the resistance may increase and the cycle life of the rechargeable lithium battery may decrease. In some embodiments, if the volume of the cylindrical can is less than or equal to about 296 cm 3 , the amount of metal dissolved varies with the type (or kind) and content of the electrolyte additive. For example, in some embodiments, the cylindrical tank may have a diameter of less than or equal to about 133 cm 3 A volume of less than or equal to about 4.6 cm in diameter and a height of less than or equal to about 8.0 cm.

[0025] A description of the electrolyte including the above two types (or categories) of additives is as follows.

[0026] The electrolyte includes a non-aqueous organic solvent, a lithium salt, a first additive, and a second additive, wherein the first additive includes a compound represented by Chemical Formula 1; the second additive includes a compound represented by Chemical Formula 2, a derivative thereof, and / or an adduct thereof; and based on 100 wt % of the electrolyte, the content of the second additive is less than about 5 wt %:

[0027] Chemical formula 1

[0028]

[0029] Wherein, in Chemical Formula 1, X1 is a halogen atom; Y1 and Y2 are each independently O or S; R1 and R2 are each independently H, a halogen atom, a substituted or unsubstituted C1-C10 alkyl group, a vinyl group, a substituted or unsubstituted C6-C10 aryl group, or a substituted or unsubstituted C2-C10 heteroaryl group containing a hetero atom of N, O or P;

[0030] Chemical formula 2

[0031]

[0032] In Chemical Formula 2, Z is N or CH.

[0033] The first additive (the compound represented by Chemical Formula 1) can stabilize the lithium salt to inhibit or reduce the side reaction of the electrolyte, and the second additive (the compound represented by Chemical Formula 2) can be absorbed on the surface of the positive electrode by the coordination of the lone pair electrons of the nitrogen atom in the additive structure with the transition metal to stabilize the positive electrode, and in some embodiments, inhibit or reduce the side reaction caused by the precipitation of the transition metal to improve the cycle life and high temperature characteristics of the rechargeable lithium battery.

[0034] However, when two types (or kinds) of additives are used simultaneously (e.g., synchronously), the content of the second additive in the electrolyte needs to be controlled to be less than about 5wt%. If the content of the second additive in the electrolyte is greater than or equal to about 5wt%, the resistance may increase, which may cause a problem in which the cycle life of the rechargeable lithium battery is reduced at high temperatures. However, if the content of the second additive in the electrolyte is less than about 5wt%, the cycle life can be ensured or improved while suppressing or reducing the increase in resistance of the rechargeable lithium battery at high temperatures.

[0035] Accordingly, when two types (or kinds) of additives are used simultaneously (e.g., synchronously) and the content of the second additive in the electrolyte is controlled to be less than about 5wt%, the high temperature characteristics of the rechargeable lithium battery are improved.

[0036] In some embodiments, the first additive includes a compound represented by Chemical Formula 1:

[0037] Chemical formula 1

[0038]

[0039] The description of chemical formula 1 is as follows:

[0040] X1 may be a halogen atom, and may be, for example, a fluorine atom.

[0041] Y1 and Y2 may each independently be O or S, and, for example, both may be O.

[0042] R1 and R2 are each independently H, a halogen atom, a substituted or unsubstituted C1-C10 alkyl group, a vinyl group, a substituted or unsubstituted C6-C10 aryl group, or a substituted or unsubstituted C2-C10 heteroaryl group including a heteroatom of N, O or P.

[0043] For example, the compound represented by Chemical Formula 1 can be represented by Chemical Formula 1-1:

[0044] Chemical formula 1-1

[0045]

[0046] In Chemical Formula 1-1, Z1 and Z2 may each independently be a substituted or unsubstituted C1 to C5 alkylene group. For example, Z1 may be *-CH2-*, and Z2 may be *-CHCH3-*, * indicating a binding site with an adjacent group.

[0047] A representative example of the first additive may be a compound represented by Chemical Formula 1-1-1:

[0048] Chemical formula 1-1-1

[0049]

[0050] Based on 100 wt % of the electrolyte, the content of the first additive may be greater than or equal to about 0.05 wt %, greater than or equal to about 0.1 wt %, or greater than or equal to about 0.5 wt %, and may be less than or equal to about 3 wt %, or less than or equal to about 2 wt %. Within this range, the effect of improving high temperature characteristics by the first additive may be significantly exhibited.

[0051] The second additive includes a compound represented by Chemical Formula 2, a derivative thereof, and / or an adduct thereof.

[0052] Chemical formula 2

[0053]

[0054] In Chemical Formula 2, Z is N or CH.

[0055] In Chemical Formula 2, when Z is N, the second additive may be a compound represented by Chemical Formula 2-1-1. In some embodiments, when Z in Chemical Formula 2 is CH, the second additive may be a compound represented by Chemical Formula 2-1-2.

[0056] The adduct of the compound represented by Chemical Formula 2 may include an adduct obtained by adding trimethylaluminum, sulfur dioxide, borate and / or hydrosilane to the compound represented by Chemical Formula 2. In some embodiments, the adduct of the compound represented by Chemical Formula 2 may be a compound represented by Chemical Formula 2-2 or Chemical Formula 2-3.

[0057] Chemical formula 2-2

[0058]

[0059] Chemical formula 2-3

[0060]

[0061] In the above Chemical Formula 2-2 and Chemical Formula 2-3, “arrow (→)” is an arrow drawn from the electron-donating atom side to the electron-receiving atom side, respectively, and means a coordinate bond.

[0062] R3 and R4 may each independently be trimethylaluminum or sulfur dioxide. Y3 to Y5 may each independently be O or S, and, for example, all of Y3 to Y5 may be O. Z1 may be B or SiH.

[0063] Representative examples of the second additive are as follows:

[0064] Chemical formula 2-1-1

[0065]

[0066] Chemical formula 2-1-2

[0067]

[0068] Chemical formula 2-2-1

[0069]

[0070] Chemical formula 2-2-2

[0071]

[0072] Chemical formula 2-3-1

[0073]

[0074] Chemical formula 2-3-2

[0075]

[0076] In 100 wt % of the electrolyte, the content of the second additive may be greater than or equal to about 0.05 wt %, greater than or equal to about 0.1 wt %, or greater than or equal to about 0.5 wt %, and may be less than or equal to about 3 wt %, or less than or equal to about 2 wt %. Within this range, the effect of improving high temperature characteristics by the second additive may be significantly exhibited.

[0077] In some embodiments, the weight ratio of the first additive to the second additive may be about 1: 0.1 to about 1: 3. Thus, when the second additive is used in an amount of about 0.1 to about 1.3 parts by weight based on 1 part by weight of the first additive, the synergistic effect of the two types (or kinds) of additives can be further increased.

[0078] The nonaqueous organic solvent serves as a medium for transporting ions participating in the electrochemical reaction of the battery.

[0079] The non-aqueous organic solvent may include a carbonate solvent, an ester solvent, an ether solvent, a ketone solvent, an alcohol solvent and / or an aprotic solvent.

[0080] Carbonate solvents may include ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. Ester solvents may include methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, decanoic acid lactone, mevalonate lactone, caprolactone, etc. Ether solvents may include dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc. Ketone solvents may include cyclohexanone, etc. Alcohol solvents may include ethanol, isopropanol, etc., and examples of aprotic solvents include nitriles (such as R-CN, where R is a C2-C20 straight chain hydrocarbon group, a branched hydrocarbon group, or a cyclic hydrocarbon group, and may include a double bond, an aromatic ring, or an ether bond), amides (such as dimethylformamide), dioxolanes (such as 1,3-dioxolane), sulfolane, etc.

[0081] A single non-aqueous organic solvent may be used or one or more thereof may be used in combination, and when one or more are used in combination, the mixing ratio may be appropriately or suitably adjusted according to appropriate or desired battery performance, which should be fully understood by those skilled in the art after reading this disclosure.

[0082] The carbonate solvent is prepared by mixing a cyclic carbonate and a chain carbonate together. The cyclic carbonate and the chain carbonate are mixed together in a volume ratio of about 5:95 to about 50:50. When the mixture is used as an electrolyte, it can have enhanced performance.

[0083] In some embodiments, ethylene carbonate (EC) may be used as the cyclic carbonate, and ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) may be used as the chain carbonate.

[0084] In some embodiments, the non-aqueous organic solvent may include a carbonate-based solvent in which ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) are mixed together. For example, the carbonate-based solvent may include ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) mixed together in a volume ratio of EC:EMC:DMC=about 1:0.5:5 to about 5:3:10, which may improve the performance of the electrolyte.

[0085] The nonaqueous organic solvent may further include an aromatic hydrocarbon solvent in addition to the carbonate-based solvent. The carbonate-based solvent and the aromatic hydrocarbon solvent may be mixed together in a volume ratio of about 1:1 to about 30:1.

[0086] In order to improve the battery cycle life, the electrolyte may further include vinylene carbonate, vinyl ethylene carbonate and / or an ethylene carbonate-based compound represented by Chemical Formula 3 as an additive for improving the cycle life.

[0087] Chemical formula 3

[0088]

[0089] In chemical formula 3, R 207 and R 208 are the same or different and are selected from hydrogen, halogen atoms, cyano (CN), nitro (NO2) and C1-C5 fluoroalkyl, provided that R 207 and R 208 At least one of them is a halogen atom, a cyano group (CN), a nitro group (NO2) or a C1-C5 fluoroalkyl group, and R 207 and R 208 Not simultaneously (eg, synchronously) hydrogen.

[0090] Examples of ethylene carbonate compounds include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, or fluoroethylene carbonate. The amount of the additive for improving the cycle life can be used within an appropriate or suitable range.

[0091] The lithium salt dissolved in the non-aqueous organic solvent supplies lithium ions in the battery, ensures the basic operation of the rechargeable lithium battery, and improves the transport of lithium ions between the positive electrode and the negative electrode. Examples of lithium salts include at least one selected from the following: LiPF6, LiBF4, LiDFOP, LiDFOB, LiPO2F2, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide: LiFSI), LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1SO2) (wherein x and y are natural numbers, such as integers of 1 to 20), LiCl, LiI, and LiB(C2O4)2 (lithium bis(oxalato)borate: LiBOB). The lithium salt may be used at a concentration in the range of about 0.1 M to about 2.0 M. When the lithium salt is included in the above concentration range, the electrolyte may have excellent performance and lithium ion mobility due to appropriate or optimal electrolyte conductivity and viscosity.

[0092] The positive electrode includes a positive electrode current collector and a positive electrode active material layer on the positive electrode current collector, and the positive electrode active material layer includes a positive electrode active material.

[0093] The positive electrode active material may include a lithiated intercalation compound that reversibly intercalates and deintercalates lithium ions.

[0094] For example, at least one composite oxide of lithium and a metal of cobalt, manganese, nickel, or a combination thereof may be used.

[0095] A composite oxide having a coating on its surface can be used, or a mixture of a composite oxide and a composite oxide having a coating can be used. The coating may include a coating element compound selected from the following: an oxide of a coating element, a hydroxide of a coating element, an oxyhydroxide of a coating element, an oxycarbonate of a coating element, or a basic carbonate of a coating element. The compound used for the coating may be amorphous or crystalline. The coating element included in the coating may be Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The coating process may include any suitable process commonly used in the art, as long as it does not (or substantially does not) cause any side effects (e.g., any undesirable side effects) to the characteristics of the positive electrode active material (e.g., spraying, dipping), which will be obvious to those of ordinary skill in the art after reading this disclosure, so it is not necessary to describe it in detail here.

[0096] In some embodiments, the positive electrode active material may include a lithium nickel-based composite oxide represented by Chemical Formula A1:

[0097] Chemical formula A1

[0098] Li a1 Ni x1 M 1 y1 M 2 z1 O 2-b1 X b1 .

[0099] In chemical formula A1, 0.9 ≤ a1 ≤ 1.2, 0.7 ≤ x1 ≤ 1, 0 ≤ y1 ≤ 0.2, 0 ≤ z1 ≤ 0.2, 0.9 ≤ x1 + y1 + z1 ≤ 1.1, and 0 ≤ b1 ≤ 0.1; M 1 and M 2 are each independently one or more elements selected from Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sr, Ti, V, W, and Zr; and X is one or more elements selected from F, P, and S.

[0100] In chemical formula A1, 0.75 ≤ x1 ≤ 1, 0 ≤ y1 ≤ 0.18, and 0 ≤ z1 ≤ 0.18; 0.85 ≤ x1 ≤ 1, 0 ≤ y1 ≤ 0.15, and 0 ≤ z1 ≤ 0.15; or 0.9 ≤ x1 ≤ 1, 0 ≤ y1 ≤ 0.1, and 0 ≤ z1 ≤ 0.1.

[0101] For example, the positive electrode active material may include a lithium nickel-based composite oxide represented by chemical formula A2. The compound represented by chemical formula A2 may be referred to as a lithium nickel cobalt-based composite oxide:

[0102] Chemical formula A2

[0103] Li a2 Ni x2 Co y2 M 3 z2 O 2-b2 X b2 .

[0104] In chemical formula A2, 0.9 ≤ a2 ≤ 1.8, 0.7 ≤ x2 < 1, 0 < y2 ≤ 0.2, 0 ≤ z2 ≤ 0.2, 0.9 ≤ x2 + y2 + z2 ≤ 1.1, and 0 ≤ b2 ≤ 0.1, M 3 is one or more elements selected from Al, B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sr, Ti, V, W, and Zr, and X is one or more elements selected from F, P, and S.

[0105] In chemical formula A2, 0.75 ≤ x2 ≤ 0.99, 0 ≤ y2 ≤ 0.15, and 0 ≤ z2 ≤ 0.15; 0.85 ≤ x2 ≤ 0.99, 0.01 ≤ y2 ≤ 0.15, and 0.01 ≤ z2 ≤ 0.15; or 0.9 ≤ x2 ≤ 0.99, 0.01 ≤ y2 ≤ 0.1, and 0.01 ≤ z2 ≤ 0.1.

[0106] As an example, the positive electrode active material may include a lithium nickel-based composite oxide represented by Chemical Formula A3. The compound represented by Chemical Formula A3 may be referred to as a lithium nickel cobalt aluminum-based oxide or a lithium nickel cobalt manganese-based oxide.

[0107] Chemical formula A3

[0108] Li a3 Ni x3 Co y3 M 4 z3 M 5 w3 O 2-b3 X b3

[0109] In the chemical formula A3, 0.9≤a3≤1.8, 0.7≤x3≤0.98, 0.01≤y3≤0.19, 0.01≤z3≤0.19, 0≤w3≤0.19, 0.9≤x3+y3+z3+w3≤1.1, and 0≤b3≤0.1, M 4 is one or more elements selected from Al and Mn, M 5 is one or more elements selected from B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mo, Nb, Si, Sr, Ti, V, W and Zr, and X is one or more elements selected from F, P and S.

[0110] In chemical formula A3, 0.75≤x3≤0.98, 0≤y3≤0.16, 0≤z3≤0.16, and 0≤w3≤0.16; 0.85≤x3≤0.98, 0.01≤y3≤0.14, 0.01≤z3≤0.14, and 0≤w3≤0.14; or 0.9≤x3≤0.98, 0.01≤y3≤0.09, 0.01≤z3≤0.09, and 0≤w3≤0.09.

[0111] As an example, the positive electrode active material may include a lithium nickel-based composite oxide represented by Chemical Formula A4. The compound represented by Chemical Formula A4 may be referred to as a lithium nickel manganese-based oxide that does not contain cobalt.

[0112] Chemical formula A4

[0113] Li a4 Ni x4 Mn y4 M 6 z4 O 2-b4 X b4

[0114] In chemical formula A4, 0.9 ≤ a4 ≤ 1.8, 0.7 ≤ x4 < 1, 0 < y4 ≤ 0.2, 0 ≤ z4 ≤ 0.2, 0.9 ≤ x4 + y4 + z4 ≤ 1.1, and 0 ≤ b4 ≤ 0.1, M 6 is one or more elements selected from Al, B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mo, Nb, Si, Sr, Ti, V, W, and Zr, and X is one or more elements selected from F, P, and S.

[0115] In some exemplary embodiments of the positive electrode, based on the total weight of the positive electrode active material layer, the content of the positive electrode active material can be about 90 wt% to about 98 wt%, about 50 wt% to about 99 wt%, about 60 wt% to about 99 wt%, about 70 wt% to about 99 wt%, about 80 wt% to about 99 wt%, or about 90 wt% to about 99 wt%.

[0116] In some embodiments of the present disclosure, the positive electrode active material layer may optionally include a conductive material (e.g., a conductivity material) and a binder. In some embodiments, based on the total weight of the positive electrode active material layer, the respective contents of the conductive material and the binder can be about 1.0 wt% to about 5.0 wt%.

[0117] The conductive material is used to impart conductivity (e.g., electrical conductivity) to the negative electrode, and any suitable conductivity material can be used as the conductive material (e.g., a conductivity material), unless it causes chemical changes in the battery (e.g., undesirable changes in a rechargeable lithium battery). Examples of the conductive material can include carbonaceous materials (such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.); metallic materials (such as metal powders or metal fibers of copper, nickel, aluminum, silver, etc.); conductive polymers (such as polyphenylene derivatives); or mixtures thereof.

[0118] The binder improves the bonding characteristics of the positive electrode active material particles to each other and the bonding characteristics of the positive electrode active material particles to the positive electrode current collector, and examples thereof can be polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, a polymer containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc., but are not limited thereto.

[0119] The positive electrode current collector can include, but is not limited to, Al foil.

[0120] The negative electrode includes a negative electrode current collector and a negative electrode active material layer, and the negative electrode active material layer includes a negative electrode active material formed on the negative electrode current collector.

[0121] The negative electrode active material can be a material that can reversibly intercalate / deintercalate lithium ions, lithium metal, a lithium metal alloy, a material that can dope and undope lithium, and / or a transition metal oxide.

[0122] Materials that can reversibly intercalate / deintercalate lithium ions include carbon materials. The carbon materials can be any suitable carbon-based negative electrode active materials commonly used in rechargeable lithium batteries. Examples of the carbon materials include crystalline carbon, amorphous carbon, and combinations thereof. The crystalline carbon can be amorphous natural graphite and / or artificial graphite, and / or flaky, sheet-like, spherical, and / or fibrous natural graphite and / or artificial graphite. The amorphous carbon can be soft carbon, hard carbon, mesophase pitch carbonization products, calcined coke, etc.

[0123] The lithium metal alloy can include lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn.

[0124] Materials that can dope and undope lithium can include Si, SiO x (0 < x < 2), Si-Q alloys (where Q is selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements other than Si, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof), Sn, SnO2, Sn-R alloys (where R is an alkali metal, alkaline earth metal, Group 13 element, Group 14 element other than Sn, Group 15 element, Group 16 element, transition metal, rare earth element, or a combination thereof), etc. At least one of them can be mixed with SiO2.

[0125] The element Q and the element R can be selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn (the element R does not include Sn), In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.

[0126] The transition metal oxide can be vanadium oxide, lithium vanadium oxide, etc.

[0127] In some exemplary embodiments, the negative electrode active material can include at least one selected from graphite and Si composites.

[0128] The Si composite can include: a core including Si particles and amorphous carbon, and for example, the Si particles can include at least one selected from Si-C composites, SiO k (0 < k ≤ 2) and Si alloys.

[0129] For example, the Si—C composite may include: a core including Si particles and amorphous carbon.

[0130] The central portion of the core may include a hole, and a radius of the central portion may correspond to about 30% to about 50% of a radius of the Si composite.

[0131] The Si particles may have an average particle diameter of about 10 nm to about 200 nm.

[0132] As used herein, the average particle size (D50) may be a particle size of 50% by volume in a cumulative size distribution curve.

[0133] When the average particle diameter of the Si particles is within the above range, volume expansion occurring during charge and discharge can be suppressed or reduced, and disconnection of a conductive path due to particle pulverization during charge and discharge can be prevented or reduced.

[0134] The Si particles may be included in an amount of about 1 wt % to about 60 wt %, for example, about 3 wt % to about 60 wt %, based on the total weight of the Si composite.

[0135] The central portion may not include amorphous carbon, but amorphous carbon may exist only on the surface portion of the negative electrode active material.

[0136] Herein, the surface portion indicates a region from the central portion of the negative electrode active material (eg, a region just outside the central portion) to the outermost surface of the negative electrode active material.

[0137] In some embodiments, the Si particles are included substantially uniformly throughout the negative electrode active material, for example, the Si particles are present in a substantially uniform concentration in the central portion and the surface portion of the negative electrode active material.

[0138] The amorphous carbon may be soft carbon, hard carbon, a mesophase pitch carbonization product, calcined coke, or a combination thereof.

[0139] The negative electrode active material may further include crystalline carbon.

[0140] When the negative electrode active material includes both Si composite and crystalline carbon, the Si composite and crystalline carbon may be included in the form of a mixture, and in some embodiments, the Si composite and crystalline carbon may be included in a weight ratio of about 1:99 to about 50:50. In some embodiments, the Si composite and crystalline carbon may be included in a weight ratio of about 3:97 to about 20:80 or about 5:95 to about 20:80.

[0141] The crystalline carbon may be, for example, graphite, and may be, for example, natural graphite, artificial graphite, or a mixture thereof.

[0142] The crystalline carbon may have an average particle size of about 5 μm to about 30 μm.

[0143] The amorphous carbon precursor may include coal-based pitch, mesophase pitch, petroleum-based pitch, coal-based oil, petroleum-based heavy oil, and / or a polymer resin (such as a phenol resin, a furan resin, and / or a polyimide resin).

[0144] In the negative electrode active material layer, the negative electrode active material may be included in an amount of about 95 wt % to about 99 wt % based on the total weight of the negative electrode active material layer.

[0145] In some example embodiments, the negative electrode active material layer may further include a binder, and may optionally include a conductive material (e.g., an electrically conductive material). In the negative electrode active material layer, the amount of the binder may be about 1 wt% to about 5 wt% based on the total weight of the negative electrode active material layer. When the negative electrode active material layer further includes a conductive material, the negative electrode active material layer may include about 90 wt% to about 98 wt% of the negative electrode active material, about 1 wt% to about 5 wt% of the binder, and about 1 wt% to about 5 wt% of the conductive material.

[0146] The binder improves the binding properties between the negative electrode active material particles and between the negative electrode active material and the current collector. The binder may be a water-insoluble binder, a water-soluble binder, or a combination thereof.

[0147] The non-water-soluble binder may be polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide-imide, polyimide or a combination thereof.

[0148] The water-soluble binder can be a rubber-based binder and / or a polymer resin binder. The rubber-based binder can be selected from styrene-butadiene rubber (SBR), acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber and a combination thereof. The polymer resin binder can be selected from polytetrafluoroethylene, ethylene-propylene copolymer, polyethylene oxide, polyvinyl pyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polystyrene, ethylene-propylene-diene copolymer, polyvinyl pyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol and a combination thereof.

[0149] When a water-soluble binder is used as a negative electrode binder, a cellulose compound may be further used as a thickener to provide viscosity. The cellulose compound includes one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, and alkali metal salts thereof. The alkali metal may be Na, K, and / or Li. Based on 100 wt % of the negative electrode active material, such a thickener may be included in an amount of about 0.1 wt % to about 3 wt %.

[0150] A conductive material is included to provide electrode conductivity (e.g., electrical conductivity) and any appropriate conductive material may be used as the conductive material (e.g., conductive material) unless it causes chemical changes (e.g., unless it causes undesirable changes in the rechargeable lithium battery). Examples thereof may be carbon-based materials (such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.); metal-based materials (such as metal powder or metal fiber of copper, nickel, aluminum, silver, etc.); conductive polymers (such as polyphenylene derivatives, etc.); or mixtures thereof.

[0151] The negative electrode current collector may be selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal (eg, an electrically conductive material), and combinations thereof.

[0152] Depending on the type (or kind) of the rechargeable lithium battery, the rechargeable lithium battery may further include a separator between the negative electrode and the positive electrode. The separator may be a porous substrate; or may be a composite porous substrate.

[0153] The porous substrate may be a substrate including pores, and lithium ions may move through the pores. The porous substrate may, for example, include a polyethylene separator, a polypropylene separator, a polyvinylidene fluoride separator, or a multilayer thereof (such as a polyethylene / polypropylene double-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, and a polypropylene / polyethylene / polypropylene three-layer separator).

[0154] The composite porous substrate may have a form including a porous substrate and a functional layer on the porous substrate. From the perspective of ensuring additional functions, the functional layer may be, for example, at least one selected from a heat-resistant layer and a bonding layer. For example, the heat-resistant layer may include a heat-resistant resin and may optionally include a filler.

[0155] In some embodiments, the tie layer may include a binder resin and, optionally, a filler.

[0156] The filler may be an organic filler and / or an inorganic filler.

[0157] refer to Figure 1 , a rechargeable lithium battery 100 according to some example embodiments includes an electrode assembly (including a negative electrode 112, a positive electrode 114 facing the negative electrode 112, a separator 113 between the negative electrode 112 and the positive electrode 114, and an electrolyte (not shown) impregnating the negative electrode 112, the positive electrode 114, and the separator 113); a battery case 120 accommodating the electrode assembly; and a sealing member 140 sealing the battery case 120. Herein, the battery case 120 is a cylindrical can.

[0158] Examples and comparative examples of the present disclosure will be described below. The following examples are merely examples of embodiments of the present disclosure, and the present disclosure is not limited to the following examples.

[0159] Preparation of electrolyte

[0160] Preparation Example 1

[0161] As for the non-aqueous organic solvent, a carbonate-based solvent was prepared by mixing together ethylene carbonate (EC): ethyl methyl carbonate (EMC): dimethyl carbonate (DMC) = 20:10:70 in a volume ratio.

[0162] To a non-aqueous organic solvent, 1.5M lithium salt (LiPF6) was added, and 1wt% of the first additive represented by Chemical Formula 1-1-1 (CAS No. 16415-09-1) and 0.5wt% of the second additive represented by Chemical Formula 2-1-1 (CAS No. 280-57-9) were added thereto to finally prepare an electrolyte.

[0163] Herein, the content (wt%) of each of the additives means the content (wt%) of each of the additives based on 100 wt% of the electrolyte. The same applies hereinafter.

[0164] Chemical formula 1-1-1

[0165]

[0166] Chemical formula 2-1-1

[0167]

[0168] Preparation Example 2

[0169] An electrolyte for a rechargeable lithium battery was manufactured in substantially the same manner as in Preparation Example 1, except that 1 wt % of the first additive represented by Chemical Formula 1-1-1 (CAS No. 16415-09-1) and 1 wt % of the second additive represented by Chemical Formula 2-1-1 (CAS No. 280-57-9) were used as additives.

[0170] Preparation Example 3

[0171] An electrolyte for a rechargeable lithium battery was manufactured in substantially the same manner as in Preparation Example 1, except that 1 wt % of the first additive represented by Chemical Formula 1-1-1 (CAS No. 16415-09-1) and 3 wt % of the second additive represented by Chemical Formula 2-1-1 (CAS No. 280-57-9) were used as additives.

[0172] Preparation Example 4

[0173] An electrolyte for a rechargeable lithium battery was manufactured in substantially the same manner as in Preparation Example 1, except that 1 wt % of the first additive represented by Chemical Formula 1-1-1 (CAS No. 16415-09-1) and 5 wt % of the second additive represented by Chemical Formula 2-1-1 (CAS No. 280-57-9) were used as additives.

[0174] Comparative Preparation Example 1

[0175] An electrolyte for a rechargeable lithium battery was prepared in substantially the same manner as in Preparation Example 1, except that no additive was used at all.

[0176] Comparative Preparation Example 2

[0177] An electrolyte for a rechargeable lithium battery was manufactured in substantially the same manner as in Preparation Example 1, except that 1 wt % of the first additive represented by Chemical Formula 1-1-1 (CAS No. 16415-09-1) was used as an additive but the second additive represented by Chemical Formula 2-1-1 (CAS No. 280-57-9) was not used.

[0178] Comparative Preparation Example 3

[0179] An electrolyte for a rechargeable lithium battery was manufactured in substantially the same manner as in Preparation Example 1, except that the first additive represented by Chemical Formula 1-1-1 (CAS No. 16415-09-1) was not used but 0.5 wt % of the second additive represented by Chemical Formula 2-1-1 (CAS No. 280-57-9) was used as an additive.

[0180] Manufacturing of rechargeable lithium battery cells

[0181] Example 1

[0182] LiNi as the positive electrode active material 0.94 Co 0.04 Al 0.02 O2, polyvinylidene fluoride as a binder, and Ketjen black as a conductive material were mixed together at a weight ratio of 97:2:1, respectively, and then dispersed in N-methylpyrrolidone to prepare a positive electrode active material slurry.

[0183] The positive electrode active material slurry was coated on a 14 μm thick Al foil, dried at 110° C., and pressed to produce a positive electrode.

[0184] A mixture of artificial graphite and Si composite at a weight ratio of 93.5:6.5 was used as a negative electrode active material, and the negative electrode active material, styrene-butadiene rubber binder, and carboxymethyl cellulose at a weight ratio of 97:1:2 were dispersed in distilled water to prepare a negative electrode active material slurry.

[0185] The negative electrode active material slurry was coated on a 10 μm thick Cu foil, dried at 100° C., and pressed to produce a negative electrode.

[0186] An electrode assembly was manufactured by assembling the manufactured positive electrode and negative electrode and a 25 μm thick polyethylene separator, and the electrode assembly was housed in a battery case having a thickness of 17 cm 3 The samples were put into a cylindrical can having a volume of 1.0 cm, a diameter of 1.8 cm, and a height of 6.5 cm, and each rechargeable lithium battery cell was manufactured by injecting the electrolyte for a rechargeable lithium battery of Preparation Example 1.

[0187] Example 2

[0188] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 1, except that the 3 A cylindrical can having a volume of , a diameter of 2.1 cm, and a height of 6.5 cm was used as a battery case.

[0189] Example 3

[0190] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 1, except that the 3 A cylindrical can having a volume of , a diameter of 4.6 cm and a height of 8.0 cm was used as a battery case.

[0191] Example 4

[0192] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 1, except that the 3 A cylindrical can having a volume of , a diameter of 5.6 cm and a height of 12.0 cm was used as a battery case.

[0193] Example 5

[0194] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 1, except that the electrolyte of Preparation Example 2 was used as an electrolyte.

[0195] Example 6

[0196] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 5, except that the 3 A cylindrical can having a volume of , a diameter of 2.1 cm and a height of 6.5 cm was used as a battery case.

[0197] Example 7

[0198] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 5, except that the 3A cylindrical can having a volume of , a diameter of 4.6 cm and a height of 8.0 cm was used as a battery case.

[0199] Example 8

[0200] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 5, except that the 3 A cylindrical can having a volume of , a diameter of 5.6 cm and a height of 12.0 cm was used as a battery case.

[0201] Example 9

[0202] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 1, except that the electrolyte of Preparation Example 3 was used as an electrolyte.

[0203] Example 10

[0204] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 9, except that the 3 A cylindrical can having a volume of , a diameter of 2.1 cm, and a height of 6.5 cm was used as a battery case.

[0205] Embodiment 11

[0206] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 9, except that the 3 A cylindrical can having a volume of , a diameter of 4.6 cm and a height of 8.0 cm was used as a battery case.

[0207] Example 12

[0208] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 9, except that the 3 A cylindrical can having a volume of , a diameter of 5.6 cm and a height of 12.0 cm was used as a battery case.

[0209] Example 13

[0210] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 1, except that the electrolyte of Preparation Example 4 was used as an electrolyte.

[0211] Embodiment 14

[0212] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 13, except that the 3 A cylindrical can having a volume of , a diameter of 2.1 cm, and a height of 6.5 cm was used as a battery case.

[0213] Embodiment 15

[0214] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 13, except that the 3 A cylindrical can having a volume of , a diameter of 4.6 cm and a height of 8.0 cm was used as a battery case.

[0215] Example 16

[0216] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 13, except that the 3 A cylindrical can having a volume of , a diameter of 5.6 cm and a height of 12.0 cm was used as a battery case.

[0217] Comparative Example 1

[0218] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 1, except that the 3 A cylindrical can having a volume of 100 cm, a diameter of 1.2 cm, and a height of 0.5 cm was used as a battery case, and the electrolyte for a rechargeable lithium battery of Comparative Preparation Example 1 was used as an electrolyte.

[0219] Comparative Example 2

[0220] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Comparative Example 1, except that the cell having a size of 17 cm 3 A cylindrical can having a volume of , a diameter of 1.8 cm and a height of 6.5 cm was used as a battery case.

[0221] Comparative Example 3

[0222] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Comparative Example 1, except that the cell having a size of 24 cm 3 A cylindrical can having a volume of , a diameter of 2.1 cm, and a height of 7.0 cm was used as a battery case.

[0223] Comparative Example 4

[0224] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Comparative Example 1, except that the 3 A cylindrical can having a volume of , a diameter of 4.6 cm and a height of 8.0 cm was used as a battery case.

[0225] Comparative Example 5

[0226] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Comparative Example 1, except that the 3 A cylindrical can having a volume of , a diameter of 5.6 cm and a height of 12.0 cm was used as a battery case.

[0227] Comparative Example 6

[0228] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Comparative Example 1, except that the electrolyte for a rechargeable lithium battery of Comparative Preparation Example 2 was used as an electrolyte.

[0229] Comparative Example 7

[0230] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Comparative Example 6, except that the cell having a size of 17 cm 3 A cylindrical can having a volume of , a diameter of 1.8 cm and a height of 6.5 cm was used as a battery case.

[0231] Comparative Example 8

[0232] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Comparative Example 6, except that the cell having a size of 24 cm 3 A cylindrical can having a volume of , a diameter of 2.1 cm, and a height of 7.0 cm was used as a battery case.

[0233] Comparative Example 9

[0234] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Comparative Example 6, except that the 3 A cylindrical can having a volume of , a diameter of 4.6 cm and a height of 8.0 cm was used as a battery case.

[0235] Comparative Example 10

[0236] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Comparative Example 6, except that the 3 A cylindrical can having a volume of , a diameter of 5.6 cm and a height of 12.0 cm was used as a battery case.

[0237] Comparative Example 11

[0238] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Comparative Example 1, except that the electrolyte for a rechargeable lithium battery of Comparative Preparation Example 3 was used as an electrolyte.

[0239] Comparative Example 12

[0240] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Comparative Example 11, except that the cell having a size of 17 cm 3 A cylindrical can having a volume of , a diameter of 1.8 cm and a height of 6.5 cm was used as a battery case.

[0241] Comparative Example 13

[0242] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Comparative Example 11, except that the 3A cylindrical can having a volume of , a diameter of 2.1 cm, and a height of 7.0 cm was used as a battery case.

[0243] Comparative Example 14

[0244] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Comparative Example 11, except that the 3 A cylindrical can having a volume of , a diameter of 4.6 cm and a height of 8.0 cm was used as a battery case.

[0245] Comparative Example 15

[0246] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Comparative Example 11, except that the 3 A cylindrical can having a volume of , a diameter of 5.6 cm and a height of 12.0 cm was used as a battery case.

[0247] Comparative Example 16

[0248] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 1, except that the 3 A cylindrical can having a volume of 1.0 cm, a diameter of 1.2 cm, and a height of 0.5 cm was used as a battery case.

[0249] Comparative Example 17

[0250] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 5, except that the 3 A cylindrical can having a volume of 1.0 cm, a diameter of 1.2 cm, and a height of 0.5 cm was used as a battery case.

[0251] Comparative Example 18

[0252] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 9, except that the 3 A cylindrical can having a volume of 1.0 cm, a diameter of 1.2 cm, and a height of 0.5 cm was used as a battery case.

[0253] Comparative Example 19

[0254] A rechargeable lithium battery cell was manufactured in substantially the same manner as in Example 13, except that the 3 A cylindrical can having a volume of 1.0 cm, a diameter of 1.2 cm, and a height of 0.5 cm was used as a battery case.

[0255] Evaluation: 60℃ high temperature storage evaluation

[0256] Each of the rechargeable lithium battery cells was subjected to initialization in the following process: The rechargeable lithium battery cell was CC-CV charged to 4.2V (0.05C cutoff) at a current of 0.2C and then discharged to 2.5V, twice.

[0257] After the formation step, the rechargeable lithium battery cells were charged to SOC 100% (SOC, state of charge = 100%) at 1C at 60°C under the conditions of 4.2V cut-off constant current and 0.05C cut-off constant voltage and stored for 60 days.

[0258] As described above, the rechargeable lithium battery cells were stored at a high temperature of 60° C., and then the Ni dissolution amount (ppm / cm 3 ), capacity retention rate (%) and resistance increase rate (%). The capacity retention rate (%) was obtained by equation 1, and the resistance increase rate (%) was obtained by equation 2. The results are shown in Table 1 below.

[0259] Equation 1

[0260] Capacity retention rate (%) = 100 × (discharge capacity after storage at 60°C for 30 days) / (initial discharge capacity)

[0261] Equation 2

[0262] Resistance increase rate (ΔDC-IR) (%) = 100 × (DC-IR after storage at 60° C. for 30 days) / (initial DC-IR)

[0263] In this article, the DC resistance (DC-IR) is calculated from the current difference and the voltage difference when different currents are applied, and specifically, in the initial fully charged state, after constant current discharge (discharging at a constant current of 10A for 10 seconds, discharging at a constant current of 1A for 10 seconds, and discharging at a constant current of 10A for 4 seconds), it is calculated from the data obtained at 18 seconds and 23 seconds according to ΔR=ΔV / ΔI.

[0264] Table 1

[0265]

[0266]

[0267]

[0268] Refer to Table 1, when the volume of the cylindrical tank exceeds 15cm 3 , for example, greater than or equal to 16cm 3 When the temperature is too low, the amount of metal dissolved changes.

[0269] In some embodiments, when two types (or types) of additives are used simultaneously (e.g., simultaneously) and the content of the second additive in the electrolyte is controlled to be less than 5 wt %, the high temperature characteristics of the rechargeable lithium battery cell are further improved compared to an embodiment in which only one additive is used or two additives are used simultaneously (e.g., synchronously) and the content of the second additive in the electrolyte is controlled to be greater than or equal to 5 wt %.

[0270] In general, the rechargeable lithium battery cells according to some example embodiments represented by Examples 1 to 16 control the volume of the cylindrical can and limit the type (or kind) and content of electrolyte additives, thereby inhibiting or reducing metal dissolution and increasing resistance at high temperatures and / or improving cycle life.

[0271] While the subject matter of the present disclosure has been described in connection with what are presently considered to be practical example embodiments, it should be understood that the disclosure is not limited to the disclosed embodiments, but on the contrary is intended to include various modifications and equivalent arrangements within the spirit and scope of the appended claims and their equivalents.

Claims

1. A rechargeable lithium battery comprising: With a diameter greater than or equal to 15cm 3 The volume of the cylindrical tank, an electrode assembly housed in the cylindrical can, and an electrolyte impregnated in the electrode assembly, The electrolyte comprises: Non-aqueous organic solvents; Lithium salts; a first additive including a compound represented by Chemical Formula 1; and A second additive comprising a compound represented by Chemical Formula 2, a derivative thereof and / or an adduct thereof, wherein the content of the second additive is less than 5 wt % based on 100 wt % of the electrolyte: Chemical formula 1 Wherein, in Chemical Formula 1, X1 is a halogen atom; Y1 and Y2 are each independently O or S; R1 and R2 are each independently H, a halogen atom, a substituted or unsubstituted C1-C10 alkyl group, a vinyl group, a substituted or unsubstituted C6-C10 aryl group, or a substituted or unsubstituted C2-C10 heteroaryl group containing a heteroatom of N, O or P; Chemical formula 2 Wherein, in Chemical Formula 2, Z is N or CH.

2. The rechargeable lithium battery according to claim 1, wherein: The volume of the cylindrical tank is 16 cm 3 ~296cm 3 .

3. The rechargeable lithium battery according to claim 2, wherein: The volume of the cylindrical tank is 16 cm 3 ~133cm 3 .

4. The rechargeable lithium battery according to claim 1, wherein: X1 is a fluorine atom.

5. The rechargeable lithium battery according to claim 1, wherein: Y 1 and Y 2 Both are O.

6. The rechargeable lithium battery according to claim 1, wherein: The compound represented by Chemical Formula 1 is represented by Chemical Formula 1-1: Chemical formula 1-1 Among them, in chemical formula 1-1, Z1 and Z2 are each independently a substituted or unsubstituted C1-C5 alkylene group.

7. The rechargeable lithium battery according to claim 6, wherein: Z1 is *-CH2-*, and Z2 is *-CHCH3-*, *Indicates the binding site with the adjacent group.

8. The rechargeable lithium battery according to claim 1, wherein: The first additive is a compound represented by Chemical Formula 1-1-1: Chemical formula 1-1-1 9. The rechargeable lithium battery according to claim 1, wherein: Based on 100 wt % of the electrolyte, the content of the first additive is 0.05 wt % to 3 wt %.

10. The rechargeable lithium battery according to claim 1, wherein: The adduct of the compound represented by Chemical Formula 2 includes an adduct obtained by adding trimethylaluminum, sulfur dioxide, borate or hydrosilane to the compound represented by Chemical Formula 2.

11. The rechargeable lithium battery according to claim 10, wherein: The adduct of the compound represented by Chemical Formula 2 is a compound represented by Chemical Formula 2-2 or Chemical Formula 2-3: Chemical formula 2-2 Chemical formula 2-3 Among them, in Chemical Formula 2-2 and Chemical Formula 2-3, R3 and R4 are each independently trimethylaluminum or sulfur dioxide, Y3-Y5 are each independently O or S; and Z1 is B or SiH.

12. The rechargeable lithium battery according to claim 11, wherein: The second additive includes at least one selected from the group consisting of a compound represented by Chemical Formula 2-1-1, a compound represented by Chemical Formula 2-1-2, a compound represented by Chemical Formula 2-2-1, a compound represented by Chemical Formula 2-2-2, a compound represented by Chemical Formula 2-3-1, and a compound represented by Chemical Formula 2-3-2: Chemical formula 2-1-1 Chemical formula 2-1-2 Chemical formula 2-2-1 Chemical formula 2-2-2 Chemical formula 2-3-1 Chemical formula 2-3-2 13. The rechargeable lithium battery according to claim 1, wherein: Based on 100 wt % of the electrolyte, the content of the second additive is 0.05 wt % to 3 wt %.

14. The rechargeable lithium battery according to claim 1, wherein: The weight ratio of the first additive to the second additive is 1:0.1 to 1:

3.

15. The rechargeable lithium battery of claim 1, wherein: The non-aqueous organic solvent includes carbonate solvents, ester solvents, ether solvents, ketone solvents, alcohol solvents and / or aprotic solvents.

16. The rechargeable lithium battery of claim 15, wherein: The non-aqueous organic solvent includes: a carbonate solvent including a mixture of a cyclic carbonate and a chain carbonate in a volume ratio of 5:95 to 50:

50.

17. The rechargeable lithium battery of claim 1, wherein: The electrode assembly comprises: a positive electrode including a positive electrode active material layer; a negative electrode including a negative electrode active material layer; and A separator is between the positive electrode and the negative electrode.

18. The rechargeable lithium battery of claim 17, wherein: The positive electrode active material layer includes a lithium nickel-based composite oxide represented by Chemical Formula A1: Chemical formula A1 Li a1 Ni x1 M 1 y1 M 2 z1 O 2-b1 X b1 , Wherein, in chemical formula A1, 0.9≤a1≤1.2, 0.7≤x1≤1, 0≤y1≤0.2, 0≤z1≤0.2, 0.9≤x1+y1+z1≤1.1, and 0≤b1≤0.1; M 1 and M 2 Each is independently one or more elements selected from Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sr, Ti, V, W and Zr; and X is one or more elements selected from F, P and S.

19. The rechargeable lithium battery of claim 17, wherein: The negative electrode active material layer includes at least one selected from graphite and Si composite.

20. The rechargeable lithium battery of claim 1, wherein: The rechargeable lithium battery further includes a sealing member sealing the cylindrical can.

Citation Information

Patent Citations

  • Shoe heel