Trimethoxy-substituted PTAA copolymer as well as preparation method and application thereof
By preparing trimethoxy-substituted PTAA copolymers as hole transport materials, the problems of low open-circuit voltage and poor stability of perovskite solar cells caused by the hydrophobicity of PTAA materials were solved, achieving high-efficiency energy conversion and long-term stability.
Patent Information
- Application Number
- CN202511160877.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-19
- Publication Date
- 2025-11-28
AI Technical Summary
Existing poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA) hole transport materials are highly hydrophobic, making it difficult to ensure uniform nucleation of perovskites, resulting in low open-circuit voltage and poor long-term stability of perovskite solar cells.
Trimethoxy-substituted PTAA copolymers were used as hole transport materials. Through the polymerization reaction of 2,4,6-trimethylaniline, 3,4,5-trimethoxyaniline and 4,4'-dibromobiphenyl under the action of palladium catalyst and auxiliaries, trimethoxy-substituted PTAA copolymers with a molecular weight distribution index of 1.1~1.5 were prepared and applied to the hole transport layer of perovskite solar cells.
This improved the open-circuit voltage of perovskite solar cells, enhanced their energy conversion efficiency, and maintained high stability during long-term use.
Smart Images

Figure CN121021829A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of copolymer technology, and particularly relates to a trimethoxy-substituted PTAA copolymer, its preparation method, and its application. Background Technology
[0002] Energy, as one of the earliest natural resources utilized by humankind, has driven the progress of civilized society and the development of the economy. Faced with the continuous depletion of non-renewable energy and the increasingly severe energy crisis, the development of green and renewable energy technologies is imperative. Single-junction perovskite solar cells (PSCs) have achieved a power conversion efficiency (PCE) of 26%. Due to their low-cost manufacturing process and remarkable photoelectric performance, perovskite solar cells are considered an important resource for next-generation photovoltaic cells.
[0003] Perovskite solar cells generally consist of a conductive substrate layer, an electron transport layer, a perovskite active layer, a hole transport layer, and an electrode layer. The hole transport layer plays a crucial role in extracting and transporting holes, thus improving the energy conversion efficiency of perovskite solar cells.
[0004] Poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA) is a relatively common hole transport material with high efficiency and has been widely used in the preparation of perovskite solar cells. However, due to its strong hydrophobicity, PTAA as a hole transport material does not ensure uniform nucleation of perovskite grown on its surface, making it difficult to achieve high open-circuit voltage of perovskite solar cells, and its long-term stability is poor. Summary of the Invention
[0005] To address the shortcomings of the prior art, a trimethoxy-substituted PTAA copolymer is provided. The perovskite solar cell prepared using this trimethoxy-substituted PTAA copolymer has a high open-circuit voltage, effectively improving the energy conversion efficiency of the perovskite solar cell.
[0006] The purpose of this invention is to provide a trimethoxy-substituted PTAA copolymer, the structural formula of which is shown in formula (I):
[0007]
[0008] Equation (Ⅰ);
[0009] Where n is 37~57 mol%.
[0010] In some embodiments of the present invention, the structural formula of the trimethoxy-substituted PTAA copolymer is shown in formula (I):
[0011]
[0012] Equation (Ⅰ);
[0013] Where n is 40~50 mol%.
[0014] In some embodiments of the present invention, the number-average molecular weight of the trimethoxy-substituted PTAA copolymer is 8000 g / mol to 30000 g / mol, and the molecular weight distribution index (PDI) is 1.1 to 1.5.
[0015] Another object of the present invention is to provide a method for preparing the trimethoxy-substituted PTAA copolymer, comprising the following steps:
[0016] Under the action of palladium catalyst and auxiliaries, 2,4,6-trimethylaniline, 3,4,5-trimethoxyaniline and 4,4'-dibromobiphenyl undergo polymerization to obtain trimethoxy-substituted PTAA copolymers;
[0017] The structure of the palladium catalyst is shown in formula (II):
[0018]
[0019] Equation (II);
[0020] Where R is either methoxy or hydrogen.
[0021] In some embodiments of the present invention, the molar ratio of the palladium catalyst, 2,4,6-trimethylaniline, 3,4,5-trimethoxyaniline and 4,4'-dibromobiphenyl is 0.01~0.03:0.3~0.7:0.3~0.7:1.
[0022] In some embodiments of the present invention, the polymerization reaction is carried out at a temperature of 100-120°C for 18-30 hours.
[0023] In some embodiments of the present invention, the auxiliary agent includes an organic base and a solvent.
[0024] In some embodiments of the present invention, the organic base is selected from potassium tert-butoxide.
[0025] In some embodiments of the present invention, the molar ratio of the 4,4'-dibromobiphenyl to the organic base is 1:1 to 5.
[0026] In some embodiments of the present invention, the solvent is toluene.
[0027] Another object of the present invention is to provide the application of the trimethoxy-substituted PTAA copolymer or the trimethoxy-substituted PTAA copolymer prepared by the method thereof in the preparation of perovskite solar cells.
[0028] Another object of the present invention is to provide a perovskite solar cell, the perovskite solar cell comprising a hole transport layer, wherein the material of the hole transport layer is the trimethoxy-substituted PTAA copolymer.
[0029] In some embodiments of the present invention, the thickness of the hole transport layer is 10~30nm.
[0030] In some embodiments of the present invention, the concentration of the trimethoxy-substituted PTAA copolymer is 1-4 mg / mL.
[0031] In some embodiments of the present invention, the perovskite solar cell further includes a transparent substrate layer, a perovskite active layer, an electron transport layer, a hole blocking layer, and a metal electrode layer.
[0032] In some embodiments of the present invention, the transparent substrate layer is ITO transparent conductive glass.
[0033] In some embodiments of the present invention, the material of the perovskite active layer is selected from FAPbI3.
[0034] In some embodiments of the present invention, the material of the electron transport layer is selected from PCBM.
[0035] In some embodiments of the present invention, the material of the hole-blocking layer is selected from BCP.
[0036] In some embodiments of the present invention, the material of the metal electrode layer is selected from silver or gold.
[0037] In some embodiments of the present invention, the thickness of the perovskite active layer is 300~500 nm.
[0038] In some embodiments of the present invention, the thickness of the electron transport layer is 10~50 nm.
[0039] In some embodiments of the present invention, the thickness of the hole blocking layer is 5~10 nm.
[0040] In some embodiments of the present invention, the thickness of the metal electrode layer is 50~200nm.
[0041] Another object of the present invention is to provide a method for preparing the perovskite solar cell, comprising the following steps:
[0042] S1. Coat a hole transport layer onto a conductive substrate;
[0043] S2. The perovskite active layer and the electron transport layer are sequentially coated on the hole transport layer;
[0044] S3. A hole blocking layer and a metal electrode layer are sequentially disposed on the electron transport layer.
[0045] In some embodiments of the present invention, in S1, the scraping speed is 3~7 mm / s.
[0046] In some embodiments of the present invention, in S1, the annealing temperature of the coating is 80~120°C and the annealing time is 5~15 min.
[0047] In some embodiments of the present invention, in S2, the coating speed of the perovskite active layer on the hole transport layer is 3~7 mm / s.
[0048] In some embodiments of the present invention, in S2, the coating speed of the electron transport layer on the perovskite active layer is 15~25 mm / s.
[0049] In some embodiments of the present invention, in S2, the annealing temperature for coating the perovskite active layer on the hole transport layer is 80~120°C, and the annealing time is 30~60 min.
[0050] Compared with the prior art, the present invention has the following beneficial effects:
[0051] (1) The perovskite solar cells prepared by the trimethoxy-substituted PTAA copolymer provided by the present invention have a high open-circuit voltage, which effectively improves the energy conversion efficiency of perovskite solar cells.
[0052] (2) The perovskite solar cells prepared by the trimethoxy-substituted PTAA copolymer provided by the present invention can maintain high energy conversion efficiency during long-term use and can maintain high stability in the atmospheric environment for a long time. Attached Figure Description
[0053] Figure 1 The 1H NMR spectrum of the trimethoxy-substituted PTAA copolymer prepared in Example 1. Detailed Implementation
[0054] To enable those skilled in the art to better understand the technical solutions of this invention, the technical solutions of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some embodiments of this invention, and not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this invention.
[0055] All raw materials used in this invention are commercially available.
[0056] Example 1
[0057] This embodiment provides a trimethoxy-substituted PTAA copolymer, the preparation method of which includes the following steps:
[0058] 2,4,6-trimethylaniline (0.5 mmol), 3,4,5-trimethoxyaniline (0.5 mmol), 4,4'-dibromobiphenyl (1 mmol), potassium tert-butoxide (3 mmol), palladium catalyst C1 (0.02 mmol), and 3 mL of toluene solution were added to a reactor, and nitrogen gas was introduced. The reaction was carried out at 110 °C for 24 h. After the reaction was completed, the mixture was cooled to room temperature, added dropwise to a methanol solution to precipitate, washed 2-3 times with methanol solution, filtered and dried to obtain a pale yellow polymer, namely a trimethoxy-substituted PTAA copolymer, with a yield of 97%. The molar percentage of trimethoxy-substituted PTAA segments (n) in the trimethoxy-substituted PTAA copolymer segments was 46.8%, the number-average molecular weight Mn was 16000 g / mol, and the molecular weight distribution index PDI was 1.43.
[0059] The structure of the palladium catalyst C1 is shown below:
[0060] ;
[0061] The structural formula of the trimethoxy-substituted PTAA copolymer is as follows:
[0062] ;
[0063] Where n = 46.8 mol%.
[0064] Example 2
[0065] This embodiment provides a trimethoxy-substituted PTAA copolymer, the preparation method of which includes the following steps:
[0066] 2,4,6-trimethylaniline (0.6 mmol), 3,4,5-trimethoxyaniline (0.4 mmol), 4,4'-dibromobiphenyl (1 mmol), potassium tert-butoxide (3.5 mmol), palladium catalyst C1 (0.015 mmol), and 3 mL of toluene solution were added to a reactor. Nitrogen gas was introduced, and the reaction was carried out at 105 °C for 22 h. After the reaction was completed, the mixture was cooled to room temperature, added dropwise to a methanol solution to precipitate, washed 2-3 times with methanol solution, filtered, and dried to obtain a pale yellow polymer, namely a trimethoxy-substituted PTAA copolymer, with a yield of 94%. The molar percentage of trimethoxy-substituted PTAA segments (n) in the trimethoxy-substituted PTAA copolymer segments was 40.3%, the number-average molecular weight Mn was 11300 g / mol, and the molecular weight distribution index PDI was 1.48.
[0067] The structure of the palladium catalyst C1 is shown below:
[0068] ;
[0069] The structural formula of the trimethoxy-substituted PTAA copolymer is as follows:
[0070] ;
[0071] Where n = 40.3 mol%.
[0072] Example 3
[0073] This embodiment provides a trimethoxy-substituted PTAA copolymer, the preparation method of which includes the following steps:
[0074] 2,4,6-trimethylaniline (0.7 mmol), 3,4,5-trimethoxyaniline (0.3 mmol), 4,4'-dibromobiphenyl (1 mmol), potassium tert-butoxide (1 mmol), palladium catalyst C1 (0.01 mmol), and 3 mL of toluene solution were added to a reactor, and nitrogen gas was introduced. The reaction was carried out at 100 °C for 18 h. After the reaction was completed, the mixture was cooled to room temperature, added dropwise to methanol solution to precipitate, washed 2-3 times with methanol solution, filtered and dried to obtain a pale yellow polymer, namely a trimethoxy-substituted PTAA copolymer, with a yield of 95%. The molar percentage of trimethoxy-substituted PTAA segments (n) in the total trimethoxy-substituted PTAA copolymer segments was 37%, the number-average molecular weight Mn was 8000 g / mol, and the molecular weight distribution index PDI was 1.45.
[0075] The structure of the palladium catalyst C1 is shown below:
[0076] ;
[0077] The structural formula of the trimethoxy-substituted PTAA copolymer is as follows:
[0078] ;
[0079] Where n = 37 mol%.
[0080] Example 4
[0081] This embodiment provides a trimethoxy-substituted PTAA copolymer, the preparation method of which includes the following steps:
[0082] 2,4,6-trimethylaniline (0.4 mmol), 3,4,5-trimethoxyaniline (0.6 mmol), 4,4'-dibromobiphenyl (1 mmol), potassium tert-butoxide (4 mmol), palladium catalyst C1 (0.025 mmol), and 3 mL of toluene solution were added to a reactor. Nitrogen gas was introduced, and the reaction was carried out at 115 °C for 28 h. After the reaction was completed, the mixture was cooled to room temperature, added dropwise to a methanol solution to precipitate, washed 2-3 times with methanol solution, filtered, and dried to obtain a pale yellow polymer, namely a trimethoxy-substituted PTAA copolymer, with a yield of 93%. The molar percentage of trimethoxy-substituted PTAA segments (n) in the trimethoxy-substituted PTAA copolymer segments was 49.8%, the number-average molecular weight Mn was 19300 g / mol, and the molecular weight distribution index PDI was 1.34.
[0083] The structure of the palladium catalyst C1 is shown below:
[0084] ;
[0085] The structural formula of the trimethoxy-substituted PTAA copolymer is as follows:
[0086] ;
[0087] Where n = 49.8 mol%.
[0088] Example 5
[0089] This embodiment provides a trimethoxy-substituted PTAA copolymer, the preparation method of which includes the following steps:
[0090] 2,4,6-trimethylaniline (0.3 mmol), 3,4,5-trimethoxyaniline (0.7 mmol), 4,4'-dibromobiphenyl (1 mmol), potassium tert-butoxide (5 mmol), palladium catalyst C1 (0.03 mmol), and 3 mL of toluene solution were added to a reactor. Nitrogen gas was introduced, and the reaction was carried out at 120 °C for 30 h. After the reaction was completed, the mixture was cooled to room temperature, added dropwise to a methanol solution to precipitate, washed 2-3 times with methanol solution, filtered, and dried to obtain a pale yellow polymer, namely a trimethoxy-substituted PTAA copolymer, with a yield of 96%. The molar percentage of trimethoxy-substituted PTAA segments (n) in the total trimethoxy-substituted PTAA copolymer segments was 57%, the number-average molecular weight Mn was 30,000 g / mol, and the molecular weight distribution index PDI was 1.20.
[0091] The structure of the palladium catalyst C1 is shown below:
[0092] ;
[0093] The structural formula of the trimethoxy-substituted PTAA copolymer is as follows:
[0094] ;
[0095] Where n = 57 mol%.
[0096] Comparative Example 1
[0097] This comparative example provides a trimethoxy-substituted PTAA homopolymer, the structural formula of which is shown below:
[0098]
[0099] The number-average molecular weight is 10845 g / mol, and the PDI is 1.5.
[0100] Comparative Example 2
[0101] This comparative example provides a PTAA, the structure of which is shown below:
[0102]
[0103] The number-average molecular weight is 13578 g / mol, and the PDI is 1.7.
[0104] Example 6
[0105] This embodiment provides a perovskite solar cell, specifically a cell structure of ITO / trimethoxy-substituted PTAA copolymer / FAPbI3 / PCBM / BCP / Ag. The specific implementation steps are as follows:
[0106] (1) Cleaning of transparent substrate: First, take out the ITO transparent conductive glass, peel off the surface plastic protective film, first wipe the surface oil stains gently with dish soap, then ultrasonically clean it for 15 minutes in a 0.2wt% dish soap aqueous solution, deionized water and isopropanol respectively, and finally blow the isopropanol on the ITO surface with nitrogen and pack it in a box for later use.
[0107] (2) Deposition of hole transport layer: The trimethoxy-substituted PTAA copolymer prepared in Example 1 was prepared as a 2.5 mg / mL precursor solution with chlorobenzene as solvent. The cleaned ITO was first placed in an ultraviolet ozone cleaner for surface hydrophilic treatment. Then, the precursor solution was pipetted out and evenly covered on the ITO surface. It was then coated onto the ITO glass by a scraping method at a scraping speed of 5 mm / s. The glass was annealed by heating at 100°C for 10 min and then naturally cooled to room temperature to obtain a 20 nm hole transport layer.
[0108] (3) Preparation of perovskite active layer: FAPbI3 was prepared into a perovskite precursor solution of 0.6 g / mL, and N-methylpyrrolidone was used as the solvent. The perovskite precursor solution was pipetted out and uniformly covered on the surface of the impregnation layer. The perovskite active layer was formed by a combination of scraping and flash evaporation. The scraping speed was 5 mm / s. Then, it was annealed at 100°C for 30~60 min on a hot stage and naturally cooled to room temperature to obtain a 400 nm perovskite active layer.
[0109] (5) Deposition of electron transport layer: Weigh 20mg PCBM and add 1mL chlorobenzene to prepare a precursor solution for electron transport layer. Deposit the precursor solution on the surface of perovskite active layer by scraping at a scraping rate of 20mm / s to obtain a 30nm electron transport layer.
[0110] (6) Deposition of hole blocking layer: Weigh 8 mg BCP and add 16 mL isopropanol to prepare a precursor solution. Then, use a pipette to evenly cover the surface of the hole blocking layer with the prepared precursor solution. The precursor solution is deposited on the surface of the electron transport layer by a scraping method with a scraping rate of 10 mm / s to obtain an 8 nm hole blocking layer.
[0111] (7) Deposition of metal electrode layer: A 100 nm thick Ag film was thermally evaporated under high vacuum. The evaporation rate was 0.3 Å / s. 20 nm was deposited at this rate, and then deposited on the hole blocking layer surface at 1 Å / s. The deposition thickness was 100 nm.
[0112] Examples 7-10
[0113] This embodiment provides a perovskite solar cell. The difference from Example 6 is that the "trimethoxy-substituted PTAA copolymer prepared in Example 1" mentioned in point (2) of Example 6 is replaced with "trimethoxy-substituted PTAA copolymer prepared in Examples 2 to 5", respectively, to obtain the perovskite solar cells of Examples 7 to 10.
[0114] Comparative Example 3
[0115] This comparative example provides a perovskite solar cell, which differs from Example 6 in that the "trimethoxy-substituted PTAA copolymer prepared in Example 1" mentioned in point (2) of Example 6 is replaced with "trimethoxy-substituted PTAA homopolymer of Comparative Example 1", thus obtaining the perovskite solar cell of Comparative Example 3.
[0116] Comparative Example 4
[0117] This comparative example provides a perovskite solar cell, which differs from Example 6 in that the "trimethoxy-substituted PTAA copolymer prepared in Example 1" mentioned in point (2) of Example 6 is replaced with "PTAA of Comparative Example 2" to obtain the perovskite solar cell of Comparative Example 4.
[0118] The performance of the perovskite solar cells of Examples 6-10 and Comparative Examples 3-4 was tested. The test methods are shown below, and the results are shown in Table 1.
[0119] (1) Current-voltage characteristic curve (JV): The JV characteristic curve of the device was measured using a Keithley 2440 light source under simulated AM1.5G spectrum.
[0120] The light intensity was calibrated by NREL using a standard silicon solar cell apparatus and a solar simulator (Newport, 91160). The effective measurement area was 0.07 cm². 2 Under both reverse and forward bias scanning, the scanning speed is 100mV / s, and the bias range is -0.2V to 1.2V.
[0121] Table 1. Performance of perovskite solar cells in Examples 6-10 and Comparative Examples 3-4.
[0122] sample Voc(V) <![CDATA[Jsc(mA / cm 2 )]]> FF(%) PCE (%) Example 6 1.24 24.28 82.40 24.81 Example 7 1.21 24.23 82.27 24.12 Example 8 1.19 24.34 82.62 23.93 Example 9 1.25 24.19 82.51 24.95 Example 10 1.27 24.45 82.36 25.57 Comparative Example 3 1.07 24.36 82.54 21.51 Comparative Example 4 0.91 21.04 78.35 15.00
[0123] As shown in Table 1, the trimethoxy-substituted PTAA copolymers prepared in Examples 6-10 of this invention can maintain a high variable open-circuit voltage under high short-circuit current density and fill factor when used to prepare perovskite solar cells, thereby significantly improving the energy conversion efficiency of the cells.
[0124] The performance of the unencapsulated perovskite solar cells of Examples 6-10 and Comparative Examples 3-4 was tested after being stored in an atmospheric environment for 30 days. The results are shown in Table 2.
[0125] Table 2. Performance of perovskite solar cells in Examples 6-10 and Comparative Examples 3-4.
[0126] sample PCE (%) Example 6 24.34 Example 7 23.66 Example 8 23.19 Example 9 24.02 Example 10 24.95 Comparative Example 3 19.13 Comparative Example 4 11.17
[0127] As shown in Tables 1 and 2, the trimethoxy-substituted PTAA copolymers prepared in Examples 6-10 of this invention can maintain a high variable open-circuit voltage when used to prepare perovskite solar cells, thereby effectively improving the energy conversion efficiency of the cells and enabling the perovskite solar cells to maintain a high energy conversion efficiency during long-term use. This also allows unencapsulated perovskite solar cells to maintain high stability in the atmospheric environment for a long time.
[0128] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that after reading this application specification, they can still modify or make equivalent substitutions to the specific implementation of the present invention, but these modifications or changes do not depart from the protection scope of the pending claims of the present invention.
Claims
1. A trimethoxy-substituted PTAA copolymer, characterized in that, The structural formula of the trimethoxy-substituted PTAA copolymer is shown in Formula (I): Equation (Ⅰ); Where n is 37~57 mol%.
2. The trimethoxy-substituted PTAA copolymer according to claim 1, characterized in that, The structural formula of the trimethoxy-substituted PTAA copolymer is shown in Formula (I): Equation (Ⅰ); Where n is 40~50 mol%.
3. The trimethoxy-substituted PTAA copolymer according to claim 1, characterized in that, The trimethoxy-substituted PTAA copolymer has a number-average molecular weight of 8000 g / mol to 30000 g / mol and a molecular weight distribution index (PDI) of 1.1 to 1.
5.
4. The method for preparing the trimethoxy-substituted PTAA copolymer according to any one of claims 1 to 3, characterized in that, Includes the following steps: Under the action of palladium catalyst and auxiliaries, 2,4,6-trimethylaniline, 3,4,5-trimethoxyaniline and 4,4'-dibromobiphenyl undergo polymerization to obtain trimethoxy-substituted PTAA copolymers; The structure of the palladium catalyst is shown in formula (II): Equation (II); Where R is either methoxy or hydrogen.
5. The method for preparing the trimethoxy-substituted PTAA copolymer according to claim 3, characterized in that, The molar ratio of the palladium catalyst, 2,4,6-trimethylaniline, 3,4,5-trimethoxyaniline, and 4,4'-dibromobiphenyl is 0.01~0.03:0.3~0.7:0.3~0.7:1; And / or, the polymerization reaction is carried out at a temperature of 100~120°C for a time of 18~30 hours; And / or, the adjuvants include organic bases and solvents.
6. The method for preparing the trimethoxy-substituted PTAA copolymer according to claim 5, characterized in that, The organic base is selected from potassium tert-butoxide; And / or, the molar ratio of the 4,4'-dibromobiphenyl to the organic base is 1:1 to 5; And / or, the solvent is toluene.
7. The application of the trimethoxy-substituted PTAA copolymer of claim 1 or the trimethoxy-substituted PTAA copolymer of any one of claims 2 to 8 in the preparation of perovskite solar cells.
8. A perovskite solar cell, characterized in that, The perovskite solar cell includes a hole transport layer, the material of which is the trimethoxy-substituted PTAA copolymer as described in any one of claims 1 to 3.
9. The perovskite solar cell as described in claim 8, characterized in that, The thickness of the hole transport layer is 10~30nm; And / or, the concentration of the trimethoxy-substituted PTAA copolymer is 1~4 mg / mL.
10. The perovskite solar cell as described in claim 8, characterized in that, The perovskite solar cell also includes a transparent substrate layer, a perovskite active layer, an electron transport layer, a hole blocking layer, and a metal electrode layer.
Citation Information
Cited By
Tertiary aminated PTAA copolymer and preparation method thereof
CN122080401A
Aldehyde-substituted copolymer and preparation method thereof
CN122103558A
An aldehyde-substituted copolymer and its preparation method
CN122103558B