Alkaline medium-coarsening micro-etching liquid and preparation method and micro-etching method thereof

By using alkaline medium-roughening micro-etching solution, the problems of discoloration of the circuit board surface after micro-etching and the easy decomposition of sulfuric acid and hydrogen peroxide are solved, a stable micro-etching rate and efficient AOI inspection are achieved, and the quality of the circuit boards and production efficiency are improved.

CN120738649AActive Publication Date: 2025-10-03SHENZHEN BANMING SCI & TECH CO LTD

Patent Information

Application Number
CN202511239951.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-09-02
Publication Date
2025-10-03
Estimated Expiration
2045-09-02

AI Technical Summary

Technical Problem

The traditional roughening process in sulfuric acid and hydrogen peroxide causes the circuit board surface to discolor after micro-etching, affecting automatic optical inspection. It is also susceptible to chloride ion contamination and decomposition, and cannot meet the circuit quality requirements of high-tech fields.

Method used

An alkaline medium-roughening micro-etching solution is used, which consists of ammonium chloride, tetramethylammonium hydroxide, ammonia water, a catalyst, a wetting agent, an accelerator, a stabilizer and a color difference regulator. Micro-etching is performed by horizontal line spraying to form a uniform rough structure, improve the bonding strength of the copper surface and the ease of detection.

Benefits of technology

It improves the color of the circuit board after micro-etching, improves the AOI inspection efficiency, reduces false positives, improves processing accuracy and finished product yield, reduces material and energy consumption, and overcomes the pollution and decomposition problems of sulfuric acid and hydrogen peroxide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120738649A_ABST
    Figure CN120738649A_ABST
Patent Text Reader

Abstract

The invention discloses an alkaline medium-coarsening micro-etching solution as well as a preparation method and a micro-etching method thereof, and relates to the technical field of printed circuit board production. The alkaline medium-coarsening micro-etching liquid is prepared from the following components in mass concentration: 5-30 g / L of ammonium chloride, 0.5-2 g / L of tetramethylammonium hydroxide, 5-15 g / L of ammonia water, 2-10% of a catalyst, 0.1-1% of a wetting agent, 0.2-2% of an accelerator, 0.3-1.5% of a stabilizer, 0.5-5% of a color difference regulator and the balance of deionized water. The invention provides an alkaline medium-coarsening micro-etching solution and a preparation method and a micro-etching method thereof, which can solve the problem of color change of a board surface after micro-etching of a circuit board and overcome the defect that a sulfuric acid hydrogen peroxide micro-etching system is easily polluted by chloride ions, and can effectively improve the problem that hydrogen peroxide is easily decomposed by replacing sulfuric acid hydrogen peroxide with an alkaline substance. And the micro-etching rate is stable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of printed circuit board production, in particular to an alkaline medium-roughening micro-etching solution and a preparation method and a micro-etching method thereof. Background Art

[0002] With the development of the global economy, especially in high-tech fields such as microelectronics, military, medical, and aerospace, the demand for circuit board (PCB) quality continues to rise. The mid-roughening process is a unique and innovative process used in the production of printed circuit boards (PCBs) to improve the adhesion of dry film / ink to the copper layer. Due to the increasing complexity of PCBs, including ultra-fine line widths / line spacings and micro-vias or blind vias, coupled with the application of new selective surface treatment processes, proper dry film / ink adhesion has become a key requirement. Traditional pre-treatment processes such as mechanical grinding, volcanic ash polishing, and conventional chemical micro-etching have reached their limits, especially when faced with new technologies, and these pre-treatment processes often cannot meet the requirements of the new technologies.

[0003] Medium roughening is a simple process that creates a uniform and finely textured organic metal surface through micro-etching. Traditionally, roughening in sulfuric acid and hydrogen peroxide results in a darker copper surface, hindering automated optical inspection and alignment processes. Furthermore, the industry has been plagued by the decomposition of hydrogen peroxide. Summary of the Invention

[0004] To address the shortcomings of existing technologies, the present invention provides an alkaline medium-roughening micro-etching solution, its preparation method, and micro-etching method. These solutions address discoloration of circuit board surfaces after micro-etching, improve the frequent false positives in the AOI (Automated Optical Inspection) process, and overcome the vulnerability of sulfuric acid and hydrogen peroxide micro-etching systems to chloride ion contamination. Replacing sulfuric acid and hydrogen peroxide with an alkaline solution effectively mitigates the problem of hydrogen peroxide's easy decomposition, resulting in a stable micro-etching rate, significantly improved quality yield, and simple and convenient operation.

[0005] In a first aspect, an alkaline medium-roughening micro-etching solution is provided, comprising the following components by mass concentration: 5-30 g / L of ammonium chloride, 0.5-2 g / L of tetramethylammonium hydroxide, 5-15 g / L of ammonia water, 2-10% of a catalyst, 0.1-1% of a wetting agent, 0.2-2% of an accelerator, 0.3-1.5% of a stabilizer, 0.5-5% of a color difference regulator, and the balance being deionized water; The catalyst is selected from at least one of tetramethylethylenediamine, ferric chloride, and cyclohexanediamine; The wetting agent is selected from at least one of sodium alkyl sulfate, polysorbate 80, and dioctyl sodium sulfosuccinate; The accelerator is selected from at least one of trilaurylmethylammonium chloride, triethanolamine, and 2-aminobenzimidazole; The stabilizer is selected from at least one of polyacrylamide, sodium dihydrogen phosphate, and lauryl amide; The color difference regulator is selected from at least one of sodium polydisulfide dipropane sulfonate, sodium methylene dinaphthalene sulfonate, and fatty amine polyoxyethylene ether.

[0006] Furthermore, the mass ratio of the catalyst to the wetting agent is 1:(0.02-0.2).

[0007] Furthermore, the mass percentage of the catalyst in the alkaline medium roughening micro-etching solution is 5-7%.

[0008] Furthermore, the mass percentage of the wetting agent in the alkaline medium roughening micro-etching solution is 0.4-0.6%.

[0009] Preferably, the mass percentage of the accelerator in the alkaline medium roughening micro-etching solution is 0.8-1.2%.

[0010] Preferably, the mass percentage of the stabilizer in the alkaline medium roughening micro-etching solution is 0.8-1.2%.

[0011] Preferably, the color difference adjusting agent accounts for 2-3% by mass of the alkaline medium roughening micro-etching solution.

[0012] Furthermore, the mass content of ammonium chloride in the alkaline medium roughening micro-etching solution is 18-22 g / L, the mass content of tetramethylammonium hydroxide in the alkaline medium roughening micro-etching solution is 0.8-1.2 g / L, and the mass content of ammonia water in the alkaline medium roughening micro-etching solution is 8-12 g / L.

[0013] Furthermore, the alkaline medium-roughening micro-etching solution is composed of the following components by mass concentration: ammonium chloride 18-22 g / L, tetramethylammonium hydroxide 0.8-1.2 g / L, ammonia water 8-12 g / L, catalyst 5-7%, wetting agent 0.4-0.6%, accelerator 0.8-1.2%, stabilizer 0.8-1.2%, color difference regulator 2-3%, and the balance is deionized water.

[0014] In a second aspect, a method for preparing the alkaline medium-roughening micro-etching solution as described in the first aspect is provided, comprising the following steps: adding ammonium chloride, tetramethylammonium hydroxide, ammonia water, a catalyst, a wetting agent, an accelerator, a stabilizer, and a color difference regulator to deionized water and mixing and stirring to obtain an alkaline medium-roughening micro-etching solution.

[0015] Preferably, the mixing and stirring time is 20-60 min.

[0016] In a third aspect, a micro-etching method using the alkaline medium-roughening micro-etching solution as described in the first aspect is provided, comprising the following steps: using the alkaline medium-roughening micro-etching solution described in the first aspect, micro-etching the circuit board surface at a micro-etching speed of 2-8 m / min in a horizontal line spraying manner.

[0017] Furthermore, the spray pressure of the horizontal spray mode is 1.5-2.5 kg / cm 2 , the micro-etching time is 0.5-1.5min.

[0018] Furthermore, the temperature of the plate surface micro-etching is 25-35°C.

[0019] Preferably, the micro-etching speed is 3-4 m / min.

[0020] Preferably, the temperature for micro-etching the plate surface is 28-32°C.

[0021] Preferably, the alkaline medium-roughening micro-etching solution is used in the micro-etching method at a concentration of 100 wt %.

[0022] The beneficial effects of the present invention are: (1) Alkaline medium-roughening micro-etching liquid uses low-toxic or non-toxic chemical components, which reduces pollution to the environment. It can also provide a more stable micro-etching effect, reduce fluctuations in the micro-etching process, and thus improve processing efficiency and precision. By optimizing the formula and process of the micro-etching liquid, the material consumption and energy consumption in the micro-etching process can be reduced, thereby reducing the overall processing cost; (2) It overcomes the disadvantage that the sulfuric acid hydrogen peroxide micro-etching system is easily contaminated by chloride ions. Using alkaline substances instead of sulfuric acid hydrogen peroxide can effectively improve the problem of hydrogen peroxide being easily decomposed; (3) Through the interaction of the effective components in the alkaline medium-roughening micro-etching solution, the microstructure of the copper surface is changed to form a uniform rough structure, so that the subsequent coating layer (such as the green oil layer) is more firmly bonded to the copper surface and prevents it from falling off. The color of the board surface after micro-etching is close to the base copper plate, which is easier to pass the post-process AOI (AOI: automatic optical inspection) scanning, reducing the number of false points, thereby saving time and improving work efficiency; (4) For precision fine lines (such as lines below 2 mil), the roughness of the line edges is improved by micro-etching and roughening, which reduces micro-short phenomena and improves the yield rate of finished products. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0024] Figure 1 This is a rendering of the production line test of the alkaline medium-roughening micro-etching solution according to Example 1 of the present invention; Figure 2 This is a rendering of the production line test of the alkaline medium-roughening micro-etching solution according to Example 2 of the present invention; Figure 3 This is a rendering of the production line test of the alkaline medium-roughening micro-etching solution of Example 3 of the present invention; Figure 4 This is a rendering of the production line test of the alkaline medium-roughening micro-etching solution of Example 4 of the present invention; Figure 5 This is a rendering of the production line test of the alkaline medium-roughening micro-etching solution of Comparative Example 1 of the present invention; Figure 6 This is a rendering of the production line test of the alkaline medium-roughening micro-etching solution of Comparative Example 2 of the present invention; Figure 7 This is a rendering of the production line test of the alkaline medium-roughening micro-etching solution of Comparative Example 3 of the present invention; Figure 8 This is a rendering of the production line test of the alkaline medium-roughening micro-etching solution of Comparative Example 4 of the present invention. DETAILED DESCRIPTION

[0025] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present invention.

[0026] It will be understood that when used in this specification and the appended claims, the terms “comprises” and “comprising” indicate the presence of described features, integers, steps, operations, elements and / or components, but do not preclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or groups thereof.

[0027] It should also be understood that the terminology used in this specification is for the purpose of describing particular embodiments only and is not intended to limit the present invention. As used in the specification and appended claims, the singular forms "a," "an," and "the" are intended to include the plural forms unless the context clearly indicates otherwise.

[0028] It should be further understood that the term "and / or" used in the present description and the appended claims refers to and includes any and all possible combinations of one or more of the associated listed items.

[0029] In order to more fully understand the technical content of the present invention, the technical solution of the present invention is further introduced and illustrated in conjunction with specific embodiments below.

[0030] Unless otherwise specified, “%” in the present invention refers to mass percentage.

[0031] Micro-etching method of alkaline medium roughening micro-etching solution: The micro-etching method of the alkaline medium-roughening micro-etching solution includes the following processes: S1 board loading; S2 pickling; S3 water washing; S4 board grinding; S5 water washing; S6 micro-etching (medium-roughening); S7 water washing; S8 drying; S9 board collection.

[0032] The S6 micro-etching step is as follows: first, the alkaline medium-roughening micro-etching solution of the embodiment or comparative example is used to open the tank on the horizontal micro-etching line and the temperature is raised to 25-35°C. Then, the circuit board is subjected to a grinding process and the circuit board surface is micro-etched in a horizontal line spraying manner at a micro-etching speed of 2-8m / min. The spraying pressure of the horizontal line spraying manner is 1.5-2.5kg / cm 2 The micro-etching time is 0.5-1.5 minutes. Finally, the micro-etched circuit board is washed with water in step S7, dried in step S8 and collected in step S9.

[0033] Preferably, the spray pressure of the horizontal spray is 1.8-2.2 kg / cm 2 .

[0034] Preferably, the heating temperature is 28-32°C.

[0035] Preferably, the micro-etching speed is 3-4 m / min.

[0036] Preferably, the concentration of the alkaline medium roughening micro-etching solution in the solution preparation tank is 100wt%.

[0037] Alkaline medium roughening micro-etching solution effect verification test (production line test): The alkaline medium roughening micro-etching solution of the embodiment and the comparative example was respectively taken on the production line at a concentration of 100wt% to form a micro-etching line tank liquid. After the micro-etching line tank liquid temperature was heated to 30°C, the circuit boards treated by the micro-etching method of the alkaline medium roughening micro-etching solution were taken and placed in the corresponding micro-etching lines respectively. The micro-etching speed was 6m / min and the spray pressure was 2.0kg / cm 2 , micro-etching time is 1min, the circuit board after micro-etching is washed and dried, and the color of the board surface is observed.

[0038] Example 1 An alkaline medium-roughening micro-etching solution is composed of the following components in mass concentrations: 18 g / L of ammonium chloride, 0.8 g / L of tetramethylammonium hydroxide, 8 g / L of ammonia water, 5% of tetramethylethylenediamine, 0.4% of sodium alkyl sulfate, 0.8% of trilaurylmethylammonium chloride, 0.8% of polyacrylamide, 2% of sodium polydisulfide propane sulfonate, and the balance being deionized water.

[0039] The preparation method of the alkaline medium-roughening micro-etching solution comprises the following steps: adding ammonium chloride, tetramethylammonium hydroxide, ammonia water, a catalyst, a wetting agent, an accelerator, a stabilizer, and a color difference regulator into deionized water, mixing and stirring for 40 minutes to obtain the alkaline medium-roughening micro-etching solution of Example 1.

[0040] The micro-etching method using the alkaline medium-roughening micro-etching solution comprises the following steps: S1 plate loading; S2 pickling; S3 water washing; S4 plate grinding; S5 water washing; S6 medium roughening; S7 water washing; S8 drying; S9 plate collection.

[0041] The S6 micro-etching process is as follows: First, use an alkaline medium-roughening micro-etching solution to open the tank at the micro-etching level and heat it to 28°C. Then, grind the circuit board and perform micro-etching on the circuit board surface in a horizontal spraying manner at a micro-etching speed of 6m / min and a spraying pressure of 1.5kg / cm 2 The micro-etching time is 1.0 min, and the amount of the alkaline medium-roughening micro-etching solution in the potion pot is 100wt%.

[0042] The preparation method of the alkaline medium roughening micro-etching solution of Examples 2-9 is the same as that of Example 1.

[0043] Example 2 An alkaline medium-roughening micro-etching solution is composed of the following components in mass concentrations: 19 g / L ammonium chloride, 0.9 g / L tetramethylammonium hydroxide, 10 g / L ammonia water, 5% ferric chloride, 0.5% polysorbate 80, 0.8% trilaurylmethylammonium chloride, 0.9% sodium dihydrogen phosphate, 2.5% sodium methylene dinaphthalene sulfonate, and the balance being deionized water.

[0044] The micro-etching method of the alkaline medium-roughening micro-etching solution of Example 2 differs from that of Example 1 in that the micro-etching step S6 of Example 2 is as follows: First, the alkaline medium-roughening micro-etching solution is used to open the pot at the micro-etching horizontal line and the temperature is raised to 29°C. Then, the circuit board is ground and the circuit board surface is micro-etched by horizontal spraying at a micro-etching speed of 4m / min and a spray pressure of 1.5kg / cm 2 The micro-etching time is 1.0 min, and the amount of the alkaline medium-roughening micro-etching solution in the potion pot is 100wt%.

[0045] Example 3 An alkaline medium-roughening micro-etching solution is composed of the following components in mass concentrations: 20 g / L of ammonium chloride, 0.8 g / L of tetramethylammonium hydroxide, 11 g / L of ammonia water, 7% of cyclohexanediamine, 0.6% of dioctyl sodium sulfosuccinate, 0.8% of trilaurylmethylammonium chloride, 0.8% of polyacrylamide, 2% of sodium polydisulfide dipropane sulfonate, and the balance being deionized water.

[0046] The micro-etching method of the alkaline medium-roughening micro-etching solution of Example 3 differs from that of Example 1 in that the micro-etching step S6 of Example 3 is as follows: First, the alkaline medium-roughening micro-etching solution is used to open the pot at the micro-etching horizontal line and the temperature is raised to 30°C. Then, the circuit board is ground and the surface of the circuit board is micro-etched by horizontal spraying at a micro-etching speed of 7m / min and a spray pressure of 1.5kg / cm 2 The micro-etching time is 1.1 min, and the amount of the alkaline medium-roughening micro-etching solution in the potion opening tank is 100wt%.

[0047] Example 4 An alkaline medium-roughening micro-etching solution is composed of the following components in mass concentrations: 19 g / L ammonium chloride, 1.2 g / L tetramethylammonium hydroxide, 8 g / L ammonia water, 5% ferric chloride, 0.6% polysorbate 80, 0.8% trilaurylmethylammonium chloride, 1.1% lauramide, 2.5% sodium methylene dinaphthalene sulfonate, and the balance being deionized water.

[0048] The micro-etching method of the alkaline medium-roughening micro-etching solution of Example 4 differs from that of Example 1 in that the micro-etching step S6 of Example 4 is as follows: First, the alkaline medium-roughening micro-etching solution is used to open the pot at the micro-etching horizontal line and the temperature is raised to 29°C. Then, the circuit board is ground and the surface of the circuit board is micro-etched by horizontal spraying at a micro-etching speed of 6m / min and a spray pressure of 1.5kg / cm 2 The micro-etching time is 1.3 min, and the amount of the alkaline medium-roughening micro-etching solution in the potion opening tank is 100 wt%.

[0049] Example 5 An alkaline medium-roughening micro-etching solution is composed of the following components in the following mass concentrations: 20 g / L ammonium chloride, 1.0 g / L tetramethylammonium hydroxide, 12 g / L ammonia water, 7% tetramethylethylenediamine, 0.7% polysorbate 80, 1.0% 2-aminobenzimidazole, 0.9% lauramide, 3% fatty amine polyoxyethylene ether, and the balance being deionized water.

[0050] The micro-etching method of the alkaline medium-roughening micro-etching solution of Example 5 differs from that of Example 1 in that the micro-etching step S6 of Example 5 is as follows: First, the alkaline medium-roughening micro-etching solution is used to open the pot at the micro-etching horizontal line and the temperature is raised to 32°C. Then, the circuit board is ground and the circuit board surface is micro-etched by horizontal spraying at a micro-etching speed of 8m / min and a spray pressure of 2kg / cm 2 The micro-etching time is 1.3 min, and the amount of the alkaline medium-roughening micro-etching solution in the potion opening tank is 100 wt%.

[0051] Example 6 An alkaline medium-roughening micro-etching solution is composed of the following components in mass concentrations: 15 g / L ammonium chloride, 0.5 g / L tetramethylammonium hydroxide, 10 g / L ammonia water, 4% ferric chloride, 0.5% dioctyl sodium sulfosuccinate, 0.8% trilaurylmethylammonium chloride, 1.2% lauramide, 3% sodium polydisulfide dipropane sulfonate, and the balance being deionized water.

[0052] The micro-etching method of the alkaline medium-roughening micro-etching solution of Example 6 differs from that of Example 1 in that the micro-etching step S6 of Example 6 is as follows: First, the alkaline medium-roughening micro-etching solution is used to open the pot at the micro-etching horizontal line and the temperature is raised to 26°C. Then, the circuit board is ground and the circuit board surface is micro-etched by horizontal spraying at a micro-etching speed of 6m / min and a spray pressure of 2.5kg / cm 2 The micro-etching time is 1.5 minutes, and the amount of the alkaline medium-roughening micro-etching solution in the potion opening tank is 100wt%.

[0053] Example 7 An alkaline medium-roughening micro-etching solution is composed of the following components in mass concentrations: 22 g / L of ammonium chloride, 1.0 g / L of tetramethylammonium hydroxide, 12 g / L of ammonia water, 8% of cyclohexanediamine, 0.6% of sodium alkyl sulfate, 1.0% of triethanolamine, 0.8% of sodium dihydrogen phosphate, 2% of sodium methylene dinaphthalene sulfonate, and the balance being deionized water.

[0054] The micro-etching method of Example 7 using an alkaline medium-roughening micro-etching solution differs from that of Example 1 in that the micro-etching step S6 of Example 7 is as follows: First, the alkaline medium-roughening micro-etching solution is used to open the tank at the micro-etching horizontal line and the temperature is raised to 30°C. Then, the circuit board is ground and the surface of the circuit board is micro-etched by horizontal spraying at a micro-etching speed of 7m / min and a spray pressure of 1.8kg / cm 2 The micro-etching time is 1.0 min, and the amount of the alkaline medium-roughening micro-etching solution in the potion pot is 100wt%.

[0055] Example 8 An alkaline medium-roughening micro-etching solution is composed of the following components in mass concentrations: 16 g / L ammonium chloride, 1.0 g / L tetramethylammonium hydroxide, 8 g / L ammonia water, 6% tetramethylethylenediamine, 0.7% sodium dioctyl sulfosuccinate, 1.0% 2-aminobenzimidazole, 1.2% lauramide, 1.5% fatty amine polyoxyethylene ether, and the balance being deionized water.

[0056] The micro-etching method of the alkaline medium-roughening micro-etching solution of Example 8 differs from that of Example 1 in that the micro-etching step S6 of Example 8 is as follows: First, the alkaline medium-roughening micro-etching solution is used to open the tank at the micro-etching horizontal line and the temperature is raised to 28°C. Then, the circuit board is ground and the circuit board surface is micro-etched by horizontal spraying at a micro-etching speed of 5m / min and a spray pressure of 1.7kg / cm 2 The micro-etching time is 1.1 min, and the amount of the alkaline medium-roughening micro-etching solution in the potion opening tank is 100wt%.

[0057] Example 9 An alkaline medium-roughening micro-etching solution is composed of the following components in mass concentrations: 21 g / L ammonium chloride, 0.8 g / L tetramethylammonium hydroxide, 11 g / L ammonia water, 6% ferric chloride, 0.7% dioctyl sodium sulfosuccinate, 1.2% trilaurylmethylammonium chloride, 1.2% lauramide, 2.3% sodium polydisulfide dipropane sulfonate, and the balance being deionized water.

[0058] The micro-etching method of the alkaline medium-roughening micro-etching solution of Example 9 differs from that of Example 1 in that the micro-etching step S6 of Example 9 is as follows: First, the alkaline medium-roughening micro-etching solution is used to open the pot at the micro-etching horizontal line and the temperature is raised to 28°C. Then, the circuit board is ground and the surface of the circuit board is micro-etched by horizontal spraying at a micro-etching speed of 8m / min and a spray pressure of 1.5kg / cm 2 The micro-etching time is 1.5 minutes, and the amount of the alkaline medium-roughening micro-etching solution in the potion opening tank is 100wt%.

[0059] In order to better illustrate the technical effects of the present invention, comparative examples 1-9 are set on the basis of Example 1. The differences between comparative examples 1-9 and Example 1 are shown in Table 1 below: Table 1 Differences between Comparative Examples 1-9 and Example 1

[0060] The difference between Comparative Examples 1-9 and Example 1 is only the components of the alkaline medium-roughening micro-etching solution, and the other conditions are the same.

[0061] In order to further illustrate the technical effects of the present invention, the following experiments were conducted for verification.

[0062] 1. Component Effect Verification Test of Alkaline Medium Roughening Micro-etching Solution 1) The circuit boards treated with the alkaline medium roughening micro-etching solution of Examples 1-9 were subjected to production line testing. The test results are shown in Table 2: Table 2 Test results of alkaline medium roughening micro-etching solution production line of Examples 1-9

[0063] 2) The circuit boards treated with the alkaline medium-roughening micro-etching solutions of Comparative Examples 1-9 were subjected to production line testing. The test results are shown in Table 3: Table 3 Comparative Examples 1-9 Alkaline Medium Roughening Micro-Etching Liquid Production Line Test Results

[0064] The effect diagram of the production line test of the alkaline medium roughening micro-etching solution in Example 1 of the present invention is as follows: Figure 1 As shown, the effect diagram of the production line test of the alkaline medium roughening micro-etching solution of Example 2 of the present invention is as follows Figure 2 As shown, the effect diagram of the production line test of the alkaline medium roughening micro-etching solution of Example 3 of the present invention is as follows Figure 3 As shown, the effect diagram of the production line test of the alkaline medium roughening micro-etching solution of Example 4 of the present invention is as follows Figure 4 As shown, the effect diagram of the production line test of the alkaline medium roughening micro-etching solution of comparative example 1 of the present invention is as follows Figure 5 As shown, the effect diagram of the production line test of the alkaline medium roughening micro-etching solution of comparative example 2 of the present invention is as follows Figure 6 As shown, the effect diagram of the production line test of the alkaline medium roughening micro-etching solution of comparative example 3 of the present invention is as follows Figure 7 As shown, the effect diagram of the production line test of the alkaline medium roughening micro-etching solution of comparative example 4 of the present invention is as follows Figure 8 As shown in the figure, the board surface color of Example 1-9 after micro-etching is lighter, close to the color of the base copper-clad laminate, which can effectively reduce the number of false points reported in the AOI process. The board surface color of Comparative Example 1-9 after micro-etching is darker, deep red, which is likely to increase the number of false points reported in the AOI process.

[0065] Depend on Figures 1-8 As shown in the test results in Tables 2-3, when one or more components of the alkaline medium-roughening micro-etching solution are missing, both the etching rate and quality are significantly affected. This indicates that the present invention utilizes the interaction between ammonium chloride, ammonia water, tetramethylammonium hydroxide, catalyst, wetting agent, stabilizer, accelerator, and color difference modifier in the alkaline medium-roughening micro-etching solution to increase the etching rate of circuit boards and reduce quality issues such as open circuits, short circuits, and gaps on circuit boards.

[0066] 2. Effects of different concentrations of ammonium chloride Comparative Examples 10-12 differ from Example 1 in the concentration of ammonium chloride, with all other conditions remaining the same. Production line tests were conducted on the circuit boards treated with the alkaline medium-roughening micro-etching solutions of Example 1 and Comparative Examples 10-12, and the test results are shown in Table 4: Table 4 Production line test results of Example 1 and Comparative Examples 10-12

[0067] As shown in the test results in Table 4, the absence of ammonium chloride in the alkaline medium-roughening micro-etching solution (Comparative Example 10) resulted in unsatisfactory production line test results. The ammonium chloride concentration was lower than 5 g / L (Comparative Example 10) or higher than 30 g / L (Comparative Example 11), resulting in unsatisfactory production line test results. Therefore, the ammonium chloride concentration in the alkaline medium-roughening micro-etching solution is preferably between 5 and 30 g / L.

[0068] 3. Effect of different catalyst mass concentrations Comparative Examples 7 and 13-14 differ from Example 1 in the catalyst concentration, with all other conditions remaining the same. Production line testing was conducted on circuit boards treated with the alkaline medium-roughening micro-etching solution of Examples 1, 7, and 13-14. The test results are shown in Table 5. Table 5 Production line test results of Example 1, Comparative Example 7, and Comparative Examples 13-14

[0069] The test results in Table 5 show that the production line test results were unsatisfactory when no catalyst was added to the alkaline medium-roughening micro-etching solution (Comparative Example 7). The production line test results were also unsatisfactory when the catalyst concentration was below 2% (Comparative Example 13) or above 10% (Comparative Example 14). Therefore, the catalyst concentration in the alkaline medium-roughening micro-etching solution is preferably between 2% and 10%.

[0070] 4. Effect of different mass concentrations of wetting agents Comparative Examples 5 and 15-16 differ from Example 1 in the mass concentration of the wetting agent, with all other conditions remaining the same. Production line testing was conducted on circuit boards treated with the alkaline medium-roughening micro-etching solution of Example 1, Comparative Examples 5, and Comparative Examples 15-16. The test results are shown in Table 6: Table 6 Production line test results of Example 1, Comparative Example 5, and Comparative Examples 15-16

[0071] The test results in Table 6 show that the alkaline medium-roughening micro-etching solution without a wetting agent (Comparative Example 5) produced unsatisfactory production line test results. The wetting agent concentration was lower than 0.1% (Comparative Example 15) or higher than 1.0% (Comparative Example 16), resulting in unsatisfactory production line test results. Therefore, the wetting agent concentration in the alkaline medium-roughening micro-etching solution is preferably between 0.1% and 1.0%.

[0072] 5. Effect of different mass concentrations of accelerator Comparative Examples 6 and 17-18 differ from Example 1 in the mass concentration of the accelerator, with all other conditions remaining the same. Production line testing was conducted on the circuit boards treated with the alkaline medium-roughening micro-etching solution of Examples 1, 6, and 17-18. The test results are shown in Table 7. Table 7 Production line test results of Example 1, Comparative Example 6, and Comparative Examples 17-18

[0073] The test results in Table 7 show that the production line test results were unsatisfactory when no accelerator was added to the alkaline medium-roughening micro-etching solution (Comparative Example 6). The production line test results were also unsatisfactory when the accelerator concentration was below 0.2% (Comparative Example 17) or above 2.0% (Comparative Example 18). Therefore, the accelerator concentration in the alkaline medium-roughening micro-etching solution is preferably between 0.2% and 2.0%.

[0074] 6. Effect of different mass concentrations of stabilizers Comparative Examples 4 and 19-20 differ from Example 1 in the concentration of the stabilizer, with all other conditions remaining the same. Production line testing was conducted on the circuit boards treated with the alkaline medium-roughening micro-etching solutions of Examples 1, 4, and 19-20. The test results are shown in Table 8. Table 8 Production line test results of Example 1, Comparative Example 4, and Comparative Examples 19-20

[0075] The test results in Table 8 show that the absence of a stabilizer in the alkaline medium-roughening micro-etching solution (Comparative Example 4) resulted in unsatisfactory production line testing results. The presence of an accelerator concentration below 0.3% (Comparative Example 19) or above 1.5% (Comparative Example 20) also resulted in unsatisfactory production line testing results. Therefore, the stabilizer concentration in the alkaline medium-roughening micro-etching solution is preferably between 0.3% and 1.5%.

[0076] 7. Effect of different mass concentrations of color difference regulator Comparative Examples 3 and 21-22 differ from Example 1 in the mass concentration of the color difference adjusting agent; all other conditions remain the same. Production line testing was conducted on circuit boards treated with the alkaline medium-roughening micro-etching solution of Examples 1, 3, and 21-22. The test results are shown in Table 9. Table 9 Production line test results of Example 1, Comparative Example 3, and Comparative Examples 21-22

[0077] The test results in Table 9 show that the production line test results were unsatisfactory when the color difference modifier was not added to the alkaline medium-roughening micro-etching solution (Comparative Example 3). The production line test results were also unsatisfactory when the color difference modifier concentration was lower than 0.5% (Comparative Example 20) or higher than 5% (Comparative Example 21). Therefore, the color difference modifier concentration in the alkaline medium-roughening micro-etching solution is preferably between 0.5% and 5%.

[0078] 8. Effect of different mass ratios of catalyst and wetting agent 1: (0.02-0.2); Comparative Examples 23-24 differ from Example 1 in the mass ratio of the catalyst to the wetting agent, with all other conditions remaining the same. Production line testing was conducted on circuit boards treated with the alkaline medium-roughening micro-etching solutions of Example 1 and Comparative Examples 23-24. The test results are shown in Table 10. Table 10 Production line test results of Example 1 and Comparative Examples 23-24

[0079] The test results in Table 10 show that when the wetting agent ratio in the alkaline medium-roughening micro-etching solution is too low (Comparative Example 22) or too high (Comparative Example 23), the production line test results are unsatisfactory. Therefore, the catalyst to wetting agent ratio in the alkaline medium-roughening micro-etching solution is preferably 1:(0.02-0.2).

[0080] In summary, the present invention provides an alkaline medium-roughening micro-etching solution, a preparation method thereof, and a micro-etching method, which can solve the problem of discoloration of the circuit board surface after micro-etching, overcome the disadvantage that the sulfuric acid hydrogen peroxide micro-etching system is easily contaminated by chloride ions, and use an alkaline substance instead of sulfuric acid hydrogen peroxide to effectively improve the problem of easy decomposition of hydrogen peroxide, thereby achieving a stable micro-etching rate.

[0081] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the technical scope disclosed in the present invention, and such modifications or substitutions are intended to be within the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be subject to the scope of protection of the claims.

Claims

1. An alkaline medium roughening micro-etching solution, characterized in that: The composition is composed of the following components by mass concentration: ammonium chloride 5-30g / L, tetramethylammonium hydroxide 0.5-2g / L, ammonia water 5-15g / L, catalyst 2-10%, wetting agent 0.1-1%, accelerator 0.2-2%, stabilizer 0.3-1.5%, color difference regulator 0.5-5%, and the balance is deionized water; The catalyst is selected from at least one of tetramethylethylenediamine, ferric chloride, and cyclohexanediamine; The wetting agent is selected from at least one of sodium alkyl sulfate, polysorbate 80, and dioctyl sodium sulfosuccinate; The accelerator is selected from at least one of trilaurylmethylammonium chloride, triethanolamine, and 2-aminobenzimidazole; The stabilizer is selected from at least one of polyacrylamide, sodium dihydrogen phosphate, and lauryl amide; The color difference regulator is selected from at least one of sodium polydisulfide dipropane sulfonate, sodium methylene dinaphthalene sulfonate, and fatty amine polyoxyethylene ether.

2. The alkaline medium roughening micro-etching solution according to claim 1, characterized in that: The mass ratio of the catalyst to the wetting agent is 1:(0.02-0.2).

3. The alkaline medium roughening micro-etching solution according to claim 1, characterized in that: The mass percentage of the catalyst in the alkaline medium roughening micro-etching solution is 5-7%.

4. The alkaline medium roughening micro-etching solution according to claim 1, characterized in that: The mass percentage of the wetting agent in the alkaline medium roughening micro-etching solution is 0.4-0.6%.

5. The alkaline medium roughening micro-etching solution according to claim 1, characterized in that: The mass content of the ammonium chloride in the alkaline medium roughening micro-etching solution is 18-22 g / L, the mass content of the tetramethylammonium hydroxide in the alkaline medium roughening micro-etching solution is 0.8-1.2 g / L, and the mass content of the ammonia water in the alkaline medium roughening micro-etching solution is 8-12 g / L.

6. The alkaline medium roughening micro-etching solution according to claim 1, characterized in that: The invention is composed of the following components in the following mass concentrations: ammonium chloride 18-22 g / L, tetramethylammonium hydroxide 0.8-1.2 g / L, ammonia water 8-12 g / L, catalyst 5-7%, wetting agent 0.4-0.6%, accelerator 0.8-1.2%, stabilizer 0.8-1.2%, color difference regulator 2-3%, and the balance is deionized water.

7. The method for preparing the alkaline medium-roughening micro-etching solution according to any one of claims 1 to 6, wherein: The following steps are involved: Ammonium chloride, tetramethylammonium hydroxide, ammonia water, a catalyst, a wetting agent, an accelerator, a stabilizer, and a color difference regulator are added into deionized water and mixed to obtain an alkaline medium-roughening micro-etching solution.

8. The micro-etching method using an alkaline medium-roughening micro-etching solution according to any one of claims 1 to 6, wherein: The following steps are involved: The alkaline medium roughening micro-etching solution according to any one of claims 1 to 6 is used to micro-etch the circuit board surface in a horizontal line spraying manner at a micro-etching speed of 2-8 m / min.

9. The micro-etching method using an alkaline medium-roughening micro-etching solution according to claim 8, wherein: The spray pressure of the horizontal spray method is 1.5-2.5kg / cm 2 , the micro-etching time is 0.5-1.5min.

10. The micro-etching method using an alkaline medium-roughening micro-etching solution according to claim 8, wherein: The temperature for micro-etching the board surface is 25-35℃.

Citation Information

Patent Citations

  • Roughening micro-etching agent for circuit board and preparation method of roughening micro-etching agent

    CN117328066A

  • Composite nano caustic soda liquid, preparation method thereof and circuit board production wastewater treatment method

    CN119874005A

  • Environment-friendly titanium alloy etching solution and preparation method and etching method thereof

    CN120041834A

  • Composition for titanium nitride hard mask removal and etch residue cleaning

    EP3599634A1

  • Catalyst application solution, electroless plating method using same, and direct plating method

    US20120171363A1

Cited By

  • Alkaline super-roughening solution, preparation method thereof and super-roughening method

    CN121575407A

  • An alkaline super-roughening solution, a method for preparing the same, and a super-roughening method

    CN121575407B