Molded pulp wire coil material and preparation method thereof

The paper pulp spool material composition with additives addresses color retention and environmental pollution, improving production efficiency and sustainability by using hydrogen peroxide, ozone, and microbial agents.

CN120310059APending Publication Date: 2025-07-15GUANGDONG HUILIN PACKAGING TECH GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510262635.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-03-06
Publication Date
2025-07-15

AI Technical Summary

Technical Problem

During the preparation process, existing pulp molded wire disk materials have problems such as impurities affecting color, weak environmental protection performance, and high drying energy consumption, resulting in insufficient color protection strength and increased production costs.

Method used

The pulp molded wire disk material consisting of waste raw materials, hydrogen peroxide, ozone, sodium pyrophosphate, degraded adsorbent materials and highly absorbent resins with specific ratios, is used to improve color protection and environmental protection through vacuum adsorption molding and drying, combined with degraded adsorbent materials and antioxidants, to achieve color protection and environmental protection performance.

Benefits of technology

It ensures the original color of the wire disk material, reduces the content of harmful substances, improves environmental protection performance, and accelerates the drying speed under the same energy consumption, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120310059A_ABST
    Figure CN120310059A_ABST
Patent Text Reader

Abstract

The invention discloses a molded pulp wire coil material and a preparation method thereof, and relates to the technical field of wire coil materials. The raw materials of the environment-friendly and environment-friendly material comprise the following components: 50%-85% of a waste raw material, 5%-20% of epoxy resin, 0.2%-2% of hydrogen peroxide, 0.5%-1% of ozone, 1%-3% of sodium pyrophosphate, 2%-5% of a degradable adsorption material, 1%-3% of super absorbent resin, 0.5%-1% of a sodium chloride solution, 0.5%-1% of a calcium chloride solution, 0.1%-0.5% of a bleaching agent and 0.5%-1% of an antioxidant. According to the paper pulp molding wire coil material and the preparation method thereof, the original color of the wire coil material can be guaranteed, meanwhile, the color protection effect can be achieved when the wire coil material is prepared, harmful substances existing in the wire coil material are reduced, the environmental protection performance of the wire coil material is improved, the water locking strength of the wire coil material is reduced, and the water removal rate can be increased under the condition of heat with the same energy consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wire coil materials, and in particular to a pulp molding wire coil material and a preparation method thereof. Background Art

[0002] The materials for making pulp molding reels mainly come from waste paper, including waste newspapers, cardboard scraps, recycled paper tubes and paper tubes, log pulp boards or sugarcane pulp residues, etc. These raw materials are mixed into a certain concentration of pulp through hydraulic pulping, batching and other processes, and then vacuum adsorbed on a special metal mold to form a wet blank product, and finally dried and hot-pressed to become a pulp molding reel with multiple protective properties such as buffering, shockproof, compression resistance and impact resistance.

[0003] At present, there are some deficiencies in the preparation of pulp plastic film reel materials, such as: the pulp raw materials have more impurities or materials that affect the original color of the pulp, these materials cannot guarantee the original color of the reel material, and the color protection effect cannot be achieved during the preparation of the reel material, resulting in weak color protection strength of the reel material; although pulp molding materials are more environmentally friendly than plastic buffer materials, the papermaking process may still cause pollution to the environment. At the same time, a large amount of paint, glue, defoamer and chlorine-containing bleaching agent will be used in the processing process. These substances may contain harmful substances such as phthalates and dioxins. Therefore, the prepared reel material will cause environmental pollution and have weak environmental protection performance; in the production process of pulp molded products, drying is an extremely energy-intensive link, because the water content of the workpiece after compression molding is as high as 55% to 60%, and the water content of the final product is 12% to 14%, so a lot of heat is needed to remove this part of the water, which not only increases the production cost, but also has a certain impact on the environment, affecting the preparation efficiency of pulp plastic film reel materials.

[0004] Therefore, a pulp molding coil material and a preparation method thereof are proposed to solve the above problems. Summary of the invention

[0005] The main purpose of the present invention is to provide a method for preparing a pulp molding wire coil material which retains the original color of pulp, has high environmental strength and fast drying speed during preparation, and is applied to the preparation of pulp molding wire coil material.

[0006] To achieve the above object, the technical solution adopted by the present invention is as follows: A pulp molding spool material, by weight percentage, its raw materials are composed of the following components: By weight percentage, its raw materials are composed of the following components: 50% to 85% of waste raw materials, 5% to 20% of epoxy resin, 0.2% to 2% of hydrogen peroxide, 0.5% to 1% of ozone, 1% to 3% of sodium pyrophosphate, 2% to 5% of degradation adsorption material, 1% to 3% of superabsorbent resin, 0.5% to 1% of sodium chloride solution, 0.5% to 1% of calcium chloride solution, 0.1% to 0.5% of bleaching agent, and 0.5% to 1% of antioxidant.

[0007] The waste raw materials include at least one of waste newspapers, carton paper, paper tube paper tubes, pure wood pulp, sugarcane pulp, bamboo pulp, and straw pulp; The mass ratio of the waste raw materials to the epoxy resin is 4:1.

[0008] The mass ratio of the hydrogen peroxide, ozone, and sodium pyrophosphate is 1:0.5:3.

[0009] The degradation adsorption material includes at least one of Pseudomonas, Bacillus, Acinetobacter, white rot fungi, photocatalyst, zero-valent iron, zero-valent aluminum, activated carbon, graphene, and carbon nanoparticles.

[0010] The mass ratio of the degradation adsorption material to the bleaching agent is 3:1; The bleaching agent includes at least one of sodium dithionite, sulfite, and borohydride.

[0011] The antioxidant includes at least one of vitamin E, sodium sulfite, potassium sulfite, sodium bisulfite, potassium bisulfite, and sodium dithionite.

[0012] The antioxidant also includes an anti-ultraviolet aging agent, and the anti-ultraviolet aging agent is pentaerythritol stearate.

[0013] The superabsorbent resin is synthesized by modifying polyacrylate and starch-acrylate polymer, with a particle size of 100 mesh to 200 mesh, and the water absorption in saturated Ca(OH)2 solution is as high as 40 to 80 g.

[0014] The mass ratio of the superabsorbent resin to the sodium chloride solution or calcium chloride solution is 2:1.

[0015] A preparation method of a pulp molding spool material, the preparation method is specifically as follows: Step 1: Prepare the original pulp solution. Remove the foreign substances on the surface of the waste raw materials, crush them, pour the waste raw materials, epoxy resin, hydrogen peroxide, and ozone into a blender according to the weight ratio, stir for 30 min - 60 min, control the temperature at 30°C to 60°C, dilute for 0.5 h - 1 h, add sodium pyrophosphate, stir again for 10 to 20 min, and grind to obtain the original pulp solution; Step 2: Add the degradation and adsorption material. Add the degradation and adsorption material to the original pulp solution according to the weight ratio, control the temperature at 30°C to 60°C, and stir for 20 to 35 min to obtain the original pulp mixture; Step 3: Molding. By the method of vacuum adsorption, add superabsorbent resin to the original pulp mixture, and add sodium chloride solution and calcium chloride solution. Then deposit the fibers of the original pulp mixture on a mesh mold and filter the water in the original pulp mixture to obtain a wet blank pulp semi-finished product; Step 4: Press the finished product. Send the wet blank pulp semi-finished product into a single-screw pulp press, increase the pulp concentration to 45% to 50%, after drying treatment, press into blocks, cut, and obtain the pulp molding line tray material.

[0016] The present invention has the following beneficial effects: 1. In the present invention, by adding hydrogen peroxide and ozone to the waste raw materials and adding sodium pyrophosphate, hydrogen peroxide is combined with sodium pyrophosphate. Sodium pyrophosphate can increase the stability of hydrogen peroxide, thereby reducing its decomposition rate and enhancing its oxidation performance. It can increase the color protection function of the line tray material. Moreover, hydrogen peroxide has dual properties of oxidation and reduction. Adding sodium pyrophosphate increases its stability, avoiding the weakening of the bleaching and oxidation effects on the pulp, ensuring the original color of the line tray material, and realizing the color protection effect during the preparation of the line tray material.

[0017] 2. In the present invention, by adding the degradation and adsorption material, among which, Bacillus and Acinetobacter in the degradation and adsorption material can effectively degrade phthalate esters and dioxin-like compounds under different conditions. Through enzymatic reactions, phthalate esters and dioxin-like compounds are decomposed into smaller molecules and finally converted into harmless substances. The toxicity of dioxin is gradually reduced through reduction reactions, reducing environmental pollution during the papermaking process, reducing harmful substances existing in the line tray material, and improving its environmental protection performance.

[0018] 3. In the present invention, adding sodium chloride solution or calcium chloride solution to the starch-acrylate polymer will change the water absorption and water retention properties of the material, thereby reducing its water locking strength. During the production process of pulp molding products, the drying efficiency is improved, the water removal rate can be increased under the same energy-consuming heat, the production cost is reduced, the impact on the environment is also reduced, and the preparation efficiency of the pulp molding line tray material is improved. Description of the Drawings

[0019] Figure 1 This is the overall process schematic diagram of a pulp molding coil material and its preparation method according to the present invention. Specific embodiments

[0020] In order to make the technical means, creative features, achieved purposes and effects of the present invention easy to understand, the present invention will be further described below in conjunction with specific embodiments.

[0021] Comparative example A pulp molding coil material, and the preparation method of the pulp molding coil material includes the following steps: Step 1: Prepare the original pulp solution. Remove the foreign matters on the surface of the waste raw materials, crush them, pour the waste raw materials, epoxy resin, hydrogen peroxide and ozone into a blender according to the weight ratio, stir for 30 min - 60 min, control the temperature at 30°C to 60°C, dilute for 0.5 h - 1 h, stir again for 10 to 20 min, and grind to obtain the original pulp solution; Step 2: Molding. By the method of vacuum adsorption, add the superabsorbent resin into the original pulp solution, and then deposit the fibers of the original pulp mixture on the mesh mold and filter the moisture in the original pulp mixture to obtain a wet blank pulp semi-finished product; Step 4: Press the finished product. Feed the wet blank pulp semi-finished product into a single-screw pulp extruder, increase the pulp concentration to 45% to 50%, after drying treatment, press into blocks, cut, and obtain the pulp molding coil material.

[0022] The comparative example is the preparation steps of the semi-finished pulp molding coil material by the prior art. Compare the comparative example with Example 1, Example 2 and Example 3. The comparison results are as follows. The comparative example lacks sodium pyrophosphate compared with Example 1. The comparative example lacks Pseudomonas marina, Bacillus, Acinetobacter, white rot fungus, photocatalyst, zero-valent iron, zero-valent aluminum, activated carbon, graphene and carbon nanoparticles compared with Example 2. The comparative example lacks polyacrylate and starch-acrylate polymer and sodium chloride solution or calcium chloride solution compared with Example 3.

[0023] Example 1 Please refer to Figure 1 As shown: A pulp molding coil material and its preparation method include the following steps: Step 1: Prepare the original pulp solution. Remove the foreign matters on the surface of the waste raw materials, crush them, pour the waste raw materials, epoxy resin, hydrogen peroxide and ozone into a blender according to the weight ratio, stir for 30 min - 60 min, control the temperature at 30°C to 60°C, dilute for 0.5 h - 1 h, add sodium pyrophosphate, stir again for 10 to 20 min, and grind to obtain the original pulp solution; Step 2: Shaping. By means of vacuum adsorption, superabsorbent resin is added to the original pulp solution, and then the fibers of the original pulp mixture are deposited on a mesh mold and the water in the original pulp mixture is filtered to obtain a semi-finished wet blank pulp. Step 4: Pressing the finished product. The semi-finished wet blank pulp is fed into a single-screw pulp extruder to increase the pulp concentration to 45% - 50%. After drying treatment, it is pressed into blocks and cut to obtain the pulp molding bobbin material.

[0024] The waste raw materials include at least one of waste newspapers, carton paper, paper tube, pure wood pulp, sugarcane pulp, bamboo pulp and straw pulp. The mass ratio of the waste raw materials to the epoxy resin is 4:1.

[0025] The mass ratio of hydrogen peroxide, ozone and sodium pyrophosphate is 1:0.5:3.

[0026] With the above ratio, there are the following advantages in the preparation of the pulp molding bobbin material in Example 1 compared with the comparative example. Combining hydrogen peroxide and sodium pyrophosphate, sodium pyrophosphate can increase the stability of hydrogen peroxide, thereby reducing its decomposition rate and enhancing its oxidation performance. It can increase the color protection function of the bobbin material. And hydrogen peroxide has the dual properties of oxidation and reduction. Hydrogen peroxide is easy to decompose into water and oxygen when exposed to light, heat or impurities. Adding sodium pyrophosphate increases its stability, avoiding the weakening of the bleaching and oxidation effects on the pulp, ensuring the original color of the bobbin material, and at the same time realizing the color protection effect during the preparation of the bobbin material, increasing the color protection intensity after bleaching during the preparation of the bobbin material.

[0027] Example 2 Please refer to Figure 1 as shown: A pulp molding bobbin material and its preparation method, including the following steps: Step 1: Preparing the original pulp solution. Remove the foreign matters on the surface of the waste raw materials, crush them, pour the waste raw materials, epoxy resin, hydrogen peroxide and ozone into a mixer according to the weight ratio, stir for 30 min - 60 min, control the temperature at 30°C to 60°C, dilute for 0.5 h - 1 h, add sodium pyrophosphate, and stir again for 10 to 20 min, then grind to obtain the original pulp solution. Step 2: Adding the degradation adsorption material. Add the degradation adsorption material to the original pulp solution according to the weight ratio, control the temperature at 30°C to 60°C, and stir for 20 to 35 min to obtain the original pulp mixture. Step 3: Shaping. By means of vacuum adsorption, superabsorbent resin is added to the original pulp mixture, and then the fibers of the original pulp mixture are deposited on a mesh mold and the water in the original pulp mixture is filtered to obtain a semi-finished wet blank pulp. Step 4: Press the finished product. Feed the semi-finished wet pulp paper into a single-screw pulp press to increase the pulp concentration to 45% to 50%. After drying, press it into blocks and cut it to obtain the pulp molding bobbin material.

[0028] The degradation and adsorption material includes at least one of Pseudomonas, Bacillus, Acinetobacter, white rot fungi, photocatalyst, zero-valent iron, zero-valent aluminum, activated carbon, graphene, and carbon nanoparticles.

[0029] The mass ratio of the degradation and adsorption material to the bleaching agent is 3:1; The bleaching agent includes at least one of sodium dithionite, sulfite, and borohydride.

[0030] With the above ratio, there are the following advantages in the preparation of the pulp molding bobbin material in Example 2 and the comparative example. Bacillus and Acinetobacter can effectively degrade phthalates and dioxins under different conditions. Through enzymatic reactions, phthalates and dioxins are decomposed into smaller molecules and finally converted into harmless substances. Zero-valent iron and zero-valent aluminum can reduce dioxins under anaerobic conditions, dechlorinate them, and gradually reduce the toxicity of dioxins through reduction reactions, reducing environmental pollution during the papermaking process, reducing harmful substances in the bobbin material, and improving its environmental performance.

[0031] Example 3 Please refer to Figure 1 as shown: A pulp molding bobbin material and its preparation method include the following steps: Step 1: Prepare the original pulp solution. Remove foreign matters on the surface of the waste raw materials, crush them, pour the waste raw materials, epoxy resin, hydrogen peroxide, and ozone into a blender according to the weight ratio, stir for 30 min - 60 min, control the temperature at 30°C to 60°C, dilute for 0.5 h - 1 h, add sodium pyrophosphate, and stir again for 10 to 20 min, then grind to obtain the original pulp solution; Step 2: Add the degradation and adsorption material. Add the degradation and adsorption material into the original pulp solution according to the weight ratio, control the temperature at 30°C to 60°C, and stir for 20 to 35 min to obtain the original pulp mixture; Step 3: Molding. By the method of vacuum adsorption, add superabsorbent resin into the original pulp mixture, and add sodium chloride solution and calcium chloride solution. Then deposit the fibers of the original pulp mixture on a mesh mold and filter the water in the original pulp mixture to obtain the semi-finished wet pulp paper; Step 4: Press the finished product. Feed the semi-finished wet pulp paper into a single-screw pulp press to increase the pulp concentration to 45% to 50%. After drying, press it into blocks and cut it to obtain the pulp molding bobbin material.

[0032] The antioxidant includes at least one of vitamin E, sodium sulfite, potassium sulfite, sodium bisulfite, potassium bisulfite and sodium dithionite.

[0033] The antioxidant also includes an anti-ultraviolet aging agent, and the anti-ultraviolet aging agent is pentaerythritol stearate.

[0034] The superabsorbent resin is synthesized by modifying polyacrylate and starch-acrylate polymer, and the particle size is 100 mesh to 200 mesh, and the water absorption in saturated Ca(OH)2 solution is as high as 40 to 80 g.

[0035] The mass ratio of the superabsorbent resin to the sodium chloride solution or calcium chloride solution is 2:1.

[0036] Through the above ratio, there are the following advantages in the preparation of the pulp molding tray material in Example 3 and the comparative example. Adding sodium chloride solution or calcium chloride solution to the starch-acrylate polymer will change the water absorption and water retention properties of the material, thereby reducing its water locking strength, making the drying efficiency in the production process of pulp molding products improved, and being able to increase the water removal rate under the same energy consumption heat, reducing production costs, and also reducing the impact on the environment, and improving the preparation efficiency of the pulp molding tray material.

[0037] The test results of the primary color grade, environmental strength and drying rate are shown in Table 1 below: Table 1: Test of primary color grade, environmental strength and drying rate:

[0038] It can be seen from the test results in the above table that the pulp molding tray materials prepared in Example 1, Example 2 and Example 3 can ensure the original color of the tray material compared with the comparative example, and at the same time can achieve a color protection effect during the preparation of the tray material, increasing the color protection strength after bleaching in the process of preparing the tray material; gradually reducing the toxicity of dioxin through a reduction reaction, reducing environmental pollution in the papermaking process, reducing harmful substances existing in the tray material, and improving its environmental protection performance; being able to increase the water removal rate under the same energy consumption heat, reducing production costs, and also reducing the impact on the environment.

[0039] In the present invention, there is provided a pulp molding coil material and a preparation method thereof. During the operation of this method, first, foreign substances on the surface of waste raw materials are removed and the materials are pulverized. Then, according to the weight ratio, the waste raw materials, epoxy resin, hydrogen peroxide, and ozone are poured into a blender and stirred for 30 min to 60 min, with the temperature controlled at 30°C to 60°C. After dilution for 0.5 h to 1 h, sodium pyrophosphate is added and stirring is continued for 10 to 20 min. Then, grinding is carried out to obtain a raw pulp solution. Combining hydrogen peroxide with sodium pyrophosphate, sodium pyrophosphate can increase the stability of hydrogen peroxide, thereby reducing its decomposition rate and enhancing its oxidation performance. It can increase the color protection function of the coil material. Moreover, hydrogen peroxide has the dual properties of oxidation and reduction. Hydrogen peroxide is prone to decompose into water and oxygen under light, heating, or when encountering impurities. Adding sodium pyrophosphate increases its stability, avoiding the weakening of the bleaching and oxidation effects on the pulp, ensuring the original color of the coil material, and simultaneously realizing the color protection effect during the preparation of the coil material, increasing the color protection intensity after bleaching during the preparation process of the coil material. According to the weight ratio, a degradation adsorption material is added to the raw pulp solution, with the temperature controlled at 30°C to 60°C, and stirring is carried out for 20 to 35 min to obtain a raw pulp mixture. Bacillus and Acinetobacter can effectively degrade phthalate esters and dioxin-like compounds under different conditions. Through enzymatic reactions, phthalate esters and dioxin-like compounds are decomposed into smaller molecules and ultimately converted into harmless substances. Zero-valent iron and zero-valent aluminum can reduce dioxin under anaerobic conditions, dechlorinate it, and gradually reduce the toxicity of dioxin through reduction reactions, reducing environmental pollution during the papermaking process, reducing harmful substances present in the pulp fiber material, and improving its environmental protection performance. By means of vacuum adsorption, a superabsorbent resin is added to the raw pulp mixture, and sodium chloride solution and calcium chloride solution are also added. Then, the fibers of the raw pulp mixture are deposited on a mesh mold and the water in the raw pulp mixture is filtered to obtain a wet blank pulp semi-finished product. Adding sodium chloride solution or calcium chloride solution to the starch-acrylate polymer will change the water absorption and water retention properties of the material, thereby reducing its water locking strength. During the production process of pulp molding products, the drying efficiency is improved, the water removal rate can be increased under the same energy consumption of heat, the production cost is reduced, and the impact on the environment is also reduced, improving the preparation efficiency of the pulp molding coil material. The wet blank pulp semi-finished product is sent into a single-screw pulp extruder to increase the pulp concentration to 45% to 50%. After drying treatment, it is pressed into blocks and cut to obtain the pulp molding coil material.

[0040] The above has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art of this industry should understand that the present invention is not limited by the above embodiments. What is described in the above embodiments and the specification only illustrates the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention will have various changes and improvements, and these changes and improvements all fall within the scope of the present invention claimed. The scope of protection claimed by the present invention is defined by the appended claims and their equivalents.

Claims

1. A pulp molding spool material, characterized in that By weight percentage, its raw materials are composed of the following components: By weight percentage, its raw materials are composed of the following components: 50% to 85% of waste raw materials, 5% to 20% of epoxy resin, 0.2% to 2% of hydrogen peroxide, 0.5% to 1% of ozone, 1% to 3% of sodium pyrophosphate, 2% to 5% of degradation and adsorption material, 1% to 3% of superabsorbent resin, 0.5% to 1% of sodium chloride solution, 0.5% to 1% of calcium chloride solution, 0.1% to 0.5% of bleaching agent and 0.5% to 1% of antioxidant.

2. The pulp molding spool material according to claim 1, characterized in that, The waste raw materials include at least one of waste newspapers, cardboard paper, paper tubes, pure wood pulp, sugarcane pulp, bamboo pulp and straw pulp; The mass ratio of the waste raw materials to the epoxy resin is 4:

1.

3. The pulp molding spool material according to claim 1, characterized in that, The mass ratio of the hydrogen peroxide, ozone and sodium pyrophosphate is 1:0.5:

3.

4. The pulp molding spool material according to claim 1, characterized in that, The degradation and adsorption material includes at least one of Pseudomonas, Bacillus, Acinetobacter, white rot fungi, photocatalyst, zero-valent iron, zero-valent aluminum, activated carbon, graphene and carbon nanoparticles.

5. The pulp molding coil material according to claim 1, characterized in that, The mass ratio of the degradation and adsorption material to the bleaching agent is 3:1; The bleaching agent includes at least one of sodium dithionite, sulfite and borohydride.

6. The pulp molding spool material according to claim 1, characterized in that, The antioxidant includes at least one of vitamin E, sodium sulfite, potassium sulfite, sodium bisulfite, potassium bisulfite and sodium dithionite.

7. The pulp molding spool material according to claim 6, wherein The antioxidant also includes an anti-ultraviolet aging agent, and the anti-ultraviolet aging agent is pentaerythritol stearate.

8. The pulp molding bobbin material according to claim 1, characterized in that, The superabsorbent resin is synthesized by modifying polyacrylate and starch-acrylate polymer, and the particle size is 100 mesh to 200 mesh, and the water absorption in saturated Ca(OH)2 solution is as high as 40 to 80 g.

9. The pulp molding spool material according to claim 8, wherein The mass ratio of the superabsorbent resin to the sodium chloride solution or calcium chloride solution is 2:

1.

10. A preparation method of a pulp molding coil material, referring to a pulp molding coil material according to any one of claims 1-9, characterized in that, The specific preparation method is as follows: Step 1: Prepare the original pulp solution. Remove the foreign matters on the surface of the waste raw materials, crush them, pour the waste raw materials, epoxy resin, hydrogen peroxide and ozone into the blender according to the weight ratio, stir for 30 min - 60 min, control the temperature at 30°C to 60°C, dilute for 0.5 h - 1 h, add sodium pyrophosphate, and stir again for 10 to 20 min, and grind to obtain the original pulp solution; Step 2: Add the degradation and adsorption material. Add the degradation and adsorption material into the original pulp solution according to the weight ratio, control the temperature at 30°C to 60°C, and stir for 20 to 35 min to obtain the original pulp mixture; Step 3: Molding. By means of vacuum adsorption, add the superabsorbent resin into the original pulp mixture, and add the sodium chloride solution and calcium chloride solution. Then deposit the fibers of the original pulp mixture on the mesh mold and filter the water in the original pulp mixture to obtain a wet blank pulp semi-finished product; Step 4: Press the finished product. Send the wet blank pulp semi-finished product into a single-screw pulp extruder, increase the pulp concentration to 45% to 50%, after drying treatment, press into blocks, cut, and obtain the pulp molding line tray material.