Curing rate adjustable supramolecular host-guest photoinitiator and epoxy adhesive
By introducing a delayed curing window into UV epoxy adhesives using supramolecular host-guest photoinitiators, the problem of curing UV epoxy adhesives on low UV transmittance substrates is solved, achieving flexible curing rate control and efficient bonding.
Patent Information
- Application Number
- CN202511177318.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-21
- Publication Date
- 2025-11-25
- Estimated Expiration
- 2045-08-21
AI Technical Summary
Existing UV epoxy adhesives cannot be effectively cured on substrates that cannot be penetrated by ultraviolet light, and existing delayed curing solutions lack universality, making it difficult to meet the delay effects and process requirements of various formulations.
A supramolecular host-guest photoinitiator is used, in which the supramolecular host compound encapsulates the guest photoinitiator to form a delayed curing window. The curing rate is adjusted by using macrocyclic structures and reactive functional groups, and flexible curing is achieved by combining UV light irradiation and temperature control.
It provides a delayed curing window, is compatible with a variety of formulations, solves the curing problem of low UV transmission components, improves bond strength and moisture barrier properties, and reduces process difficulty.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_4
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the field of adhesives, in particular to a supramolecular host-guest photoinitiator with adjustable curing rate and an epoxy adhesive, and a preparation method and application of the epoxy adhesive. BACKGROUND
[0002] In recent decades, UV epoxy curing adhesives have been widely used in the field of precision electronic device packaging due to their fast curing speed, easy operation, and large bonding strength. However, when the substrate to be bonded cannot be penetrated by ultraviolet light, such as when the adhesive is applied to non-transparent substrates or substrates with added UV absorbers, the photoinitiator cannot be activated by light and cannot be successfully cured by UV, greatly limiting the use of UV-curable adhesives.
[0003] To solve the above problems, the skilled in the art have proposed solutions combining UV with other curing methods, such as UV / humidity dual curing and UV / thermal dual curing. However, these solutions all have their own drawbacks, such as poor compatibility between material components, difficulty in dispersion, insufficient bonding strength, limitation of material types to avoid unwanted side reactions, and inapplicability to some environments with special construction requirements. Another relatively effective solution is to develop a delayed curing adhesive that does not immediately cure after light exposure and only starts to cure after the lapping of the substrate is completed. In recent years, based on specific formulation design, resin structure design, and selection of photoinitiators, people have developed some UV delayed curing adhesives. For example, invention patent application CN118307767A discloses an epoxy resin UV delayed curing agent for preparing a resin composition for display element packaging, which has excellent properties such as delayed curing, strong water vapor barrier ability, and strong adhesion ability, and can provide better protection for display elements when applied to the packaging of display elements. This invention can achieve a certain delay time by designing the structure of the epoxy compound. For another example, invention patent CN115895549B discloses a UV delayed curing adhesive for sealing cylindrical batteries, a preparation method and application thereof. The adhesive includes naphthalene-type epoxy resin, bridged cyclic epoxy resin, toughening agent, active diluent, photoinitiator, etc. This invention obtains a UV delayed curing adhesive by compounding fast-curing epoxy resin with slow-curing epoxy resin. The above-mentioned solutions are mainly focused on the modification or compounding of epoxy resins, and better achieve the adjustment of curing rate and delayed curing. However, these strategies are only effective for some specific formulations, and when the formulation contains highly reactive resins (such as aliphatic epoxy resins), the system will still cure rapidly, so the universality of the above-mentioned solutions is still insufficient.
[0004] In summary, how to provide a comprehensive solution for UV delayed curing, which can meet the delayed effect of most formulations, and according to the actual process requirements, the delay window and the whole curing process can be artificially controlled, has become a technical problem urgently to be solved in the field. SUMMARY
[0005] In view of the defects in the prior art, the present application provides a supramolecular host-guest photoinitiator with adjustable curing rate, a UV epoxy adhesive and a preparation method and application thereof. The supramolecular host-guest photoinitiator including a supramolecular host compound and a guest photoinitiator encapsulated therein is added to an epoxy adhesive composition to obtain a UV epoxy adhesive with adjustable curing rate. After light irradiation, the UV epoxy adhesive has obvious delayed curing characteristics. Based on different sizes of the host macrocycle, the initiator can provide an adjustable delay window period. After complete curing, the curing system has the advantages of high adhesive force and good water vapor barrier.
[0006] In a first aspect, the present application provides a supramolecular host-guest photoinitiator with adjustable curing rate, including a supramolecular host compound and a guest photoinitiator encapsulated therein. The supramolecular host compound has a macrocyclic structure with a repeat unit number of 2-30. The guest photoinitiator includes a cationic photoinitiator. In the supramolecular host-guest photoinitiator, the molar ratio of the supramolecular host compound to the guest photoinitiator is (0.8-1.5):1, and the mass percentage of carbon and hydrogen elements is (40-75):(3-8).
[0007] The supramolecular host compound is a kind of macrocyclic compound, which can form a relatively stable host-guest complex with some small molecule guest compounds through electrostatic, hydrogen bond, π-π and other non-covalent interactions. Based on this, a series of photoinitiators with supramolecular host-guest structure are prepared. After UV irradiation, the guest photoinitiator molecules are photolyzed to generate active species that induce epoxy cationic polymerization. However, unlike traditional photoinitiators, the active species are bound by the macrocyclic host molecules at the beginning and cannot efficiently induce polymerization, thus providing a delay window period of 3-30 min, preferably 5-20 min. Due to the existence of chemical reaction equilibrium, a small amount of active species induces slow polymerization. When the polymerization reaches a certain degree and / or the system temperature rises, the reaction equilibrium is broken, and the active species are released, thereby inducing accelerated polymerization speed.
[0008] For the specific type of cationic photoinitiator, different photoinitiators can be selected according to the polymerization mechanism of different polymerized monomers, including but not limited to iodonium salt, sulfonium salt, ferrocenium salt, quaternary ammonium salt, diazonium salt, phosphonium salt, bromonium salt, chloronium salt, and any initiator capable of generating cations under UV light. The inclusion of the supramolecular host compound with the photoinitiator actually provides a slow-release effect, which can overall exhibit better delayed curing universality. Moreover, by selecting the type and amount of the supramolecular host compound and guest photoinitiator, the delayed curing window period can be effectively adjusted according to the use requirements.
[0009] Further, the supramolecular host compound has a structure shown in Formula I:
[0010] R1 is independently selected from at least one repeating unit of a host structure of a cycloparaphenylene, a crown ether, a calixarene, a pillararene, a cyclodextrin, and a cucurbituril, and n is a positive integer selected from 2-30; R2 and Ra independently include at least one of a hydrogen atom, a substituted or unsubstituted alkyl group, a substituted or unsubstituted heteroalkyl group, a substituted or unsubstituted aromatic ring group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted alkylthio group, a substituted or unsubstituted cycloalkyl group, a halogen atom, a hydroxyl group, a carbonyl group, a carboxyl group, an ester group, an acyl group, an amino group, a mercapto group, and a carboxylate salt, and * is a bonding point of Ra and the macrocyclic structure.
[0011] Further, Ra includes a structure shown in Formula II:
[0012] Rb includes at least one of a hydrogen atom, a substituted or unsubstituted C1-C10 alkyl group, a substituted or unsubstituted C1-C10 heteroalkyl group, and a substituted or unsubstituted C1-C6 alkoxy group; R5 is independently selected from one of the following groups: .
[0013] The present application not only uses the supramolecular host compound to encapsulate and release the guest photoinitiator therein, but also introduces a reactive functional group (such as an epoxy group R5) on the macrocycle of the supramolecular host compound, further extending the delayed curing window period. Moreover, by utilizing the reactivity of the high-activity reactive functional group and the epoxy group, the modified supramolecular host-guest photoinitiator can induce polymerization while the supramolecular host compound can participate in the epoxy curing reaction, effectively avoiding the migration of the supramolecular host compound causing adhesion failure.
[0014] Preferably, the supramolecular host-guest photoinitiator has a structure shown in Formula III:
[0015] R3 + R3 is a cationic moiety in the cationic photoinitiator, selected from at least one of iodonium ion, sulfonium ion, ferrocenium ion, quaternary ammonium ion, diazonium ion, phosphonium ion, bromonium ion, and chloronium ion; R4 is a substituent of the cationic moiety in the cationic photoinitiator, selected from at least one of hydrogen atom, substituted or unsubstituted alkyl group, substituted or unsubstituted heteroalkyl group, substituted or unsubstituted aromatic ring group, substituted or unsubstituted alkoxy group, substituted or unsubstituted alkylthio group, substituted or unsubstituted cycloalkyl group, halogen atom, hydroxyl group, carbonyl group, carboxyl group, ester group, acyl group, amino group, mercapto group, and carboxylate salt; X - X represents an anion or anion group as a counterion of the cationic photoinitiator.
[0016] After being combined with the supramolecular host compound, the affinity of the cationic photoinitiator to the resin and other materials is significantly enhanced, and it is more easily dissolved in various adhesive formulations used subsequently, solving the problems of poor solubility and high process difficulty of some cationic photoinitiators.
[0017] Preferably, X - selected from at least one of BF4 - , PF6 - , SbF6 - , B(Ar)4 - , halogen and halogen-like ions, p-toluenesulfonate (-OTs) and its derivatives, triflate (-OTf) and its derivatives, methanesulfonate (-OMs) and its derivatives.
[0018] The reaction equation for introducing a high-activity reactive functional group on the macrocycle of the supramolecular host compound and forming a high-activity supramolecular host-guest photoinitiator can be referred to the following formula:
[0019] wherein the halogenating reagent includes all halogenating reagents, including but not limited to hydrochloric acid, hydrobromic acid, p-toluenesulfonyl chloride, hydroiodic acid, phosphorus pentachloride, phosphorus trichloride, phosphorus tribromide, thionyl chloride, oxalyl chloride, etc.
[0020] Taking [8]-CPP∝I as an example, the following reaction equation shows the delayed curing mechanism of the supramolecular host-guest photoinitiator:
[0021] When [8]-CPP∝I is exposed to UV light, the guest photoinitiator molecule is photolyzed to generate the active species HPF6 which induces cationic polymerization of the epoxide. However, at the beginning, the active species is bound by the supramolecular host macrocycle and cannot induce polymerization efficiently, forming a delay curing window period at the beginning of the reaction. Under the chemical reaction equilibrium, a small amount of active species is released from the binding to induce slow polymerization. When the polymerization reaches a certain degree and / or the temperature of the system rises, the reaction equilibrium is broken, and the active species is rapidly released, showing the usual polymerization speed of UV light curing.
[0022] In the second aspect, the present application further provides a UV epoxy adhesive with adjustable curing rate, comprising the following components in mass parts: Epoxy resin 1-10 parts; Supramolecular host-guest photoinitiator 0.1-0.5 parts; Silane coupling agent 0.01-5 parts; Photosensitizer 0-0.3 parts; Active diluent 0-10 parts; The supramolecular host-guest photoinitiator is the aforementioned supramolecular host-guest photoinitiator.
[0023] Specifically, the epoxy resin is selected from any epoxy resin, including but not limited to at least one of bisphenol A type glycidyl ether type epoxy resin, bisphenol F type glycidyl ether type epoxy resin, bisphenol A type and bisphenol F glycidyl ether type epoxy resin mixture, rubber toughening type glycidyl ether epoxy resin, aliphatic epoxy resin, alicyclic epoxy resin. The present application uses a supramolecular host-guest photoinitiator with adjustable curing rate, thereby significantly reducing the limitation of the specific type and performance of the epoxy resin, effectively breaking through the technical bottleneck of traditional material selection limitation and curing rate not easy to control.
[0024] The silane coupling agent is selected from any silane coupling agent, including but not limited to 3-glycidyloxypropyltrimethoxysilane, γ-(2,3-epoxypropoxy) propyltrimethoxysilane, (3-epoxypropylpropoxy) trimethoxysilane, (3-epoxypropylpropoxy) triethoxysilane, 2-(3,4-epoxycyclohexyl) ethyl trimethoxysilane, etc.
[0025] The photosensitizer is selected from any photosensitizer, including but not limited to 2-isopropylthioxanthone, camphorquinone, anthraquinone and its derivatives, methylene blue, porphyrin and its derivatives, etc.
[0026] The active diluent is selected from any active diluent, including but not limited to benzyl glycidyl ether (and its derivatives), alkyl glycidyl ether, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, allyl glycidyl ether, trifunctional glycidyl ether, tetrafunctional glycidyl ether, etc.
[0027] The UV epoxy adhesive provided by the present application has adjustable curing rate. After UV light irradiation initiation, due to the inclusion and slow release of the guest photoinitiator by the supramolecular host compound, the UV epoxy adhesive does not immediately cure like traditional photo-curable adhesives, but provides a delayed curing function, that is, a delayed curing window period is formed before the curing rate rapidly rises, and the curing rate of the adhesive is very low (for example, below 15%) in the window period, the adhesive has excellent flow and coating performance, and can meet the flexible gluing requirements; the UV epoxy adhesive can also be irradiated by UV light after gluing to leave more time for the low-UV-transmission component to be bonded.
[0028] Preferably, after the UV light irradiation with a wavelength of 200-500 nm and a curing energy of 200-20000 mJ / cm 2 , the UV epoxy adhesive is delayed cured, the delayed curing window period is 5 min or more and 30 min or less, and the degree of curing in the window period is 10% or less. The gluing thickness is not particularly limited, and can be determined according to the bonding requirements, and the UV light irradiation time can be determined for different gluing thicknesses, for example, when the gluing thickness is 0.2-1 mm, the UV light irradiation can be performed for 2-20 s. After the window period, the subsequent curing can be slowly cured at room temperature without light, for example, the adhesive can reach a large enough initial strength after UV light irradiation at room temperature for about 15-35 min, and is completely cured in about 1 h; or the adhesive can be rapidly cured under heating conditions, for example, the adhesive can be heated to 50-70℃, and can be substantially completely cured in 1 min or less. The heating means can also be used in the window period, and when all the curing preparations are ready, the window period can be broken by increasing the temperature to improve the work efficiency.
[0029] Based on the use of the supramolecular host-guest photoinitiator with adjustable curing rate, the present application can effectively control the curing rate of the UV epoxy adhesive by various means such as initiator component design, gluing condition regulation, light source regulation, temperature regulation, etc., and has great use advantages and popularization value.
[0030] In a third aspect, the present application also provides a preparation method of the UV epoxy adhesive with adjustable curing rate, comprising the following steps: S1, dissolving the guest photoinitiator, adding the supramolecular host compound to the solution, and reacting to precipitate crystals; S2, removing the solvent, washing the crystals, and vacuum drying to obtain the supramolecular host-guest photoinitiator; S3, mixing the supramolecular host-guest photoinitiator, the epoxy resin, the silane coupling agent, and optionally the photosensitizer and the reactive diluent to obtain the UV epoxy adhesive.
[0031] Further, in step S1, the guest photoinitiator is dissolved in a solvent, which includes but is not limited to at least one of methanol, ethanol, acetone, chloroform, water, diethyl ether, toluene, benzene, 1,4-dioxane, N,N-dimethylacetamide, tetrahydrofuran, acetonitrile, dichloromethane, ethyl acetate, petroleum ether, n-hexane, isopropyl alcohol, and tert-butyl alcohol. Preferably, a low-boiling-point solvent is used to facilitate subsequent removal.
[0032] Further, in step S1, the reaction is carried out at a temperature of -20 to 200°C and a rotation speed of 10 to 2000 rpm, and the reaction atmosphere is selected from at least one of helium, nitrogen, oxygen, and air.
[0033] Further, in step S2, after removing part of the solvent, the residual liquid is cooled to room temperature, an inert solvent is added, filtered, and the crystal filter cake is washed and filtered multiple times with the aforementioned solvent, and then dried in a vacuum oven.
[0034] Further, removing part of the solvent includes removing 30 to 70% of the total amount of the solvent.
[0035] Further, the inert solvent includes but is not limited to at least one of n-hexane, petroleum ether, diethyl ether, and n-heptane, which is used to promote further precipitation of the reaction product generated in step S1.
[0036] In a fourth aspect, based on the aforementioned supramolecular host-guest photoinitiator and the UV epoxy adhesive with adjustable curing rate, the application provides an application of the UV epoxy adhesive with adjustable curing rate to bonding low-UV-transmission components.
[0037] Preferably, the application includes the following steps: irradiating the UV epoxy adhesive with UV light and initiating the UV epoxy adhesive, and the UV epoxy adhesive enters a window period of delayed curing; in the window period, the UV epoxy adhesive is combined with the low-UV-transmission component; the UV epoxy adhesive is selected from any of the following post-curing modes: (1) room temperature light-free slow curing; (2) rapid curing by increasing the temperature; (3) controlling the heating temperature to adjust the curing rate.
[0038] Further, before, after, or simultaneously with the irradiation of the UV epoxy adhesive with UV light to enter the window period of delayed curing, the UV epoxy adhesive is applied to the substrate.
[0039] The low UV transmission component generally refers to a component with a UV transmittance lower than 20%, such as a non-light-transmitting substrate (such as metal, ceramic, carbon fiber, black / dark plastic, etc.), a substrate containing a UV absorber (such as certain weather-resistant coatings, sunscreen packaging materials, optical protective films, etc.), a multi-layer composite substrate (such as glass with a UV shielding layer, an ultraviolet-proof film, etc.), and the like. In specific applications, the UV transmittance of some medical packaging, electronic display screen protective films, high-end optical films, etc. needs to be controlled to be lower than 5%, and the transmittance of some aerospace optical windows needs to be controlled to be lower than 1%.
[0040] The UV epoxy adhesive with adjustable curing rate of the present application actually exhibits at least two adjustment modes in the application process. One adjustment is to obtain an adjustable window period by selecting a supermolecular host-guest photoinitiator and other material components, thereby providing a basic setting for delayed curing. The second adjustment is to adjust the curing temperature of the post-curing process, thereby adjusting the starting point and curing rate of the post-curing, and realizing flexible setting of the curing rate throughout the process.
[0041] The present application at least includes the following beneficial effects: (1) The supermolecular host-guest photoinitiator of the present application forms a delayed curing window period by the inclusion and slow-release effect of the supermolecular host compound on the guest photoinitiator, and does not immediately induce rapid polymerization on the initiation object. A small amount of active species induces slow polymerization in the window period. When the polymerization reaches a certain degree and / or the system temperature rises, the reaction equilibrium is broken, the window period ends, and the active species is rapidly released to accelerate polymerization, thereby providing a light-curing polymerization technology with adjustable curing rate. Moreover, according to the difference of the macrocyclic structure of the supermolecular host compound, the delayed window period can be artificially controlled, thereby providing different operation window periods according to the specific process requirements, greatly improving the convenience and friendliness of construction.
[0042] (2) The UV epoxy adhesive of the present application utilizes the adjustable curing rate of the supermolecular host-guest photoinitiator, and can be applied to the surface of the substrate before, after or simultaneously with UV light excitation. The adhesive remains in a flow state in the delayed curing window period, combines the low UV transmission component with the adhesive, and can complete the post-curing at room temperature without light, thereby solving the problem that the low UV transmission component cannot be cured with a UV adhesive.
[0043] (3) The present application improves the affinity of the cationic photoinitiator and the resin and other materials through the macrocyclic structure of the supermolecular host compound, so that it is more easily dissolved in the adhesive formulation, thereby solving the problem of high process difficulty caused by poor solubility of the cationic photoinitiator.
[0044] (4) The application also introduces a reactive functional group on the macrocycle of the supramolecular host compound, which not only further prolongs the window period of delayed curing, but also utilizes the reactivity of the high-activity reactive functional group and the epoxy group to make the modified supramolecular host-guest photoinitiator not only induce polymerization, but also enable the supramolecular host compound to participate in the epoxy curing reaction, effectively avoiding the migration of the supramolecular host compound to cause bonding failure. DETAILED DESCRIPTION
[0045] In order to better understand the above technical solutions, the above technical solutions will be described in detail in combination with the description and specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present application, not all. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative labor are within the scope of protection of the present application.
[0046] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include the plural forms, unless the context clearly indicates otherwise. "Multiple" generally includes at least two.
[0047] It should also be noted that the term "comprise", "include" or any other variant thereof is intended to cover non-exclusive inclusion, so that the product or device including a series of elements not only includes those elements, but also includes other elements not explicitly listed or inherent to such product or device. Without more limitations, the element defined by the sentence "including a" does not exclude the presence of other identical elements in the product or device including the element.
[0048] A supramolecular host-guest photoinitiator with adjustable curing rate, comprising a supramolecular host compound and a guest photoinitiator encapsulated therein, the molar ratio of the supramolecular host compound and the guest photoinitiator is (0.8-1.5):1, the mass percentage of carbon and hydrogen is (40-75):(3-8), and the supramolecular host-guest photoinitiator has the structure shown in formula III:
[0049] (1) The supramolecular host compound has a macrocyclic structure with a repeat unit number of 2-30, preferably as shown in formula I:
[0050] R1 is independently selected from at least one of the repeating units of the host structures of cycloparaphenylene, crown ether, calixarene, pillararene, cyclodextrin, cucurbituril, n is a positive integer selected from 2 to 30; R2, Ra independently include at least one of hydrogen atom, substituted or unsubstituted alkyl group, substituted or unsubstituted heteroalkyl group, substituted or unsubstituted aromatic ring group, substituted or unsubstituted alkoxy group, substituted or unsubstituted alkylthio group, substituted or unsubstituted cycloalkyl group, halogen atom, hydroxyl group, carbonyl group, carboxyl group, ester group, acyl group, amino group, mercapto group, carboxylate, and * is the bonding point of Ra to the macrocyclic structure. Preferably, Ra includes the structure shown in Formula II:
[0051] Rb includes at least one of hydrogen atom, substituted or unsubstituted C1-C10 alkyl group, substituted or unsubstituted C1-C10 heteroalkyl group, and substituted or unsubstituted C1-C6 alkoxy group; R5 is independently selected from one of the following groups: .
[0052] (2) The guest photoinitiator includes a cationic photoinitiator, which is represented as follows in the structural formula III of the supramolecular host-guest photoinitiator: R3 + is a cationic moiety in the cationic photoinitiator, and is selected from at least one of iodonium ion, sulfonium ion, ferrocenium ion, quaternary ammonium ion, diazonium ion, phosphonium ion, bromonium ion, and chloronium ion; R4 is a substituent of the cationic moiety in the cationic photoinitiator, and is selected from at least one of hydrogen atom, substituted or unsubstituted alkyl group, substituted or unsubstituted heteroalkyl group, substituted or unsubstituted aromatic ring group, substituted or unsubstituted alkoxy group, substituted or unsubstituted alkylthio group, substituted or unsubstituted cycloalkyl group, halogen atom, hydroxyl group, carbonyl group, carboxyl group, ester group, acyl group, amino group, mercapto group, and carboxylate; X - represents an anion or anion group as a counterion of the cationic photoinitiator, and preferably, X - is selected from at least one of BF4 - , PF6-, SbF6 - , B(Ar)4 - , halogen and halogen-like ion, p-toluene sulfonate (-OTs) and its derivatives, trifluoromethane sulfonate (-OTf) and its derivatives, and methanesulfonate (-OMs) and its derivatives.
[0053] Specifically, the supramolecular host-guest photoinitiator with adjustable curing rate of the present application includes, but is not limited to, the following kinds: (1) [7]-CPP∝I, [8]-CPP∝I, [9]-CPP∝I, [9]-CPP∝OI, etc. based on cyclophane, for example: (1.1) [9]-CPP∝I has the following structure:
[0054] (1.2) [9]-CPP∝OI has the following structure:
[0055] (2) 18-C-6∝Fe, 18-C-6∝S, 24-C-8∝S, etc. based on crown ether, for example: (2.1) 18-C-6∝Fe has the following structure:
[0056] (2.2) 24-C-8∝S has the following structure:
[0057] (3) CA[6]∝I, etc. based on calixarene, CA[6]∝I has the following structure:
[0058] (4) Supramolecular host-guest photoinitiators with high activity reactive functional groups on the supramolecular host macrocycle, for example: (4.1) 18-C-6∝Fe with side chain epoxy substitution (also known as epoxy-18-C-6∝Fe), has the following structure:
[0059] (4.2) 18-C-6∝Fe with side chain unsaturated double bond (also known as ene-18-C-6∝Fe), has the following structure:
[0060] (4.3) 18-C-6∝S with side chain oxetane (also known as ox-18-C-6∝S), has the following structure:
[0061] A UV epoxy adhesive with adjustable curing rate, including the following components by mass fraction: (1) 1-10 parts of epoxy resin selected from at least one of any epoxy resin, such as bisphenol A type glycidyl ether type epoxy resin, bisphenol F type glycidyl ether type epoxy resin, bisphenol A type and bisphenol F glycidyl ether type epoxy resin mixture, rubber toughened glycidyl ether epoxy, aliphatic epoxy resin, alicyclic epoxy resin; (2) 0.1-0.5 parts of the aforementioned supramolecular host-guest photoinitiator; (3) 0.01-5 parts of a silane coupling agent, any silane coupling agent, such as 3-glycidyloxypropyltrimethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, (3-epoxypropylpropoxy)trimethoxysilane, (3-epoxypropylpropoxy)triethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, etc.; (4) 0-0.3 parts of a photosensitizer, any photosensitizer, such as 2-isopropylthioxanthone, camphorquinone, anthraquinone and its derivatives, methylene blue, porphyrin and its derivatives, etc.; (5) 0-10 parts of an active diluent, any active diluent, such as benzyl glycidyl ether (and its derivatives), alkyl glycidyl ether, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, allyl glycidyl ether, trifunctional glycidyl ether, tetrafunctional glycidyl ether, etc.
[0062] The glue thickness and UV light source can be selected according to actual needs. Generally, a glue thickness of 0.2-1 mm can meet the bonding requirements, the wavelength of the UV light is selected to be 200-500 nm, and the curing energy is selected to be 200-20000 mJ / cm 2 , which can meet the initiation and curing requirements and the curing degree is easy to control.
[0063] After the aforementioned UV epoxy adhesive formulation is irradiated by UV light with a wavelength of 200-500 nm and a curing energy of 200-20000 mJ / cm 2 for about 2-20 s at a glue thickness of 0.2-1 mm, the UV epoxy adhesive is cured with a delay, the window period of the delayed curing is 5 min or more and 30 min or less, and the curing degree in the window period is 10% or less. After the window period, the subsequent curing can be slow curing at room temperature without light, for example, the adhesive can reach a large initial strength after UV light irradiation at room temperature for about 15-35 min, and completely cured in about 1 h; or rapid curing under heating conditions, for example, the adhesive can be basically completely cured in 1 min or less when heated to 50-70℃, and the heating means can also be used in the window period, and when all the curing preparations are ready, the window period can be broken by increasing the temperature to improve the work efficiency.
[0064] A preparation method of the aforementioned UV epoxy adhesive with adjustable curing rate, comprising the following steps: S1, dissolving the guest photoinitiator in a solvent, adding a supramolecular host compound to the solution, and reacting to precipitate crystals at a temperature of -20-200℃ and a rotation speed of 10-2000 rpm; S2, remove part of the solvent by rotary evaporation and cool to room temperature, add inert solvent to the residual liquid, filter, wash the crystal filter cake with a small amount of the aforementioned solvent several times (at least 3 times), filter, and then place in a vacuum oven to dry, to obtain the supramolecular host-guest photoinitiator; S3, mix the supramolecular host-guest photoinitiator with the epoxy resin, silane coupling agent, and optionally photosensitizer and reactive diluent to obtain the UV epoxy adhesive.
[0065] An application of the aforementioned UV epoxy adhesive with adjustable curing rate for bonding low UV transmission components, comprising the following application steps: Before, after or simultaneously with the application of the UV epoxy adhesive to the substrate, irradiate and initiate the UV epoxy adhesive with UV light, and the UV epoxy adhesive enters the window period of delayed curing; In the window period, join the UV epoxy adhesive with the low UV transmission component; The UV epoxy adhesive is selected in any of the following post-curing modes: (1) room temperature light-free slow curing, after UV light irradiation for about 15-35 min, the adhesive can reach a large enough initial strength, and completely cure in about 1 h; (2) rapid curing by heating, such as heating the adhesive to 50-70℃, which can be substantially completely cured in 1 min; (3) control the heating temperature to adjust the curing rate.
[0066] Example 1 The supramolecular host-guest photoinitiator and UV epoxy adhesive sample with adjustable curing rate of Example 1 are prepared by the following steps: (1) synthesis of supramolecular host-guest photoinitiator Dissolve 2 mmol of diphenyl iodonium hexafluorophosphate in methanol, then add 2 mmol of 8-cycloparaphenylene ([8]-CPP) to the solution, and [8]-CPP dissolves and crystals are precipitated. After the reaction is complete, remove half of the methanol by rotary evaporation, cool to room temperature, add n-hexane, filter, wash the filter cake with a small amount of methanol three times, and finally place in a vacuum oven to dry to obtain colorless crystals of 8-[CPP]∝I.
[0067] The reaction equation for synthesizing 8-[CPP]∝I is as follows:
[0068] Elemental analysis: Theoretical value: C 61 H 46 F6IP: %C (69.72), %H (4.41); Actual value: %C (69.65), %H (4.55).
[0069] (2) Preparation of UV epoxy adhesive 0.2 parts by mass of the supramolecular host-guest photoinitiator 8-[CPP]αI, 0.1 parts by mass of the photosensitizer ITX, 2.5 parts by mass of bisphenol A epoxy resin, 2.5 parts by mass of 2021p epoxy resin, and 0.05 parts by mass of silane coupling agent were thoroughly stirred and mixed uniformly to obtain the UV epoxy adhesive.
[0070] Example 2 The supramolecular host-guest photoinitiator with adjustable curing rate and the UV epoxy adhesive sample of Example 2 were prepared by the following steps: (1) Synthesis of supramolecular host-guest photoinitiator 2 mmol of diphenyliodonium hexafluorophosphate was dissolved in methanol, and then 2 mmol of 7-cycloparaphenylene ([7]-CPP) was added to the solution. Crystals were precipitated during the dissolution reaction. After the reaction was complete, half of the methanol was removed by rotary evaporation, and the solution was cooled to room temperature. Normal hexane was added, and the mixture was filtered. The filter cake was washed with a small amount of methanol three times. Finally, the mixture was dried in a vacuum oven to obtain colorless crystals of 7-[CPP]αI.
[0071] The reaction equation for synthesizing 7-[CPP]αI is as follows:
[0072] Elemental analysis: Theoretical value: C 54 H 38 F6IP: %C (67.65), %H (4.00); Actual value: %C (67.56), %H (4.12). (2) Preparation of UV epoxy adhesive The difference between Example 1 and Example 2 is that 0.19 parts by mass of 7-[CPP]αI was used as the supramolecular host-guest photoinitiator.
[0073] Example 3 The supramolecular host-guest photoinitiator with adjustable curing rate and the UV epoxy adhesive sample of Example 3 were prepared by the following steps: (1) Synthesis of supramolecular host-guest photoinitiator 2 mmol of diphenyliodonium hexafluorophosphate was dissolved in methanol, and then 2 mmol of 9-cycloparaphenylene ([9]-CPP) was added to the solution. Crystals were precipitated during the dissolution reaction. After the reaction was complete, half of the methanol was removed by rotary evaporation, and the solution was cooled to room temperature. Normal hexane was added, and the mixture was filtered. The filter cake was washed with a small amount of methanol three times. Finally, the mixture was dried in a vacuum oven to obtain colorless crystals of 9-[CPP]αI.
[0074] The reaction equation for synthesizing [9]-CPP∝I is as follows:
[0075] Elemental analysis: Theoretical value: C 67 H 50 F6IP: %C (71.40), %H (4.47); Actual value: %C (71.46), %H (4.39).
[0076] (2) Preparation of UV epoxy adhesive The difference from Example 1 is that 0.22 parts by mass of 9-[CPP]∝I is used as the supramolecular host-guest photoinitiator.
[0077] Example 4 The supramolecular host-guest photoinitiator with adjustable curing rate and the UV epoxy adhesive sample of Example 4 are prepared by the following steps: (1) Synthesis of supramolecular host-guest photoinitiator 2 mmol of methoxy-substituted diphenyl iodonium antimonate is dissolved in methanol, and then 2 mmol of 9-cycloparaphenylene ([9]-CPP) is added to the solution. Crystals are precipitated after the dissolution reaction of [9]-CPP. After the reaction is complete, half of the methanol is removed by rotary evaporation, and the solution is cooled to room temperature. Then, n-hexane is added, and the mixture is filtered. The filter cake is washed with a small amount of methanol three times. Finally, the colorless crystals of 9-[CPP]∝OI are obtained by drying in a vacuum oven.
[0078] The reaction equation for synthesizing [9]-CPP∝OI is as follows:
[0079] Elemental analysis: Theoretical value: C 66 H 46 F6IOSb: %C (65.33), %H (3.93); Actual value: %C (65.01), %H (4.02).
[0080] (2) Preparation of UV epoxy adhesive The difference from Example 1 is that 0.24 parts by mass of 9-[CPP]∝OI is used as the supramolecular host-guest photoinitiator.
[0081] Example 5 The supramolecular host-guest photoinitiator with adjustable curing rate and the UV epoxy adhesive sample of Example 5 are prepared by the following steps: (1) Synthesis of supramolecular host-guest photoinitiator 2 mmol of bis-p-tolylphenyl iodonium salt was dissolved in methanol, then 2 mmol of calix[6]arene (CA[6]) was added into the solution, and crystals were precipitated in the solution after the dissolution reaction. After the reaction was completed, half of the methanol was removed by rotary evaporation, and the solution was cooled to room temperature. Then, n-hexane was added, and the mixture was filtered. The filter cake was washed with a small amount of methanol three times. Finally, the mixture was placed in a vacuum oven to dry, and colorless crystals of CA[6]@I were obtained.
[0082] The reaction equation for synthesizing CA[6]@I is as follows:
[0083] Elemental analysis: Theoretical value: C 80 H 50 BF 20 IO6: %C (59.13), %H (3.10); Actual value: %C (58.88), %H (3.11).
[0084] (2) Preparation of an adhesive composition Different from Example 1, the supramolecular host-guest photoinitiator used was 0.31 parts by mass of CA[6]@I.
[0085] Example 6 The supramolecular host-guest photoinitiator with adjustable curing rate and the UV epoxy adhesive sample of Example 6 were prepared by the following steps: (1) Synthesis of a supramolecular host-guest photoinitiator 2 mmol of ferrocenium hexafluorophosphate was dissolved in methanol, then 2 mmol of 18-crown-6 (18-C-6) was added into the solution, and crystals were precipitated in the solution after the dissolution reaction. After the reaction was completed, half of the methanol was removed by rotary evaporation, and the solution was cooled to room temperature. Then, n-hexane was added, and the mixture was filtered. The filter cake was washed with a small amount of methanol three times. Finally, the mixture was placed in a vacuum oven to dry, and colorless crystals of 18-C-6@Fe were obtained.
[0086] The reaction equation for synthesizing 18-C-6@Fe is as follows:
[0087] Elemental analysis: Theoretical value: C 22 H 34 F6FeO6P: %C (44.39), %H (5.76); Actual value: %C (44.44), %H (5.81).
[0088] (2) Preparation of a UV epoxy adhesive 0.12 parts by mass of the supramolecular host-guest photoinitiator 18-C-6∝Fe, 2.5 parts by mass of the bisphenol F epoxy resin, 2.5 parts by mass of the 2021p epoxy resin, and 0.05 parts by mass of the silane coupling agent were stirred and mixed uniformly to obtain the UV epoxy adhesive.
[0089] Example 7 The supramolecular host-guest photoinitiator with adjustable curing rate and the UV epoxy adhesive sample of Example 7 were prepared by the following steps: (1) Synthesis of supramolecular host-guest photoinitiator The antimonate of sulfonium salt was dissolved in methanol, and then 2 mmol of 18-crown-6 (18-C-6) was added to the solution. After the dissolution reaction, crystals of 18-C-6 were precipitated. After the reaction was completed, half of the methanol was removed by rotary evaporation, and the solution was cooled to room temperature. Then, n-hexane was added, and the mixture was filtered. The filter cake was washed with a small amount of methanol three times. Finally, the mixture was dried in a vacuum oven to obtain colorless crystals of 18-C-6∝S.
[0090] The reaction equation for synthesizing 18-C-6∝S is as follows:
[0091] Elemental analysis: Theoretical value: C 31 H 41 F6O6S2Sb: %C (74.8), %H (5.11).
[0092] Actual value: %C (74.23), %H (4.98).
[0093] (2) Preparation of UV epoxy adhesive The difference between Example 6 and Example 7 is that the supramolecular host-guest photoinitiator used in Example 7 is 0.16 parts by mass of 18-C-6∝S.
[0094] Example 8 The supramolecular host-guest photoinitiator with adjustable curing rate and the UV epoxy adhesive sample of Example 8 were prepared by the following steps: (1) Synthesis of supramolecular host-guest photoinitiator The antimonate of sulfonium salt was dissolved in methanol, and then 2 mmol of 18-crown-6 (18-C-6) was added to the solution. After the dissolution reaction, crystals of 18-C-6 were precipitated. After the reaction was completed, half of the methanol was removed by rotary evaporation, and the solution was cooled to room temperature. Then, n-hexane was added, and the mixture was filtered. The filter cake was washed with a small amount of methanol three times. Finally, the mixture was dried in a vacuum oven to obtain colorless crystals of 18-C-6∝S.
[0095] The reaction equation for synthesizing 18-C-6∝S is as follows: The reaction equation for synthesizing 18-C-6∝S is as follows:
[0096] Elemental analysis: Theoretical value: C 35 H 49 F6O8S2Sb: %C (46.83), %H (5.50); Actual value: %C (46.54), %H (5.23).
[0097] (2) Preparation of UV epoxy adhesive 0.17 parts by mass of 24-C-8αS, 5 parts by mass of 2021p epoxy resin, and 0.05 parts by mass of silane coupling agent were fully stirred and uniformly mixed to obtain the UV epoxy adhesive.
[0098] Example 9 The sample of the curing rate-adjustable supramolecular host-guest photoinitiator and UV epoxy adhesive of Example 9 was prepared by the following steps: (1) Synthesis of supramolecular host-guest photoinitiator epoxy-18-C-6αFe, the reaction equation is as follows:
[0099] S1, 2 mmol of hydroxymethyl-substituted 18-crown-6 (18-C-6) was dissolved in dichloromethane, then 2.5 mmol of p-toluenesulfonyl chloride TsCl and a catalytic amount of DMAP were added to the solution. After TLC monitoring of the complete reaction, the reaction liquid was poured into water, extracted with dichloromethane, and the solvent was dried and evaporated to obtain the crude product which was directly used in the next step.
[0100] S2, 2 mmol of epoxypropanol was dissolved in tetrahydrofuran, then NaH was added at 0°C, and the reaction was restored to room temperature for half an hour. The crude product obtained in step S1 was added to the reaction liquid. After the reaction was completed, the reaction was quenched with water, extracted with dichloromethane, dried, and evaporated. The crude product was further column chromatographed to obtain the side chain epoxy-substituted 18-crown-6 (supramolecular host compound with reactive functional groups).
[0101] S3, the steps of synthesizing supramolecular host-guest photoinitiator epoxy-18-C-6αFe using side chain epoxy-substituted 18-crown-6 and ferrocene hexafluorophosphate were consistent with Example 6.
[0102] Elemental analysis: Theoretical value: C 26 H 40 F6FeO8P: %C (45.83), %H (5.92); Actual value: %C (45.66), %H (5.79).
[0103] (2) Preparation of UV epoxy adhesive Different from Example 6, the supramolecular host-guest photoinitiator used 0.13 parts by mass of epoxy-18-C-6∝Fe.
[0104] Example 10 The supramolecular host-guest photoinitiator with adjustable curing rate and the UV epoxy adhesive sample of Example 10 were prepared by the following steps: (1) Synthesis of supramolecular host-guest photoinitiator ene-18-C-6∝Fe, the reaction equation is as follows:
[0105] The specific synthesis method of ene-18-C-6∝Fe is similar to that of Example 9, except that in step S2, 2 mmol of hydroxypropyl vinyl ether is dissolved in tetrahydrofuran.
[0106] Elemental analysis: Theoretical value: C 28 H 44 F6FeO8P: %C (47.40), %H (6.85); Actual value: %C (47.29), %H (6.68).
[0107] (2) Preparation of UV epoxy adhesive Different from Example 6, the supramolecular host-guest photoinitiator used 0.14 parts by mass of ene-18-C-6∝Fe.
[0108] Example 11 The supramolecular host-guest photoinitiator with adjustable curing rate and the UV epoxy adhesive sample of Example 11 were prepared by the following steps: (1) Synthesis of supramolecular host-guest photoinitiator ox-18-C-6∝S, the reaction equation is as follows:
[0109] The specific synthesis method of ox-18-C-6∝S is similar to that of Example 9, except that in step S2, 2 mmol of 3-methyl-3-hydroxymethyl oxetane is dissolved in tetrahydrofuran.
[0110] Elemental analysis: Theoretical value: C 37 H 51 F6O8S2Sb: %C (48.11), %H (5.57); Actual value: %C (48.01), %H (5.55).
[0111] (2) Preparation of UV epoxy adhesive The difference between this example and Example 6 is that the supramolecular host-guest photoinitiator used is 0.18 parts by mass of ox-18-C-6 © S.
[0112] Comparative Example 1 This comparative example provides an adhesive composition, the difference from Example 1 is that the supramolecular host-guest photoinitiator is not used, and 0.1 parts by mass of diphenyl iodonium hexafluorophosphate is directly added.
[0113] Comparative Example 2 This comparative example provides an adhesive composition, the difference from Example 6 is that the supramolecular host-guest photoinitiator is not used, and 0.06 parts by mass of ferrocene hexafluorophosphate is directly added.
[0114] Comparative Example 3 This comparative example provides an adhesive composition, the difference from Example 8 is that the supramolecular host-guest photoinitiator is not used, and 0.08 parts by mass of antimonate of sulfonium salt is directly added.
[0115] Comparative Example 4 This comparative example provides an adhesive composition, the difference from Example 6 is that the supramolecular host-guest photoinitiator is not used, but 0.07 parts by mass of ferrocene hexafluorophosphate and 0.05 parts by mass of 18-crown-6 ether are respectively mixed with other materials when preparing the adhesive composition.
[0116] Test and result 1. Test the acid production performance of the supramolecular host-guest photoinitiator used in Examples 1 to 11, and the initiators used in Comparative Examples 1 to 3.
[0117] Prepare an acetonitrile dilute solution with a concentration of 1.5 x 10 -5 mol / L of photoinitiator, add photosensitizer ITX at the same time, the molar ratio of photosensitizer to photoinitiator is 0.5:1, add a few drops of rhodamine B solution as pH indicator, mix well, then place the prepared mixed solution under 365 nm ultraviolet light (light intensity is 300 mW / cm 2 ) for irradiation, and record the time of solution discoloration (unit: min). The test results are shown in Table 1.
[0118] Table 1
[0119] The solution discoloration time of each of Examples 1-11 is more than 5 min, which shows obvious delay effect compared with Comparative Examples 1-3 in which the corresponding cationic photoinitiator is directly added, and the main reason is the inclusion and slow release of the supramolecular host compound to the guest photoinitiator, and because the composition and ratio of the supramolecular host-guest photoinitiator of each example are different, a large range of different delay discoloration times are also shown, which particularly advantageously provides a delay window period that can adapt to different curing needs, and has great practical application value.
[0120] 2. The adhesive samples obtained in each of the examples and comparative examples were evaluated in the following aspects, and the test results are shown in Table 2: 2.1. Delay window: a 0.5 mm thick adhesive layer was prepared using a coating machine, and was irradiated under 365 nm ultraviolet light (light intensity: 300 mW / cm 2 ) for 10 s. The adhesive layer was gently picked up with a toothpick every 1 min, and the time when the adhesive layer began to pull out was defined as the window period of delayed curing (unit: min).
[0121] 2.2. Time required to reach 0.1 MPa strength: the sample was prepared by the chip shear method, and glass substrates were bonded to glass substrates with a bonding area of 3 mm x 3 mm. The above cured adhesive was tested every 2 min using a Dage chip thrust machine, and the time required for the strength value to be greater than 0.1 MPa for the first time (unit: min) was recorded, as well as the actual strength value (unit: MPa) tested at that time.
[0122] 2.3. Bonding strength after 5 min: the adhesive film was heated at 60°C for 1 min, and the shear strength after 5 min (unit: MPa) was tested.
[0123] 2.4. Final strength: the shear strength after 24 h (unit: MPa) was recorded.
[0124] Table 2
[0125] As can be seen, the adhesive samples of Examples 1-11 show a delay curing window period corresponding to the delay discoloration time in Table 1, which indicates the effectiveness and reliability in adhesive applications. Comparative Examples 1-3 do not have a window period, and it is observed in the experiment that their adhesive samples are rapidly cured after UV irradiation, and the curing is basically completed within 1 min, and a high bonding strength value is reached at 2 min.
[0126] Comparative Example 4 incorporated the same supramolecular host compound and guest photoinitiator as Example 6. The macrocyclic structure of the supramolecular host compound also exhibited a certain delay effect on the guest photoinitiator. However, since the two did not react in advance to form a stable supramolecular host-guest photoinitiator, the window of delayed curing was too short. In practical applications, there was not enough time to perform accurate bonding operations. It can be seen that the simple mixed slow-release effect is limited. Only by using the supramolecular host compound to encapsulate the guest photoinitiator to prepare a supramolecular host-guest photoinitiator can it have a practical delayed curing effect and application value.
[0127] The preferred embodiments of the present invention have been described above, which are intended to make the spirit of the present invention clearer and easier to understand, and are not intended to limit the present invention. All modifications, substitutions and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A supramolecular host-guest photoinitiator with adjustable curing rate, characterized in that, This includes supramolecular host compounds and guest photoinitiators encapsulated within them; The supramolecular host compound has a macrocyclic structure with 2-30 repeating units; Guest photoinitiators include cationic photoinitiators; In the supramolecular host-guest photoinitiator, the molar ratio of the supramolecular host compound to the guest photoinitiator is (0.8-1.5):1, and the mass percentage of carbon and hydrogen is (40-75):(3-8).
2. The supramolecular host-guest photoinitiator as described in claim 1, characterized in that, The supramolecular host compound has the structure shown in Formula I: ; R1 is an independent repeating unit selected from at least one main structure of cyclophenylene, crown ether, calixarene, columnar aromatics, cyclodextrin, and cucurbituril, where n is a positive integer selected from 2 to 30; R2 and Ra independently include at least one of the following: hydrogen atom, substituted or unsubstituted alkyl group, substituted or unsubstituted heterochain alkyl group, substituted or unsubstituted aromatic ring group, substituted or unsubstituted alkoxy group, substituted or unsubstituted alkylthio group, substituted or unsubstituted cycloalkyl group, halogen atom, hydroxyl group, carbonyl group, carboxyl group, ester group, acyl group, amino group, mercapto group, and carboxyl salt. * is the bonding site between Ra and the macrocyclic structure.
3. The supramolecular host-guest photoinitiator as described in claim 2, characterized in that, Ra includes the structure shown in Equation II: ; Rb includes at least one of hydrogen atom, substituted or unsubstituted C1-C10 alkyl, substituted or unsubstituted C1-C10 heterochain alkyl, and substituted or unsubstituted C1-C6 alkoxy. R5 is independently selected from one of the following groups: 。 4. The supramolecular host-guest photoinitiator as described in claim 2 or 3, characterized in that, Supramolecular host-guest photoinitiators have the structure shown in Formula III: ; R3 + The cationic portion of the cationic photoinitiator is selected from at least one of iodonium ion, thionium ion, ferrocene ion, quaternary ammonium ion, diazo ion, phosphonium ion, bromium ion, and chloride ion; R4 is a substituent of the cationic moiety in a cationic photoinitiator, selected from at least one of the following: hydrogen atom, substituted or unsubstituted alkyl group, substituted or unsubstituted heterochain alkyl group, substituted or unsubstituted aromatic ring group, substituted or unsubstituted alkoxy group, substituted or unsubstituted alkylthio group, substituted or unsubstituted cycloalkyl group, halogen atom, hydroxyl group, carbonyl group, carboxyl group, ester group, acyl group, amino group, mercapto group, and carboxyl salt. X - This refers to anion or anionic group that acts as a counterion to a cationic photoinitiator.
5. The supramolecular host-guest photoinitiator as described in claim 4, characterized in that, X - Selected from BF4 - PF6 - SbF6 - B(Ar)4 - At least one of the following: halogens and halide-like ions, p-toluenesulfonate and its derivatives, trifluoromethanesulfonate and its derivatives, and methanesulfonate and its derivatives.
6. A UV epoxy adhesive with adjustable curing rate, characterized in that, Based on parts by weight, it includes the following components: 1-10 parts epoxy resin; 0.1-0.5 parts of supramolecular host-guest photoinitiator; 0.01-5 parts of silane coupling agent; 0-0.3 parts photosensitizer; 0-10 parts of reactive diluent; The supramolecular host-guest photoinitiator is the supramolecular host-guest photoinitiator according to any one of claims 1-5.
7. The UV epoxy adhesive with adjustable curing rate as described in claim 6, characterized in that, When the adhesive thickness is 0.2-1mm, a wavelength of 200-500nm and a curing energy of 200-20000mJ / cm are used. 2 After being irradiated with UV light, the UV epoxy adhesive undergoes delayed curing, with a delayed curing window of more than 5 minutes and less than 30 minutes, and the degree of curing within the window is less than 10%.
8. A method for preparing a UV epoxy adhesive with adjustable curing rate as described in claim 6 or 7, characterized in that, Includes the following steps: S1. After dissolving the guest photoinitiator, a supramolecular host compound is added to the solution, and crystals are precipitated by the reaction. S2. Remove the solvent, clean the crystal and vacuum dry it to obtain the supramolecular host-guest photoinitiator; S3. Mix the supramolecular host-guest photoinitiator with epoxy resin, silane coupling agent, and optionally photosensitizer and reactive diluent to obtain the UV epoxy adhesive.
9. An application of a UV epoxy adhesive with adjustable curing rate for bonding low UV transmittance components, characterized in that, The UV epoxy adhesive with adjustable curing rate is selected from... At least one of the UV epoxy adhesives as described in claim 6 or 7, and the UV epoxy adhesives prepared by the method described in claim 8.
10. The application of the UV epoxy adhesive with adjustable curing rate as described in claim 9 for bonding low UV transmittance components, characterized in that, The application steps include the following: The UV epoxy adhesive is irradiated with UV light and then initiated, allowing it to enter a delayed curing window. During the window period, the UV epoxy adhesive is bonded to the low UV transmission component; The UV epoxy adhesive may be selected using any of the following post-curing methods: (1) Room temperature, light-free, slow curing; (2) Rapid curing upon heating; (3) Control the heating temperature and adjust the curing rate.
Citation Information
Patent Citations
UV delayed-curing adhesives, their preparation methods and applications
CN115895549B
Epoxy resin UV delayed curing agent and composition thereof
CN118307767A
Delayed-curing photocurable resin composition, and sealing material
CN108368238A
UV adhesive with controllable curing time
CN116676063A
Water soluble cyclic dextrin clathrate complex initiator and its preparing method
CN1944472A
Cited By
UV (ultraviolet) delayed curing electrolyte-resistant adhesive tape as well as preparation method and application thereof
CN121271472A
Uv delayed curing electrolyte resistant adhesive tape, its preparation method and application
CN121271472B