Reductive amination catalyst as well as preparation method and application thereof
By loading a nickel-non-precious metal alloy catalyst onto layered Al2O3, the problem of low selectivity of existing catalysts was solved, and the efficient conversion of 5-hydroxymethylfurfural to 5-hydroxymethylfurfural was achieved, thus improving the selectivity and conversion rate of the catalyst.
Patent Information
- Application Number
- CN202511350223.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-22
- Publication Date
- 2025-12-16
AI Technical Summary
Existing catalysts exhibit low selectivity during the reduction amination of 5-hydroxymethylfurfural, making it difficult to effectively convert them into 5-hydroxymethylfurfural.
Layered Al2O3 was used as a support to load nickel and non-precious metal elements (Cu, Mg, Ca, Co, Zn) alloy catalysts. The catalysts were prepared by hydrothermal reaction, calcination and reduction. The charge structure of the metal sites was adjusted to suppress excessive hydrogenation reaction and improve selectivity.
The catalyst exhibits excellent performance and is easy to operate, achieving high selectivity and high conversion rate of 5-hydroxymethylfurfural to 5-hydroxymethylfurfuralamine.
Smart Images

Figure CN121130894A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the field of catalysis, in particular to a reductive amination catalyst and a preparation method and application thereof. BACKGROUND
[0002] 5-hydroxymethylfurfurylamine (HMFA) has a wide range of applications in the fields of medicine, organic synthesis and polymer materials. The conversion of 5-hydroxymethylfurfural (HMF) into HMFA through catalytic reductive amination has become one of the important paths for the preparation of HMFA.
[0003] The catalysts used for reductive amination include NiZr / γ-Al2O3, Ni y AlO x , alumina-supported carbon-doped Ni. However, most of these catalysts have the disadvantage of low selectivity. SUMMARY
[0004] The present application provides a reductive amination catalyst and a preparation method and application thereof. The reductive amination catalyst of the present application has high selectivity.
[0005] The present application provides a reductive amination catalyst, comprising layered Al2O3 and an alloy supported on the surface of the layered Al2O3. The elements in the alloy include a nickel element and a non-noble metal element; the non-noble metal element includes one or more of Cu, Mg, Ca, Co and Zn.
[0006] Preferably, the molar ratio of the nickel element to the non-noble metal element is 1:(0.1-4).
[0007] Preferably, the ratio of the total amount of substance of the nickel element and the non-noble metal element to the amount of substance of the aluminum element is 2:1.
[0008] The present application also provides a preparation method of the reductive amination catalyst described in the above technical solution, comprising the following steps: mixing a soluble nickel salt, a soluble non-noble metal salt, a soluble aluminum salt, a precipitating agent and an alcohol solvent to perform a hydrothermal reaction to obtain a hydrotalcite; successively performing calcination and reduction on the hydrotalcite to obtain the reductive amination catalyst.
[0009] Preferably, the soluble nickel salt, the soluble non-noble metal salt and the soluble aluminum salt are nitrate salts. The alcohol solvent includes methanol; and the precipitating agent includes urea.
[0010] Preferably, the mass ratio of the alcohol solvent to the soluble nickel salt is 100:(1-20). The mass ratio of the soluble nickel salt to the soluble non-noble metal salt, the mass ratio of the soluble nickel salt to the soluble aluminum salt, and the mass ratio of the soluble nickel salt to the precipitant are independently 1:(0.05-20).
[0011] Preferably, the temperature of the hydrothermal reaction is 50-210℃, and the holding time is 8-48 h. The temperature of the calcination is 400-700℃, and the holding time is 2-10 h. The reduction is performed in an atmosphere containing a reducing gas, the temperature of the reduction is 300-550℃, and the holding time is 0.5-6 h; the reducing gas comprises hydrogen.
[0012] The application also provides the use of the reduction amination catalyst in the above technical solution or the reduction amination catalyst prepared by the preparation method in the above technical solution in the preparation of 5-hydroxymethylfurfurylamine by reduction amination of 5-hydroxymethylfurfural.
[0013] The application also provides a method for preparing 5-hydroxymethylfurfurylamine by reduction amination of 5-hydroxymethylfurfural, comprising the following steps: The reduction amination reaction of the mixture of the methanol solution of ammonia, 5-hydroxymethylfurfural and the reduction amination catalyst is performed in hydrogen to obtain the 5-hydroxymethylfurfurylamine. The reduction amination catalyst is the reduction amination catalyst in the above technical solution or the reduction amination catalyst prepared by the preparation method in the above technical solution.
[0014] Preferably, the concentration of the methanol solution of ammonia is 0.4-7 mol / L. The mass ratio of the 5-hydroxymethylfurfural to the methanol solution of ammonia is 0.003-0.1:1. The mass ratio of the 5-hydroxymethylfurfural to the reduction amination catalyst is 2-50:1. The temperature of the reduction amination reaction is 30-150℃, the pressure is 0.5-6 MPa, and the time is 0.5-10 h.
[0015] The application alloys nickel with specific non-noble metals to adjust the charge structure of metal sites, so that the HMF is inhibited from excessive hydrogenation during catalysis, and it is ensured that only the aldehyde group of HMF undergoes the reduction amination reaction, thereby improving the selectivity of HMFA.
[0016] The results of the examples show that, at 90℃, the selectivity and yield of the product 5-hydroxymethylfurfurylamine (HMFA) of the catalytic reduction amination reaction are as high as 98.7%.
[0017] Hydrotalcite (Ni m M nThe composition of the Al-LDH is flexible and diverse, and the cations in the layer are uniformly dispersed. The application forms a high-dispersion (high dispersion of metal active sites) stable supported catalyst by taking the hydrotalcite as a precursor. In addition, the Ni m M n The Al-LDH has high adsorption capacity, especially the alloy produced after calcination and reduction, thereby improving the catalytic activity of the active metal in the reduction amination reaction of 5-hydroxymethylfurfural (HMF) and the conversion rate of HMF.
[0018] The results of the examples show that the conversion rate of the raw material HMF in the catalytic reduction amination reaction can reach 100% at 90℃.
[0019] The method provided by the application is simple and easy to operate, and the obtained catalyst has excellent catalytic performance. BRIEF DESCRIPTION OF DRAWINGS
[0020] Figure 1 It is a scanning electron microscope image of the Ni2Co1Al-LDH precursor in Example 1. Figure 2 It is a transmission electron microscope image of the Ni2Co1Al catalyst in Example 1. Figure 3 It is an X-ray powder diffraction pattern of the Ni2Co1Al catalyst in Example 1. DETAILED DESCRIPTION
[0021] The application provides a reduction amination catalyst, which comprises layered Al2O3 and an alloy supported on the surface of the layered Al2O3. The alloy comprises a nickel element and a non-noble metal element; the non-noble metal element comprises one or more of Cu, Mg, Ca, Co and Zn.
[0022] In the application, the reduction amination catalyst comprises layered Al2O3.
[0023] In the application, the reduction amination catalyst comprises an alloy supported on the surface of the layered Al2O3; the alloy comprises a nickel element and a non-noble metal element; the molar ratio of the Ni element to the non-noble metal element is preferably 1:(0.1-4), and in specific embodiments of the application, can be 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3 or 1:3.5; the active component comprises nickel and a non-noble metal; the non-noble metal comprises one or more of Cu, Mg, Ca, Co and Zn; and the ratio of the total amount of substance of the nickel and the non-noble metal to the amount of substance of the aluminum element is 2:1.
[0024] In the application, the preparation raw material of the reduction amination catalyst is preferably Ni m M nAl-LDH (i.e., the precursor of the reducing amination catalyst), where m and n are the molar ratio of Ni to non-noble metals, and Ni m M n The preferred morphology of Al-LDH is a nanoflower-like morphology.
[0025] This invention also provides a method for preparing the reducing amination catalyst described in the above technical solution, comprising the following steps: A hydrothermal reaction is carried out by mixing a soluble nickel salt, a soluble non-precious metal salt, a soluble aluminum salt, a precipitant, and an alcohol solvent to obtain hydrotalcite. The hydrotalcite was sequentially calcined and reduced to obtain the reduced amination catalyst.
[0026] This invention involves mixing a soluble nickel salt, a soluble non-precious metal salt, a soluble aluminum salt, a precipitant, and an alcohol solvent and carrying out a hydrothermal reaction to obtain hydrotalcite.
[0027] In this invention, the mass ratio of the alcohol solvent to the soluble nickel salt is preferably 100:(1~20). In specific embodiments of this invention, it can be 100:2, 100:4, 100:6, 100:8, 100:10, 100:12, 100:14, 100:16 or 100:18. The alcohol solvent includes methanol, and the soluble nickel salt preferably includes nickel nitrate.
[0028] In this invention, the mass ratio of the soluble nickel salt to the soluble non-precious metal salt is preferably 1:(0.05~20). In specific embodiments of this invention, it can be 1:1, 1:2, 1:4, 1:6, 1:8, 1:10, 1:12, 1:14, 1:16 or 1:18. The soluble non-precious metal salt preferably includes nitrates.
[0029] In this invention, the mass ratio of the soluble nickel salt to the soluble aluminum salt is preferably 1:(0.05~20), and in specific embodiments of this invention, it can be 1:1, 1:2, 1:4, 1:6, 1:8, 1:10, 1:12, 1:14, 1:16 or 1:18. The soluble aluminum salt preferably includes aluminum nitrate.
[0030] In this invention, the mass ratio of the soluble nickel salt to the precipitant is preferably 1:(0.05~20), and in specific embodiments of this invention it can be 1:1, 1:2, 1:4, 1:6, 1:8, 1:10, 1:12, 1:14, 1:16 or 1:18. The precipitant preferably includes urea.
[0031] In this invention, the preferred temperature of the hydrothermal reaction is 50~210℃, and the preferred holding time is 8~48h. In specific embodiments of this invention, the temperature of the hydrothermal reaction can be 70℃, 90℃, 100℃, 120℃, 130℃, 150℃, 170℃, 190℃ or 200℃, and the holding time can be 10h, 15h, 18h, 20h, 24h, 28h, 30h, 32h, 36h, 38h, 40h, 42h or 45h.
[0032] After the hydrothermal reaction, the present invention preferably cools the hydrothermal reaction system to room temperature, filters and washes it, and then dries the resulting wet solid to obtain the hydrotalcite.
[0033] After obtaining hydrotalcite, the present invention sequentially calcines and reduces the hydrotalcite to obtain the reduced amination catalyst.
[0034] In this invention, the preferred calcination temperature is 400-700℃, and the preferred holding time is 2-10 hours. In specific embodiments of this invention, the calcination temperature can be 420℃, 480℃, 500℃, 520℃, 550℃, 580℃, 600℃, 620℃, 650℃, or 680℃, and the holding time can be 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, or 9 hours. Calcination produces metal oxides.
[0035] In this invention, the reduction is carried out in an atmosphere containing a reducing gas, which includes hydrogen. The volume fraction of hydrogen in the atmosphere containing the reducing gas is preferably 10%, and the atmosphere containing the reducing gas preferably also includes argon. The reduction temperature is preferably 300~550℃, and the holding time is preferably 0.5~6h. In specific embodiments of this invention, the calcination temperature can be 320℃, 350℃, 380℃, 400℃, 420℃, 450℃, 480℃, 500℃, or 520℃, and the holding time can be 0.5h, 1h, 2h, 3h, 4h, 5h, or 6h.
[0036] The present invention also provides the application of the reducing amination catalyst described in the above technical solution or the reducing amination catalyst prepared by the preparation method described in the above technical solution in the reducing amination of 5-hydroxymethylfurfural to prepare 5-hydroxymethylfurfural.
[0037] The present invention also provides a method for preparing 5-hydroxymethylfurfural by reducing and amination, comprising the following steps: A methanol solution of ammonia, 5-hydroxymethylfurfural, and a reducing amination catalyst were mixed and then subjected to a reducing amination reaction in hydrogen to obtain the 5-hydroxymethylfurfural. The reducing amination catalyst is the reducing amination catalyst described in the above technical solution or the reducing amination catalyst prepared by the preparation method described in the above technical solution.
[0038] In this invention, the mass ratio of 5-hydroxymethylfurfural to the methanol solution of ammonia is preferably 0.003 to 0.1:1, and in specific embodiments of this invention, it can be 0.01:1, 0.02:1, 0.03:1, 0.04:1, 0.05:1, 0.06:1, 0.07:1, 0.08:1, or 0.09:1; the concentration of the methanol solution of ammonia is preferably 0.4 to 7 mol / L, and in specific embodiments of this invention, it can be 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, or 6 mol / L.
[0039] In this invention, the mass ratio of 5-hydroxymethylfurfural to the reducing amination catalyst is preferably 2 to 50:1, and in specific embodiments of this invention, it can be 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 35:1, 40:1 or 45:1.
[0040] In this invention, the temperature of the reductive amination reaction is preferably 30~150℃, the pressure is preferably 0.5~6MPa, and the time is preferably 0.5~10h. In specific embodiments of this invention, the temperature of the reductive amination reaction can be 50℃, 80℃, 100℃ or 120℃, the pressure can be 1MPa, 2MPa, 3MPa, 4MPa, 5MPa or 6MPa, and the time can be 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h or 9h.
[0041] The equation for the reductive amination reaction is shown below: The following examples illustrate the reducing amination catalyst, its preparation method, and its application provided by the present invention in detail, but these should not be construed as limiting the scope of protection of the present invention.
[0042] In the examples, the numbers in the subscripts represent the molar ratio. For example, “Ni2Co1Al” in Example 1 represents a molar ratio of Ni to Co of 2:1.
[0043] Example 1 47.5 g methanol, 1.94 g nickel nitrate, 0.97 g cobalt nitrate, 1.87 g aluminum nitrate and 2.1 g urea were weighed and stirred vigorously at room temperature for 30 min to form a homogeneous mixed solution. The solution was kept at 150 ℃ for 12 h in a crystallization kettle, cooled to room temperature, filtered, washed and dried, calcined at 600 ℃ for 6 h in a muffle furnace, and then reduced at 500 ℃ for 2 h in a tube furnace under a 10% H2 / Ar atmosphere (with a hydrogen volume fraction of 10%) to obtain the Ni2Co1Al catalyst.
[0044] Figure 1 The image shows a scanning electron microscope (SEM) image of the Ni2Co1Al-LDH precursor, which exhibits a nanoflower-like morphology, indicating the successful synthesis of the hydrotalcite layered material.
[0045] Figure 2 The image shows a transmission electron microscope (TEM) image of the Ni2Co1Al catalyst. The alloy particles are loaded on the support, and the layered structure is not destroyed.
[0046] Figure 3 The image shows the X-ray powder diffraction (XRD) pattern of the Ni2Co1Al catalyst. The characteristic diffraction peaks at 44° and 52° correspond to the 111 and 200 crystal planes of the NiCo bimetallic crystal, respectively.
[0047] Example 2 47.5 g methanol, 0.97 g nickel nitrate, 1.94 g cobalt nitrate, 1.87 g aluminum nitrate and 2.1 g urea were weighed and stirred vigorously at room temperature for 30 min to form a homogeneous mixed solution. The solution was kept at 100 °C for 36 h in a crystallization vessel, cooled to room temperature, filtered, washed and dried, calcined at 600 °C for 10 h in a muffle furnace, and then reduced at 500 °C for 1 h in a tube furnace under a 10% H2 / Ar atmosphere to obtain the Ni1Co2Al catalyst.
[0048] Example 3 47.5 g methanol, 1.94 g nickel nitrate, 0.85 g magnesium nitrate, 1.87 g aluminum nitrate and 2.1 g urea were weighed and stirred vigorously at room temperature for 30 min to form a homogeneous mixed solution. The solution was kept at 150 ℃ for 48 h in a crystallization kettle, cooled to room temperature, filtered, washed and dried, calcined at 550 ℃ for 6 h in a muffle furnace, and then reduced at 500 ℃ for 4 h in a tube furnace under a 10% H2 / Ar atmosphere to obtain the Ni2Mg1Al catalyst.
[0049] Example 4 47.5 g methanol, 1.45 g nickel nitrate, 1.49 g zinc nitrate, 1.87 g aluminum nitrate and 2.1 g urea were weighed and stirred vigorously at room temperature for 30 min to form a homogeneous mixed solution. The solution was kept at 200 °C for 24 h in a crystallization vessel, cooled to room temperature, filtered, washed and dried, calcined at 550 °C for 8 h in a muffle furnace, and then reduced at 500 °C for 2 h in a tube furnace under a 10% H2 / Ar atmosphere to obtain the Ni1Zn1Al catalyst.
[0050] Example 5 47.5 g methanol, 0.97 g nickel nitrate, 1.61 g copper nitrate, 1.87 g aluminum nitrate and 2.1 g urea were weighed and stirred vigorously at room temperature for 30 min to form a homogeneous mixed solution. The solution was kept at 130 ℃ for 12 h in a crystallization kettle, cooled to room temperature, filtered, washed and dried, calcined at 650 ℃ for 2 h in a muffle furnace, and then reduced at 500 ℃ for 4 h in a tube furnace under a 10% H2 / Ar atmosphere to obtain the Ni1Cu2Al catalyst.
[0051] Example 6 47.5 g methanol, 1.45 g nickel nitrate, 1.18 g calcium nitrate, 1.87 g aluminum nitrate and 2.1 g urea were weighed and stirred vigorously at room temperature for 30 min to form a homogeneous mixed solution. The solution was kept at 150 ℃ for 8 h in a crystallization kettle, cooled to room temperature, filtered, washed and dried, calcined at 400 ℃ for 3 h in a muffle furnace, and then reduced at 500 ℃ for 6 h in a tube furnace under a 10% H2 / Ar atmosphere to obtain the Ni1Ca1Al catalyst.
[0052] Comparative Example 1 1.16 g of cobalt nitrate and 2.33 g of nickel nitrate were weighed and impregnated onto a commercially available γ-Al2O3 support in equal volumes. The impregnation was carried out at room temperature for 4 h, filtered, washed and dried, and then calcined in a muffle furnace at 600 ℃ for 6 h. Finally, the catalyst was reduced in a tube furnace at 500 ℃ for 2 h in a 10% H2 / Ar atmosphere to obtain the Ni2Co1 / γ-Al2O3 catalyst.
[0053] Comparative Example 2 Weigh 150 g of water, 5.4 g of glucose and 3.75 g of aluminum nitrate, dry them in a water bath at 80 °C for 4 h, cool them to room temperature, and calcine them in a tube furnace at 1000 °C for 3 h in an air atmosphere to obtain the Al2O3 support.
[0054] 0.78 g of cobalt nitrate and 1.55 g of nickel nitrate were weighed and impregnated onto the Al2O3 support synthesized in Comparative Example 2 by equal volume. The impregnation was carried out at room temperature for 10 h, filtered, washed and dried, calcined at 600 ℃ in a muffle furnace for 6 h, and then reduced at 500 ℃ in a tube furnace under a 10% H2 / Ar atmosphere for 2 h to obtain the Ni2Co1 / Al2O3 catalyst.
[0055] Application Example 1 The Ni₂Co₁Al catalyst synthesized in Example 1 was evaluated in a batch reactor. 20 mL of a 4 mol / L ammonia-methanol solution, 3 mmol HMF, and 50 mg of catalyst were added to a batch stainless steel reactor. After thorough mixing, the reactor was sealed, and the catalytic reduction amination reaction was carried out for 6 h under a hydrogen atmosphere, at a pressure of 2 MPa and a temperature of 90 °C. The product was analyzed by offline gas chromatography. Under these reaction conditions, the HMF conversion reached 100%, and the selectivity and yield of the product HMFA were as high as 98.7%.
[0056] Application Example 2 The Ni₂Co₁Al catalyst synthesized in Example 1 was evaluated in a batch reactor. 20 mL of a 7 mol / L ammonia-methanol solution, 3 mmol HMF, and 50 mg of catalyst were added to a batch stainless steel reactor. After thorough mixing, the reactor was sealed, and the catalytic reduction amination reaction was carried out for 6 h under a hydrogen atmosphere, at a pressure of 1 MPa and a temperature of 80 °C. The product was analyzed by offline gas chromatography. Under these reaction conditions, the HMF conversion reached 100%, and the selectivity and yield of the product HMFA were 93.4%.
[0057] Application Example 3 The Ni₂Co₁Al catalyst synthesized in Example 1 was evaluated in a batch reactor. 30 mL of a 4 mol / L ammonia-methanol solution, 3 mmol HMF, and 100 mg of catalyst were added to a batch stainless steel reactor. After thorough mixing, the reactor was sealed, and the catalytic reduction amination reaction was carried out for 8 h under a hydrogen atmosphere, at a pressure of 1 MPa and a temperature of 120 °C. The product was analyzed by offline gas chromatography. Under these reaction conditions, the HMF conversion reached 100%, and the selectivity and yield of the product HMFA were 94.7%.
[0058] Application Example 4 The Ni₂Co₁Al catalyst synthesized in Example 1 was evaluated in a batch reactor. 20 mL of a 2 mol / L ammonia-methanol solution, 3 mmol HMF, and 20 mg of catalyst were added to a batch stainless steel reactor. After thorough mixing, the reactor was sealed, and the catalytic reduction amination reaction was carried out for 4 h under a hydrogen atmosphere, at a pressure of 2 MPa and a temperature of 120 °C. The product was analyzed by offline gas chromatography. Under these reaction conditions, the HMF conversion reached 100%, and the selectivity and yield of the product HMFA were 82.6%.
[0059] Application Example 5 The Ni1Co2Al catalyst synthesized in Example 2 was evaluated in a batch reactor. 10 mL of a 2 mol / L ammonia-methanol solution, 1 mmol HMF, and 80 mg of catalyst were added to a batch stainless steel reactor. After thorough mixing, the reactor was sealed, and the catalytic reduction amination reaction was carried out for 10 h under a hydrogen atmosphere, at a pressure of 2 MPa and a temperature of 90 °C. The product was analyzed by offline gas chromatography. Under these reaction conditions, the HMF conversion reached 100%, and the selectivity and yield of the product HMFA were 70.7%.
[0060] Application Example 6 The Ni1Co2Al catalyst synthesized in Example 2 was evaluated in a batch reactor. 20 mL of a 4 mol / L ammonia-methanol solution, 3 mmol HMF, and 30 mg of catalyst were added to a batch stainless steel reactor. After thorough mixing, the reactor was sealed, and the catalytic reduction amination reaction was carried out for 2 h under a hydrogen atmosphere, at a pressure of 2 MPa and a temperature of 60 °C. The product was analyzed by offline gas chromatography. Under these reaction conditions, the HMF conversion reached 100%, and the selectivity and yield of the product HMFA were 22.2%.
[0061] Application Example 7 The Ni2Mg1Al catalyst synthesized in Example 3 was evaluated in a batch reactor. 50 mL of a 4 mol / L ammonia-methanol solution, 3 mmol HMF, and 100 mg of catalyst were added to a batch stainless steel reactor. After thorough mixing, the reactor was sealed, and the catalytic reduction amination reaction was carried out for 8 h under a hydrogen atmosphere, at a pressure of 4 MPa and a temperature of 120 °C. The product was analyzed by offline gas chromatography. Under these reaction conditions, the HMF conversion reached 100%, and the selectivity and yield of the product HMFA were 82.9%.
[0062] Application Example 8 The Ni2Mg1Al catalyst synthesized in Example 3 was evaluated in a batch reactor. 20 mL of a 7 mol / L ammonia-methanol solution, 3 mmol HMF, and 100 mg of catalyst were added to a batch stainless steel reactor. After thorough mixing, the reactor was sealed, and the catalytic reduction amination reaction was carried out for 6 h under a hydrogen atmosphere, at a pressure of 6 MPa and a temperature of 90 °C. The product was analyzed by offline gas chromatography. Under these reaction conditions, the HMF conversion reached 100%, and the selectivity and yield of the product HMFA were 85.5%.
[0063] Application Example 9 The Ni1Zn1Al catalyst synthesized in Example 4 was evaluated in a batch reactor. 20 mL of a 2 mol / L ammonia-methanol solution, 2 mmol HMF, and 10 mg of catalyst were added to a batch stainless steel reactor. After thorough mixing, the reactor was sealed, and the catalytic reduction amination reaction was carried out for 0.5 h under a hydrogen atmosphere, at a pressure of 1 MPa and a temperature of 60 °C. The product was analyzed by offline gas chromatography. Under these reaction conditions, the conversion of HMF reached 100%, and the selectivity and yield of the product HMFA were 15.1%.
[0064] Application Example 10 The Ni1Zn1Al catalyst synthesized in Example 4 was evaluated in a batch reactor. 60 mL of a 0.4 mol / L ammonia-methanol solution, 3 mmol HMF, and 10 mg of catalyst were added to a batch stainless steel reactor. After thorough mixing, the reactor was sealed, and the catalytic reduction amination reaction was carried out for 8 h under a hydrogen atmosphere, at a pressure of 4 MPa and a temperature of 150 °C. The product was analyzed by offline gas chromatography. Under these reaction conditions, the HMF conversion reached 100%, and the selectivity and yield of the product HMFA were 65.4%.
[0065] Application Example 11 The Ni1Cu2Al catalyst synthesized in Example 5 was evaluated in a batch reactor. 20 mL of a 2 mol / L ammonia-methanol solution, 3 mmol HMF, and 20 mg of catalyst were added to a batch stainless steel reactor. After thorough mixing and sealing, the reactor was subjected to a catalytic reduction amination reaction for 6 h under a hydrogen atmosphere, at a pressure of 2 MPa and a temperature of 70 °C. The product was analyzed by offline gas chromatography. Under these reaction conditions, the HMF conversion reached 100%, and the selectivity and yield of the product HMFA were 38.1%.
[0066] Application Example 12 The Ni1Cu2Al catalyst synthesized in Example 5 was evaluated in a batch reactor. 100 mL of a 7 mol / L ammonia-methanol solution, 3 mmol HMF, and 70 mg of catalyst were added to a batch stainless steel reactor. After thorough mixing, the reactor was sealed, and the catalytic reduction amination reaction was carried out for 2 h under a hydrogen atmosphere, at a pressure of 2 MPa and a temperature of 100 °C. The product was analyzed by offline gas chromatography. Under these reaction conditions, the HMF conversion reached 100%, and the selectivity and yield of the product HMFA were 74.8%.
[0067] Application Example 13 The Ni1Ca1Al catalyst synthesized in Example 6 was evaluated in a batch reactor. 20 mL of a 4 mol / L ammonia-methanol solution, 3 mmol HMF, and 40 mg of catalyst were added to a batch stainless steel reactor. After thorough mixing, the reactor was sealed, and the catalytic reduction amination reaction was carried out for 2 h under a hydrogen atmosphere, at a pressure of 2 MPa and a temperature of 50 °C. The product was analyzed by offline gas chromatography. Under these reaction conditions, the HMF conversion reached 100%, and the selectivity and yield of the product HMFA were 38.1%.
[0068] Application Example 14 The Ni1Ca1Al catalyst synthesized in Example 6 was evaluated in a batch reactor. 20 mL of a 4 mol / L ammonia-methanol solution, 3 mmol HMF, and 100 mg of catalyst were added to a batch stainless steel reactor. After thorough mixing, the reactor was sealed, and the catalytic reduction amination reaction was carried out for 4 h under a hydrogen atmosphere, at a pressure of 2 MPa and a temperature of 140 °C. The product was analyzed by offline gas chromatography. Under these reaction conditions, the HMF conversion reached 100%, and the selectivity and yield of the product HMFA were 69.5%.
[0069] Comparative Application Example 1 The Ni₂Co₁ / γ-Al₂O₃ catalyst synthesized in Comparative Example 1 was evaluated in a batch reactor. 20 mL of a 4 mol / L ammonia-methanol solution, 3 mmol HMF, and 50 mg of catalyst were added to a batch stainless steel reactor. After thorough mixing, the reactor was sealed, and the catalytic reduction amination reaction was carried out for 6 h under a hydrogen atmosphere, at a pressure of 2 MPa and a temperature of 90 °C. The product was analyzed by offline gas chromatography. Under these reaction conditions, the HMF conversion reached 100%, and the selectivity and yield of the product HMFA were 87.8%.
[0070] Comparative Application Example 2 The Ni₂Co₁ / Al₂O₃ catalyst synthesized in Comparative Example 2 was evaluated in a batch reactor. 20 mL of a 4 mol / L ammonia-methanol solution, 3 mmol HMF, and 50 mg of catalyst were added to a batch stainless steel reactor. After thorough mixing and sealing, the reactor was subjected to a catalytic reduction amination reaction for 6 h under a hydrogen atmosphere, at a pressure of 2 MPa and a temperature of 90 °C. The product was analyzed by offline gas chromatography. Under these reaction conditions, the HMF conversion reached 100%, and the selectivity and yield of the product HMFA were 64.1%.
[0071] As can be seen from Application Examples 1-14 and Comparative Application Examples 1-2, compared with commercially available γ-Al2O3 supported NiCo catalyst (Ni2Co1 / γ-Al2O3) and Ni2Co1 / Al2O3 synthesized by the conventional impregnation method, the NiCo bimetallic catalyst (Ni2Co1Al) prepared in this invention has superior reaction performance and significantly improved HMFA selectivity.
[0072] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A reductive amination catalyst, characterized in that, It includes layered Al2O3 and an alloy supported on the surface of the layered Al2O3; The alloy contains elements including nickel and non-precious metal elements; the non-precious metal elements include one or more of Cu, Mg, Ca, Co and Zn.
2. The reductive amination catalyst according to claim 1, characterized in that, The molar ratio of nickel to non-precious metal elements is 1:(0.1~4).
3. The reductive amination catalyst according to claim 1 or 2, characterized in that, The ratio of the total amount of nickel and non-precious metal elements to the amount of aluminum is 2:
1.
4. The method for preparing the reductive amination catalyst according to any one of claims 1 to 3, characterized in that, Includes the following steps: A hydrothermal reaction is carried out by mixing a soluble nickel salt, a soluble non-precious metal salt, a soluble aluminum salt, a precipitant, and an alcohol solvent to obtain hydrotalcite. The hydrotalcite was sequentially calcined and reduced to obtain the reduced amination catalyst.
5. The preparation method according to claim 4, characterized in that, The soluble nickel salt, soluble non-precious metal salt, and soluble aluminum salt are nitrates; The alcohol solvent includes methanol; the precipitant includes urea.
6. The preparation method according to claim 4 or 5, characterized in that, The mass ratio of the alcohol solvent to the soluble nickel salt is 100:(1~20); The mass ratio of the soluble nickel salt to the soluble non-precious metal salt, the mass ratio of the soluble nickel salt to the soluble aluminum salt, and the mass ratio of the soluble nickel salt to the precipitant are independently 1:(0.05~20).
7. The preparation method according to claim 4, characterized in that, The hydrothermal reaction temperature is 50~210℃, and the holding time is 8~48 h; The calcination temperature is 400~700℃, and the holding time is 2~10h; The reduction is carried out in an atmosphere containing a reducing gas, at a temperature of 300~550℃, and for a holding time of 0.5~6h; the reducing gas includes hydrogen.
8. The use of the reductive amination catalyst according to any one of claims 1 to 3 or the reductive amination catalyst prepared by the preparation method according to any one of claims 4 to 7 in the reductive amination of 5-hydroxymethylfurfural to prepare 5-hydroxymethylfurfural.
9. A method for preparing 5-hydroxymethylfurfural by reducing and amination, characterized in that, Includes the following steps: A methanol solution of ammonia, 5-hydroxymethylfurfural, and a reducing amination catalyst were mixed and then subjected to a reducing amination reaction in hydrogen to obtain the 5-hydroxymethylfurfural. The reducing amination catalyst is the reducing amination catalyst according to any one of claims 1 to 3 or the reducing amination catalyst prepared by the preparation method according to any one of claims 4 to 7.
10. The method according to claim 9, characterized in that, The concentration of the ammonia in methanol solution is 0.4~7 mol / L; The mass ratio of the 5-hydroxymethylfurfural to the methanol solution of ammonia is 0.003~0.1:1; The mass ratio of 5-hydroxymethylfurfural to the reducing amination catalyst is 2~50:1; The reductive amination reaction is carried out at a temperature of 30~150℃, a pressure of 0.5~6MPa, and a time of 0.5~10h.
Citation Information
Cited By
Method for preparing primary amine chemicals by hydrogenation amination of aldehyde and ketone through platinum group monatomic doped nickel-based layered hydroxide catalyst
CN121537241A