Electrolyte for rechargeable lithium battery and rechargeable lithium battery including same
By using specific electrolytes, including a combination of non-aqueous organic solvents and specific additives in rechargeable lithium batteries, the film on the surface of the electrode is solved, and the problems of positive electrode deterioration and side reactions at high voltages are improved, and the safety of the battery is improved and cycle life.
Patent Information
- Application Number
- CN202410433111.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-06-05
- Filing Date
- 2024-04-11
- Publication Date
- 2024-12-06
AI Technical Summary
Under high voltage, the positive electrode of the rechargeable lithium battery deteriorates under severe conditions, resulting in lithium crystal branches growth, accelerated side reactions, gas generation, and reduced the cycle life and safety of the battery.
An electrolyte comprising a non-aqueous organic solvent, a lithium salt and a specific additive is used. The additive consists of a compound represented by Chemical Formula 1 and Chemical Formula 2. The weight ratio of the first compound to the second compound is about 1:0.3 to 1:1.3, and is formed at The film on the electrode surface suppresses side reactions and electrode structure collapse, and reduces the dissolution of positive electrode active substances and gas generation.
Effectively prevent the dissolution of positive electrode active substances, reduce the increase in internal resistance, ensure the safety and high temperature reliability of the battery at high voltage, and improve capacity characteristics and cycle life.
Smart Images

Figure CN119092820A_ABST
Abstract
Description
Technical Field
[0001] Disclosed are an electrolyte for a rechargeable lithium battery and a rechargeable lithium battery including the same. Background Art
[0002] Recently, with the rapid popularization of electronic devices using batteries (such as mobile phones, notebook computers and electric vehicles), the demand for rechargeable lithium batteries with high energy density and high capacity has increased rapidly. Accordingly, research and development for improving the performance of rechargeable lithium batteries is being actively carried out.
[0003] The rechargeable lithium battery includes positive and negative electrodes including active materials capable of intercalating and deintercalating lithium ions, and an electrolyte, and generates electric energy through oxidation and reduction reactions when lithium ions are intercalated / deintercalated at the positive and negative electrodes.
[0004] Recently, in order to use the rechargeable lithium battery as a driving power source for a hybrid vehicle or an electric vehicle or as a power source for power storage, research on a rechargeable lithium battery having high capacity, high energy density, and high safety is being actively conducted.
[0005] In rechargeable lithium batteries, electrolyte plays an important role in delivering lithium ions, among which one type (or kind) of electrolyte containing organic solvent and lithium salt shows extremely high ion conductivity and is generally used. The electrolyte plays an important role in determining or contributing to the safety and performance of rechargeable lithium batteries.
[0006] Recently, with the demand or expectation for high-capacity and high-energy-density batteries, it is necessary or desirable to design a battery with a high-density electrode operable at a high voltage of 4.5 V or higher. However, the positive electrode deteriorates under severe conditions such as high voltage, while lithium dendrites grow on the surface of the negative electrode, accelerating the side reaction between the electrode and the electrolyte and causing problems such as reduced cycle life of the battery and deterioration of battery safety due to gas generation, etc.
[0007] In order to solve this problem, a method of protecting the electrode and inhibiting or reducing the side reaction with the electrolyte by surface treatment has been proposed. However, it has been reported that under high voltage driving conditions, the surface treatment of the positive electrode lacks a protective effect, and the surface treatment of the negative electrode can deteriorate the capacity. Therefore, when designing a high-capacity electrode that can be driven at a high voltage, it is required or expected to develop an electrolyte that can improve battery safety and performance. Summary of the invention
[0008] Embodiments of the present disclosure provide an electrolyte for a rechargeable lithium battery, which inhibits or reduces side reactions of the electrolyte and collapse of the electrode structure, effectively prevents or reduces the dissolution of positive electrode active materials, and inhibits or reduces the increase in internal resistance due to gas generation, thereby ensuring the safety and high-temperature reliability of the battery under high-voltage driving conditions, and improving capacity characteristics and cycle life characteristics.
[0009] Another embodiment provides a rechargeable lithium battery including an electrolyte.
[0010] Embodiments provide an electrolyte for a rechargeable lithium battery, which includes a non-aqueous organic solvent, a lithium salt, and an additive, wherein the additive includes a first compound represented by Chemical Formula 1 and CsPF 6 Or a second compound of the compound represented by Chemical Formula 2, and a weight ratio of the first compound to the second compound is about 1:0.3 to about 1:1.3.
[0011] Chemical formula 1
[0012]
[0013] In Chemical Formula 1, Ar is a substituted or unsubstituted C6-C30 aryl group or a substituted or unsubstituted C2-C30 heterocyclic group, and R 1 It is O or S.
[0014] Chemical formula 2
[0015]
[0016] In chemical formula 2, R 2 and R 3 Each is independently a fluoro group or a C1-C4 fluoroalkyl group substituted by at least one fluoro group.
[0017] In another embodiment, a rechargeable lithium battery includes: a positive electrode including a positive electrode active material; a negative electrode including a negative electrode active material; a separator between the positive electrode and the negative electrode; and the aforementioned electrolyte.
[0018] The electrolyte for a rechargeable lithium battery according to an embodiment inhibits or reduces side reactions of the electrolyte and collapse of the electrode structure, effectively prevents or reduces the dissolution of the positive electrode active material, and inhibits or reduces the increase in internal resistance due to gas generation, thereby ensuring the safety and high temperature reliability of the battery under high voltage driving conditions, and improving capacity characteristics and cycle life characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Features will become apparent to those skilled in the art by describing exemplary embodiments in detail with reference to the accompanying drawings, in which:Figure 1 to Figure 4 is a schematic diagram of a rechargeable lithium battery according to an embodiment.
[0020] Description of Reference Numerals
[0021] 100: Rechargeable lithium battery 10: Positive electrode
[0022] 11: Positive electrode lead tab 12: Positive terminal
[0023] 20: Negative electrode 21: Negative electrode lead lug
[0024] 22: Negative terminal 30: Separator
[0025] 40: electrode assembly 50: shell
[0026] 60: Sealing member 70: Electrode terminal piece
[0027] 71: Positive electrode terminal tab 72: Negative electrode terminal tab DETAILED DESCRIPTION
[0028] Example embodiments will now be described more fully hereinafter with reference to the accompanying drawings; however, they may be embodied in different forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey exemplary implementations to those skilled in the art.
[0029] In the accompanying drawings, the dimensions of layers and regions may be exaggerated for clarity of illustration. It will also be understood that when a layer or element is referred to as being "on" another layer or substrate, it may be directly on the other layer or substrate, or there may also be intervening layers. Further, it will be understood that when a layer is referred to as being "below" another layer, it may be directly below the other layer, and there may also be one or more intervening layers. In addition, it will also be understood that when a layer is referred to as being "between" two layers, it may be the only layer between the two layers, or there may also be one or more intervening layers. The same reference numerals refer to the same elements throughout.
[0030] As used herein, when no specific limitations are provided otherwise, it will be understood that when an element (such as a layer, film, region or substrate) is referred to as being "on" another element (such as a layer, film, region or substrate), it can be directly on the other element (such as a layer, film, region or substrate) or intervening elements (such as layers, films, regions or substrates) may also be present.
[0031] Unless otherwise specified in the specification, what is indicated in the singular may also include the plural. In addition, unless otherwise specified, "A or B" may indicate "including A, including B, or including A and B".
[0032] As used herein, "combinations thereof" may refer to mixtures, laminates, composites, copolymers, alloys, blends, reaction products, and the like, of the components.
[0033] As used in this article, when not otherwise provided for limitation, particle diameter may be average particle diameter.Term " particle diameter " may refer to average particle diameter (D50).Term " D50 " refers to the diameter of the particle with 50 volume % cumulative volume in particle size distribution.Mean particle diameter (D50) can be measured by methods well known to those skilled in the art (such as, for example, by particle size analyzer or by transmission electron microscope image or scanning electron microscope image).In some implementations, dynamic light scattering measurement device can be used for data analysis, and the number of particles of each particle size range can be counted.From this calculation, average particle diameter (D50) value can be easily obtained.In some implementations, laser diffraction method can be used to measure particle diameter.More specifically, when particle diameter is measured by laser diffraction method, particles to be measured can be dispersed in a dispersion medium, and then commercially available laser diffraction particle diameter measuring device (for example, Microtrac MT 3000) can be introduced. Ultrasonic waves of about 28 kHz with an output of 60 W may be irradiated to calculate an average particle size (D50) based on 50% of the particle size distribution in the measuring device.
[0034] As used herein, when no limitation is otherwise provided, the term "substituted" refers to that at least one hydrogen in a substituent or a compound is replaced by deuterium, halogen, hydroxyl, amino, C1-C30 amine, nitro, C1-C40 silyl, C1-C30 alkyl, substituted or unsubstituted C2-C20 alkenyl, substituted or unsubstituted C2-C20 alkynyl, C1-C10 alkylsilyl, C6-C30 arylsilyl, C3-C30 cycloalkyl, C3-C30 heterocycloalkyl, C6-C30 aryl, C2-C30 heteroaryl, C1-C20 alkoxy, C1-C10 fluoroalkyl, cyano or a combination thereof.
[0035] As used herein, the term "substituted" may refer to at least one hydrogen in a substituent or compound being replaced by deuterium, halogen, C1-C30 alkyl, C1-C10 alkylsilyl, C6-C30 arylsilyl, C3-C30 cycloalkyl, C3-C30 heterocycloalkyl, C6-C30 aryl, C2-C30 heteroaryl, C1-C10 fluoroalkyl or cyano. For example, the term "substituted" may refer to at least one hydrogen in a substituent or compound being replaced by deuterium, halogen, C1-C20 alkyl, C6-C30 aryl, C1-C10 fluoroalkyl or cyano. In some embodiments, the term "substituted" may refer to at least one hydrogen in a substituent or compound being replaced by deuterium, halogen, C1-C5 alkyl, C6-C18 aryl, C1-C5 fluoroalkyl or cyano. For example, the term "substituted" may refer to a substituent or compound in which at least one hydrogen is replaced by deuterium, cyano, halogen, methyl, ethyl, propyl, butyl, phenyl, biphenyl, terphenyl, trifluoromethyl, or naphthyl.
[0036] Embodiments provide an electrolyte for a rechargeable lithium battery, which includes a non-aqueous organic solvent, a lithium salt, and an additive, wherein the additive includes a first compound represented by Chemical Formula 1 and CsPF 6 Or a second compound of the compound represented by Chemical Formula 2, and a weight ratio of the first compound to the second compound is about 1:0.3 to about 1:1.3.
[0037] Chemical formula 1
[0038]
[0039] In Chemical Formula 1, Ar is a substituted or unsubstituted C6-C30 aryl group or a substituted or unsubstituted C2-C30 heterocyclic group, and R 1 It is O or S.
[0040] Chemical formula 2
[0041]
[0042] In chemical formula 2, R 2 and R 3 Each is independently a fluoro group or a C1-C4 fluoroalkyl group substituted by at least one fluoro group.
[0043] The electrolyte may include the additive in an amount of, for example, about 0.1 wt % to about 30.0 wt %, about 1.0 wt % to about 20.0 wt % or about 2.0 wt % to about 15.0 wt % based on the total weight of the electrolyte for a rechargeable lithium battery.
[0044] The weight ratio between the first compound and the second compound may be about 1:0.3 to about 1:1.3, and, for example, may be about 1:0.5 to about 1:1.25. The electrolyte for a rechargeable lithium battery includes the first compound and the second compound in the aforementioned weight ratio range as additives and thus suppresses or reduces the side reaction of the electrolyte and the structural collapse of the electrode, effectively prevents or reduces the dissolution of the positive electrode active material, and suppresses or reduces the increase in internal resistance due to gas generation, resulting in ensuring the safety and high temperature reliability of the battery under high voltage driving conditions, and improving capacity characteristics, cycle life characteristics, etc. For example, when the weight ratio of the second compound to the first compound is less than about 0.3, the cycle life characteristics and high temperature storage characteristics may be deteriorated because the battery thickness increase rate according to charging and discharging is not properly or sufficiently suppressed or reduced. When the weight ratio of the second compound to the first compound is greater than about 1.3, the battery thickness increase rate according to charging and discharging may be greatly increased because the synergistic effect generated by the combination of the two compounds may be greatly deteriorated, resulting in the cycle life characteristics and high temperature storage characteristics being deteriorated.
[0045] First Compound
[0046] The first compound may be a compound having an isocyanate (—NCO) functional group or an isothiocyanate (—NCS) functional group. The isocyanate functional group or the isothiocyanate functional group acts as an anion receptor and induces anions of lithium salts (e.g., PF 6 - ) and, for example, by stabilizing lithium salts such as LiPF 6 ), the generation of byproducts (such as HF) due to the decomposition of the lithium salt can be suppressed or reduced. Accordingly, the decomposition of the lithium salt on the positive electrode surface and the electrolyte oxidation reaction that can occur during the high temperature cycle operation of the rechargeable lithium battery can be suppressed, prevented or reduced, thereby improving the high rate charge / discharge characteristics and swelling characteristics. In addition, the first compound forms a film on the positive electrode surface and thus suppresses or reduces the side reaction with the electrolyte and the structural collapse of the electrode to improve the performance and also effectively prevent or reduce the dissolution of the metal component in the positive electrode active material.
[0047] The first compound is represented by Chemical Formula 1.
[0048] Chemical formula 1
[0049]
[0050] In Chemical Formula 1, Ar is a substituted or unsubstituted C6-C30 aryl group or a substituted or unsubstituted C2-C30 heterocyclic group, and R 1 It is O or S.
[0051] For example, the first compound may be represented by Chemical Formula 1A.
[0052] Chemical formula 1A
[0053]
[0054] In Chemical Formula 1A, R A , R B , R C , R D and R E are each independently hydrogen, halogen, hydroxyl, cyano, nitro, substituted or unsubstituted C1-C20 alkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted C2-C20 alkenyl, substituted or unsubstituted C2-C20 alkynyl, substituted or unsubstituted C3-C20 cycloalkyl, substituted or unsubstituted C6-C20 aryl or substituted or unsubstituted C2-C20 heteroaryl, and R 1 It is O or S.
[0055] For example, in Formula 1A, R A , R B , R C , R D and R E They may each independently be hydrogen, halogen or substituted or unsubstituted C1-C10 alkyl.
[0056] As an example, the first compound may be represented by any one selected from Chemical Formula 1A-1 to Chemical Formula 1A-3.
[0057] Chemical formula 1A-1
[0058]
[0059] Chemical formula 1A-2
[0060]
[0061] Chemical formula 1A-3
[0062]
[0063] In Chemical Formulas 1A-1 to 1A-3, R 1 It is O or S.
[0064] Based on the total weight of the electrolyte for a rechargeable lithium battery, the amount of the first compound included in the electrolyte may be about 0.1 wt% to about 10.0 wt%. For example, based on 100 wt% of the electrolyte, the amount of the first compound included may be about 0.25 wt% to about 10.0 wt%, about 0.5 wt% to about 10.0 wt%, about 0.5 wt% to about 5.0 wt%, or about 0.5 wt% to about 2.5 wt%, for example, about 0.5 wt% to about 2.0 wt%. When the first compound is included within the above range, high rate charge / discharge characteristics and swelling characteristics can be effectively improved.
[0065] Second compound
[0066] The second compound may include cesium hexafluorophosphate (CsPF 6 ) and / or a compound of cesium sulfonimide salt. The second compound decomposes in the electrolyte and forms a film on the surface of the electrode to effectively control the dissolution of lithium ions generated from the positive electrode, so as to prevent or reduce the decomposition of the electrode. In some embodiments, the second compound is reduced and decomposed earlier than the carbonate solvent included in the non-aqueous organic solvent, and forms an SEI (solid electrolyte interface) film on the negative electrode to prevent or reduce the decomposition of the electrolyte and the resulting decomposition reaction of the negative electrode, thereby inhibiting or reducing the increase in internal resistance due to gas generation. The SEI film formed on the negative electrode is partially decomposed by a reduction reaction during charging and discharging, and then moves to the surface of the positive electrode and forms a film on the surface of the positive electrode by an oxidation reaction, so as to prevent or reduce the decomposition of the positive electrode surface and the oxidation reaction of the electrolyte, thereby helping to improve the high temperature cycle life characteristics.
[0067] The second compound is represented by Chemical Formula 2.
[0068] Chemical formula 2
[0069]
[0070] In chemical formula 2, R 2 and R 3 Each is independently a fluoro group or a C1-C4 fluoroalkyl group substituted by at least one fluoro group.
[0071] For example, R in Formula 2 2 and R 3 Each of them may independently be a fluoro group or a C1-C4 fluoroalkyl group substituted by at least two fluoro groups.
[0072] For example, R in Formula 2 2 and R 3 Each independently may be a fluoro group or a C1-C4 fluoroalkyl group substituted by at least three fluoro groups.
[0073] As an example, R in Formula 2 2 and R 3 Each of them may independently be a fluoro group or a C1-C3 fluoroalkyl group substituted by at least three fluoro groups.
[0074] As an example, R in Formula 2 2 and R 3 Each independently may be a fluoro group or a C1-C2 fluoroalkyl group substituted by at least three fluoro groups.
[0075] For example, the compound represented by Chemical Formula 2 may be represented by Chemical Formula 2-1 or Chemical Formula 2-2.
[0076] Chemical formula 2-1
[0077]
[0078] Chemical formula 2-2
[0079]
[0080] Based on the total weight of the electrolyte for a rechargeable lithium battery, the amount of the second compound included in the electrolyte may be about 0.01 wt% to about 5 wt%. For example, based on 100 wt% of the electrolyte, the amount of the second compound included may be about 0.05 wt% to about 5 wt%, about 0.1 wt% to about 5 wt%, about 0.25 wt% to about 5 wt%, or about 0.25 wt% to about 2.5 wt%, for example, about 0.25 wt% to about 1.25 wt%. When the second compound is included within the above range, the dissolution of lithium ions is effectively controlled and the increase in internal resistance due to gas generation is suppressed or reduced, thereby contributing to the improvement of high temperature cycle life characteristics.
[0081] The third compound
[0082] The additive may further include a third compound.
[0083] The third compound has a structure including a cesium fluorosulfonyl imide salt and can be decomposed in the electrolyte to form a film on the surface of the positive electrode and the negative electrode, respectively. In some embodiments, the film on the surface of the positive electrode can prevent or reduce the decomposition of the positive electrode by effectively controlling the dissolution of lithium ions generated from the positive electrode.
[0084] In addition, the third compound is reduced and decomposed earlier than the carbonate solvent included in the non-aqueous organic solvent to form an SEI film on the negative electrode, thereby preventing or reducing the decomposition of the electrolyte and the resulting decomposition reaction of the electrode, and inhibiting or reducing the increase in internal resistance due to gas generation. The SEI film formed on the negative electrode is partially decomposed by a reduction reaction during charging and discharging, moves to the surface of the positive electrode, and forms a film on the surface of the positive electrode by an oxidation reaction to prevent or reduce the decomposition of the surface of the positive electrode and the oxidation of the electrolyte, thereby improving high temperature and low temperature cycle life characteristics.
[0085] The third compound is represented by Chemical Formula 3.
[0086] Chemical formula 3
[0087]
[0088] In Chemical Formula 3, X is C(=O) or S(=O) 2 And Y 1 and Y 2 Each is independently a fluoro group or a C1-C5 fluoroalkyl group substituted by at least one fluoro group.
[0089] For example, the third compound may be represented by any one selected from Chemical Formula 3-1 to Chemical Formula 3-8.
[0090] Chemical formula 3-1
[0091]
[0092] Chemical formula 3-2
[0093]
[0094] Chemical formula 3-3
[0095]
[0096] Chemical formula 3-4
[0097]
[0098] Chemical formula 3-5
[0099]
[0100] Chemical formula 3-6
[0101]
[0102] Chemical formula 3-7
[0103]
[0104] Chemical formula 3-8
[0105]
[0106] In Chemical Formulae 3-3 to 3-8, R a , R b , R c and R d Each is independently a hydrogen or fluoro group, and n and m are each independently one integer selected from 0 to 4.
[0107] For example, the third compound may be represented by Chemical Formula 3-1 or Chemical Formula 3-2.
[0108] Based on the total weight of the electrolyte for a rechargeable lithium battery, the amount of the third compound included in the electrolyte may be about 0.05 wt % to about 5 wt %, for example, about 0.1 wt % to about 5.0 wt %, about 0.2 wt % to about 5.0 wt %, or about 0.5 wt % to about 5.0 wt %, for example, about 0.5 wt % to about 2.5 wt %. When the third compound is included within the above range, a rechargeable lithium battery having improved cycle life characteristics and low temperature output characteristics can be implemented by preventing or reducing resistance increase during long-term charge / discharge or at low temperatures.
[0109] Other additives
[0110] The electrolyte for a rechargeable lithium battery may further include other additives than those described above. When other additives are further included, high temperature storage characteristics (such as effective control of gas generated from the positive electrode and the negative electrode during high temperature storage) may be improved.
[0111] Other additives may include at least one selected from the following: vinylene carbonate (VC), fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), chloroethylene carbonate (CEC), dichloroethylene carbonate (DCEC), bromethylene carbonate (BEC), dibromoethylene carbonate (DBEC), nitroethylene carbonate, cyanoethylene carbonate, vinylethylene carbonate (VEC), succinonitrile (SN), adiponitrile (AN), 1,3,6-hexanetrinitrile (HTCN), propene sultone (PST), propane sultone (PS), lithium tetrafluoroborate (LiBF 4 ), lithium difluorophosphate (LiPO 2 F 2 ) and 2-fluorobiphenyl (2-FBP), but are not limited thereto.
[0112] Based on the total weight of the electrolyte for the rechargeable lithium battery, the amount of other additives included in the electrolyte may be about 0.2 wt% to about 30 wt%. For example, the amount of other additives included may be about 0.2 wt% to about 15 wt%, for example, about 0.2 wt% to about 10 wt%. When the other additives included are within the above range, a rechargeable lithium battery with improved high temperature storage characteristics (such as effectively controlling the gas generated from the positive electrode and the negative electrode) can be implemented.
[0113] Electrolyte
[0114] An electrolyte for a rechargeable lithium battery may include a non-aqueous organic solvent and a lithium salt.
[0115] The nonaqueous organic solvent may be used as a medium for transporting ions participating in the electrochemical reaction of the battery.
[0116] The non-aqueous organic solvent may be a carbonate solvent, an ester solvent, an ether solvent, a ketone solvent or an alcohol solvent, an aprotic solvent or a combination thereof.
[0117] The carbonate solvents may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc.
[0118] The ester solvents may include methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, propyl propionate, decanoic acid lactone, mevalonolactone, valerolactone, caprolactone, and the like.
[0119] Ether solvents may include dibutyl ether, tetraglyme, diglyme, dimethoxyethane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, tetrahydrofuran, etc. In addition, ketone solvents may include cyclohexanone, etc. Alcohol solvents may include ethanol, isopropanol, etc. and aprotic solvents may include nitriles (such as R-CN, where R is a C2-C20 straight chain hydrocarbon group, a branched hydrocarbon group or a cyclic hydrocarbon group, and may include a double bond, an aromatic ring or an ether bond, etc.); amides (such as dimethylformamide); dioxolanes (such as 1,3-dioxolanes, 1,4-dioxolanes, etc.); sulfolane, etc.
[0120] A single nonaqueous organic solvent may be used or a combination of two or more may be used.
[0121] In addition, when a carbonate-based solvent is used, a cyclic carbonate and a chain carbonate may be mixed and used, and the cyclic carbonate and the chain carbonate may be mixed in a volume ratio of about 1:1 to about 1:9.
[0122] The lithium salt dissolved in the organic solvent supplies lithium ions in the battery, ensures the basic operation of the rechargeable lithium battery, and improves the transport of lithium ions between the positive electrode and the negative electrode. Examples of the lithium salt include those selected from LiPF 6 , LiBF 4 、LiSbF 6 、LiAsF 6 、LiClO 4 、LiAlO 2 、LiAlCl 4 、LiPO 2 F 2 、LiCl、LiI、LiN(SO 3 C 2 F 5 ) 2 、Li(FSO 2 ) 2 N(lithium bis(fluorosulfonyl)imide, LiFSI), LiC 4 F 9 SO 3 、LiN(C x F 2x+1 SO 2 )(C y F 2y+1 SO 2 )(wherein x and y are one of integers selected from 1 to 20), at least one of lithium trifluoromethanesulfonate, lithium tetrafluoroethanesulfonate, lithium difluorobis(oxalato)phosphate (LiDFOB) and lithium bis(oxalato)borate (LiBOB).
[0123] Rechargeable lithium battery
[0124] Embodiments provide a rechargeable lithium battery including a positive electrode including a positive electrode active material, a negative electrode including a negative electrode active material, a separator between the positive electrode and the positive electrode, and the aforementioned electrolyte.
[0125] The rechargeable lithium battery may be classified into a cylindrical, prismatic, pouch or coin type battery, etc., depending on the shape of the rechargeable lithium battery. Figure 1 to Figure 4 A schematic diagram for explaining a rechargeable lithium battery according to an embodiment. Figure 1 A cylindrical battery is shown, Figure 2 A prismatic cell is shown, and Figure 3 and Figure 4 A pouch type battery is shown. Figure 1 to Figure 4 , the rechargeable lithium battery 100 may include: an electrode assembly 40 including a separator 30 between a positive electrode 10 and a negative electrode 20; and a case including the electrode assembly 40. The positive electrode 10, the negative electrode 20, and the separator 30 may be impregnated with an electrolyte (not shown). Figure 1 As shown in FIG. 1 , the rechargeable lithium battery 100 may include a sealing member 60 that seals the housing 50. Figure 2 In the embodiment, the rechargeable lithium battery 100 may include a positive electrode lead tab 11, a positive terminal 12, a negative electrode lead tab 21, and a negative terminal 22. Figure 3 and Figure 4 As shown in FIG. 1 , the rechargeable lithium battery 100 may include an electrode tab 70 (see FIG. Figure 4 ), which may be, for example, a positive electrode tab 71 (see Figure 3 ) and negative electrode terminal tab 72 (see Figure 3 ).
[0126] The rechargeable lithium battery according to the embodiment may be applied to vehicles, mobile phones, and / or various types of electronic devices as non-limiting examples.
[0127] Positive electrode active material
[0128] The positive electrode active material may include a compound capable of intercalating and deintercalating lithium (lithiated intercalation compound). Specifically, at least one composite oxide of lithium and a metal selected from cobalt, manganese, nickel, and a combination thereof may be used.
[0129] The composite oxide may be a lithium transition metal composite oxide. Specific examples of the composite oxide may include lithium nickel-based oxides, lithium cobalt-based oxides, lithium manganese-based oxides, lithium iron phosphate-based compounds, nickel manganese-based oxides not containing cobalt, or combinations thereof.
[0130] As an example, the following compounds represented by any one of the following chemical formulas may be used. a A 1-b X b O 2-c D c (0.90≤a≤1.8, 0≤b≤0.5, and 0≤c≤0.05); Li a Mn 2-b X b O 4-c D c (0.90≤a≤1.8, 0≤b≤0.5, and 0≤c≤0.05); Li a Ni 1-b-c Co b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, and 0<α<2); Li a Ni 1-b-c Mn b Xc O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, and 0<α<2); Li a Ni b Co c L 1 d G e O 2 (0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, and 0≤e≤0.1); Li a NeG b O 2 (0.90≤a≤1.8 and 0.001≤b≤0.1); Li a CoG b O 2 (0.90≤a≤1.8 and 0.001≤b≤0.1); Li a Mn 1-b G b O 2 (0.90≤a≤1.8 and 0.001≤b≤0.1); Li a Mn 2 G b O 4 (0.90≤a≤1.8 and 0.001≤b≤0.1); Li a Mn 1-g G g PO 4 (0.90≤a≤1.8 and 0≤g≤0.5); Li (3-f) Fe 2 (PO 4 ) 3 (0≤f≤2); or Li a FePO 4( 0.90≤a≤1.8).
[0131] In the above chemical formula, A is Ni, Co, Mn or a combination thereof; X is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element or a combination thereof; D is O, F, S, P or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof; and L 1 It is Mn, Al or a combination thereof.
[0132] The positive electrode active material may be, for example, a high nickel-based positive electrode active material having a nickel content of about 80 mol% or more, about 85 mol% or more, about 90 mol% or more, about 91 mol% or more, or about 94 mol% or more and about 99 mol% or less based on 100 mol% of metals other than lithium in the lithium transition metal composite oxide. The high nickel-based positive electrode active material may be capable of achieving high capacity and may be applied to high capacity, high density rechargeable lithium batteries.
[0133] In an embodiment, the positive electrode active material may include a lithium cobalt oxide. A positive electrode using a lithium cobalt oxide as a positive electrode active material, when used with the aforementioned electrolyte, can suppress or reduce battery resistance and improve overall battery performance by exhibiting a synergistic effect in a 4.5V class high voltage design or a fast charging system.
[0134] The lithium cobalt-based oxide may be represented by Chemical Formula 4, for example.
[0135] Chemical formula 4
[0136] Li a1 Co x1 M 1 1-x1 O 2
[0137] In Chemical Formula 4, 0.9≤a1≤1.8, and 0.7≤x1≤1, and M 1 It is one or more elements selected from Al, B, Ba, Ca, Ce, Cr, Cu, F, Fe, Mg, Mn, Mo, Ni, P, S, Se, Si, Sr, Ti, V, W, Y, Zn and Zr.
[0138] In Chemical Formula 4, x1 represents a molar content of cobalt and may be, for example, 0.8≤x1≤1, 0.9≤x1≤1, or 0.95≤x1≤1.
[0139] Positive electrode
[0140] The positive electrode for a rechargeable lithium battery may include a positive electrode current collector and a positive electrode active material layer on the positive electrode current collector. The positive electrode active material layer may include a positive electrode active material and may further include a binder and / or a conductive material (eg, an electrically conductive material).
[0141] For example, the positive electrode may further include additives so as to be usable as a sacrificial positive electrode.
[0142] The amount of the positive electrode active material may be about 90 wt % to about 99.5 wt % based on 100 wt % of the positive electrode active material layer, and the amount of the binder and the conductive material may be about 0.5 wt % to about 5 wt % based on 100 wt % of the positive electrode active material layer, respectively.
[0143] The binder is used to make the positive electrode active material particles well attached to each other and also to make the positive electrode active material well attached to the positive electrode current collector. Examples of binders may include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers including ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, (meth) acrylated styrene-butadiene rubber, epoxy resin, (meth) acrylic resin, polyester resin, nylon, etc. as non-limiting examples.
[0144] Conductive materials can be used to impart conductivity (e.g., electrical conductivity) to electrodes. Any material that does not cause chemical changes (e.g., does not cause undesirable chemical changes in rechargeable lithium batteries) and conducts electrons can be used in the battery. Examples of conductive materials may include carbon-based materials (such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanofibers, and carbon nanotubes); metal-based materials containing copper, nickel, aluminum, silver, etc. in the form of metal powder or metal fiber; conductive polymers (such as polyphenylene derivatives); or mixtures thereof.
[0145] Al foil may be used as a positive electrode current collector, but is not limited thereto.
[0146] Negative electrode active material
[0147] The negative electrode active material may include a material that reversibly intercalates / deintercalates lithium ions, lithium metal, a lithium metal alloy, a material capable of doping / dedoping lithium, or a transition metal oxide.
[0148] The material that reversibly intercalates / deintercalates lithium ions may include a carbon-based negative electrode active material (such as, for example, crystalline carbon, amorphous carbon, or a combination thereof). The crystalline carbon may be graphite (such as amorphous, flaky, sheet-like, spherical, or fibrous natural graphite or artificial graphite). The amorphous carbon may be soft carbon, hard carbon, mesophase pitch carbonization product, calcined coke, etc.
[0149] Lithium metal alloys include alloys of lithium and a metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn.
[0150] The material capable of doping / dedoping lithium can be an Si-based negative electrode active material or an Sn-based negative electrode active material. The Si-based negative electrode active material can include silicon, silicon-carbon composite, SiO x (0 < x < 2), Si-Q alloy (where Q is selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements (excluding Si), Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof). The Sn-based negative electrode active material can include Sn, SnO 2 , Sn-based alloy, or a combination thereof.
[0151] The silicon-carbon composite can be a composite of silicon and amorphous carbon. According to an embodiment, the silicon-carbon composite can be in the form of silicon particles and amorphous carbon coated on the surface of the silicon particles. For example, the silicon-carbon composite can include secondary particles (cores) in which primary silicon particles are assembled and an amorphous carbon coating (shell) on the surface of the secondary particles. The amorphous carbon can also be between the primary silicon particles, and, for example, the primary silicon particles can be coated with amorphous carbon. The secondary particles can be dispersed in the amorphous carbon matrix.
[0152] The silicon-carbon composite can further include crystalline carbon. For example, the silicon-carbon composite can include: a core including crystalline carbon and silicon particles and an amorphous carbon coating on the surface of the core.
[0153] The Si-based negative electrode active material or the Sn-based negative electrode active material can be used in combination with a carbon-based negative electrode active material.
[0154] Negative electrode
[0155] The negative electrode for a rechargeable lithium battery can include a negative electrode current collector and a negative electrode active material layer on the negative electrode current collector. The negative electrode active material layer can include a negative electrode active material and can further include a binder and / or a conductive material (e.g., a conductive material).
[0156] For example, the negative electrode active material layer can include about 90 wt% to about 99 wt% of the negative electrode active material, about 0.5 wt% to about 5 wt% of the binder, and about 0 wt% to about 5 wt% of the conductive material.
[0157] The binder can be used to make the negative electrode active material particles adhere well to each other and also make the negative electrode active material adhere well to the negative electrode current collector. The binder can include a non-aqueous binder, an aqueous binder, a dry binder, or a combination thereof.
[0158] The non-aqueous binder can include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene-propylene copolymer, polystyrene, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or a combination thereof.
[0159] The aqueous binder can be selected from styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, (meth)acrylonitrile-butadiene rubber, (meth)acrylic rubber, butyl rubber, fluororubber, polyethylene oxide, polyvinyl pyrrolidone, polyepichlorohydrin, polyphosphazene, poly(meth)acrylonitrile, ethylene propylene diene copolymer, polyvinyl pyridine, chlorosulfonated polyethylene, latex, polyester resin, (meth)acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol and combinations thereof.
[0160] When the aqueous binder is used as the negative electrode binder, a cellulose compound capable of imparting viscosity may be further included. The cellulose compound may include at least one of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, and an alkali metal salt thereof. The alkali metal may include Na, K, or Li.
[0161] The dry binder may be a polymer material capable of being fiberized. For example, the dry binder may be polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, or a combination thereof.
[0162] Conductive materials can be used to impart conductivity (e.g., electrical conductivity) to electrodes. Any material that does not cause chemical changes (e.g., does not cause undesirable chemical changes in rechargeable lithium batteries) and conducts electrons can be used in the battery. Non-limiting examples thereof may include carbon-based materials (such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanofiber, and carbon nanotube); metal-based materials containing copper, nickel, aluminum, silver, etc. in the form of metal powder or metal fiber; conductive polymers (such as polyphenylene derivatives); or mixtures thereof.
[0163] The negative electrode current collector may include copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, or a combination thereof.
[0164] Diaphragm
[0165] Depending on the type of rechargeable lithium battery, the separator may be present between the positive electrode and the negative electrode. The separator may include a polyethylene separator, a polypropylene separator, a polyvinylidene fluoride separator, or a multilayer separator of two or more layers thereof, and a mixed multilayer film (such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, a polypropylene / polyethylene / polypropylene three-layer separator, etc.).
[0166] The separator may include a porous substrate and a coating layer including an organic material, an inorganic material, or a combination thereof on one surface or both surfaces of the porous substrate.
[0167] The porous substrate may be a polymer film formed from any one selected from the following: polyolefins (such as polyethylene and polypropylene), polyesters (such as polyethylene terephthalate and polybutylene terephthalate), polyacetals, polyamides, polyimides, polycarbonates, polyether ketones, polyaryletherketones, polyetherimides, polyamideimides, polybenzimidazoles, polyethersulfones, polyoxyxylenes, cyclic olefin copolymers, polyphenylene sulfide, polyethylene naphthalate, glass fibers, Teflon and polytetrafluoroethylene, or copolymers or mixtures of two or more thereof.
[0168] The organic material may include a polyvinylidene fluoride-based polymer or a (meth)acrylic polymer.
[0169] The inorganic material may include inorganic particles selected from the following: Al 2 O 3 、SiO 2 、TiO 2 SnO 2 、CeO 2 , MgO, NiO, CaO, GaO, ZnO, ZrO 2 , Y 2 O 3 、SrTiO 3 、BaTiO 3 Mg(OH) 2 , boehmite, and combinations thereof, but are not limited thereto.
[0170] An organic material and an inorganic material may be mixed in one coating layer, or a coating layer including an organic material and a coating layer including an inorganic material may be stacked.
[0171] The following examples and comparative examples are provided to emphasize the characteristics of one or more embodiments, but it will be understood that the examples and comparative examples are not to be construed as limiting the scope of the embodiments, nor are the comparative examples to be construed as being outside the scope of the embodiments. Further, it will be understood that the embodiments are not limited to the specific details described in the examples and comparative examples.
[0172] Example 1
[0173] 1. Preparation of electrolyte
[0174] After preparing a nonaqueous organic solvent by sequentially mixing ethylene carbonate (EC), propylene carbonate (PC), ethyl propionate (EP), and propyl propionate (PP) in a volume ratio of 10:15:30:45, 1.3 M lithium salt LiPF 6 dissolved therein to prepare a basic electrolyte.
[0175] To the base electrolyte, the first compound represented by Chemical Formula 1A-1a and the second compound represented by Chemical Formula 2-1 were added to prepare an electrolyte according to Example 1. Herein, 1 wt% of the first compound and 0.5 wt% of the second compound were added based on the total amount of the electrolyte.
[0176] Chemical formula 1A-1a
[0177]
[0178] 2. Manufacturing of rechargeable lithium battery cells
[0179] LiCoO as the positive electrode active material 2 , polyvinylidene fluoride as a binder and ketjen black as a conductive material were mixed together in a weight ratio of 97:2:1, and then dispersed in N-methylpyrrolidone to prepare a positive electrode active material slurry. The positive electrode active material slurry was coated on a 14 μm thick Al foil positive electrode current collector, dried at 110°C, and pressed to manufacture a positive electrode.
[0180] In addition, a negative electrode active material slurry was prepared by mixing artificial graphite as a negative electrode active material, styrene-butadiene rubber as a binder, and carboxymethyl cellulose as a thickener in a weight ratio of 97:1:2, and the mixture was dispersed in distilled water. The negative electrode active material slurry was coated on a 10 μm thick Cu foil negative electrode current collector, dried at 100° C., and pressed to manufacture a negative electrode.
[0181] A 25 μm thick separator having a polyethylene-polypropylene multilayer structure was inserted between the positive electrode and the negative electrode to manufacture an electrode assembly, and a 4.5V-class rechargeable lithium battery cell was manufactured by inserting the electrode assembly into a pouch type battery case and injecting the prepared electrolyte therein.
[0182] The fabricated rechargeable lithium battery cell had a total thickness of about 50 μm.
[0183] Examples 2 to 3 and Comparative Examples 1 to 7
[0184] Respective electrolytes and respective rechargeable lithium battery cells were prepared in substantially the same manner as in Example 1, except that the electrolytes were prepared by changing the contents of the first compound and the second compound and changing the weight ratio of the first compound to the second compound as shown in Table 1.
[0185] Table 1
[0186]
[0187] Evaluation Example 1: Evaluation of the thickness increase rate of a rechargeable lithium battery cell after charge / discharge cycles
[0188] At 25° C., the rechargeable lithium battery cells according to Examples 1 to 3 and Comparative Examples 1 to 7 were charged to an upper limit of 4.5 V under a constant current condition of 0.2 C, paused for 10 minutes, and discharged to 3.0 V under a condition of 0.2 C, which was used as initial charge and discharge. Subsequently, the rechargeable lithium battery cells were repeatedly charged and discharged 200 times at 1.5 C / 1.0 C in the range of 3.0 V to 4.5 V at 45° C.
[0189] Herein, each rechargeable lithium battery cell was measured for thickness just after manufacturing and thickness after 200 cycles for calculating a thickness increase rate (%) after charge / discharge cycles according to Equation 1, and the results are shown in Table 2.
[0190] The thickness of the rechargeable lithium battery cell of Example 1 just after initial charge and discharge was 50 μm, and the thickness of the rechargeable lithium battery cell after 200 cycles was 52.8 μm.
[0191] Equation 1
[0192] Thickness increase rate after charge / discharge cycle (%) = {(thickness of rechargeable lithium battery cell after 200 cycles) - (thickness of rechargeable lithium battery cell just after initial charge / discharge)} / (thickness of rechargeable lithium battery cell just after initial charge / discharge) × 100%
[0193] Evaluation Example 2: Evaluation of high temperature cycle life characteristics
[0194] The rechargeable lithium battery cells according to Examples 1 to 3 and Comparative Examples 1 to 7 were initially charged and discharged and then subjected to 200 cycles of charge and discharge in substantially the same manner as in Evaluation Example 1. The ratio of the discharge capacity at the 200th cycle to the initial discharge capacity was calculated and provided as a high temperature capacity retention rate (%) in Table 2.
[0195] Evaluation Example 3: Evaluation of high temperature storage characteristics
[0196] The rechargeable lithium battery cells according to Examples 1 to 3 and Comparative Examples 1 to 7 were measured for ΔV / ΔI (voltage change / current change) as the initial DC internal resistance (DCIR), and after being fully charged (SOC 100%) as the maximum energy state and stored at high temperature (60°C) for 28 days, the DC internal resistance was also measured in the same manner as for measuring the initial DC internal resistance, for calculating the DCIR increase rate (%) after high temperature storage according to Equation 2, and the results are shown in Table 2.
[0197] Equation 2
[0198] DCIR increase rate after high temperature storage (%) = (DCIR after 28 days / initial DCIR) × 100%
[0199] Table 2
[0200]
[0201] Referring to Table 2, Comparative Example 1 excluding the first and second compounds and Comparative Examples 2 and 3 using one selected from the first and second compounds exhibited a thickness increase rate of more than 10% and worse high temperature cycle life characteristics and high temperature storage characteristics.
[0202] Compared with the embodiment, the comparative example 4 in which the ratio of the second compound to the first compound is greater than 1.3 shows a higher thickness increase rate after the charge / discharge cycle, and shows poor high temperature cycle life characteristics and high temperature storage characteristics compared with the embodiment. Comparative Examples 5 to 7 in which the ratio of the second compound to the first compound is less than 0.3 show almost no or insignificant thickness increase rate after the charge / discharge cycle and thus show unsatisfactory high temperature cycle life characteristics and high temperature storage characteristics. In contrast, the embodiment in which the weight ratio of the first compound to the second compound is in the range of 1:0.3 to 1:1.3 shows a thickness increase rate after the charge / discharge cycle of about 8%, an improved high temperature capacity retention rate of about 90%, and a DCIR increase rate after the reduced high temperature storage of about 130% compared with the comparative example. According to one embodiment, an electrolyte prepared by applying two types (or kinds) of additives in a set ratio can be applied to improve the high temperature cycle life characteristics during fast charging at a high voltage of 4.5V and effectively suppress or reduce the resistance increase during high temperature storage.
[0203] Example embodiments have been disclosed herein, and although specific terms are employed, they are used and interpreted in a generic and descriptive sense only, and not for purposes of limitation. In some cases, as will be apparent to one of ordinary skill in the art at the time of filing this application, features, characteristics, and / or elements described in conjunction with a particular embodiment may be used alone or in combination with features, characteristics, and / or elements described in conjunction with other embodiments, unless specifically indicated otherwise. Accordingly, those skilled in the art will understand that various changes in form and details may be made without departing from the spirit and scope of the invention as set forth in the claims.
Claims
1. An electrolyte for a rechargeable lithium battery, comprising: Non-aqueous organic solvents, lithium salts and additives, wherein the additive comprises a first compound represented by Chemical Formula 1 and a second compound which is CsPF6 or a compound represented by Chemical Formula 2, and The weight ratio of the first compound to the second compound is 1:0.3 to 1:1.3: Chemical formula 1 Wherein, in Chemical Formula 1, Ar is a substituted or unsubstituted C6-C30 aryl group or a substituted or unsubstituted C2-C30 heterocyclic group, and R 1 is O or S, Chemical formula 2 In the chemical formula 2, R 2 and R 3 Each is independently a fluoro group or a C1-C4 fluoroalkyl group substituted by at least one fluoro group.
2. The electrolyte for a rechargeable lithium battery according to claim 1, wherein: The weight ratio of the first compound to the second compound is 1:0.5 to 1:1.
25.
3. The electrolyte for a rechargeable lithium battery according to claim 1, wherein: The electrolyte for a rechargeable lithium battery includes the first compound in an amount of 0.1 wt % to 10.0 wt % based on the total weight of the electrolyte for a rechargeable lithium battery.
4. The electrolyte for a rechargeable lithium battery according to claim 1, wherein: The electrolyte for a rechargeable lithium battery includes the second compound in an amount of 0.01 wt % to 5 wt % based on the total weight of the electrolyte for a rechargeable lithium battery.
5. The electrolyte for a rechargeable lithium battery according to claim 1, wherein: The first compound is represented by Chemical Formula 1A: Chemical formula 1A Wherein, in Chemical Formula 1A, R A , R B , R C , R D and R E are each independently hydrogen, halogen, hydroxyl, cyano, nitro, substituted or unsubstituted C1-C20 alkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted C2-C20 alkenyl, substituted or unsubstituted C2-C20 alkynyl, substituted or unsubstituted C3-C20 cycloalkyl, substituted or unsubstituted C6-C20 aryl or substituted or unsubstituted C2-C20 heteroaryl, and R 1 It is O or S.
6. The electrolyte for a rechargeable lithium battery according to claim 5, wherein: In Chemical Formula 1A, R A , R B , R C , R D and R E Each is independently hydrogen, halogen or substituted or unsubstituted C1-C10 alkyl.
7. The electrolyte for a rechargeable lithium battery according to claim 1, wherein: The first compound is represented by any one selected from Chemical Formula 1A-1 to Chemical Formula 1A-3: Chemical formula 1A-1 Chemical formula 1A-2 Chemical formula 1A-3 Among them, in Chemical Formula 1A-1 to Chemical Formula 1A-3, R 1 It is O or S.
8. The electrolyte for a rechargeable lithium battery according to claim 1, wherein: The compound represented by Chemical Formula 2 is represented by Chemical Formula 2-1 or Chemical Formula 2-2: Chemical formula 2-1 Chemical formula 2-2 9. The electrolyte for a rechargeable lithium battery according to claim 1, wherein: The additive further includes a third compound represented by Chemical Formula 3: Chemical formula 3 Wherein, in Chemical Formula 3, X is C(=O) or S(=O)2, and Y 1 and Y 2 Each is independently a fluoro group or a C1-C5 fluoroalkyl group substituted by at least one fluoro group.
10. The electrolyte for a rechargeable lithium battery according to claim 9, wherein: The third compound is represented by any one selected from Chemical Formula 3-1 to Chemical Formula 3-8: Chemical Formula 3-1 Chemical formula 3-2 Chemical formula 3-3 Chemical formula 3-4 Chemical formula 3-5 Chemical formula 3-6 Chemical formula 3-7 Chemical formula 3-8 Among them, in Chemical Formula 3-3 to Chemical Formula 3-8, R a , R b , R c and R d are each independently hydrogen or fluoro, and n and m are each independently one integer selected from 0-4.
11. The electrolyte for a rechargeable lithium battery according to claim 1, wherein: The electrolyte for a rechargeable lithium battery further comprises other additives, and The other additives include at least one selected from the following: vinylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, vinylethylene carbonate, succinonitrile, adiponitrile, 1,3,6-hexanetrinitrile, propylene sultone, propane sultone, lithium tetrafluoroborate, lithium difluorophosphate and 2-fluorobiphenyl.
12. A rechargeable lithium battery comprising: a positive electrode including a positive electrode active material; a negative electrode including a negative electrode active material; a separator between the positive electrode and the negative electrode; as well as An electrolyte for a rechargeable lithium battery according to any one of claims 1 to 11.
13. The rechargeable lithium battery according to claim 12, wherein: The positive electrode active material includes a lithium cobalt-based oxide.
14. The rechargeable lithium battery according to claim 13, wherein: The lithium cobalt oxide is represented by Chemical Formula 4: Chemical formula 4 Li a1 Yes x1 M 1 1-x1 O2, Wherein, in chemical formula 4, 0.9≤a1≤1.8, 0.7≤x1≤1, and M 1 It is one or more elements selected from Al, B, Ba, Ca, Ce, Cr, Cu, F, Fe, Mg, Mn, Mo, Ni, P, S, Se, Si, Sr, Ti, V, W, Y, Zn and Zr.
15. The rechargeable lithium battery of claim 12, wherein: The negative electrode active material includes crystalline carbon.