Polar marine corrosion environment simulation system
By designing a polar marine corrosion environment simulation system, the problem of the inability to effectively simulate the polar marine environment in the existing technology is solved, precise control and directional corrosion of the corrosion environment are achieved, and the testing efficiency and convenience of material corrosion research are improved.
Patent Information
- Application Number
- CN202510588579.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-08
- Publication Date
- 2025-07-25
- Estimated Expiration
- 2045-05-08
AI Technical Summary
The existing marine corrosion simulation system cannot effectively simulate the polar marine environment, resulting in large test workload, long periods, uncontrollable conditions, and inability to achieve local directional corrosion and efficient material corrosion research.
A polar marine corrosion environment simulation system was designed, including a test chamber, air conditioner, refrigerator and temperature control system, with light mode, ice flotation mode, current mode and freeze-thaw mode. The control unit regulates the purple light, refrigerator and air conditioner to achieve multi-faceted simulation of the polar marine environment.
It realizes precise control of the corrosion environment, can corrode the samples in a direction, shorten the experimental cycle, save test space, reduce costs, and is suitable for corrosion research of a variety of materials.
Smart Images

Figure CN120369586A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polar marine corrosion environment simulation, and specifically provides a polar marine corrosion environment simulation system. Background Art
[0002] With the continuous development of society and the gradual exhaustion of land resources, people have begun to pay more attention to the development and utilization of marine resources. Contact with the ocean necessarily requires the use of various materials, and seawater is a complex electrolyte with strong corrosiveness. All kinds of materials are constantly facing the test of harsh conditions in the marine environment. According to statistics, the losses caused by marine corrosion each year account for about one-third of the total corrosion losses. At present, the seawater corrosion test of materials mainly relies on seawater natural environment test stations and is carried out by the method of hanging specimens in the sea. Seawater natural environment test stations have been built in many places in China, covering the seawater environmental characteristics of different sea areas from north to south, accumulating a large amount of material corrosion data, and providing a scientific basis and important technical support for material design and selection and new material development in the fields of marine ships, platform ports, and docks. However, it is very difficult to conduct tests on the polar marine environment because there is no such marine environment in the adjacent sea areas of China, and in-situ sea tests cannot be carried out nearby. Moreover, although in-situ sea tests have the advantages of being real and accurate, they also have the following deficiencies: First, the test workload is large, consuming a large amount of manpower and material resources; second, the test cycle is long and cannot meet the needs of new material development in a timely manner; third, the test conditions are uncontrollable and it is difficult to conduct systematic research. Therefore, it is urgent to develop and design experimental equipment for simulating the corrosion of the polar marine environment to fill this gap. By developing a corrosion simulation test system for seawater environments in different zones, on the one hand, it can be an important supplement to in-situ sea tests, and on the other hand, it can combine other research methods in the laboratory to achieve a comprehensive understanding of the corrosion behavior and mechanism of materials.
[0003] Most of the current marine corrosion simulation systems on the market are of closed design and can only immerse or spray-corrode the specimens as a whole. If the specimens are long, the volume of the corrosion chamber needs to be increased accordingly, which not only cannot achieve local directional corrosion of the specimens but also occupies a large amount of test site space, resulting in increased costs. In addition, the simulation environment reduction degree of these systems is low, the automation degree is insufficient, and the operation mode is single and difficult. Therefore, it is particularly important to carry out research on a polar marine environment corrosion simulation test system, especially one that can more comprehensively and realistically simulate the corrosion state of the polar marine environment, so as to more accurately and conveniently obtain information on the corrosion behavior and mechanism of marine materials. Summary of the Invention
[0004] Aiming at the defects in the prior art, the object of the present invention is to provide a polar marine corrosion environment simulation system, including a test chamber, a cold air chamber, a refrigerator, and a temperature control system. A test bucket is arranged in the test chamber, and the temperature control system includes a control unit and an ultraviolet lamp;
[0005] The polar marine corrosion environment simulation system is provided with a light mode, an ice floe mode, an ocean current mode and a freeze-thaw mode; when the light mode is selected, the control unit controls the ultraviolet lamp to increase the light, simulating the long-term light or no-light state in the polar marine area; when the ice floe mode is selected, the control unit controls the refrigerator and the cold air box to start working, rapidly cooling down to make the simulated corrosion solution in the test barrel generate ice floes; when the ocean current mode is selected, the control unit controls the rotation speed of the test barrel to simulate the seabed ocean current in the polar marine environment; when the freeze-thaw mode is selected, the freeze-thaw temperature range and the number of freeze-thaw cycles are selected through the temperature control system, and the control unit controls the refrigerator and the ultraviolet lamp to work in a cycle, and the freeze-thaw cycle simulation of the polar marine environment is carried out by selecting the freeze-thaw temperature range and the number of freeze-thaw cycles.
[0006] In a preferred embodiment, a plurality of ice-breaking rods are installed in the test barrel, and the plurality of ice-breaking rods are circumferentially installed at the bottom of the test barrel; through the rotation of the ice-breaking rods and the test barrel, ice floes are generated on the surface of the solution.
[0007] In a preferred embodiment, the polar marine corrosion environment simulation system further includes: a seawater tank, a workbench, a solution pipe and a cold air pipe; the test chamber and the cold air box are installed on the workbench; the seawater tank and the refrigerator are installed under the workbench; the refrigerator and the seawater tank are connected to the test barrel through the solution pipe to transport the simulated corrosion solution; the refrigerator is connected to the cold air box through the cold air pipe to transport cold air.
[0008] In a preferred embodiment, the polar marine corrosion environment simulation system is in a closed state, and the light is provided by the ultraviolet lamp in the temperature control system, and the phenomenon of polar day and polar night in the polar region is simulated by controlling the working duration of the ultraviolet lamp.
[0009] In a preferred embodiment, a temperature sensor is arranged inside the test chamber; the temperature sensor transmits the detected temperature information to the control unit, and the control unit selects to start the ultraviolet lamp or the refrigerator according to the received temperature information.
[0010] In a preferred embodiment, the polar marine corrosion environment simulation system includes a specimen rack, and the specimen rack includes: a ball screw, an upper tray, a specimen clamp and a lower tray; according to the size of the target test area of the specimen to be tested, the distance between the upper tray and the lower tray is adjusted by rotating the ball screw, the simulated corrosion solution is added into the test barrel, and the movement of the specimen clamp is controlled, so as to realize the control of the corrosion area.
[0011] Compared with the prior art, the present invention has the following beneficial effects:
[0012] 1. The present invention can achieve precise control of the temperature in the corrosive environment, can also perform directional corrosion on the middle part of the specimen without affecting other areas, and can adjust the corrosion area through the specimen holder as needed to achieve precise control of the corrosion area.
[0013] 2. The present invention has multiple modes, realizing multi - function in one machine, and can comprehensively simulate and reproduce the polar environment in the laboratory, which is of great significance for the research on polar marine corrosion.
[0014] 3. The present invention can achieve batch - scale corrosion loading on the premise of realizing directional corrosion of the target area.
[0015] 4. The structure of the present invention is flexible, saving test space, with low cost and strong practicability. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 is a schematic structural view of the present invention without the test chamber 3 installed;
[0017] Figure 2 is the front view of the present invention;
[0018] Figure 3 is the internal top - view structure diagram of the present invention;
[0019] Figure 4 is a schematic structural view of the specimen holder 6;
[0020] Figure 5 is a schematic view of the surface of the temperature control box;
[0021] Figure 6 is a schematic internal structure diagram of the test barrel 4;
[0022] Figure 7 is the top - view of the slidable box wall panel 3 - 1 and the silicone strip;
[0023] Figure 8 is the comparison of the cumulative charge change of high - strength steel (left) and high - strength aluminum alloy (right) under freeze - thaw environment;
[0024] Figure 9 is the macroscopic morphology and the morphology after rust removal of three high - strength steels after one cycle of accelerated environmental spectrum corrosion;
[0025] Figure 10 is the corrosion rate of three high - strength steels after one cycle of accelerated corrosion in the indoor accelerated test spectrum environment;
[0026] Figure 11 、 Figure 12 and Figure 13 are the surface microscopic morphologies of the corrosion products of high - strength steels No. 1, No. 2, and No. 3 respectively after one cycle of accelerated environmental spectrum corrosion;
[0027] Figure 14 、 Figure 15 、 Figure 16 are respectively the cross-sectional morphologies of the corrosion products and the EDS surface scan results after 1 cycle of accelerated environmental spectrum corrosion of three high-strength steels, namely 1#, 2#, and 3#.
[0028] Reference numerals: seawater tank 1; workbench 2; test chamber 3; slidable chamber wall plate 3-1; temperature display screen 3-2; temperature controller button 3-3; electric control switch 3-4; test barrel 4; solution pipe 5; specimen holder 6; ball screw 6-1; upper tray 6-2; specimen clamp 6-3; lower tray 6-4; temperature sensor 7; ultraviolet lamp 8; cage 9; cold air box 10; fan 11; cold air pipe 12; refrigerator 13. Detailed implementation manners
[0029] The present invention will be described in detail below with reference to specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but do not limit the present invention in any form. It should be noted that for those of ordinary skill in the art, without departing from the concept of the present invention, several changes and improvements can still be made. These all belong to the protection scope of the present invention.
[0030] Embodiment 1
[0031] As Figure 1 、 Figure 2The shown polar ocean corrosion environment simulation system includes a test chamber 3, a workbench 2, a cold air box 10, a fan 11, a refrigerator 13, a seawater tank 1, a solution pipe 5, a cold air pipe 12, a test bucket 4, a cage 9, a specimen holder 6 and a temperature control system. The test bucket 4 is used to hold the required simulated corrosion solution (artificially simulated seawater solution). The test bucket 4 is installed in the test chamber 3 and is embedded in the workbench 2. The test chamber 3 mainly serves to protect the test bucket 4 and isolate the environment for heat preservation, mainly to maintain temperature stability when simulating the polar ocean environment. The test chamber 3 and the cold air box 10 are installed on the workbench 2. The refrigerator 13 and the seawater tank 1 are placed under the workbench. The workbench 2 mainly plays a supporting role. The refrigerator 13 and the seawater tank 1 are connected to the cold air box 10 and the test bucket 4 through pipes to complete the work of transporting cold air and simulated corrosion solution. The fan 11 is installed on the left box wall of the cold air box 10 opposite to the ventilation opening on its right box wall. The rotation of the fan 11 is used to realize the air exchange between the two boxes and achieve the function of cooling. The floating ice mode and freeze-thaw mode of the system mainly rely on the refrigerator 13 and the temperature control system to achieve. By inputting temperature parameters in advance in the temperature control system and controlling the working time of the refrigerator 13, the temperature of the solution in the test bucket 4 is reduced to achieve the effect of freezing or freeze-thawing, and then the state of the polar ocean environment is simulated. The specimen holder 6 is installed on the ball screw 6-1 and can move up and down to realize simulated corrosion experiments on different regions of the specimen. The specimen holder 6 is composed of upper and lower parts, and the interval length between the two parts is adjustable. Therefore, the present invention can achieve corrosion tests on the experimental target areas of test specimens with different thicknesses and lengths, with flexible structure, high test efficiency, saving test space and strong practicability.
[0032] One or more specimen clips 6-3 can be installed on the specimen holder 6. When multiple specimen clips 6-3 are installed, multiple groups of experiments can be carried out simultaneously, saving experimental time and experimental costs.
[0033] Specifically, the test specimens include various magnesium-aluminum alloys and various low-alloy steel materials.
[0034] As Figure 6 shown, an arc-shaped groove is provided on the bottom surface of the slidable box wall plate 3-1, and a silica gel strip is provided in the arc-shaped groove. Through the cooperation of the arc-shaped groove and the silica gel strip, on the one hand, the edges and corners can be eliminated, and at the same time, good sealing can be achieved to prevent cold air leakage.
[0035] Specifically, the temperature control system can control the temperature in the test chamber 3 to be constant according to the target temperature. When the temperature in the test chamber 3 is lower than the target temperature, the temperature control system automatically heats the inside of the test chamber 3. When the temperature in the test chamber 3 reaches the target temperature, the temperature control system automatically stops heating the inside of the test chamber 3.
[0036] In a preferred embodiment, the temperature control system includes a control unit, an ultraviolet lamp 8, and a temperature sensor 7; the control unit is installed outside the test chamber 3; the ultraviolet lamp 8 and the temperature sensor 7 are both installed inside the test chamber 3; the temperature sensor 7 can transmit the detected temperature information to the control unit, and the control unit selects to start the ultraviolet lamp 8 for heating or the refrigerator 13 for cooling according to the received temperature information.
[0037] Specifically, as Figure 4 shown, a plurality of specimen clamps 6-3 are circumferentially installed on the specimen holder 6, and the specimens are clamped and positioned through the reserved clamping holes and set screws.
[0038] Specifically, as Figure 3 shown, a control box is provided outside the test chamber 3; a temperature display screen 3-2, a temperature controller button 3-3, and an electric control switch 3-4 are sequentially arranged on the control box from top to bottom; the control unit is installed inside the control box; the electric control switch 3-4 controls the power on or off of the temperature controller button 3-3 and the temperature display screen 3-2 respectively; the target temperature can be set by operating the temperature controller button 3-3; the temperature display screen 3-2 can display the temperature inside the test chamber 3.
[0039] The working principle of the present invention is as follows:
[0040] First, select a specific environmental simulation mode according to the experimental requirements. After selection, wait for 2 to 4 hours for the system to complete the environmental simulation. Then, according to the size of the target test area of the specimen to be tested, adjust the distance between the upper tray 6-2 and the lower tray 6-4 by rotating the ball screw 6-1, add the prepared simulated corrosion solution into the test bucket 4 through the water inlet pipe, and observe the scale in the test bucket 4 until the simulated corrosion solution reaches the required position. Precise control the movement of the specimen holder 6 through the control system, so as to achieve the control of the corrosion area. The process of environmental simulation is mainly as follows: Turn on the electric control switch 3-4 and set the target temperature through the temperature controller button 3-3.
[0041] The system has 4 simulation modes: (1) light mode (2) floating ice mode (3) ocean current mode (4) freeze-thaw mode;
[0042] (1) Light mode: When the light mode is selected, through the control system, the ultraviolet lamp 8 starts to work under the control of the control unit. The light is mainly provided by the ultraviolet lamp 8, and the light duration is determined according to specific experimental parameters, and the long-term light or no-light state in polar ocean regions can be simulated. Among them, the temperature controller button 3-3 and the temperature sensor 7 are connected, and the temperature in the test chamber 3 is displayed on the temperature display screen 3-2 in real time. When the required light duration for the experiment is reached, the ultraviolet lamp 8 stops working.
[0043] The light exposure time depends on the light radiation intensity on the surface of the test piece in the test chamber and the amount of light radiation received during one exposure cycle in the real outdoor environment. The conventional solar irradiation test intensity is taken as the same irradiation intensity as the CASS spectrum, W = (60 ± 10) W / m 2 . When the light radiation intensity in the test chamber is 60 W / m 2 , and the total annual irradiation dose QT = 306.45 MJ / m 2 in the environmental total spectrum of the service environment, the required irradiation time for each test cycle is:
[0044]
[0045] Based on the total annual light radiation intensity at Zhongshan Station, Antarctica being 214.7 MJ / m 2 , it can be obtained that:
[0046]
[0047] That is, the action time of the irradiation experiment is 41 d.
[0048] (2) Floating ice mode:
[0049] Low-temperature freezing test environmental conditions: Since the corrosion is slow during the low-temperature process, the influence of the low-temperature process on electrochemical corrosion is relatively slight. However, in the polar environment, it is necessary to reproduce the influence of the low-temperature process on material damage: First, research shows that there is still an electrochemical process at low temperatures; second, the low-temperature process will affect the expansion of the corrosion front medium and the corrosion situation during subsequent melting; third, the low temperature has a certain impact on mechanical properties. Therefore, the floating ice mode is retained in the accelerated test environmental spectrum for the polar environment.
[0050] When the floating ice mode is selected, through the control system, under the control of the control unit, the cooler 13 and the fan 11 in the cold air box 10 start to work. According to the parameters required for the experiment, the working intensity of the specific cooler and fan is determined. Through the blowing of the fan, the cold air directly contacts the simulated corrosion solution in the test barrel, which can achieve the effect of rapid cooling, causing the simulated corrosion solution to form floating ice, greatly reducing the time required for environmental simulation, shortening the experimental cycle. In addition, the ice-breaking rod in the test barrel can effectively prevent the occurrence of large-scale icing in the test barrel.
[0051] This embodiment is designed taking Zhongshan Station as an example. The temperature range where the environmental task corrosion at Zhongshan Station is very slow is below -10°C. The temperature spectrum results show that the annual minimum temperature at Zhongshan Station is about -40°C. To fully reflect the influence of low temperature, -40°C is selected as the low-temperature test environment in the accelerated spectrum, and the time is selected based on the actual statistical temperature annual spectrum at Zhongshan Station. The total number of days from -30 to -40°C is used as the low-temperature freezing time for indoor freezing:
[0052] t 冰冻= 1 + 5 = 6 (d)
[0053] Since the accelerating effect on corrosion within the range of -10 to -20°C can be ignored and the influence of low temperature is weaker than that at -40°C, this -40°C low-temperature freezing acceleration method of the present accelerated test spectrum can not only magnify the influence of low temperature but also meet the acceleration requirements for material damage and failure in terms of the acceleration time.
[0054] From the equivalent conversion of the polar atmospheric environment spectrum and the accelerated corrosion environment spectrum, the equivalent acceleration relationship:
[0055] t 合金钢 = 3 (d) + 5 (d) + 5 (d) + 6 (d) += 19 (d)
[0056] t 铝合金 = 3 (d) + 4 (d) + 4 (d) + 6 (d) = 17 (d)
[0057] (3) Ocean current mode: When selecting the ocean current mode, according to specific experimental parameters, the rotation speed of the test barrel is selected through the control system. If simulating the Antarctic Circumpolar Current, a 4-pole motor (pole pair number \(p = 2\)) can be selected, and then the synchronous speed \(n=(60×50) / 2 = 1500\) revolutions per minute. If simulating the Arctic Ocean cold current, on this basis, the rotation speed can be appropriately reduced through the transmission system, etc. For example, a 6-pole motor (pole pair number \(p = 3\)) is used, and its synchronous speed \(n=(60×50) / 3 = 1000\) revolutions per minute.
[0058] Through the rotation of the test barrel, a vortex is generated in the simulated corrosion solution, thereby completing the phenomenon of the seabed ocean current in the polar ocean environment inside the barrel.
[0059] (4) Freeze-thaw mode
[0060] The freeze-thaw conversion process is carried out according to one freeze-thaw cycle within a day in the Antarctic summer. After corroding for 6 hours at -5°C, the temperature is raised to 5°C for corrosion for 18 hours, and the change in corrosion current within 24 hours is continuously measured and recorded. The laboratory acceleration condition is to corrode for 2 hours at -10°C and then raise the temperature to 10°C for corrosion for 2 hours (as Figure 8 shown). The temperatures during the freeze-thaw days in summer at Zhongshan Station are mainly -5°C to 5°C. There is a liquid film-ice layer transformation on the surface of the specimen's corrosion medium, and the rust layer may have deterioration behavior. The test is set with a freeze-thaw cycle every 4 hours, freezing at -10°C for 2 hours and then raising the temperature to 10°C for heat preservation for 2 hours.
[0061] The average number of freeze-thaw days per year at Zhongshan Station is 30 days. It is considered that only one freeze-thaw process occurs within 24 hours. An accelerated freeze-thaw cycle includes a 2-hour temperature range of -10°C and a 2-hour temperature range of 10°C. The corrosion charge within one accelerated freeze-thaw cycle is equivalent to the cumulative charge within one day of simulated Antarctic freeze-thaw. Therefore, when the accelerated freeze-thaw condition is freezing at -10°C for 2 hours and then warming to 10°C for melting for 2 hours, the number of accelerated freeze-thaw times required for each test cycle is 30 times, and the total freeze-thaw time t is as follows:
[0062] High-strength steel: t 冻融 =(2 + 2)×30 / 24 = 5(d)
[0063] Aluminum alloy: t 冻融 =(1.5 + 1.5)×30 / 24 ≈ 4(d)
[0064] When selecting the freeze-thaw mode, according to specific experimental parameters, the freeze-thaw temperature range and the number of freeze-thaw times are selected through the temperature control system. Through the cyclic operation of the refrigerator and the ultraviolet lamp, the freeze-thaw cycle simulation of the polar marine environment is completed.
[0065] When the system is working, when the target temperature is reached inside the experimental chamber, the ultraviolet lamp 8 will stop heating and switch to the heat preservation mode. When the temperature is too high, the refrigerator 13 starts to work to reduce the temperature inside the test chamber 3 to the target temperature. The temperature control system realizes the real-time control of the temperature through the coordinated work of the temperature controller button 3-3, the temperature sensor 7, the ultraviolet lamp 8 and the refrigerator 13.
[0066] Example 2
[0067] Based on the accelerated test spectrum constructed in the laboratory, indoor accelerated tests were carried out on three types of high-strength steels. Among them, the three high-strength steels of 1#, 2#, and 3# are alloy steels with different strengths. The test process refers to the "Test Outline for Verifying the Applicability of the Accelerated Test Environment Spectrum in the Polar Environment". The corrosion weight loss, corrosion rate, corrosion products, and corrosion morphology after accelerated corrosion are analyzed.
[0068] Analyze the results of the accelerated corrosion of the three high-strength steels of 1#, 2#, and 3# in the indoor accelerated test spectrum environment. Figure 9 The macroscopic morphologies (a-c) and the morphologies after rust removal (d-f) of the three high-strength steels of 1# (a, d), 2# (b, e), and 3# (c, f) after one cycle of corrosion by the accelerated environment spectrum are shown. The corrosion products of the three steels are reddish-brown, and the areas where the rust layer peels off are gray-green, indicating that the external rust layer is mainly composed of corrosion products of iron ions, and the internal rust layer is ferrous ion products. After rust removal, the surfaces of 1# steel and 2# steel are more uneven, with obvious corrosion pits, and the surface of 3# steel is more flat and uniform after corrosion.
[0069] Figure 10It is the corrosion rate of three high-strength steels after one cycle of accelerated corrosion in the indoor accelerated test spectrum environment. Since one cycle of environmental spectrum acceleration is equivalent to one year outdoors, the unit of corrosion rate here is unified from μm / period to μm / year. It can be seen from the results in the figure that after one cycle of accelerated corrosion of Steel 1#, the corrosion rate is about 11.30 μm / period (μm / year). The corrosion rates of Steel 2# and Steel 3# are relatively high, being 15.02 and 15.49 μm / period (μm / year) respectively.
[0070] Figure 11 、 Figure 12 and Figure 13 are the surface microtopographies of the corrosion products of three high-strength steels, namely Steel 1#, Steel 2#, and Steel 3# after one cycle of accelerated environmental spectrum corrosion. Table 4-1 shows the EDS results at different positions. The main corrosion products on the surface of Steel 1# are cluster-shaped γ-FeOOH and hemispherical and denser α-FeOOH. At the same time, the EDS results show that there is a relatively large amount of Ni element in the rust layer at Point P1. The composition of the corrosion products on the surface of Steel 2# is similar to that of Steel 1#, consisting of hemispherical α-FeOOH and cluster-shaped γ-FeOOH. There is an obvious delamination phenomenon in the rust layer. The outer layer is a loose outer layer, and the fact that no Ni element is detected by EDS indicates that there is no Ni element enrichment area in the outer loose rust layer. The corrosion product layer of Steel 3# is significantly looser, with delamination and spalling of the corrosion products. The corrosion products are composed of loose γ-FeOOH phase (at Position P5) and needle-shaped β-FeOOH phase (at Position P6). The main elements in the rust layer are Fe, O, and C, and no alloying elements that can improve the protection of the rust layer are detected. Figure 14 、 Figure 15 、 Figure 16 are the cross-sectional morphologies of the corrosion products of three high-strength steels, namely Steel 1#, Steel 2#, and Steel 3# after one cycle of accelerated environmental spectrum corrosion and their EDS surface scan results. The thickness of the rust layer of the three materials is about 40 μm. The outer part of the rust layer of Steel 1# is loose and the inner part is denser, but there are cracks at the interface with the substrate. The EDS results show that the Ni content in the inner rust layer is significantly higher than that in the outer rust layer. The rust layer of Steel 2# is tightly bonded to the substrate, but the thickness of the rust layer is uneven, and there are also cracking phenomena in the rust layer. The rust layer of Steel 3# has obvious cracks and cavities, and the rust layer structure is easily damaged, which is also consistent with the result that the corrosion rate of Steel 3# is relatively fast. Summarizing the morphologies of the surface corrosion products and EDS results of the three high-strength steels, it can be found that the corrosion product layer of Steel 1# contains more Ni elements and has better protection, which is mutually verified with the corrosion rate results.
[0071] Table 1 EDS test results at different positions of the corrosion products of three high-strength steels
[0072]
[0073]
[0074] In the description of the present application, it should be understood that the orientation or positional relationship indicated by the terms "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", etc. is based on the orientation or positional relationship shown in the drawings, and is only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the system or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be construed as a limitation to the present application.
[0075] The specific embodiments of the present invention have been described above. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various changes or modifications within the scope of the claims, which do not affect the essence of the present invention. Without conflict, the embodiments of the present application and the features in the embodiments can be combined with each other arbitrarily.
Claims
1. A polar marine corrosion environment simulation system, characterized in that, It includes a test chamber, a cold air chamber, a refrigerator and a temperature control system. A test barrel is arranged inside the test chamber. The temperature control system includes a control unit and an ultraviolet lamp. The polar marine corrosion environment simulation system is provided with a light mode, an ice floe mode, an ocean current mode and a freeze-thaw mode. When the light mode is selected, the control unit controls the ultraviolet lamp to increase the light, simulating the long-time light or no-light state in the polar marine area. When the ice floe mode is selected, the control unit controls the refrigerator and the cold air chamber to start working, rapidly cooling down to make the simulated corrosion solution in the test barrel generate ice floes. When the ocean current mode is selected, the control unit controls the rotation speed of the test barrel to simulate the seabed ocean current in the polar marine environment. When the freeze-thaw mode is selected, the freeze-thaw temperature range and the number of freeze-thaw cycles are selected through the temperature control system. The control unit controls the refrigerator and the ultraviolet lamp to work in a cycle, and simulates the freeze-thaw cycle of the polar marine environment by selecting the freeze-thaw temperature range and the number of freeze-thaw cycles.
2. The polar marine corrosion environment simulation system according to claim 1, wherein A plurality of ice-breaking rods are installed inside the test barrel, and the plurality of ice-breaking rods are circumferentially installed at the bottom of the test barrel. Ice floes are generated on the surface of the solution through the rotation of the ice-breaking rods and the test barrel.
3. The polar marine corrosion environment simulation system according to claim 1, characterized in that, The polar marine corrosion environment simulation system further includes: a seawater tank, a workbench, a solution pipe and a cold air pipe. The test chamber and the cold air chamber are installed on the workbench. The seawater tank and the refrigerator are installed under the workbench. The refrigerator and the seawater tank are connected to the test barrel through the solution pipe to transport the simulated corrosion solution. The refrigerator is connected to the cold air chamber through the cold air pipe to transport cold air.
4. The polar marine corrosion environment simulation system according to claim 1, wherein The polar marine corrosion environment simulation system is in a closed state. The light is provided by the ultraviolet lamp in the temperature control system, and the polar day and polar night phenomena in the polar region are simulated by controlling the working duration of the ultraviolet lamp.
5. The polar marine corrosion environment simulation system according to claim 1, wherein A temperature sensor is arranged inside the test chamber. The temperature sensor transmits the detected temperature information to the control unit, and the control unit selects to start the ultraviolet lamp or the refrigerator according to the received temperature information.
6. The polar marine corrosion environment simulation system according to claim 1, wherein The polar marine corrosion environment simulation system includes a specimen holder, and the specimen holder includes: a ball screw, an upper tray, a specimen clamp and a lower tray. According to the size of the target test area of the specimen to be tested, the distance between the upper tray and the lower tray is adjusted by rotating the ball screw, the simulated corrosion solution is added into the test barrel, and the movement of the specimen clamp is controlled, so as to realize the control of the corrosion area.
Citation Information
Patent Citations
Testing method and testing system for simulating ocean multi-environmental-factor coupling corrosion
CN104390905A
Erosion-corrosion experiment device for simulating spray splashing area
CN104849198A
Polar region corrosion environment spectrum determination method, system, equipment and medium
CN115950812A
Stress corrosion experiment device and method for polar region complex environment
CN117367940A
Circulation accelerated test device of simulation seawater corrosion
CN204831987U