High-energy water reaction metal fuel propellant as well as preparation method and application thereof
By preparing a high-energy water-reactive metal fuel propellant and using novel binders and combustion promoters, the problem of difficult aluminum/water reaction start-up was solved, achieving high-density, high-efficiency combustion and adjustable burning rate, making it suitable for equipment such as water-ramjet engines.
Patent Information
- Application Number
- CN202511473755.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-10-15
- Publication Date
- 2025-11-18
AI Technical Summary
Existing water-reacting metallic fuel propellants are difficult to start in the aluminum/water reaction. The reaction product Al2O3 adheres and prevents the reaction from proceeding further, resulting in poor combustion performance. Moreover, existing research mainly focuses on engine models and theories, lacking systematic research on energy performance and combustion performance.
A high-energy water-reactive metal fuel propellant is prepared by using a system of binders, oxidants, metallic fuels, curing agents, combustion promoters, and pressure index regulators, through mixing and curing processes. This includes the controlled proportions of burning rate regulators, pressure index regulators, and process aids.
It improves the density and combustion efficiency of the propellant, has good mechanical properties, adjustable burning rate, and adjustable dynamic pressure index, making it suitable for water ramjet engines, underwater vehicles, and torpedoes, with an overall improved burning rate.
Smart Images

Figure SMS_3 
Figure SMS_4 
Figure SMS_5
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the propellant technical field, in particular, it relates to a kind of high-energy water reaction metal fuel propellant and its preparation method and application. BACKGROUND
[0002] Water reaction metal fuel propellant is the key technology to realize super-speed torpedo powerful propulsion system, is the main fuel of water ramjet system, plays a decisive role in the comprehensive performance of water ramjet, and it is of great significance to develop water reaction metal fuel propellant.
[0003] Although the energy of aluminum-based water reaction metal fuel is higher than that of magnesium-based water reaction metal fuel, the aluminum surface is covered with a very dense alumina film, so that the aluminum / water reaction is difficult: (1) it is difficult to start Al / H2O reaction. (2) there is great difficulty in continuous Al / H2O reaction, because the reaction product Al2O3 can be firmly attached to the surface of aluminum, preventing further reaction. Therefore, in order to ensure the combustion, the ambient temperature of combustion must be higher than the melting point of alumina. Gorbunov of Russia studied the combustion reaction performance of Al / H2O and Mg / H2O, and the results showed that the combustion performance of "metal / water" mixture was related to the difficulty of oxidation of metal powder, and the oxidation degree of metal powder depended on the water fuel ratio (mass ratio of water to metal fuel in the mixture), and it was found that the aggregation state (condensed phase or gas phase) of water did not affect the oxidation degree of metal powder. Risha of the United States found that the flame temperature of Al / H2O reaction was lower than the gasification temperature of Al, while the flame temperature of Al in air or oxygen was higher than the gasification temperature of Al, which indicated that there was difference in reaction mechanism between the two, and the Al water reaction was more similar to the combustion of solid carbon, and the mixing of gas phase had little effect on the reaction, and the reaction was carried out on the surface of aluminum particles, and the combustion time was proportional to the diameter of aluminum particles. At present, the research on water reaction metal fuel in China mainly focuses on the test parameters, engine model, working principle and theoretical research of water ramjet. Therefore, it is urgent to carry out systematic research on the energy performance and combustion performance of water reaction metal fuel propellant and its adjusting method. SUMMARY
[0004] The purpose of the present application is to overcome the above-mentioned shortcomings of the prior art, and to provide a kind of high-energy water reaction metal fuel propellant and its preparation method and application.
[0005] The technical problem of the present application is solved by using the following technical scheme.
[0006] The application provides a high-energy water reaction metal fuel propellant, which comprises a binder system composed of a binder and a plasticizer, an oxidizer, a metal fuel, a curing agent and a combustion promoter, and further comprises a pressure index regulator system and a network regulator, wherein the pressure index regulator system comprises a burning rate regulator, a pressure index regulator and a process aid, and the mass ratio of the burning rate regulator, the pressure index regulator and the process aid is (1.0-3):(0.1-0.3):(0.02-0.04).
[0007] The application provides a preparation method of the high-energy water reaction metal fuel propellant, which comprises the following steps: mixing components in proportion to obtain a slurry, vacuum casting the slurry into a mold or a water ram solid rocket engine, and obtaining the high-energy water reaction metal fuel propellant after curing. Preferably, the mixing temperature is 40-60 DEG C, the mixing time is 70-120 min, the curing temperature is 50-60 DEG C, and the curing time is 4-8 days.
[0008] The application provides an application of the high-energy water reaction metal fuel propellant in a water ram engine, an underwater vehicle or a torpedo.
[0009] The application has the following beneficial effects: The application provides a high-energy water reaction metal fuel propellant, a preparation method and an application thereof, wherein the high-energy water reaction metal fuel propellant with excellent comprehensive performance is obtained by introducing a pressure index regulator system and a network regulator, the actual density of the high-energy water reaction metal fuel propellant is not less than 1.87 g / cm 3 , the one-time combustion injection efficiency is not less than 97%, the mechanical property is good, the burning rate and the dynamic pressure index are adjustable, in addition, the comprehensive burning rate of the water ram rocket engine can be improved by embedding metal wires, and the high-energy water reaction metal fuel propellant can be widely used in water ram engines, underwater vehicles or torpedoes and the like. DETAILED DESCRIPTION
[0010] In order to make the purpose, technical scheme and advantages of the embodiments of the application more clear, the technical scheme in the embodiments of the application will be clearly and completely described below. If the specific conditions are not indicated in the embodiments, the conventional conditions or the conditions suggested by the manufacturers are adopted. If the reagents or instruments are not indicated by the manufacturers, they are all conventional products which can be purchased in the market.
[0011] The high-energy water reaction metal fuel propellant, the preparation method and the application thereof provided by the embodiments of the application will be specifically described below.
[0012] In a first aspect, the embodiments of the present application provide a high-energy water reaction metal fuel propellant, comprising: a binder system composed of a binder and a plasticizer, an oxidizer, a metal fuel, a curing agent and a combustion promoter, further comprising a pressure exponent regulator system and a network regulator, the pressure exponent regulator system comprising a burning rate regulator, a pressure exponent regulator and a process aid, the mass ratio of the burning rate regulator, the pressure exponent regulator and the process aid being (1.0-3):(0.1-0.3):(0.02-0.04).
[0013] In some alternative embodiments, the burning rate regulator is one of 2,2-bis(ethyl ferrocene) propane (GFP), BH-01 or a combination thereof, the general formula of BH-01 being: 10 H 10 -CH2-OOC(CH2) n CH3, 12≤n≤16, wherein B 10 H 10 The structural formula of GFP is as follows: .
[0014] In some alternative embodiments, the pressure exponent regulator is TAP, the particle size d 50 ≤5μm, the general formula of TAP being: (C6H 14 N2)2X(NH4)(ClO4)6, wherein: X is any one of Li, Na, K, and the structural formula of TAP is as follows: .
[0015] In some alternative embodiments, the process aid is one of 1,2-diamino propane, 2-hydroxyethylamine or a combination thereof.
[0016] In some alternative embodiments, the binder is one of hydroxyl-terminated polybutadiene (HTPB), hydroxyl-terminated polyisoprene (HTPC) or a combination thereof, and the plasticizer is one of dioctyl sebacate (DOS), dioctyl adipate (DOA) or a combination thereof. Preferably, the viscosity of the hydroxyl-terminated polybutadiene and the hydroxyl-terminated polyisoprene is less than 6 Pa•s, the hydroxyl value is 0.5 mmol / g-0.7 mmol / g, the number average molecular weight of the hydroxyl-terminated polybutadiene is 3000-3500, the number average molecular weight of the hydroxyl-terminated polyisoprene is 3500-4500, and the average functionality is 2.0±0.1.
[0017] In some alternative embodiments, the curing agent is one of toluene diisocyanate (TDI), hexamethylene polyisocyanate (HDI) or a combination thereof.
[0018] In some alternative embodiments, the combustion promoter is lithium fluoride (LiF), the particle size d 50 ≤ 3 μm In some alternative embodiments, the metal fuel is one of aluminum powder (Al), aluminum-magnesium alloy powder (Al-Mg), aluminum-lithium alloy powder (Al-Li), or a combination thereof. Preferably, the particle size d 50 ≤ 5 μm. Preferably, the mass percentage of aluminum to magnesium in the aluminum-magnesium alloy powder is 1:1, and the particle size of the aluminum-magnesium alloy powder is between 13 μm and 27 μm. Preferably, the mass percentage of lithium in the aluminum-lithium alloy powder is 2.0%-3.0%, the mass percentage of magnesium is 0.2%-0.5%, the mass percentage of scandium (Sc) is 0.2%-0.5%, and the mass percentage of iridium (Y) is 0.2%-0.5%, the particle size of the aluminum-lithium alloy powder is between 13 μm and 27 μm, and the small amount of scandium and iridium in the aluminum-lithium alloy powder can improve the stability of the aluminum-lithium alloy powder. Preferably, when the metal fuel is a combination of aluminum powder (Al), aluminum-magnesium alloy powder (Al-Mg), and aluminum-lithium alloy powder (Al-Li), the mass percentage of the aluminum powder in the metal fuel is 5%-10%, the mass percentage of the aluminum-magnesium alloy powder in the metal fuel is 20%-30%, and the mass percentage of the aluminum-lithium alloy powder in the metal fuel is 60%-75%.
[0019] In some alternative embodiments, the oxidizer is ammonium perchlorate (AP). Preferably, the ammonium perchlorate includes coarse-grained ammonium perchlorate and medium-grained ammonium perchlorate, the particle size d 50 of the coarse-grained ammonium perchlorate is 300±10 μm, and the particle size d 50 of the medium-grained ammonium perchlorate is 100±5 μm, and the mass percentage of the coarse-grained ammonium perchlorate in the oxidizer is 50%-60%.
[0020] In some alternative embodiments, the network regulator is one of 1,6-hexanediamine, BA-01, tris(2-methylaziridine)oxophosphine (MAPO), and boron trifluoride triethanolamine complex (T313), or a combination thereof, wherein the structural formula of BA-01 is as follows:
[0021] The degree of polymerization n is 35-45.
[0022] In some alternative embodiments, the high-energy water reaction metal fuel propellant includes the following components in the following mass percentages: Binder: 5.5%-7.0%; Metal fuel: 50%-60%; Oxidizer: 26%-36%; Plasticizer: 2.0%-3.8%; Curing agent: 0.3%-0.4%; Burning rate regulator: 1.0%-3%; Pressure index regulator: 0.1%-0.3%; Process aid: 0.02%-0.04%; Network regulator: 1.0%-3.0%; Combustion promoter: 0.1%-0.3%.
[0023] In a second aspect, the embodiment of the present application provides a preparation method of the high-energy water-reactive metal fuel propellant, comprising the following steps: (1) weighing the components according to the selected formula proportion; (2) putting the components into a vertical mixer for mixing, the mixing temperature is 40-60℃, the mixing time is 70-110min, and a slurry is obtained; (3) vacuum casting the slurry into a mold or a water ram solid rocket engine, and then placing it in an oven at 50-60℃ for curing for 7-8 days.
[0024] In a third aspect, the embodiment of the present application provides an application of the high-energy water-reactive metal fuel propellant in a water ram engine, an underwater vehicle or a torpedo.
[0025] As can be seen, the embodiment of the present application provides a high-energy water-reactive metal fuel propellant, which has the following advantages compared with the prior art: (1) The water-reactive metal fuel propellant provided by the present application can significantly improve the solid content of the water-reactive metal fuel propellant by using a new binder and a process aid, thereby improving the density of the propellant, and the propellant of the present application has a test density not less than 1.87g / cm 3 ; (2) The water-reactive metal fuel propellant provided by the present application can make the one-time injection efficiency of the water-reactive metal fuel propellant not less than 97% by using a combustion promoter; (3) The water-reactive metal fuel propellant provided by the present application can make the interior ballistic performance of the water-reactive metal fuel propellant better by using a burning rate regulator, and the burning rate is adjustable at 10-30mm / s (4MPa); (4) The water reaction metal fuel propellant provided by the application can significantly improve the mechanical properties of the water reaction metal fuel propellant by using a new binder and a network regulator, the maximum tensile strength (20℃, 100mm / min) can be adjusted in the range of 0.6MPa-2MPa, and the maximum elongation (20℃, 100mm / min) can be adjusted in the range of 30%-60%; (5) The water reaction metal fuel propellant provided by the application has good combustion stability, and the dynamic pressure index can be adjusted in the range of 0.2-0.5 (1-9MPa) by using a dynamic pressure index regulator; (6) The water reaction metal fuel propellant provided by the application has high energy, and the measured specific impulse of the water ramjet engine (the inner diameter of the combustion chamber charge is not less than Φ300mm, and the length of the combustion chamber charge is not less than 2500mm) is not less than 545s (the combustion chamber pressure is 4MPa, the ambient pressure is 0.101325MPa, and the mass ratio of water to metal fuel is between 4.0-4.5); (7) The water reaction metal fuel propellant provided by the application can increase the comprehensive burning rate of the engine to more than 50mm / s (4MPa) by embedding metal wires (silver wires, copper wires).
[0026] The high-energy water reaction metal fuel propellant provided by the application, the preparation method and the application thereof will be described in detail in combination with the embodiments below, but they cannot be understood as the limitation of the protection scope of the application.
[0027] The high-energy water reaction metal fuel propellant and the preparation method thereof have the following formula composition (calculated in percentage by mass): Table 1 Formula composition and performance of Example 1
[0028] Table 2 Formula composition and performance of Example 2
[0029] Table 3 Formula composition and performance of Example 3
[0030] Table 4 Formula composition and performance of Example 4
[0031] Table 5 Formula composition and performance of Example 5 .
[0033] In summary, this invention provides a high-energy water-reacting metal fuel propellant, its preparation method, and its application. The high-energy water-reacting metal fuel propellant comprises the following components by mass percentage: binder: 5.5%-7.0%; metal fuel: 50%-60%; oxidant: 26%-36%; plasticizer: 2.0%-3.8%; curing agent: 0.3%-0.4%; burning rate regulator: 1%-3%; pressure index regulator: 0.1%-0.2%; process aid: 0.02%-0.04%; network regulator: 1%-3%; and combustion promoter: 0.1%-0.3%. The water-reacting metal fuel propellant provided by this invention has a high energy density, with a measured density of not less than 1.87 g / cm³. 3 The water-rammed rocket engine (combustion chamber propellant inner diameter not less than Φ300mm, combustion chamber propellant length not less than 2500mm) has a measured specific impulse of not less than 545s (combustion chamber pressure 4MPa, ambient pressure 0.101325MPa, water to metal fuel mass ratio between 3.5 and 4.5), and a single-stage combustion injection efficiency of not less than 97%. It possesses excellent formulation and process performance, good mechanical properties, and its maximum tensile strength (20℃, 100mm / min) is adjustable within the range of 0.6MPa-2MPa, and its maximum elongation (20℃, 100mm / min) is adjustable within the range of 30%-60%. The burning rate is adjustable within the range of 10mm / s-30mm / s (7MPa), and the dynamic pressure index is adjustable between 0.2 and 0.5 (1-9MPa). This propellant can be used to increase the engine's overall burning rate to over 50mm / s (4MPa) by embedding metal wires (silver wire, copper wire).
[0034] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A high-energy water-reactive metal fuel propellant, comprising: An adhesive system, oxidant, metallic fuel, curing agent, and combustion promoter composed of adhesives and plasticizers, characterized in that it further includes a pressure index regulator system and a network regulator, wherein the pressure index regulator system includes a burning rate regulator, a pressure index regulator, and a process aid, and the mass ratio of the burning rate regulator, the pressure index regulator, and the process aid is (1.0-3):(0.1-0.3):(0.02-0.04).
2. The high-energy water-reactive metal fuel propellant according to claim 1, characterized in that, The combustion rate regulator is one or a combination of 2,2-bis(ethylferrocene)propane (GFP) and BH-01, wherein the general formula of BH-01 is: B 10 H 10 -CH2-OOC(CH2) n CH3, 12≤n≤16, where B 10 H 10 The structural formula is shown below: 。 3. The high-energy water-reactive metal fuel propellant according to claim 1, characterized in that, The pressure index regulator is TAP, with a particle size of d. 50 ≤5μm, the general formula for TAP is: (C6H 14 N2)2X(NH4)(ClO4)6, where X is any one of Li, Na, and K. The structural formula of TAP is shown below: 。 4. The high-energy water-reactive metal fuel propellant according to claim 1, characterized in that, The process aid is one or a combination of 1,2-diaminopropane and 2-hydroxyethylamine.
5. The high-energy water-reactive metal fuel propellant according to claim 1, characterized in that, The adhesive is one or a combination of hydroxyl-terminated polybutadiene (HTPB) and hydroxyl-terminated polyisoprene (HTPC), and the plasticizer is one or a combination of dioctyl sebacate (DOS) and dioctyl adipate (DOA). Preferably, the viscosity of the hydroxyl-terminated polybutadiene and the hydroxyl-terminated polyisoprene is less than 6 Pa•s, and the hydroxyl value is 0.5 mmol / g-0.7 mmol / g; the number average molecular weight of the hydroxyl-terminated polybutadiene is 3000-3500, the number average molecular weight of the hydroxyl-terminated polyisoprene is 3500-4500, and the average functionality is 2.0±0.
1.
6. The high-energy water-reactive metal fuel propellant according to claim 1, characterized in that, The curing agent is one or a combination of toluene diisocyanate (TDI) and hexamethylene polyisocyanate (HDI), and the combustion promoter is lithium fluoride (LiF), wherein the particle size d of the lithium fluoride is... 50 ≤3μm, wherein the metal fuel is one or a combination of aluminum powder (Al), aluminum-magnesium alloy powder (Al-Mg), and aluminum-lithium alloy powder (Al-Li), and the oxidant is ammonium perchlorate (AP); Preferably, the particle size d of the aluminum powder 50 ≤5μm; Preferably, the mass percentage of aluminum to magnesium in the aluminum-magnesium alloy powder is 1:1; the particle size of the aluminum-magnesium alloy powder is between 13μm and 27μm. Preferably, the aluminum-lithium alloy powder contains 2.0%-3.0% lithium by mass, 0.2%-0.5% magnesium by mass, 0.2%-0.5% scandium (Sc) by mass, and 0.2%-0.5% iridium (Y) by mass; the particle size of the aluminum-lithium alloy powder is between 13μm and 27μm. Preferably, when the metal fuel is a combination of aluminum powder (Al), aluminum-magnesium alloy powder (Al-Mg), and aluminum-lithium alloy powder (Al-Li), the mass percentage of aluminum powder in the metal fuel is 5%-10%, the mass percentage of aluminum-magnesium alloy powder in the metal fuel is 20%-30%, and the mass percentage of aluminum-lithium alloy powder in the metal fuel is 60%-75%. Preferably, the ammonium perchlorate includes coarse-grained ammonium perchlorate and medium-grained ammonium perchlorate; the coarse-grained ammonium perchlorate has a d... 50 The d of medium-sized ammonium perchlorate with a particle size of 300±10μm is 50 The particle size is 100±5μm; the mass percentage of the coarse-grained ammonium perchlorate in the oxidant is 50%-60%.
7. The high-energy water-reactive metal fuel propellant according to claim 1, characterized in that, The network regulator is one or a combination of 1,6-hexanediamine, BA-01, tris(2-methylaziridine)phosphine oxide (MAPO) and boron trifluoride triethanolamine complex (T313), wherein the structural formula of BA-01 is shown below: The degree of polymerization, n, is 35-45.
8. The high-energy water-reactive metal fuel propellant according to any one of claims 1-7, characterized in that, Components include the following percentage by weight: Adhesive: 5.5%-7.0%; Metal fuels: 50%-60%; Oxidizing agent: 26%-36%; Plasticizer: 2.0%-3.8%; Hardener: 0.3%-0.4%; Burn rate modifier: 1.0%-3%; Pressure index regulator: 0.1%-0.3%; Processing aids: 0.02%-0.04%; Network regulator: 1.0%-3.0%; Combustion accelerator: 0.1%-0.3%.
9. A method for preparing a high-energy water-reactive metal fuel propellant according to any one of claims 1-8, characterized in that, The process includes the following steps: mixing the components in a specific ratio to obtain a slurry; vacuum casting the slurry into a mold or a water-pressed solid rocket motor; and after curing, obtaining a propellant strip. Preferably, the mixing temperature is 40℃-60℃, the mixing time is 70min-120min, the curing temperature is 50℃-60℃, and the curing time is 4-8 days; Preferably, the method further includes embedding a metal wire during the strip forming process to obtain a metal wire-embedded strip.
10. The application of the high-energy water-reactive metal fuel propellant according to any one of claims 1-8, characterized in that, The high-energy water-reactive metal fuel propellant is applied to water ramjet engines, underwater vehicles, or torpedoes; Preferably, the measured density of the high-energy water-reactive metal fuel propellant is not less than 1.87 g / cm³. 3 The single-stage combustion injection efficiency is no less than 97%.