Encapsulated corrosion inhibitors
By using microcapsule technology surrounded by polymer shells in aqueous coatings, the toxicity and solubility problems of corrosion inhibitors in the prior art are solved, and excellent corrosion protection and water resistance in the case of thin layers are achieved, and suitable for various metals application.
Patent Information
- Application Number
- CN202380036122.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-26
- Filing Date
- 2023-04-25
- Publication Date
- 2024-12-06
AI Technical Summary
Corrosion inhibitors for direct metal applications in the prior art conventional compositions do not provide sufficient corrosion protection and water resistance, especially in thin layers, and conventionally used corrosion inhibitors have toxicity and environmental problems and are water-insoluble. Corrosion inhibitors are difficult to use in aqueous coatings.
Using a package structure, the core formed by the preferred corrosion inhibitory component is surrounded by a polymer shell to form microcapsules in aqueous coatings, and the interaction with the metal surface is improved by using functional groups, and corrosion protection and adhesion are improved.
It achieves excellent corrosion protection and water resistance in thin layers, avoids the use of toxic substances, improves the stability and adhesion of water-based coatings, and is suitable for various types of direct metal applications.
Smart Images

Figure BDA0005099990720000291 
Figure BDA0005099990720000311 
Figure BDA0005099990720000321
Abstract
Description
[0001] The present invention relates to capsules containing corrosion inhibiting compounds, a process for their preparation and the use of these capsules for releasing corrosion inhibiting components. Background Art
[0002] Today, metal substrates made of, for example, aluminum, aluminum alloys, steel and / or steel alloys are typically often subjected to anti-corrosion and / or adhesion promoting pretreatment processes for a variety of different applications, wherein an organic coating is formed directly on the surface of the metal (direct-to-metal application).
[0003] An example of such direct metal application is the organic dip coating technique, in which coating films with a dry film thickness of about 20 μm are formed on the surface of metal substrates, in particular metal substrates made of galvanized steel or cold rolled steel (CRS) or made of aluminum, which coating films are usually pigmented with black and / or white pigments (such as carbon black and / or titanium dioxide pigments).
[0004] Another example of direct metal application is the so-called permanent coating (PC) technology, in which the metal surface of the substrate and in particular the galvanized surface is treated with an acidic Cr-free thin and usually pigment-free coating formulation to form a thin permanent coating (PC) for corrosion protection, anti-fingerprint properties, water resistance and / or other properties (such as paint adhesion on the substrate surface). Such permanent coatings are usually transparent layers applied with a dry film thickness of about 1 to <2 μm, i.e., with a significantly lower thickness than in the case of the conventional organic dip coating method described above. In particular, on steel surfaces (such as surfaces made of galvanized steel), the applied coating formulation is typically acidic and contains inorganic components (such as metal-fluoride complexes) and formulation additives (such as defoamers and wetting additives) in addition to the polymer dispersion for film-forming ability. However, corresponding alkaline coating formulations can also be used, especially on aluminum-based or aluminum-containing substrate surfaces, and these alkaline coating formulations are usually formulated as 2K coating systems. Polymer dispersions alone are usually not enough to ensure sufficient corrosion protection in each case. Therefore, further inorganic components are usually added to meet corrosion protection requirements, especially industrially, since these inorganic components can react with metal surfaces to form a protective (conversion) layer on the surface. The combination of the above inorganic components with the polymer dispersion produces a uniform film that uniformly covers the metal surface.
[0005] US2012 / 0171402 A1 relates to a method for coating metal surfaces by contacting these surfaces with an aqueous composition, the aqueous composition containing in particular at least one organic film-forming ionomer polymer or copolymer and a low-temperature corrosion inhibiting crosslinking agent having a pH value of 6 to 10.5 and being free of any wax and oil. US2012 / 0171402 A1 aims to provide a corrosion protection coating at a temperature below 80°C PMT (peak metal temperature) at low cost.
[0006] US2013 / 0177768A1 discloses a method for coating a metal surface, comprising the step of applying to the surface an aqueous composition having a pH value of 1 to 4, the composition comprising, inter alia, an inorganic component and a polymer dispersion. US2013 / 0177768A1 aims to provide protective layers formed from the composition on substrates, which protective layers exhibit high moisture resistance and good corrosion resistance.
[0007] WO 2008 / 110480 A1 relates to a method for coating metal surfaces with an aqueous composition which comprises, inter alia, an organic film former, a long-chain alcohol as film-forming aid, an inorganic crosslinker and a lubricant. WO 2008 / 110480 A1 is particularly intended to provide a method which has a high coating speed and uses a composition which does not contain any chromium (VI) and, as far as possible, does not contain inorganic and organic acids.
[0008] WO 2016 / 154680 A1 discloses a method for protecting a substrate from corrosion, the method comprising applying a corrosion inhibitor composition to the surface of the substrate, wherein the corrosion inhibitor composition comprises at least one metal salt or mixed metal salt and at least one organic heterocyclic compound as a corrosion inhibitor. WO 2016 / 154680 A1 aims to provide a chromate-free corrosion inhibitor composition which provides good corrosion protection.
[0009] Conventional compositions disclosed in the prior art, which are generally useful for direct metal applications, in particular for use in the field of organic dip coating and permanent coating technology, do not always provide adequate corrosion protection and / or water resistance and / or adhesion to the substrate and / or to further layers applied thereto. In the case of permanent coating technology, conventional compositions are also not always suitable for providing permanent coatings (PC), in particular when applied at rather thin dry film thicknesses, such as thicknesses of only about 1 μm or less. In particular, when applying conventional compositions on steel surfaces, significant white rust formation can often be observed, which exceeds the amount that can be tolerated by customer requirements, such as those of the coil and appliance industry. In some cases, the amount of white rust formed can be reduced by applying the composition at a higher dry film thickness, for example up to or exceeding 2 μm. However, such higher dry film thicknesses are in turn unacceptable due to customer requirements for permanent coatings for other reasons.
[0010] It is further known to include corrosion inhibitors in conventional compositions for direct metal applications disclosed in the prior art in order to further improve corrosion protection. However, conventionally used corrosion inhibitors known in the prior art often have the following disadvantages: For example, many conventionally used known corrosion inhibitors are labeled as toxic, such as chromium (VI) compounds. Other hazardous or environmentally problematic components for corrosion protection are also known, such as inorganic pigments, for example phosphates, molybdates and other inorganic complexes. Therefore, the use of such corrosion inhibitors is undesirable for ecological reasons, but also for safety and health reasons regarding the personnel handling and using these compounds.
[0011] Furthermore, although a considerable number of corrosion inhibitors (such as various organic compounds) are not necessarily toxic or hazardous - as is the case with the inorganic compounds mentioned above, these compounds are often water-insoluble or substantially water-insoluble. While this may not be considered a problem with respect to the application of solvent-borne compositions, it is certainly disadvantageous for applications where aqueous compositions are to be used and applied, as these types of corrosion inhibitors cannot be used and incorporated into such aqueous compositions, which may be used, for example, to provide a PC layer, due to their low or absent solubility in water, thus limiting their use in aqueous formulations.
[0012] It would therefore be desirable to provide novel corrosion inhibitors for use in and incorporation into aqueous coating compositions for direct metal applications which allow the use of conventionally effective corrosion inhibitors (although these corrosion inhibitors are known to be insoluble or substantially insoluble in water or to have only low water solubility), whereby the resulting aqueous coating compositions should be particularly suitable for providing thin permanent coatings on substrates exhibiting at least the same, but preferably improved, corrosion and / or water resistance, adhesion to the substrate and adhesion to any layers applied thereto as compared to conventionally used aqueous coating compositions.
[0013] question
[0014] It is therefore an object of the present invention to provide novel corrosion inhibitors for use in and incorporation into aqueous coating compositions for direct metal applications which allow the use of conventionally effective corrosion inhibitors (although these corrosion inhibitors are known to be insoluble or substantially insoluble in water or to have only low water solubility), whereby the resulting aqueous coating compositions should be particularly suitable for providing thin permanent coatings on substrates exhibiting at least the same but preferably improved corrosion and / or water resistance, substrate adhesion and adhesion to any layers applied thereto as compared to conventionally used aqueous coating compositions.
[0015] Solution
[0016] This object has been solved by the subject matter of the claims of the present application and by its preferred embodiments disclosed in the present description, ie by the subject matter described herein.
[0017] A first subject of the present invention is a package structure comprising a polymer shell and a core within the shell, wherein
[0018] The shell is obtainable by polymerization of at least one (meth)acrylic monomer or a monomer mixture comprising the at least one (meth)acrylic monomer in the presence of the core, and
[0019] The core comprises at least one preferably corrosion inhibiting component having a water solubility of less than 50 g / L at 23°C in its non-encapsulated state, wherein the core optionally further comprises at least one non-aqueous solvent.
[0020] Solubility in water was measured according to the method disclosed below in the "Methods" section.
[0021] Another subject of the present invention is a method for preparing a package structure according to the present invention, characterized in that the method comprises at least steps a) and b), namely
[0022] a) providing a mixture of (i) at least one (meth)acrylic monomer suitable for forming a polymer shell or a monomer mixture comprising the at least one (meth)acrylic monomer, (ii) at least one preferred corrosion inhibiting component suitable for forming a core, wherein the preferred corrosion inhibiting component may optionally be present in a mixture further comprising at least one non-aqueous solvent, the mixture being suitable for forming an oil phase, and then emulsifying into (iii) water as an aqueous continuous phase, wherein at least one emulsifier and / or surfactant is optionally present, preferably in the aqueous continuous phase (iii) and / or in the mixture formed by (i) and (ii), and
[0023] b) polymerizing the at least one (meth)acrylic monomer or the monomer mixture comprising the at least one (meth)acrylic monomer to form the shell of the encapsulating structure, the encapsulating structure comprising the at least one preferred corrosion inhibiting component as a core within the shell formed upon polymerization, wherein the core may optionally further comprise at least a portion of the at least one non-aqueous solvent.
[0024] A further subject of the present invention is the use of the encapsulation structure of the invention as releasable capsules of corrosion-inhibiting components, in particular for releasing the corrosion-inhibiting compounds present in the shell of the encapsulation structure after at least partial application of an aqueous coating composition containing the encapsulation structure to the surface of an optionally precoated metal substrate to at least partially form a coating film on said surface.
[0025] It has surprisingly been found that corrosion inhibitors which have a solubility in water of ≤5 g / L or are substantially insoluble or insoluble in water can nevertheless be used effectively as corrosion inhibitors in aqueous systems, in particular aqueous acidic coating compositions, but also in corresponding alkaline coating compositions, which are suitable in each case for direct metal application, but in particular for providing thin permanent coatings (PC) on metal substrates, when, before incorporation into the aqueous systems, these corrosion inhibitors are encapsulated into encapsulating structures as the core of the structures, which core is surrounded by or embedded in a polymer shell which is formed at least partially from (meth)acrylic monomers. It has further been found that it is possible and advantageous to prepare shells with monomer units which contain functional groups, such as OH groups and / or COOH groups, and / or groups containing sulfur atoms, such as thioether groups, and / or groups containing phosphorus atoms, such as phosphonic acid groups. When the encapsulation structure is incorporated into an aqueous composition, which is then applied to a metal surface to provide a permanent coating, such functional groups can further serve as anchors to the metal surface for complexing inorganic components present therein, such as H2TiF6 and / or H2ZrF6 and / or fluoride-free Zr- and / or Ti-complexes, and for improving adhesion to any additional coating film applied on top of the PC layer, for example by forming covalent bonds. In addition, the presence of functional groups (such as COOH-groups) and / or groups containing sulfur atoms in the shell can not only lead to a further increase in corrosion protection performance, but can also improve the stability of the coating composition and / or allow the composition to interact better with the metal surface once applied.
[0026] It has been found, particularly surprisingly, that aqueous coating compositions containing at least one encapsulation structure of the present invention are suitable for use in various types of direct metal applications, but are particularly suitable for use as permanent coating compositions which in turn can be used to provide a permanent coating on the surface of a substrate, in particular on metal surfaces such as steel including galvanized steel surfaces. It has been found, in particular, that the encapsulation structure is very stable in acidic media.
[0027] Furthermore, it has been found, particularly surprisingly, that organic coatings (e.g. permanent coatings) formed directly on metal substrates obtained from aqueous coating compositions comprising the encapsulation structure of the invention exhibit excellent corrosion protection and / or water / humidity resistance when present on metal surfaces (e.g. surfaces made of steel), even when applied at a dry film thickness of less than 1.5 μm (e.g. less than 1.3 μm). In particular, no significant white rust formation or even no white rust formation at all is observed in this case. It has been found that encapsulated corrosion inhibitors (e.g. encapsulated benzothiazoles and / or quercetin) enhance the corrosion protection of, in particular, Cr-free PC layers on steel, in particular galvanized steel such as HDG (hot dip galvanized steel). When using corresponding aqueous alkaline coating compositions, in particular on aluminum-based or aluminum-containing substrate surfaces (e.g. ) A similar effect can be observed on aqueous alkaline coating compositions containing the encapsulation structure of the invention. An additional advantage of using such aqueous alkaline coating compositions containing the encapsulation structure of the invention is that such compositions can be used as 1K compositions and the use of, for example, organosilanes conventionally used as corrosion inhibitors in alkaline compositions can be avoided, which have to be added / stored in the form of separate components and therefore require the use of 2K coating systems.
[0028] Furthermore, it has been found, particularly unexpectedly, that the organic coating obtained from the aqueous coating composition comprising the encapsulation structure of the present invention and applied to a metal surface exhibits excellent paint adhesion when any additional coating film (such as a powder coating film) is applied thereon, even when the organic coating is a PC layer applied at a dry film thickness of less than 1.5 μm (such as less than 1.3 μm), and also when the organic coating is applied at a higher dry film thickness (for example, at about 20 μm, which is a typical thickness for organic dip coating applications, especially on galvanized steel or cold rolled steel).
[0029] Furthermore, it has been found that the incorporation of the encapsulation structure of the invention into an aqueous coating composition does not lead to any compatibility problems with its further components, in particular with respect to the inorganic components, and with the at least one film-forming polymer, in particular when at least two different film-forming polymers are used, such as for example at least one (meth)acrylic polymer or copolymer and at least one polyurethane. In particular, no undesirable precipitation of the at least one film-forming polymer is observed. Furthermore, in the case of using at least two different film-forming polymers, such as for example at least one (meth)acrylic polymer or copolymer and at least one polyurethane, no stability problems due to the pH value of the composition and any stabilizing groups of these polymers are observed.
[0030] Furthermore, it has been found that in the case of the use of aqueous coating compositions containing at least two different film-forming polymers, such as for example at least one (meth)acrylic polymer or copolymer and at least one polyurethane, the incorporation of the encapsulation structure of the invention allows at least partial replacement of the polyurethane (e.g. up to 50% of the amount of polyurethane used) without any adverse effect on the water resistance and / or corrosion resistance and adhesion to metal surfaces, and also without any adverse effect on the paint adhesion in the case of the application of an additional coating film on top of the PC layer formed from the aqueous acidic coating composition. This is particularly advantageous for economic reasons, since commercially available and suitable polyurethanes that are stable at acidic pH values are relatively expensive. DETAILED DESCRIPTION
[0031] In the sense of the present invention, the term "comprising", for example in connection with, for example, an aqueous coating composition, preferably has the meaning of "consisting of". For example, with respect to an aqueous coating composition, in addition to all mandatory components present therein, one or more further optional components as identified below may also be included therein. In each case, all components may be present in its preferred embodiments, as identified below.
[0032] The proportions and amounts in wt.-% (weight %) of any components given below that are present in each aqueous coating composition add up to 100 wt.-%, based in each case on the total weight of the aqueous coating composition.
[0033] Package structure
[0034] A first subject of the present invention is an encapsulated structure comprising a polymer shell and a core within the shell, wherein the shell is obtainable by polymerization of at least one (meth)acrylic monomer or a monomer mixture comprising the at least one (meth)acrylic monomer in the presence of the core, and the core comprises at least one preferably corrosion inhibiting component having a water solubility of less than 50 g / L at 23° C. in its non-encapsulated state, wherein the core optionally further comprises at least one non-aqueous solvent. The core is surrounded by or embedded in the polymer shell. The solubility in water is measured according to the method disclosed below in the “Methods” section.
[0035] The encapsulation structure is also referred to herein as a "capsule" or "microcapsule". Capsules and methods for preparing them are known, for example, from US2020 / 108367 A1 and US2019 / 159448 A1.
[0036] Preferably, the encapsulated structure has an average median d50 particle size diameter in the range of 0.1 to 30 μm, more preferably 0.2 to 20 μm, even more preferably 0.3 to 15 μm, still more preferably 0.4 to 10 μm, yet more preferably 0.5 to 7.5 μm, yet more preferably 0.5 to 5.5 μm, yet more preferably 0.5 to 4.0 μm, yet more preferably 0.5 to 3.5 μm, most preferably 0.6 to 3.0 μm. The method for determining the average median d50 particle size diameter is described below in the "Methods" section.
[0037] Preferably, the amount of the shell is in the range of 1 to 70 wt.-%, more preferably 2 to 65 wt.-%, still more preferably 3 to 60 wt.-%, even more preferably 4 to 55 wt.-%, yet more preferably 5 to 50 wt.-%, in each case based on the total weight of the encapsulation structure including shell and core. The total weight of the encapsulation structure can be calculated by adding the weights of the shell and core components used to make the encapsulation structure.
[0038] Preferably, the encapsulated structure is present in an aqueous mixture, more preferably an aqueous dispersion, with water, the mixture preferably having a solids content in the range of 1 to 70 wt.-%, more preferably 2 to 65 wt.-%, even more preferably 3 to 60 wt.-%, still more preferably 5 to 55 wt.-%, yet more preferably 10 to 50 wt.-%, in each case based on the total weight of the aqueous mixture. Preferably, the solids of the solids content of the mixture are due to the encapsulated structure present in the mixture.
[0039] Package structure core
[0040] Preferably, the at least one corrosion inhibiting component present in the core has, in its non-encapsulated state, a water solubility at 23°C of less than 40 g / L, more preferably less than 30 g / L, even more preferably less than 20 g / L, still more preferably less than 15 g / L, even more preferably less than 10 g / L, still more preferably less than 7.5 g / L, still more preferably less than 5.0 g / L, still more preferably less than 2.5 g / L, and most preferably less than 1 g / L.
[0041] Preferably, the corrosion inhibiting component itself is a solid or liquid at 23°C and atmospheric pressure.
[0042] Some suitable corrosion inhibiting components are described, for example, in S. Gangopadhyay et al., J. Coat. Technol. Res. [Journal of Coating Technology and Research] 2018, 15(4), pp. 789-807; ML Zheludkevich et al., Chem. Mater. [Material Chemistry] 2007, 19, pp. 402-411 and SB Ulaeto et al., Progress in Organic Coatings [Progress in Organic Coatings] 2019, 136, 105276.
[0043] Preferably, the corrosion inhibiting component is an inorganic or organic component, more preferably an organic compound, even more preferably an organic compound having at least one alicyclic, heteroalicyclic, aromatic and / or heteroaromatic moiety, still more preferably having at least one C3-C 40 -alicyclic moiety, at least one C3-C 40 -heteroalicyclic moiety, at least one C5-C 40 - an aromatic moiety and / or at least one C5-C 40 -heteroaromatic moiety, the at least one C3-C 40 - the heteroalicyclic moiety comprises at least one heteroatom and / or at least one heteroatom group - wherein the heteroatom is preferably selected in each case from O, N and S, the at least one C5-C 40 The heteroaromatic moiety comprises at least one heteroatom and / or at least one heteroatom group, wherein the heteroatom is preferably selected in each case from O, N and S. Still more preferably, the organic compound comprises at least one C3-C 25 -alicyclic moiety, at least one C3-C 25 -heteroalicyclic moiety, at least one C5-C 25 - an aromatic moiety and / or at least one C5-C 25 -heteroaromatic moiety, the at least one C3-C 25 - the heteroalicyclic moiety comprises at least one heteroatom and / or at least one heteroatom group - wherein the heteroatom is preferably selected in each case from O, N and S, the at least one C5-C 25 The heteroaromatic moiety comprises at least one heteroatom and / or at least one heteroatom group—wherein the heteroatom is preferably selected from O, N and S in each case.
[0044] Examples of corrosion inhibiting components are compounds containing an azole moiety, such as benzotriazole and / or benzothiazole. Further examples are 3-methylsalicylic acid, 4-methylsalicylic acid, 5-methylsalicylic acid, 6-methylsalicylic acid, 3-sulfosalicylic acid, 4-sulfosalicylic acid, 5-sulfosalicylic acid, 6-sulfosalicylic acid, 3-aminosalicylic acid, 4-aminosalicylic acid, 5-aminosalicylic acid, 6-aminosalicylic acid and their salts. Additional examples are benzimidazole, 1-methylbenzimidazole, 1-phenylbenzimidazole, 2-phenyl-benzimidazole, quinaldic acid, nicotinic acid, 1-pyrrolidinedithiocarboxylic acid ammonium salt, catechol, 1H-benzotriazole, 2-phosphonobutane-1,2,4-tricarboxylate ( S particles), iminodiacetic acid, copper iron reagent, 8-hydroxyquinoline, sodium metavanadate, 2-phosphonobutane-1,2,4-tricarboxylic acid ( AM), DL-tartaric acid, iron sulfate heptahydrate, phosphonoformic acid 1,1-diethoxy-ethyl ester-1-oxide, glutaric acid, L-(+)-ascorbic acid, L-(-)-malic acid, mercaptosuccinic acid, resorcinol, rosin / kollophonium, salicylaldehyde oxime, succinic acid, tannic acid, acetylacetonatovanadium, zinc nitrate hexahydrate, 3,4,5-trihydroxybenzoic acid (gallic acid), 4-amino-3-hydroxy-1-naphthalenesulfonic acid, aminosulfonic acid, quercetin, quercetin dihydrate, 2,5-dimercapto-1,3,4-thiadiazole, 2-amino-6-methylbenzothiazole, 2,4-pentanedione barium hydrate, benzimidazole, benzoin oxime, benzothiazole, biuret, CHE-COAT-CI L8AF, CHE-COAT-CI L8NF, ciprofloxacin, hydroquinone, N,N′-bis(salicylidene)-1,2-propylenediamine, N,N′-bis(salicylidene)ethylenediamine, N,N′-dibutylthiourea, N,N′-diethylthiourea, nitrile acetic acid, RIMA-FLASH OGP, 2-mercaptobenzothiazole, 2-nitrophenol, 3-amino-1H-triazole, 3-amino-5-mercapto-1,2,4-triazole, 3-hydroxy-3-methyl-2-butanone oxime, 4-hydroxybenzoic acid, 4-hydroxychalcone, bis(cyclohexanone) oxalyldihydrazone, choline hydroxide, dimethyl maleate, dimethyloxamide, dithiooxamide, dithizone, guanidine nitrate, guanidine thiocyanate, 570, 2-(1,3-Benzothiazol-2-ylthio)succinic acid ( Flash-X350D), urea, hexafluorotitanic acid, imidazole, propargyl alcohol alkoxylate ( PM and PP), benzylpyridine-3-carboxylate, N-allylthiourea, N-guanylthiourea, naphthalene-2-sulfonic acid, neodymoxid, thiosalicylic acid, thiourea, thioacetamide, semicarbazide, trithiocyanuric acid, HighTAC additive G50, methyl-2-thiourea, quinoline, disodium dithiothiazolidine ( NATD), N,N-bis(2-ethylhexyl)-4-methyl-1H-benzotriazole-1-methylamine ( 303), alkylthiadiazole ( 484), 826, 1352, 1351, 1651, Coconut oil alkyl quaternary amine ethoxylate dibutyl thiourea (Armohib CI-31), TT-50, 3-(1H-tetrazolyl-5-yl)aniline, 1-(4-hydroxyphenyl)-5-mercaptotetrazole, 7-hydroxy-5-methyl[1,2,4]triazolo[1,5-a]pyrimidine, 1,2,4-triazole, 5-methyl-1H-benzotriazole, TT-HG, 5-aminotetrazole monohydrate, 5-mercapto-1-methyltetrazole, 3-mercapto-1,2,4-triazole, ASI 80, 4-aminobenzoic acid (PABA), ON-60V, AEP (α-hydrogen-ω-hydroxy-poly(oxy-1,2-ethanediyl) mono-C12-14-alkyl ether, phosphate), dinonylnaphthalenesulfonic acid / carboxylate barium (NaSul BSN-HAT), benzyldimethyltetradecylammonium bromide, benzylcetyldimethylammonium bromide, alkylbenzyldimethylammonium chloride, MI 6627, triaminooctanoic acid triazine ( RC 5402), arylsulfonic acid ( RC 5428), RC 4810, RC 8239, 2-mercaptobenzimidazole (MBI) and 1,2,4-triazole-3-thiol (TT). In addition to benzothiazole and benzotriazole, ciprofloxacin and quercetin are preferred.
[0045] Preferably, the core comprises the at least one corrosion-inhibiting component in an amount of at least 10 wt.-%, more preferably at least 20 wt.-%, still more preferably at least 30 wt.-%, even more preferably at least 40 wt.-%, still more preferably at least 60 wt.-%, even more preferably at least 70 wt.-%, still more preferably at least 80 wt.-%, yet more preferably at least 90 wt.-%, more preferably at least 95 wt.-%, yet more preferably at least 98 wt.-%, in each case based on the total weight of the core. In particular, the core consists of or essentially consists of the at least one corrosion-inhibiting component.
[0046] The core optionally further comprises at least one non-aqueous solvent. The non-aqueous solvent preferably acts as a carrier for dissolving the corrosion inhibiting component to produce a dispersed liquid oil phase before polymerization and to produce an encapsulated core-shell structure thereafter, as will be outlined in detail below. The carrier can further assist in the encapsulation of the at least one corrosion inhibiting component by assisting the at least one corrosion inhibiting component to remain in the core phase during the polymerization of the shell or later during the application process: the presence of the carrier in the core can increase the retention of the corrosion inhibiting component in the capsule. For example, some corrosion inhibiting components can be quite polar and may tend to have a faster release. The use of a carrier can help ensure that the corrosion inhibiting component stays in the core (for a longer time) via a favorable distribution and / or can assist in the distribution between the polymer shell and the core by producing a liquid mixture that is incompatible with the polymer.
[0047] Preferably, the at least one non-aqueous solvent optionally present in the core and preferably present in the core has a boiling point at atmospheric pressure of >100°C, more preferably >125°C, still more preferably >150°C, even more preferably >175°C, still more preferably >200°C, yet more preferably >225°C, most preferably >250°C.
[0048] Preferably, the at least one non-aqueous solvent optionally present in the core (preferably present in the core) has a water miscibility of less than 5 g / L, preferably less than 2.5 g / L, more preferably less than 2.0 g / L, even more preferably less than 1.5 g / L, most preferably less than 1.0 g / L at 23° C. in its non-encapsulated state. The miscibility with water is measured according to the method disclosed below in the “Methods” section.
[0049] Preferably, the at least one non-aqueous solvent optionally present in the core (preferably present in the core) has a water miscibility at 23°C in its non-packaged state, which is lower in g / L than the water solubility at 23°C of the at least one corrosion inhibiting component present in the core (in its non-packaged state).
[0050] Preferably, the core comprises the at least one non-aqueous solvent in an amount of at most 80 wt.-%, more preferably at most 50 wt.-%, even more preferably at most 30 wt.-%, yet more preferably at most 20 wt.-%, yet more preferably at most 10 wt.-%, more preferably at most 5 wt.-%, yet more preferably at most 2 wt.-%, in each case based on the total weight of the core. In particular, the core does not comprise or essentially does not comprise the at least one non-aqueous solvent.
[0051] Preferably, the at least one non-aqueous solvent is a hydrocarbon, more preferably an aliphatic hydrocarbon, wherein the hydrocarbon may, however, optionally further contain one or more heteroatoms or one or more heteroatom groups in addition to carbon atoms and hydrogen atoms, wherein the heteroatoms are in each case preferably selected from N, S and O. More preferably, the at least one non-aqueous solvent has at least one aliphatic and / or heteroaliphatic moiety, still more preferably at least one C5-C 40 - an aliphatic moiety, at least one C5-C 40 -heteroaliphatic moiety, the at least one C5-C 40 The heteroaliphatic moiety comprises at least one heteroatom and / or at least one heteroatom group-wherein the heteroatom is preferably in each case selected from O, N and S. The at least one nonaqueous solvent may preferably be selected from ethers, esters and amides and mixtures thereof.
[0052] Examples of the at least one nonaqueous solvent are in particular: Guerbet alcohols based on fatty alcohols having 6 to 18, preferably 8 to 10, carbon atoms, linear C6-C 22 -Fatty acids with straight or branched C6-C 22 -Amides or branched C6-C 13 -Carboxylic acid with straight or branched C6-C 22 - Amides of fatty amines, amines having 6 to 18, preferably 8 to 10, carbon atoms, linear C6-C 22 -Fatty acids with straight or branched C6-C 22 -Fatty alcohol esters or branched C6-C 13 -Carboxylic acid with straight or branched C6-C 22- esters of fatty alcohols, such as, for example, myristyl myristate, myristyl palmitate, myristyl stearate, myristyl isostearate, myristyl oleate, myristyl behenate, myristyl erucate, cetyl myristate, cetyl palmitate, cetyl stearate, cetyl isostearate, cetyl oleate, cetyl behenate, cetyl erucate, stearyl myristate, stearyl palmitate, stearyl stearate, stearyl isostearate, stearyl oleate, stearyl behenate, stearyl erucate, isostearyl myristate, isostearyl palmitate, isostearyl stearate Suitable are isostearyl isostearate, isostearyl oleate, isostearyl behenate, isostearyl oleate, oleyl myristate, oleyl palmitate, oleyl stearate, oleyl isostearate, oleyl oleate, oleyl behenate, oleyl erucate, behenyl myristate, behenyl palmitate, behenyl stearate, behenyl isostearate, behenyl oleate, behenyl behenate, behenyl erucate, erucyl myristate, erucyl palmitate, erucyl stearate, erucyl isostearate, erucyl oleate, erucyl behenate and erucyl erucate. Also suitable are straight chain C6-C 22 - Esters of fatty acids and branched alcohols (especially 2-ethylhexanol), C 18 -C 38 -alkyl hydroxycarboxylic acid with a straight or branched C6-C 22 - esters of fatty alcohols, in particular dioctyl malate, esters of linear and / or branched fatty acids with polyols (such as, for example, propylene glycol, dimer diol or trimer triol) and / or Guerbet alcohols, based on C6-C 10 -Triglycerides of fatty acids, based on C6-C 18 -Liquid mono / di / triglyceride mixture of fatty acids, C6-C 22 - esters of fatty alcohols and / or Guerbet alcohols with aromatic carboxylic acids, in particular benzoic acid, C2-C 12 - esters of dicarboxylic acids with straight-chain or branched alcohols having 1 to 22 carbon atoms or polyols having 2 to 10 carbon atoms and 2 to 6 hydroxyl groups, vegetable oils, branched primary alcohols, substituted cyclohexanes, straight-chain and branched C6-C 22 - fatty alcohol carbonates, such as, for example, dicaprylyl carbonate ( CC), Guerbet carbonates based on fatty alcohols having 6 to 18, preferably 8 to 10, carbon atoms, benzoic acid and linear and / or branched C6-C 22 -esters of alcohols, linear or branched, symmetrical or asymmetrical dialkyl ethers (such as dioctyl ether, for example), each alkyl radical having 6 to 22 carbon atoms, ring-opening products of epoxidized fatty acid esters and polyols, silicone oils (cyclomethicone, polysiloxane polymethicone grades, etc.), aliphatic or cycloalkane (such as squalane, squalene or dialkylcyclohexanes), and / or mineral oils. In one form, the oil preferably comprises an aliphatic or cycloalkane, and / or a mineral oil.
[0053] An example of a suitable non-aqueous solvent is BASF or Series, such as B. OE, Sensoft and AMD 10 is a commercial product. AMD 10 is N,N-dimethyldecane-1-amide. OE is dioctyl ether, Sensoft is 2-propylheptyl octanoate and B is a liquid adipate. These solvents are considered "green" solvents.
[0054] Encapsulation structure shell
[0055] The shell of the encapsulating structure is polymeric. In the case that only one monomer is used, such as exactly one (meth)acrylic monomer m1, for preparing the shell, the shell may be a homopolymer. However, it may also be a copolymer and preferably a copolymer prepared from more than one monomer.
[0056] The term "(meth)acryloyl" means "acryloyl" and / or "methacryloyl". Similarly, "(meth)acrylate" means acrylate and / or methacrylate. The shell is a "(meth)acryloyl polymer" which is at least partly formed from "acryloyl monomers" and / or "methacryloyl monomers", but may additionally contain non-acryloyl and non-methacryloyl monomer units if other ethylenically unsaturated monomers (such as vinyl monomers) are additionally used for its preparation. Preferably, the shell is formed from more than 40 wt.-%, even more preferably more than 50 wt.-%, still more preferably more than 60 wt.-% of (meth)acryloyl monomers.
[0057] Preferably, the shell is obtainable from at least one (meth)acrylic monomer m1, from at least a monomer m2, from a monomer mixture comprising the at least one (meth)acrylic monomer m1 and optionally at least one further monomer m2 and / or optionally at least one further monomer m3, or from a monomer mixture comprising the at least one monomer m2 and optionally at least one further monomer m1 and / or optionally at least one further monomer m3, m2 and m3 both being different from each other and from the monomer m1,
[0058] The at least one (meth) acrylic monomer m1 is a non-functional (meth) acrylic monomer, preferably an aliphatic C1-C 30 - (meth)acrylates of monohydric alcohols,
[0059] The monomer m2 optionally present in the monomer mixture is a monomer having at least one ethylenically unsaturated group and further having at least one functional group, wherein the at least one functional group is preferably selected from hydroxyl groups, ether groups, carbonyl groups, amino groups, epoxy groups, carboxylic acid groups, sulfur-containing functional groups and phosphorus-containing groups, wherein the monomer m2 is preferably a (meth)acrylic monomer, and
[0060] Among the monomers m3 optionally present in the monomer mixture are monomers having at least two ethylenically unsaturated groups.
[0061] Monomer m1 is preferably a (meth)acrylic monomer with a hydrophobic group. Preferably, m1 contains exactly one (meth)acrylic group. 30 Examples of (meth)acrylic acid esters of monohydric alcohols are methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, lauryl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 3-propylheptyl (meth)acrylate, stearyl (meth)acrylate, behenyl (meth)acrylate, benzyl (meth)acrylate, cyclohexyl (meth)acrylate and isobornyl (meth)acrylate.
[0062] Monomer m2 is used so as to preferably functionalize the shell of the encapsulation structure. Monomer m2 is preferably a monomer selected from vinyl monomers and / or (meth) acrylic monomers. Preferably, m2 contains just one (meth) acrylic acid group or just one vinyl group. Examples of groups containing sulfur atoms present as the functional group of monomer m2 are thiol groups, thioether groups, thioester groups and thiocarboxylic acid groups and mixtures thereof, more preferably thioether groups, thioester groups and thiocarboxylic acid groups and mixtures thereof. Examples of groups containing phosphorus atoms present as the functional group of monomer m2 are phosphonic acid groups, phosphoric acid groups and mixtures thereof. Examples of monomers that can be used as monomer m2 are 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 3-hydroxypropyl acrylate, 3-hydroxypropyl methacrylate, 4-hydroxybutyl acrylate, 4-hydroxybutyl methacrylate, 3-phenoxy-2-hydroxypropyl (meth)acrylate, glyceryl mono(meth)acrylate, N-(2-hydroxypropyl) (meth)acrylamide, allyl alcohol, hydroxystyrene, hydroxyalkyl vinyl ethers (e.g., hydroxybutyl vinyl ether) and vinylbenzyl alcohol as well as acrylic acid and methacrylic acid, vinyl mercapto alcohol (e.g., vinylmercaptoethanol), vinylthiazole and vinylthiophene, glycidyl (meth)acrylate, N,N-dimethylaminoethyl acrylate, N,N-dimethylaminoethyl methacrylate, N,N-dimethylaminopropyl acrylate, N,N-dimethylaminopropyl methacrylate, 2-(N,N-diethylamino)ethyl (meth)acrylate, 2-(N,N-dimethylamino)ethyl (meth)acrylate, N -[3-(N,N-dimethylamino)propyl](meth)acrylamide, 3-dimethylaminoneopentyl(meth)acrylate, 2-N-morpholinoethyl(meth)acrylate, N-[3-(N,N-dimethylamino)propyl](meth)acrylamide, 2-(N,N-diethylamino)ethyl(meth)acrylamide, 2-(tert-butylamino)ethyl(meth)acrylate, 2-diisopropylaminoethyl(meth)acrylate, N-dodecylacrylamide and N-[2-(N,N-dimethylamino)ethyl](meth)acrylamide, N,N-dimethyl(meth)acrylamide, 2-vinylpyridine, 4-vinylpyridine, allylamine, (meth)acrylamide and vinylimidazole, N-vinyl-pyrrolidone, vinyl acetate, N-vinylformamide, as well as N,N-diethylaminostyrene (all isomers) and N,N-diethylamino-α-methylstyrene (all isomers) and vinylphosphonic acid. Vinylmercaptoethanol is particularly preferred.
[0063] It is also possible to introduce, for example, sulfur-containing groups later in a polymer-analogous reaction. Preferably, in the case of introducing the moiety after the polymerization reaction has taken place, a monomer containing a moiety suitable for subsequent modification is used as monomer m2 for the polymerization. Preferably, at least one monomer selected from the group consisting of preferably (meth) acrylic monomers having at least one epoxy group is used. Most preferably, glycidyl (meth) acrylate. In order to introduce at least one sulfur-containing moiety, a suitable S-containing compound is used, preferably a compound having at least one thiol group. The thiol group can react with the epoxide moiety after the ring opening of the epoxy group and form at least one sulfur-containing moiety. Preferably, the S-containing compound is selected from the group consisting of dithiols (such as 1,2-ethanedithiol), mercapto alcohols (such as mercaptoethanol), thiocarboxylic acids (such as thioacetic acid (CH3-C(=O)SH), mercapto acids (such as HS-CH2-C(=O)OH), mercapto esters (such as HS-CH2-C(=O)R, wherein R is a hydrocarbon group, preferably an aliphatic group) and mercapto-functional compounds with more than one additional functional group (such as both at least one amino group and at least one carboxylic acid group) (e.g. L-cysteine).
[0064] As outlined above, monomer m3 has at least two ethylenically unsaturated groups, which are preferably non-conjugated. If there are just two ethylenically unsaturated groups, the monomer represents a difunctional monomer. The difunctional monomer can be a limited small molecule or can be based on a polymer. For example, a linear end functional polymer can be modified to produce a difunctional crosslinking agent, and then used as a difunctional monomer. In some cases, vinyl bonds can also be introduced into the main polymer chain during polymer synthesis. The difunctional monomer based on polymer can be described as a difunctional monomer. If there are more than two ethylenically unsaturated groups, the monomer represents a multifunctional monomer. The multifunctional monomer can be a limited small molecule or can be based on a polymer. For example, a branched or hyperbranched end functional polymer can be modified to produce a multifunctional crosslinking agent, and then used as a multifunctional monomer. In some cases, vinyl bonds can also be introduced into the main polymer chain during polymer synthesis. The multifunctional monomer based on a polymer can be described as a multifunctional monomer. Monomer m3 is preferably a monomer selected from vinyl monomers and / or (meth) acrylic monomers. Monomer m3 is preferably used as a crosslinking monomer because it carries at least two ethylenically unsaturated groups when forming a polymer shell. Preferably, it has at least two vinyl groups or at least two (meth) acrylic acid groups. Suitable difunctional monomers are divinylbenzene (DVB), divinylcyclohexane, the diester of glycol and (meth) acrylic acid and the diallyl ether and divinyl ether of such glycols, such as ethylene glycol di(meth)acrylate, ethylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, methallyl methacrylamide and allyl (meth)acrylate. Suitable difunctional monomers are PEG di(meth)acrylate, PPG di(meth)acrylate, polyglycerol di(meth)acrylate, polyurethane di(meth)acrylate resin and polyester di(meth)acrylate. Suitable multifunctional monomers are PEG with more than two (meth)acrylate groups, PPG with more than two (meth)acrylate groups, polyglycerol with more than two (meth)acrylate groups, polyurethane with more than two (meth)acrylate groups, and polyester with more than two (meth)acrylate groups. Other suitable multifunctional monomers are polyesters of polyols and (meth)acrylic acid, as well as polyallyl ethers and polyvinyl ethers of such polyols, trivinylbenzene, and trivinylcyclohexane. Specific examples of difunctional monomers m3 are 1,4-butylene glycol diacrylate (BDDA), 1,4-butylene glycol dimethacrylate, 1,5-pentanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, methacrylic anhydride (MAA), divinylbenzene (DVB), and divinylcyclohexane. Specific examples of the multifunctional monomer m3 are trivinylbenzene, trivinylcyclohexane, trimethylolpropane tri(meth)acrylate, pentaerythritol tetraallyl ether and pentaerythritol tri(meth)acrylate.The incorporation of monomer unit mu3 derived from monomer m3 is advantageous since its presence avoids an early release of the corrosion inhibiting compound upon storage of the microcapsule dispersion by creating a dense crosslinked polymer network around the core. However, upon application to a metal surface, mu3 facilitates the release of the corrosion inhibiting compound from the polymer shell of the encapsulating structure or optimizes the release rate of the corrosion inhibiting compound, if necessary, for example at the corrosion front. For example, BDDA is sensitive to alkaline pH, where corrosion occurs. The higher the amount of monomer unit mu3 in the shell, the slower the early release before application, since the shell is more "crosslinked". However, at the corrosion front where the pH is higher, the crosslinker will hydrolyze, resulting in a change in the polarity of the shell and an optimal release of the corrosion inhibiting compound. On the other hand, the amount of monomer unit mu3 should preferably not be too high since this could lead to undesirable aggregate formation during microcapsule manufacturing.
[0065] Additional monomers, such as at least one monomer m4, may optionally further be used to prepare the shell. Examples of such monomers m4 are non-functional, such as non-(meth)acrylic non-functional monomers, for example styrene.
[0066] Preferably, monomers m3 are used in addition to the monomers m1 for preparing the shell. As a result of the use of monomers m3, the polymer shell is therefore preferably at least branched or completely crosslinked.
[0067] Preferably, the shell
[0068] contains only monomer units mu1 derived from the at least one (meth)acrylic monomer m1, and contains no other monomer units except the monomer units m1,
[0069] or containing monomer units mu1 derived from the at least one (meth)acrylic monomer m1 in an amount in the range of 60 to 99 wt.-%, preferably 65 to 95 wt.-%, more preferably 70 to 90 wt.-% and monomer units mu2 derived from the at least one monomer m2 in an amount in the range of 1 to 40 wt.-%, preferably 5 to 35 wt.-%, more preferably 10 to 30 wt.-%,
[0070] or containing monomer units mu1 derived from the at least one (meth)acrylic monomer m1 in an amount in the range of 40 to 99 wt.-%, preferably 50 to 95 wt.-%, more preferably 50 to 90 wt.-% and monomer units mu3 derived from the at least one monomer m3 in an amount in the range of 1 to 60 wt.-%, preferably 5 to 50 wt.-%, more preferably 10 to 50 wt.-%,
[0071] Or contains monomer units mu1 derived from the at least one (meth)acrylic monomer m1 in an amount ranging from 30 to 98 wt.-%, preferably 36 to 92 wt.-%, more preferably 44 to 86 wt.-%, monomer units mu2 derived from the at least one monomer m2 in an amount ranging from 1 to 35 wt.-%, preferably 4 to 32 wt.-%, more preferably 5 to 25 wt.-% and monomer units mu3 derived from the at least one monomer m3 in an amount ranging from 1 to 50 wt.-%, preferably 2 to 45 wt.-%, more preferably 5 to 40 wt.-%.
[0072] Of course, the sum of all monomers used for preparing the shell amounts to 100 wt.-% in each case.
[0073] Preferably, the amount of monomer units mu1 in the shell exceeds by wt.-% the amount of any monomer units mu2 and / or mu3 also present.
[0074] Preparation of packaging structure
[0075] Another subject of the present invention is a method for preparing a package structure according to the present invention, characterized in that the method comprises at least steps a) and b), namely
[0076] a) providing a mixture of (i) at least one (meth)acrylic monomer suitable for forming a polymer shell or a monomer mixture comprising the at least one (meth)acrylic monomer, (ii) at least one preferred corrosion inhibiting component suitable for forming a core, wherein the preferred corrosion inhibiting component may optionally be present in a mixture further comprising at least one non-aqueous solvent, the mixture being suitable for forming an oil phase, and then emulsifying into (iii) water as an aqueous continuous phase, wherein at least one emulsifier and / or surfactant is optionally present, preferably in the aqueous continuous phase (iii) and / or in the mixture (oil phase) formed by (i) and (ii), and
[0077] b) polymerizing the at least one (meth)acrylic monomer or the monomer mixture comprising the at least one (meth)acrylic monomer to form the shell of the encapsulating structure, the encapsulating structure comprising the at least one preferred corrosion inhibiting component as a core within the shell formed upon polymerization, wherein the core may optionally further comprise at least a portion of the at least one non-aqueous solvent.
[0078] All the preferred embodiments described above in conjunction with the packaging structure of the present invention and its preferred embodiments are also preferred embodiments of the preparation method thereof of the present invention.
[0079] In step a), (i) and (ii) are dispersed in water (iii). (i) and (ii) form a hydrophobic phase (oil phase), while (iii) forms an aqueous phase used as a continuous phase. Therefore, when two phases are present, the process of the present invention comprising steps a) and b) is preferably an oil-in-water emulsion polymerization. When the corrosion-inhibiting compound is liquid at 23° C. and atmospheric pressure, the compound can be used in particular as (ii) without any non-aqueous solvent. In the case where the compound is solid at 23° C. and atmospheric pressure and the monomers used to prepare the shell cannot dissolve the compound, it is preferably dissolved with the aid of at least one non-aqueous solvent so as to produce a liquid oil phase, which is then emulsified into water.
[0080] As outlined above, the process of the present invention comprising steps a) and b) is preferably an oil-in-water emulsion polymerization, especially when a mixture of a corrosion inhibiting component and at least one non-aqueous solvent is used. During the formation of the microcapsules, the shell monomers are polymerized to form a polymer shell around the core. Polymerizing the shell monomers can form microcapsules comprising a core of an oil phase within a polymer shell. Preferably, during the emulsification and polymerization process, the shell monomers are present in the oil phase.
[0081] One or more emulsifiers and / or one or more surfactants may be used to produce a stable emulsion and / or suspension. These may be dissolved into the aqueous continuous phase and / or the oil phase to assist in the emulsification of the oil phase.
[0082] One or more polymeric stabilizers can be used. The polymeric stabilizer can be included in the continuous aqueous phase and / or the oil phase, preferably in the aqueous phase. The polymeric stabilizer can be a hydrophilic polymer, for example a polymer containing hydroxyl groups, such as polyvinyl alcohol. Polyvinyl alcohol can be used in the form of its aqueous solution. Polyvinyl alcohol can be derived from polyvinyl acetate, wherein some or all of the vinyl acetate groups are hydrolyzed into vinyl alcohol units. Other types of polymeric stabilizers are suitable nanoparticles that allow pickering stabilization.
[0083] Preferably, the polymerization is a free radical polymerization. Thus, preferably, one or more initiator compounds are used, such as redox initiators and / or thermal initiators. Suitable thermal initiators are, for example, dialkyl peroxides, hydroperoxides, peroxyesters, peroxyketals, diacyl peroxides, peroxy(di)carbonates, persulfates and / or azo initiators. Redox initiators may include reducing agents, such as sodium sulfite, sulfur dioxide; and oxidizing compounds, such as ammonium persulfate or suitable peroxy compounds (such as tert-butyl hydroperoxide).
[0084] Preferably, step b) is carried out at a temperature in the range of 5 to 100°C, more preferably 40 to 95°C.
[0085] Purpose of packaging structure
[0086] A further subject of the present invention is the use of the encapsulation structure of the invention as releasable capsules of corrosion-inhibiting components, in particular for releasing the corrosion-inhibiting compounds present in the shell of the encapsulation structure after at least partial application of an aqueous coating composition containing the encapsulation structure to the surface of an optionally precoated metal substrate to at least partially form a coating film on said surface.
[0087] All preferred embodiments described above in conjunction with the inventive packaging structure, its method for production and in each case its preferred embodiments are also preferred embodiments of the inventive use.
[0088] The metal substrate is preferably a substrate made at least partially of steel, preferably galvanized steel, steel alloys, aluminum, aluminum alloys, zinc, zinc alloys and mixtures thereof; more preferably a substrate made at least partially of steel, and / or steel alloys, and / or zinc, and / or zinc and aluminum alloys, and / or zinc, aluminum and magnesium alloys. Preferably, the metal substrate is not pre-coated.
[0089] The aqueous coating composition containing the encapsulation structure used is preferably an acidic or alkaline aqueous coating composition, more preferably an acidic aqueous coating composition. Preferably, it contains, in addition to water, at least one film-forming polymer, at least one metal ion selected from the group of titanium ions, zirconium ions, hafnium ions and mixtures thereof (preferably in the form of their complex fluorides) and at least one encapsulation structure according to the invention.
[0090] In the sense of the present invention, the term "aqueous" with respect to a composition preferably means that the composition is a composition which contains at least 50 wt.-%, preferably at least 60 wt.-%, more preferably at least 70 wt.-%, in particular at least 80 wt.-%, most preferably at least 90 wt.-% of water, based on its total content of organic and inorganic solvents including water. Thus, the composition may contain at least one organic solvent other than water, however, in an amount lower than the amount of water present. Preferably, the acidic aqueous composition contains at least 50 wt.-%, preferably at least 60 wt.-%, more preferably at least 65 wt.-%, in particular at least 70 wt.-%, most preferably at least 70 and at most 90 wt.-% of water, in each case based on its total weight. The total amount of all components present in the composition according to the invention amounts to 100 wt.-%.
[0091] The term "acidic" means that the composition has a pH value of less than 7 at room temperature (23°C). Preferably, the aqueous coating composition has a pH value in the range of 0.1 to <7.0, more preferably 0.5 to 6.5, still more preferably 1.0 to 6.0, even more preferably 1.5 to 5.5, still more preferably 2.0 to 5.0, yet more preferably 2.5 to 4.5, most preferably 3.0 to 4.0. The pH can preferably be adjusted by using nitric acid, ammonia and / or sodium carbonate. The term "alkaline" means that the composition has a pH value of ≥7 at room temperature (23°C). Preferably, when alkaline, the aqueous coating composition has a pH in the range of ≥7.0 to 14.0, more preferably >7.0 to 13.5, still more preferably >7.0 to 13.0, even more preferably >7.0 to 12.5, still more preferably >7.0 to 12.0, yet more preferably 7.5 to 11.5, yet more preferably 8.0 to 11.0, yet more preferably 8.5 to 10.5.
[0092] The composition may be a dispersion or a solution. Preferably, it is a dispersion.
[0093] Film-forming polymers represent adhesives. For purposes of the present invention, the term "adhesive" is preferably understood as a non-volatile (solid) component of a coating composition according to DIN EN ISO 4618 (German version, date: March 2007), which is responsible for film formation. The term includes crosslinking agents (crosslinking agent / crosslinker) and additives such as catalysts (if they represent non-volatile components). Pigments and / or fillers are not included under the term "adhesive" because these are not responsible for film formation. The term "polymer" is also known to those skilled in the art and for purposes of the present invention, covers addition polymers and polymerizates and polycondensates. The term "polymer" includes both homopolymers and copolymers.
[0094] Preferably, the aqueous coating composition does not comprise any pigment and / or filler.Preferably, the aqueous coating composition contains no or substantially no chromium (VI) ions, more preferably contains no or substantially no chromium ions.
[0095] Preferably, the aqueous coating composition contains the at least one encapsulation structure according to the invention in an amount in the range of 0.1 to 20 wt.-%, more preferably 0.2 to 18 wt.-%, still more preferably 0.3 to 16 wt.-%, even more preferably 0.4 to 14 wt.-%, still more preferably 0.5 to 12 wt.-%, yet more preferably 0.6 to 10 wt.-%, yet more preferably 0.7 to 9.5 wt.-%, yet more preferably 0.8 to 9.0 wt.-%, yet more preferably 0.9 to 8.5 wt.-%, most preferably 1.0 to 8.0 wt.-%, in each case based on the total weight of the aqueous coating composition.
[0096] Preferably, the aqueous coating composition has a solids content in the range of 15 to 45 wt.-%, more preferably 20 to 40 wt.-%, even more preferably 20 to 35 wt.-%.The solids content is determined according to the method disclosed in the "Methods" section.
[0097] The aqueous coating composition preferably comprises at least one metal ion selected from the group of titanium ion, zirconium ion, hafnium ion and mixtures thereof. When the aqueous coating composition is acidic, the at least one metal ion preferably exists or is used in the form of at least its complex fluoride in each case. When the aqueous coating composition is alkaline, the at least one metal ion preferably exists or is used in the form of at least its carbonate and / or complex carbonate and / or its lactate in each case, preferably exists or is used in the form of fluoride-free in each case. Particularly preferred are titanium ion and zirconium ion and mixtures thereof. When the metal substrate mentioned above has or contains aluminum, zirconium ion is most preferred. When the metal substrate mentioned above has or contains steel, and / or zinc, and / or zinc and aluminum alloy, and / or zinc, aluminum and magnesium alloy, titanium ion is most preferred. Preferably, the at least one metal ion selected from the group of titanium ions, zirconium ions, hafnium ions and mixtures thereof, preferably selected from the group of zirconium ions and titanium ions, is present in the composition in an amount in the range of 50 to 50000 ppm, more preferably 75 to 40000 ppm, still more preferably 100 to 30000 ppm, even more preferably 125 to 20000 ppm, yet more preferably 150 to 15000 ppm, in particular 175 to 10000 ppm, more particularly 200 to 8000 ppm, most preferably 300 to 6000 ppm, in each case calculated as metal. This content can be monitored and determined by ICP-OES (Inductively Coupled Plasma Optical Emission Spectroscopy). Preferably, a precursor metal compound is used to generate the metal ions. Preferably, the precursor metal compound is water-soluble. Particularly preferred titanium compounds, zirconium compounds and hafnium compounds used as precursor metal compounds are complex fluorides of these metals, in particular when the aqueous composition is acidic. The term "complex fluoride" includes monoprotonated and polyprotonated forms as well as deprotonated forms. Mixtures of such complex fluorides can also be used. In the sense of the present invention, complex fluorides are complexes of titanium, zirconium and / or hafnium formed with fluoride ions in the composition (for example by coordination of fluoride anions to titanium, zirconium and / or hafnium cations in the presence of water). In addition, zirconium can also be added in the form of: zirconyl compounds, for example as zirconyl nitrate and zirconyl acetate; or zirconium carbonate or zirconium nitrate, the latter being particularly preferred, especially when the aqueous composition is acidic. The same applies to titanium and hafnium. As outlined above, other precursor compounds can also be used, such as, for example, zirconium carbonate, especially when the aqueous composition is alkaline.
[0098] The aqueous coating composition preferably comprises at least one film-forming polymer, which is preferably different from the polymer shell of the encapsulation structure. Any type of film-forming polymer can be used. In particular, the polymer disclosed in US 2013 / 0177768A 1 is suitable. Most preferably, cationic and / or nonionic polymers. Preferably, the aqueous coating composition comprises at least two different film-forming polymers, more preferably at least one (meth) acrylic polymer or copolymer and at least one polymer comprising at least one polyurethane part. In this case, preferably, the amount of the (meth) acrylic polymer or copolymer present preferably exceeds the amount of the at least one polymer comprising at least one polyurethane part. Any type of (meth) acrylic polymer or copolymer can be used. Copolymers are preferred. These copolymers can include monomer units from non-(meth) acrylic monomers (such as ethylene monomers). The polymer comprising at least one polyurethane part preferably has a certain content of polyether, preferably polycarbonate. Cationic polymers comprising at least one polyurethane part are particularly preferred. Examples are polyester-polyurethane, polyester-polyurethane-poly (meth) acrylate, polycarbonate-polyurethane and / or polycarbonate-polyurethane-poly (meth) acrylate. Preferably, the hydrophilic cationic groups are incorporated into the backbone and / or side chains of the cationic polymer comprising at least one polyurethane part via at least one amine, in particular via at least one alkanolamine, such as, for example, N-alkyldialkanolamine. Preferably, quaternary ammonium groups are incorporated into the backbone of the cationic polymer comprising at least one polyurethane part. These groups may optionally have acid groups as anionic counterions, and / or quaternizing agent groups, which are formed when, for example, acetic acid and / or phosphoric acid are used as acids and / or when, for example, dibutyl sulfate and / or benzyl chloride are used as quaternizing agents.
[0099] The aqueous composition may contain additional components as listed below. The aqueous composition preferably contains free fluoride. These may be produced by the presence of metal ions as mentioned above (i.e., particularly when there are complex fluorides of Ti, Zr and / or Hf), but may also or alternatively be produced by the presence of other optional components as described below. Preferably, the aqueous composition contains free fluoride in an amount in the range of 1 to 500 ppm, more preferably 1.5 to 200 ppm, even more preferably 2 to 100 ppm, particularly 2.5 to 50 ppm. The free fluoride content is determined by a fluoride ion sensitive electrode.
[0100] Optionally, the aqueous composition further comprises at least one metal cation selected from the group of cations of metals of the 1st to 3rd subgroups (copper, zinc and scandium) and the 5th to 8th subgroups (vanadium, manganese and iron) of the periodic table (including lanthanides) and the 2nd main group (alkaline earth metal group) of the periodic table, lithium and bismuth. Optionally, the aqueous composition further comprises at least one pH-adjusting substance, which is preferably selected from the group consisting of nitric acid, sulfuric acid, methanesulfonic acid, acetic acid, ammonia water, sodium hydroxide and sodium carbonate, wherein nitric acid, phosphoric acid, ammonia water and sodium carbonate are preferred. Depending on the pH of the aqueous composition, the above compounds can be present in their fully or partially deprotonated form or in a protonated form.
[0101] Optionally, the aqueous composition further comprises at least one complexing agent. An example is 1-hydroxyethane-1,1-diphosphonic acid (HEDP).
[0102] Alternatively, the aqueous composition further comprises at least one water-soluble fluorine compound. Examples of such water-soluble fluorine compounds are fluorides and hydrofluoric acid. In particular, when the above-mentioned one or more metal ions are not present in the composition in the form of complex fluorides of titanium, zirconium and / or hafnium, such compounds are present in the composition. Alternatively, the aqueous composition further comprises at least one organosilane. Examples are such as (3-aminopropyl) trimethoxysilane, (3-aminopropyl) triethoxysilane, N-2-aminoethyl-3-aminopropyl trimethoxysilane, (3-mercaptopropyl) trimethoxysilane, (3-mercaptopropyl) triethoxysilane, (3-glycidyloxypropyl) trimethoxysilane and / or (3-glycidyloxypropyl) triethoxysilane, vinyl trimethoxysilane, particularly when the aqueous composition is acidic. Optionally, The aqueous composition further comprises at least one organic acid, preferably at least one organic acid having at least two carboxylic acid groups and / or at least one organic acid having at least one carboxylic acid group and at least one further functional group having at least one donor atom (such as an OH-group), such as lactic acid, in particular when the aqueous composition is alkaline. The presence of such compounds can contribute to the stabilization of at least one metal ion (such as a Zr cation) in the composition. The aqueous composition can further comprise at least one of the following components: one or more waxes, one or more wetting agents and one or more defoamers.
[0103] method
[0104] 1. Solid content
[0105] The solids content (non-volatile content) was determined via DIN EN ISO 3251:2008-06 at 105° C. for 120 min.
[0106] 2. Average particle diameter
[0107] The particle size distribution of the capsules was measured by laser diffraction using a Malvern Mastersizer 2000 according to ISO 13320 EN: 2020-01. The data were processed using the "General Model" provided by Malvern Instruments according to Mie-Theory by software. The important parameters are the dn values d10, d50 and d90 values for n=10, 50 and 90. The d50 value is the median d50 particle size diameter based on the average volume.
[0108] 3. Neutral Salt Spray (NSS) Test
[0109] The NSS test is used to determine the corrosion resistance of coatings on substrates. According to DIN EN ISO 9227:2017-07, the analyzed samples are in a chamber where a 5% strength sodium chloride salt solution with a controlled pH is sprayed continuously at a temperature of 50°C for a duration of 120 hours. The spray is deposited on the analyzed samples, covering them with a corrosive film of the salt water. The degree of corrosion can be evaluated based on characteristic values in the range of 0 (no corrosion) to 5 (significant corrosion). Each test is performed three times and the average value is determined.
[0110] 4. Wet stack test
[0111] The wet stack test is performed at 60°C for 240 h and simulates storage and transportation of coils in hot and humid areas.
[0112] 5. Cross-cutting testing
[0113] According to DIN EN ISO 2409:2020-12, a cross-cut test is used to determine the adhesion strength of the coating on the substrate. The cutter spacing is 2 mm. Based on the characteristic cross-cut value in the range of 0 (very good adhesion) to 5 (very poor adhesion), the evaluation is performed. According to DIN EN ISO 6270-2CH:2018-04, a cross-cut test is performed before and after exposure to a condensing climate for 240 hours. Each test is performed three times and the average value is determined.
[0114] 6. water solubility
[0115] The water solubility, in particular of the corrosion inhibiting components, is measured at 23° C. (at atmospheric pressure and pH 7.0). The measurement method including sample preparation is described in OECD Guideline 105.
[0116] 7. Water miscibility
[0117] Water miscibility, in particular of non-aqueous solvents, is measured at 23° C. (at atmospheric pressure and pH 7.0) according to ASTM D1722.
[0118] Examples
[0119] The following examples further illustrate the present invention but should not be construed as limiting its scope.
[0120] 1. Preparation of Encapsulated Corrosion Inhibitors
[0121] 1.1 General preparation scheme
[0122] Water and a commercially available aqueous solution of polyvinyl alcohol (10 wt.-%) were mixed to obtain mixture 1. The pH was adjusted to a pH in the range of pH 2.5 to 3.5 with an aqueous solution of sulfuric acid (20 wt.-% solution). Mixture 1 contained polyvinyl alcohol in an amount of 7.5 wt.-%, based on the total weight of mixture 2 described below. Separately, a mixture 2 of a corrosion inhibitor to be encapsulated, a carrier and a monomer to be used for preparing the shell (wall) of the capsule (such as, for example, at least one hydrophobic monomer and at least one monomer having at least one functional group) and optionally a crosslinking agent (such as a crosslinking monomer) was prepared. Mixture 2 was then emulsified in mixture 1 at 26.000 rpm for 5 min using a silent crusher (rotor stator dispersion tool). The temperature of the emulsion was maintained below 35° C. using an ice bath during the emulsification step. The emulsion was then transferred to a round-bottom flask equipped with a half-moon stirrer and a water condenser and stirred at 150 rpm. Nitrogen was flowed in the reactor throughout the polymerization. A free radical initiator (thermal initiator) is then added to the medium and the temperature is increased: starting from 20° C., 75° C. is reached over 60 minutes (linear rate). This temperature is maintained for 2 hours. The temperature is then increased to 85° C. (linear rate) within 15 min and maintained for 60 min. Afterwards, the system is cooled to room temperature (23° C.). At the beginning of cooling, an initiator (redox initiator partner) is added to the medium to reduce the residual monomer content.
[0123] 1.2 Various capsules were prepared according to the protocol defined above. The following components were used:
[0124] Carrier: OE, Sensoft, AMD 10.
[0125] Monomers: MMA (methyl methacrylate; an example of a hydrophobic monomer); VME (vinyl mercaptoethanol; an example of a monomer having at least one functional group).
[0126] Crosslinking agent: BDDA (1,4-butylene glycol diacrylate), DVB (divinylbenzene), MAA (methacrylic anhydride).
[0127] Corrosion inhibitors: benzothiazole, benzotriazole, quercetin.
[0128] AMD 10 is N,N-dimethyldecane-1-amide with a boiling point of 291° C. (1,013 hPa). OE is dioctyl ether having a boiling point of 292°C. Sensoft is 2-propylheptyl octanoate and has a boiling point of 319° C. Benzothiazole has a solubility in water of about 4.3 mg / mL at 23° C. Benzotriazole has a solubility in water of about 20 mg / mL at 23° C. Quercetin is substantially insoluble in water at 23° C.
[0129] The following capsules were prepared in this manner according to the general preparation protocol:
[0130] Example E1:
[0131] The capsule shell was prepared from MMA and BDDA as a crosslinker utilized in a 4:1 wt.-% ratio. The core consisted of benzothiazole as a corrosion inhibitor and OE was composed of a 3:1 wt.-% mixture. The target core-shell ratio was 85 / 15 wt.-%. E1 had a solids content of 23.8 wt.-%. The "target active substance content" as the content of corrosion inhibitor in the emulsion was 19.8 wt.-%.
[0132] Example E2:
[0133] The capsule shell was prepared from MMA and BDDA as a crosslinker utilized in a 4:1 wt.-% ratio. The core was composed of benzothiazole as a corrosion inhibitor and The target core-shell ratio is 75 / 25 wt.-%. E2 has a solids content of 19.8 wt.-%. The "target active substance content" is 17.2 wt.-%.
[0134] Example E3:
[0135] The capsule shell was prepared from MMA and BDDA as a crosslinker utilized in a 7:3 wt.-% ratio. The core consisted of benzothiazole as a corrosion inhibitor and The target core-shell ratio is 80 / 20 wt.-%. E3 has a solids content of 15.8 wt.-%. The "target active substance content" is 18.4 wt.-%.
[0136] Example E4:
[0137] The capsule shell was prepared from MMA and BDDA as a crosslinker utilized in a 4:1 wt.-% ratio. The core consisted of benzothiazole as a corrosion inhibitor and The target core-shell ratio is 80 / 20 wt.-%. E4 has a solids content of 26.4 wt.-%. The "target active substance content" is 11.9 wt.-%.
[0138] Example E5:
[0139] The capsule shell was prepared from MMA and BDDA as a crosslinker utilized in a 3:2 wt.-% ratio. The core was composed of benzothiazole as a corrosion inhibitor and Sensof is composed of a 3:1 wt.-% mixture by weight. The target core-shell ratio is 80 / 20 wt.-%. E5 has a solid content of 9.9 wt.-%. The "target active substance content" is 18.3 wt.-%.
[0140] Example E6:
[0141] The capsule shell was prepared from MMA, VME and BDDA as a crosslinker utilized in a 5:1:4 wt.-% ratio. The core consisted of benzothiazole as a corrosion inhibitor and The target core-shell ratio is 80 / 20 wt.-%. E6 has a solids content of 18.1 wt.-%. The "target active substance content" is 18.3 wt.-%.
[0142] Example E7:
[0143] The capsule shell was prepared from MMA and MAA as crosslinking agent utilized in a 3:2 wt.-% ratio. The core was composed of benzothiazole as corrosion inhibitor and Sensof. The target core-shell ratio is 80 / 20 wt.-%. E7 has a solids content of 9.2 wt.-%. The "target active substance content" is 18.3 wt.-%.
[0144] Example E8:
[0145] The capsule shell was prepared from MMA and BDDA as a crosslinking agent utilized in a 85:15 wt.-% ratio. The core was composed of 1,2,3-benzotriazole as a corrosion inhibitor and AMD 10. The target core-shell ratio is 80 / 20 wt.-%. E8 has a solids content of 24.1 wt.-%. The "target active substance content" is 12.7 wt.-%.
[0146] Example E9:
[0147] The capsule shell was prepared from MMA and MAA as cross-linking agents utilized in a 3:2 wt.-% ratio. The core consisted of quercetin as a corrosion inhibitor and AMD 10. The target core-shell ratio is 80 / 20 wt.-%. E9 has a solids content of 9.2 wt.-%. The "target active substance content" is 8.3 wt.-%.
[0148] 1.3 Capsule characteristics
[0149] The average particle size diameters of Examples E1 to E9 were determined according to the method disclosed above. The determined values are summarized in Table 1.
[0150] Table 1:
[0151]
[0152] 2. Preparation of waterborne coating compositions suitable for providing permanent coatings
[0153] 2.1 In addition to water, the following components were used to prepare these compositions:
[0154] Additive 1: Commercially available silicone surfactant.
[0155] Additive 2: Commercially available defoamer.
[0156] Wax: Cationic emulsion of a commercially available oxidized HD polyethylene wax (solids content: 30 wt.-%).
[0157] HGE: hydrophobic glycol ether (commercially available).
[0158] AR: Commercially available (meth)acrylic resin dispersion with a solids content of 40.0 wt.-%.
[0159] PUR: commercially available aqueous aliphatic cationic polycarbonate-polyurethane dispersion with a solids content of 35.0 wt.-%.
[0160] Inorganic aqueous mixtures (IAM): mixtures which, in addition to water, comprise, inter alia, organosilanes and H2TiF6 and / or H2ZrF6.
[0161] 2.2 General preparation scheme
[0162] An aqueous polymer dispersion was prepared from water, additives 1 and 2, a mixture of AR and PUR, a mixture of wax, HGE and IAM and one of the capsules E1 to E7 and E9. A reference composition RE containing no capsules was also prepared in this way.
[0163] 2.3 Various acidic aqueous coating compositions PC1 to PC8 were prepared according to the scheme set out above, each having a pH value in the range of 3.0 to 4.0. The compositions are summarized in Table 2. All given amounts are given in pbw. All compositions had a VOC content of 0 wt.-%.
[0164] 2.4 After 1 day of storage at room temperature, the storage stability of all compositions PC1 to PC8 and RE was very good. Compositions PC1 to PC3, PC5, PC6, PC7 and RE were further investigated with regard to their storage stability after 15 days and after 30 days: in all cases, excellent storage stability was observed.
[0165]
[0166] 3. Permanent coatings obtained from coating compositions and their properties.
[0167] 3.1 Each of the acidic aqueous coating compositions PC1 to PC8 and RE was applied to the surface of a panel made of galvanized steel (HDG) using a doctor blade or a roller coater at room temperature (23°C). The coated substrate was then dried at a peak metal temperature of 60°C (oven temperature 210°C) for about 10 seconds. The resulting permanent coating had a dry layer film thickness of about 1.2 μm as measured by XRF using a tracer element. The coating weight was between 1.1 and 1.2 g / m 2 The coated substrates obtained from PC1 to PC7 and RE were subjected to NSS test and wet stack (WS) test, both as described in the "Methods" section. The results are shown in Table 3.
[0168] Table 3
[0169]
[0170] 3.2 Each of the resulting coated panels obtained as outlined in item 3.1 was further coated with a powder coating composition (commercial product 771). The cross-section test was then performed before or after the condensation climate test as described in the "Methods" section. The results are shown in Table 4.
[0171] Table 4
[0172]
[0173]
[0174] 3.3 Each of the acidic aqueous coating compositions PC1 to PC7 and RE was applied to the surface of a panel made of Galvalume (aluminum-rich galvanized steel) using a doctor blade or a roller coater at room temperature (23°C). The coated substrate was then dried at a peak metal temperature of 60°C (oven temperature 210°C) for about 10 seconds. The resulting permanent coating had a dry layer film thickness of about 1.2 μm as measured by XRF using a tracer element. The coating weight was between 1.1 and 1.2 g / m 2 The coated substrates were subjected to NSS testing and wet stack (WS) testing, both as described in the "Methods" section. The results are shown in Table 5. No darkening or dark spots were observed.
[0175] Table 5
[0176]
Claims
1. A packaging structure comprising a polymer shell and a core within the shell, in, The shell is obtainable by polymerization of at least one (meth)acrylic monomer or a monomer mixture comprising the at least one (meth)acrylic monomer in the presence of the core, and The core comprises at least one corrosion inhibiting component having a water solubility of less than 50 g / L at 23° C. in its non-encapsulated state, wherein the core optionally further comprises at least one non-aqueous solvent.
2. The packaging structure according to claim 1, It is characterized in that The at least one corrosion inhibiting component present in the core has, in its non-encapsulated state, a water solubility at 23°C of less than 40 g / L, preferably less than 30 g / L, more preferably less than 20 g / L, yet more preferably less than 15 g / L, even more preferably less than 10 g / L, yet more preferably less than 7.5 g / L, yet more preferably less than 5.0 g / L, yet more preferably less than 2.5 g / L, and most preferably less than 1 g / L.
3. The packaging structure according to one or more of claims 1 and 2, It is characterized in that The corrosion inhibiting component is an inorganic or organic component, preferably an organic compound, more preferably an organic compound having at least one alicyclic, heteroalicyclic, aromatic and / or heteroaromatic moiety, and still more preferably having at least one C 3 -C 40 - alicyclic moiety, at least one C 3 -C 40 -heteroalicyclic moiety, at least one C 5 -C 40 - an aromatic moiety and / or at least one C 5 -C 40 -heteroaromatic moiety, most preferably selected from benzothiazole and quercetin, wherein at least one C 3 -C 40 - the heteroalicyclic moiety comprises at least one heteroatom and / or at least one heteroatom group - wherein the heteroatom is in each case preferably selected from O, N and S, the at least one C 5 -C 40 The heteroaromatic moiety comprises at least one heteroatom and / or at least one heteroatom group—wherein the heteroatom is preferably selected from O, N and S in each case.
4. The package structure according to one or more of the preceding claims, It is characterized in that The encapsulated structure has an average median d50 particle size diameter in the range of 0.1 to 30 μm, preferably 0.2 to 20 μm, more preferably 0.3 to 15 μm, still more preferably 0.4 to 10 μm, yet more preferably 0.5 to 7.5 μm, yet more preferably 0.5 to 5.5 μm, yet more preferably 0.5 to 4.0 μm, yet more preferably 0.5 to 3.5 μm, most preferably 0.6 to 3.0 μm.
5. The package structure according to one or more of the preceding claims, It is characterized in that The amount of the shell is in the range of 1 to 70 wt.-%, preferably 2 to 65 wt.-%, more preferably 3 to 60 wt.-%, even more preferably 4 to 55 wt.-%, yet more preferably 5 to 50 wt.-%, in each case based on the total weight of the encapsulated structure including shell and core.
6. Package structure according to one or more of the preceding claims, It is characterized in that The at least one non-aqueous solvent optionally present in and preferably present in the core has a boiling point of >100°C, preferably >125°C, more preferably >150°C, even more preferably >175°C, still more preferably >200°C, yet more preferably >225°C, most preferably >250°C at atmospheric pressure, and / or the at least one non-aqueous solvent has a water miscibility of less than 5 g / L, preferably less than 2.5 g / L, more preferably less than 2.0 g / L, even more preferably less than 1.5 g / L, most preferably less than 1.0 g / L at 23°C in its non-packaged state.
7. The package structure according to one or more of the preceding claims, It is characterized in that the shell being obtainable from at least one (meth)acrylic monomer m1, from at least one monomer m2, from a monomer mixture comprising the at least one (meth)acrylic monomer m1 and optionally at least one further monomer m2 and / or optionally at least one further monomer m3, or from a monomer mixture comprising the at least one monomer m2 and optionally at least one further monomer m1 and / or optionally at least one further monomer m3, m2 and m3 both being different from each other and from the monomer m1, The at least one (meth) acrylic monomer m1 is a non-functional (meth) acrylic monomer, preferably an aliphatic C 1 -C 30 - (meth)acrylates of monohydric alcohols, wherein the monomer m2 optionally present in the monomer mixture is a monomer having at least one ethylenically unsaturated group and further carrying at least one functional group, the at least one functional group being preferably selected from hydroxyl groups, ether groups, carbonyl groups, amino groups, epoxy groups, carboxylic acid groups, sulfur-containing functional groups and phosphorus-containing groups, and Among the monomers m3 optionally present in the monomer mixture are monomers having at least two ethylenically unsaturated groups.
8. The package structure according to one or more of the preceding claims, It is characterized in that The Shell contains only monomer units mu1 derived from the at least one (meth)acrylic monomer m1, and contains no other monomer units except the monomer units m1, or containing monomer units mu1 derived from the at least one (meth)acrylic monomer m1 in an amount in the range of 60 to 99 wt.-%, preferably 65 to 95 wt.-%, more preferably 70 to 90 wt.-% and monomer units mu2 derived from the at least one monomer m2 in an amount in the range of 1 to 40 wt.-%, preferably 5 to 35 wt.-%, more preferably 10 to 30 wt.-%, or containing monomer units mu1 derived from the at least one (meth)acrylic monomer m1 in an amount in the range of 40 to 99 wt.-%, preferably 50 to 95 wt.-%, more preferably 50 to 90 wt.-% and monomer units mu3 derived from the at least one monomer m3 in an amount in the range of 1 to 50 wt.-%, preferably 5 to 50 wt.-%, more preferably 10 to 50 wt.-%, or containing monomer units mu1 derived from the at least one (meth)acrylic monomer m1 in an amount in the range of 30 to 98 wt.-%, preferably 36 to 92 wt.-%, more preferably 44 to 86 wt.-%, monomer units mu2 derived from the at least one monomer m2 in an amount in the range of 1 to 35 wt.-%, preferably 4 to 32 wt.-%, more preferably 7 to 28 wt.-% and monomer units mu3 derived from the at least one monomer m3 in an amount in the range of 1 to 50 wt.-%, preferably 2 to 45 wt.-%, more preferably 5 to 40 wt.-%, The sum of all monomers used for preparing the shell amounts in each case to 100 wt.-%.
9. The packaging structure according to claim 8, It is characterized in that The amount of monomer units mu1 in the shell exceeds by wt.-% the amount of any monomer units mu2 and / or mu3 also present.
10. The package structure according to one or more of the preceding claims, It is characterized in that The core of the encapsulated structure comprises the at least one corrosion inhibiting component in an amount of at least 50 wt.-%, more preferably at least 60 wt.-%, even more preferably at least 70 wt.-%, still more preferably at least 80 wt.-%, yet more preferably at least 90 wt.-%, more preferably at least 95 wt.-%, yet more preferably at least 98 wt.-%, in each case based on the total weight of the core.
11. The package structure according to one or more of the preceding claims, It is characterized in that The encapsulated structure is present in an aqueous mixture, preferably an aqueous dispersion, the mixture preferably having a solids content in the range of 1 to 70 wt.-%, preferably 2 to 65 wt.-%, even more preferably 3 to 60 wt.-%, still more preferably 5 to 55 wt.-%, yet more preferably 10 to 50 wt.-%, in each case based on the total weight of the aqueous mixture.
12. A method for producing a package structure according to one or more of the preceding claims, It is characterized in that The method comprises at least steps a) and b), namely a) providing a mixture of (i) the at least one (meth)acrylic monomer or a monomer mixture comprising the at least one (meth)acrylic monomer suitable for forming the polymer shell, (ii) the at least one corrosion inhibiting component suitable for forming the core, wherein the corrosion inhibiting component may optionally be present in a mixture further comprising at least one non-aqueous solvent, said mixture being suitable for forming an oil phase, and then emulsified into (iii) water as an aqueous continuous phase, wherein optionally at least one emulsifier and / or surfactant is present in the aqueous continuous phase (iii) and / or in the mixture formed by (i) and (ii), and b) polymerizing the at least one (meth)acrylic monomer or the monomer mixture comprising the at least one (meth)acrylic monomer to form the shell of the encapsulating structure, the encapsulating structure comprising the at least one corrosion inhibiting component as a core within the shell formed upon polymerization, wherein the core may optionally further comprise at least a portion of the at least one non-aqueous solvent.
13. The method according to claim 12, It is characterized in that At least one of an emulsifier, a surfactant and a polymer stabilizer is used in the preparation of the encapsulation structure.
14. Use of a packaging structure according to one or more of claims 1 to 11 as releasable capsules of corrosion inhibiting components.
15. The use according to claim 14, It is characterized in that The use is for releasing the corrosion inhibiting compound present in the shell of the encapsulation structure after at least partially applying an aqueous coating composition containing the encapsulation structure to the surface of an optionally pre-coated metal substrate to at least partially form a coating film on the surface.
Citation Information
Patent Citations
Process for the coating of metallic components with an aqueous organic composition
US20120171402A1
Method for coating metallic surfaces with a coating agent containing a polymer, the coating agent, and use thereof
US20130177768A1
Releasable Encapsulation Compositions
US20190159448A1
microcapsules
US20200108367A1
Method for coating metal surfaces using an aqueous compound having polymers, the aqueous compound, and use of the coated substrates
WO2008110480A1