A method for preparing ordered oriented short fiber molded carbon / carbon board
By modifying short-cut carbon fibers with nano-Fe3O4 and using magnetic field orientation, combined with the blending of short and long carbon fibers, the problem of insufficient mechanical and thermal conductivity properties in the thickness direction of carbon/carbon composite plates was solved, and a significant performance improvement was achieved.
Patent Information
- Application Number
- CN202511229345.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-29
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2045-08-29
AI Technical Summary
Existing carbon/carbon composite panels have weak mechanical and thermal properties in the thickness direction, which are difficult to improve effectively through existing molding processes.
Short-cut carbon fibers were modified with nano-Fe3O4 and oriented in a direction perpendicular to the surface of the board using a magnetic field. By combining short-cut and long carbon fibers, ordered oriented short-fiber molded carbon/carbon boards were prepared through directional magnetic field arrangement and hot pressing.
It significantly improves the interlayer mechanical properties and thermal conductivity in the thickness direction of the plate, achieving an approximately isotropic performance distribution.
Abstract
Description
Technical Field
[0001] This invention relates to a method for preparing ordered oriented short fiber molded carbon / carbon sheet, belonging to the field of carbon / carbon composite material preparation technology. Background Technology
[0002] Carbon / carbon composites are a class of high-performance composite materials using carbon fiber (or its fabric) as reinforcement and chemical vapor deposition (CVD) pyrolytic carbon or resin carbon as the matrix. Due to their low density, high specific strength, high specific modulus, excellent high-temperature mechanical properties (maintaining temperatures above 2500℃ in an inert atmosphere), good thermal shock resistance and tribological properties, low coefficient of thermal expansion, and good biocompatibility, carbon / carbon composites have irreplaceable and important application value in aerospace (such as rocket engine nozzles, throat liners, thermal protection systems, and aircraft brake discs), nuclear energy, high-temperature furnace components, and biomedicine.
[0003] Currently, the main manufacturing processes for carbon / carbon composite sheets involve either needle-punching to create preforms followed by densification, or carbon fiber layup molding to create preforms followed by densification. Needle-punched preforms are the primary production method for carbon / carbon composites, offering advantages such as high scalability and ease of operation. Carbon / carbon sheets prepared by continuous long fiber layup molding fully utilize the in-plane reinforcement of continuous fibers, achieving excellent in-plane mechanical and thermal conductivity properties. However, the mechanical properties (such as interlaminar shear strength) and thermal conductivity of this layered carbon / carbon sheet structure are typically very weak because the thickness direction relies mainly on matrix carbon or a small amount of Z-axis needle-punched fibers for connection. Furthermore, while introducing Z-axis needle-punched fiber bundles during preform layup can improve the thickness direction performance, the needle-punching process damages the continuous fibers in the plane, significantly reducing in-plane mechanical properties. Continuous long fibers are prone to wrinkling and breakage at bends during molding, leading to delamination and hindering the molding of high-precision, complex parts. Short fibers have excellent flowability, making them less prone to wrinkling, breakage, and delamination during molding. They can also achieve near-size molding and easily produce sheets with near-isotropic properties. However, the layered structure still cannot effectively improve the mechanical properties and thermal conductivity in the thickness direction. Summary of the Invention
[0004] To address the issue that the mechanical properties and thermal conductivity of carbon / carbon sheets prepared by current molding processes need further improvement, this invention provides a method for preparing ordered oriented short fiber molded carbon / carbon sheets. The method involves modifying the surface of short-cut carbon fibers with nano-Fe3O4, and then using a magnetic field to orient the modified short-cut carbon fibers in a direction perpendicular to the sheet surface. This effectively improves the interlayer mechanical properties and thermal conductivity along the thickness direction of the sheet.
[0005] The objective of this invention is achieved through the following technical solutions.
[0006] A method for preparing ordered oriented short fiber molded carbon / carbon board includes the following steps:
[0007] Nano-Fe3O4 is loaded onto the surface of chopped carbon fibers to form modified chopped carbon fibers;
[0008] Modified short-cut carbon fibers, long carbon fibers, dispersant, and resin are mixed evenly to obtain a resin mixture solution;
[0009] A directional magnetic field is applied to a resin mixture solution, and the modified short-cut carbon fibers in the resin mixture solution are oriented along the direction of the magnetic field. During the application of the magnetic field, excess resin is removed to obtain a prepreg containing ordered oriented short fibers, and the directional arrangement direction of the modified short-cut carbon fibers is parallel to the thickness direction of the prepreg.
[0010] The prepreg is laid into a mold and hot-pressed to obtain a molded preform;
[0011] The molded preform is carbonized to obtain a carbonized preform;
[0012] The carbonized preform is densified to obtain carbon / carbon preform;
[0013] The carbon / carbon preform is graphitized to obtain ordered oriented short fiber molded carbon / carbon board.
[0014] Preferably, the modified short-cut carbon fibers are prepared using the following method:
[0015] Short-cut carbon fibers are immersed in a first acidic solution with oxidizing properties for oxidation treatment. After being removed from the first acidic solution and washed, oxidized short-cut carbon fibers are obtained. Nano-Fe3O4, a silane coupling agent containing amino and siloxy groups and a solvent are mixed evenly and stirred at 60-80°C for 6-12 hours under a protective atmosphere. After that, the solvent is removed and the mixture is washed to obtain modified Fe3O4.
[0016] An aqueous solution of oxidized short-cut carbon fiber was mixed with an aqueous solution of modified Fe3O4, and the pH of the mixed solution was adjusted to 4.5-5.5 using a second acidic solution. The mixture was then stirred and reacted at 30-50°C for 30-60 minutes, allowing the modified Fe3O4 to be loaded onto the surface of the oxidized short-cut carbon fiber through electrostatic adsorption. After removing the water, the mixture was washed and dried to obtain the modified short-cut carbon fiber.
[0017] Preferably, the mass ratio of modified Fe3O4 to oxidized short-cut carbon fibers in the mixed solution is (1.5~2.5):1.
[0018] Preferably, the silane coupling agent containing amino and siloxy groups is (3-aminopropyl)triethoxysilane or (3-aminopropyl)trimethoxysilane.
[0019] Preferably, the pH of the aqueous solution of oxidized chopped carbon fibers is adjusted to 4.5–5.5 using a second acidic solution; then, an aqueous solution of modified Fe3O4 is added dropwise to the aqueous solution of oxidized chopped carbon fibers with a pH of 4.5–5.5, and the pH of the mixed solution of the aqueous solution of oxidized chopped carbon fibers and the aqueous solution of modified Fe3O4 is adjusted to 4.5–5.5 using the second acidic solution. Alternatively, a conventional dilute acid solution, such as dilute hydrochloric acid or dilute acetic acid, can be used as the second acidic solution.
[0020] Preferably, in the resin mixture, the mass ratio of modified short-cut carbon fibers to long carbon fibers is 10:90 to 20:80.
[0021] Preferably, the length of the chopped carbon fibers is 1–8 mm, and the length of the long carbon fibers is 2–10 cm. More preferably, the length of the chopped carbon fibers is 1–3 mm, and the length of the long carbon fibers is 3–5 cm.
[0022] Preferably, the strength of the directional magnetic field applied to the resin mixture is 2 to 6 T.
[0023] Preferably, the short-cut carbon fibers and long carbon fibers are each independently at least one of PAN-based carbon fibers, pitch-based carbon fibers, and rayon carbon fibers.
[0024] Preferably, the resin in the resin solution includes phenolic resin, furan resin, or polyimide resin.
[0025] Preferably, in the resin solution, the mass ratio of the sum of the masses of the modified short-cut carbon fibers and long fibers to the mass of the resin is 1:(15-20).
[0026] Preferably, the dispersant in the resin solution is a polyether-modified siloxane, polyvinylpyrrolidone, or sodium dodecylbenzenesulfonate.
[0027] Preferably, the mass fraction of the dispersant in the resin solution is 0.2% to 0.7%.
[0028] Preferably, a portion of excess resin is first removed by vacuum filtration, and then excess resin is further removed by applying pressure.
[0029] Preferably, the resin mass percentage in the prepreg is 75-85%.
[0030] Preferably, the molding ratio of the prepreg during the hot pressing process is 1:2 to 1:5.
[0031] Preferably, the following heating procedure is adopted during the hot pressing process: first, the temperature is raised to 80-90℃ at a heating rate of 50-60℃ / h and held for 1-2 hours; then, the pressure is increased to 10-15MPa; after pressurization, the temperature is raised to 120-130℃ at a heating rate of 20-30℃ / h and held for 1-2 hours; finally, the temperature is raised to 180-200℃ at a heating rate of 20-30℃ / h and held for 1-2 hours.
[0032] Preferably, the carbonization process employs the following heating procedure: first, the temperature is raised to 120–130°C at a heating rate of 80–90°C / h and held for 1–2 hours; then, the temperature is raised to 200–220°C at a heating rate of 20–30°C / h and held for 1–2 hours; then, the temperature is raised to 890–930°C at a heating rate of 5–15°C / h and held for 4–6 hours. The carbonization process must be carried out under a nitrogen or inert gas protective atmosphere.
[0033] Preferably, the carbonized preform is subjected to multiple cycles of treatment in the order of resin impregnation followed by carbonization until it is densified to the required density.
[0034] Preferably, the resin used for resin impregnation includes furan resin, phenolic resin, or asphalt; in each cycle of treatment, the resin impregnation pressure is 0.1–0.2 MPa, the resin impregnation time is 4–6 h, the carbonization temperature is 890–930 °C, and the carbonization time is 4–6 h.
[0035] Preferably, after densification treatment, the density of the char / char preform increases by 0.5–0.8 g / cm³ relative to the density of the carbonized preform. 3 .
[0036] Preferably, the graphitization temperature is 2000–2200℃, and the graphitization time is 4–6 hours.
[0037] Preferably, the thickness of the ordered oriented short fiber molded carbon / carbon board is 2-5 mm.
[0038] Beneficial effects:
[0039] (1) This application uses nano-Fe3O4 to modify the surface of short-cut carbon fibers. The main advantage is the magnetic properties of Fe3O4, which allows the modified short-cut carbon fibers to achieve directional orientation under a directional magnetic field. This enables the short-cut carbon fibers to be oriented along the direction perpendicular to the thickness of the substrate, thereby improving the interlayer mechanical properties and thermal conductivity along the thickness direction. Furthermore, to avoid excessive nano-Fe3O4 affecting the interfacial bonding between the carbon fibers and the carbon matrix, and because the presence of nano-Fe3O4 increases phonon scattering, thus affecting the mechanical and thermal properties of the substrate, the amount of nano-Fe3O4 loaded on the short-cut carbon fibers must be controlled according to actual requirements.
[0040] (2) This application introduces oxygen-containing functional groups (-COO-, -O-, -SO3-, etc.) into carbon fibers by acid washing and oxidation treatment, making them negatively charged in solution; Fe3O4 is modified by using silane coupling agent to make it positively charged in solution, so that nano Fe3O4 can be loaded on the surface of short-cut carbon fibers by electrostatic adsorption. Based on electrostatic adsorption, it is easier to load nano Fe3O4 on the surface of short-cut carbon fibers and ensure the loading effect.
[0041] (3) Since the length of short carbon fiber is too short, it is impossible to strengthen the matrix carbon through the entanglement and interlacing of fibers. Therefore, long carbon fiber needs to be introduced to achieve the strengthening effect on the matrix carbon. Short carbon fiber mainly improves the interlayer mechanical properties and thermal conductivity of the plate in the thickness direction through its directional arrangement in the thickness direction of the plate. Therefore, this application uses short carbon fiber and long carbon fiber in combination.
[0042] (4) By adjusting parameters such as the mixing ratio of short carbon fiber and long carbon fiber, the length of short carbon fiber, the length of long carbon fiber, and the strength of directional magnetic field, this application can control the reinforcing effect of long carbon fiber and the improvement effect of short carbon fiber on the interlayer mechanical properties and thermal conductivity of the plate in the thickness direction. Detailed Implementation
[0043] The present invention will be further described below with reference to specific embodiments. Unless otherwise specified, the methods described are conventional methods, and the raw materials described are obtainable from publicly available commercial sources.
[0044] Example 1
[0045] Short carbon fibers with a length of 1 mm were soaked in a 65 wt.% nitric acid solution for 2 hours to induce oxidation. After soaking, the short carbon fibers were filtered out and washed with deionized water until neutral to obtain oxidized short carbon fibers.
[0046] 100 mg of nano Fe3O4 was dispersed in 50 mL of ethanol and sonicated for 30 min. Then, 1 mL of (3-aminopropyl)triethoxysilane (APTES) was added, and the mixture was stirred at 70 °C for 6 h under N2 atmosphere. After the reaction was completed, the solid and liquid were separated by magnetic separation, and the solid product was washed with ethanol until neutral to obtain modified Fe3O4.
[0047] 5g of oxidized chopped carbon fibers were dispersed in 500mL of deionized water and sonicated for 30min to ensure uniform dispersion. Dilute acetic acid was then added to adjust the pH of the aqueous solution containing oxidized chopped carbon fibers to 5, resulting in an aqueous solution of oxidized chopped carbon fibers. 7.5g of modified Fe3O4 was dispersed in 500mL of deionized water and sonicated for 30min to ensure uniform dispersion, resulting in an aqueous solution of modified Fe3O4. The aqueous solution of modified Fe3O4 was added dropwise to the aqueous solution of oxidized chopped carbon fibers. Under the control of dilute acetic acid, the pH of the mixed solution after the complete addition of the modified Fe3O4 aqueous solution was maintained in the range of 4.5-5.5. The mixture was stirred at 500rpm for 60min under a water bath at 30℃. After the reaction was completed, the solid product was collected by filtration, washed with deionized water, and then dried at 60℃ to obtain modified chopped carbon fibers.
[0048] Polyether-modified siloxane was added to acetaminophen-formaldehyde resin and stirred until homogeneous. Then, modified short-cut carbon fibers and long carbon fibers with a length of 3 cm were added and stirred until homogeneous to obtain a resin mixture solution. The mass ratio of modified short-cut carbon fibers to long carbon fibers was 15:85, and the mass ratio of the sum of the modified short-cut carbon fibers and long carbon fibers to the mass of acetaminophen-formaldehyde resin was 1:15. The modified short-cut carbon fibers and long carbon fibers were both of the grade SYT45T. The content of polyether-modified siloxane in the resin mixture solution was 0.5 wt.%.
[0049] A directional magnetic field with a strength of 4T is applied to the resin mixture solution. Under the action of the directional magnetic field, the modified short-cut carbon fibers in the resin mixture solution are oriented along the direction of the magnetic field. During the application of the magnetic field, a portion of the excess resin in the resin mixture solution is first filtered out by vacuum filtration. Then, a 30kg pressure plate is used to cover the surface of the filtered solid product for extrusion to further extrude the excess resin, resulting in a prepreg containing ordered oriented short fibers. The mass fraction of resin in the prepreg is approximately 80%.
[0050] Based on a compression ratio of 1:3, a multi-layer prepreg with a total thickness of 9mm is stacked and placed in a mold with a depth of 3mm for hot pressing to obtain a molded preform. The heating procedure for hot pressing is as follows: first, the temperature is raised to 85℃ at a heating rate of 60℃ / h, and held at 85℃ for 1h. Then, the pressure is increased to 10MPa, and after pressurization, the temperature is raised to 125℃ at a heating rate of 26℃ / h, and held at 125℃ for 1h. Finally, the temperature is raised to 180℃ at a heating rate of 27℃ / h, and held at 180℃ for 1h.
[0051] The molded preform is carbonized to obtain a carbonized preform. The carbonization heating procedure is as follows: first, the temperature is increased to 120℃ at a heating rate of 90℃ / h and held at 120℃ for 2h; then, the temperature is increased to 200℃ at a heating rate of 30℃ / h and held at 200℃ for 2h; then, the temperature is increased to 900℃ at a heating rate of 10℃ / h and held at 900℃ for 4h. The carbonization process must be carried out under a nitrogen protective atmosphere.
[0052] The carbonized preform was subjected to two cycles of treatment, first resin impregnation followed by carbonization, to obtain a carbon / carbon preform; wherein the density of the carbon / carbon preform increased by 0.6 g / cm³ compared to the density of the carbonized preform. 3 The impregnation resin is furan resin, and the impregnation pressure, impregnation time and carbonization temperature are 900℃ and 4h respectively in each cycle of treatment.
[0053] The carbon / carbon preform was graphitized at 2100℃ for 4 hours and then machined according to the actual size requirements to obtain ordered oriented short fiber molded carbon / carbon board.
[0054] According to GB / T 41501-2022 standard, samples were prepared using the ordered oriented short fiber molded carbon / carbon sheet prepared in Example 1, and the interlaminar shear strength was measured to be 10 MPa.
[0055] Samples were prepared using the ordered oriented short fiber molded carbon / carbon sheet prepared in Example 1 according to the Q / G260-2012 standard, and the thermal conductivity in the thickness direction of the sheet was measured to be 29.3 W / (mK).
[0056] Comparative Example 1
[0057] Based on Example 1, except for the preparation steps of unmodified chopped carbon fibers and the preparation conditions of the resin mixture solution, all other steps and process conditions are the same as in Example 1, and chopped fiber molded carbon / carbon board is obtained accordingly; wherein, the preparation steps of the resin mixture solution in Comparative Example 1 are as follows;
[0058] Polyether-modified siloxane was added to acetaminophen-formaldehyde resin and stirred until homogeneous. Then, long carbon fibers (3 cm in length, grade SYT45T) were added and stirred until homogeneous to obtain a resin mixture solution. The mass ratio of long carbon fibers to acetaminophen-formaldehyde resin was 1:15, and the content of polyether-modified siloxane in the resin mixture solution was 0.5 wt.%.
[0059] Compared with Example 1, Comparative Example 1 did not add modified short-cut carbon fibers to the acetophenolic resin, and therefore did not require the preparation of modified short-cut carbon fibers.
[0060] According to GB / T 41501-2022 standard, a sample was prepared using the non-chopped fiber molded carbon / carbon board prepared in Comparative Example 1, and the interlaminar shear strength was measured to be 8.5 MPa.
[0061] According to the Q / G260-2012 standard, a sample was prepared using the non-chopped fiber molded carbon / carbon sheet prepared in Comparative Example 1. The thermal conductivity in the thickness direction of the sheet was measured to be 26 W / (mK).
[0062] Comparative Example 2
[0063] Based on Example 1, except for the preparation steps of unmodified short-cut carbon fibers and the preparation conditions of the resin mixture solution, all other steps and process conditions are the same as in Example 1, and disordered oriented short fiber molded carbon / carbon board is obtained accordingly; wherein, the preparation steps of the resin mixture solution in Comparative Example 2 are as follows;
[0064] Polyether-modified siloxane was added to acetaminophen-formaldehyde resin and stirred until homogeneous. Then, 1 mm long short carbon fibers and 3 cm long long carbon fibers were added and stirred until homogeneous to obtain a resin mixture solution. The mass ratio of short carbon fibers to long carbon fibers was 15:85, and the mass ratio of the sum of the mass of short carbon fibers and long carbon fibers to the mass of acetaminophen-formaldehyde resin was 1:15. Both the short carbon fibers and long carbon fibers were of the grade SYT45T. The content of polyether-modified siloxane in the resin mixture solution was 0.5 wt.%.
[0065] Compared to Example 1, Comparative Example 2 directly adds unmodified short-cut carbon fibers to acetophenolic resin, thus eliminating the need to prepare modified short-cut carbon fibers.
[0066] According to GB / T 41501-2022 standard, a sample was prepared using the long fiber molded carbon / carbon board prepared in Comparative Example 2, and the interlaminar shear strength was measured to be 7.9 MPa.
[0067] According to the Q / G260-2012 standard, the long fiber molded carbon / carbon sheet prepared in Comparative Example 2 was used to prepare the sample, and the thermal conductivity in the thickness direction of the sheet was measured to be 26.7 W / (mK).
[0068] Example 2
[0069] Based on Example 1, except that the length of the chopped carbon fiber was replaced with 2 mm and the mass ratio of modified chopped carbon fiber to long carbon fiber was replaced with 12.5:87.5, all other steps and process conditions were the same as in Example 1, and ordered oriented short fiber molded carbon / carbon board was obtained accordingly.
[0070] According to GB / T 41501-2022 standard, samples were prepared using the ordered oriented short fiber molded carbon / carbon sheet prepared in Example 2, and the interlaminar shear strength was measured to be 11.2 MPa.
[0071] Samples were prepared using the ordered oriented short fiber molded carbon / carbon sheet prepared in Example 2 according to the Q / G260-2012 standard, and the thermal conductivity in the thickness direction of the sheet was measured to be 30.5 W / (mK).
[0072] Example 3
[0073] Based on Example 1, except that the length of the chopped carbon fiber is replaced with 3 mm and the mass ratio of modified chopped carbon fiber to long carbon fiber is replaced with 10:90, all other steps and process conditions are the same as in Example 1, and ordered oriented short fiber molded carbon / carbon board is obtained accordingly.
[0074] According to GB / T 41501-2022 standard, samples were prepared using the ordered oriented short fiber molded carbon / carbon sheet prepared in Example 3, and the interlaminar shear strength was measured to be 10.5 MPa.
[0075] Samples were prepared using the ordered oriented short fiber molded carbon / carbon sheet prepared in Example 3 according to the Q / G260-2012 standard, and the thermal conductivity in the thickness direction of the sheet was measured to be 30 W / (mK).
[0076] Example 4
[0077] Based on Example 1, except that the mass ratio of modified short-cut carbon fiber to long carbon fiber was replaced with 12.5:87.5 and the directional magnetic field strength was replaced with 2T, all other steps and process conditions were the same as in Example 1, and ordered oriented short fiber molded carbon / carbon board was obtained accordingly.
[0078] According to GB / T 41501-2022 standard, samples were prepared using the ordered oriented short fiber molded carbon / carbon sheet prepared in Example 4, and the interlaminar shear strength was measured to be 9.3 MPa.
[0079] According to the Q / G260-2012 standard, samples were prepared using the ordered oriented short fiber molded carbon / carbon sheet prepared in Example 4, and the thermal conductivity in the thickness direction of the sheet was measured to be 28.7 W / (mK).
[0080] Example 5
[0081] Based on Example 1, except that the mass ratio of modified short-cut carbon fiber to long carbon fiber was replaced with 12.5:87.5 and the directional magnetic field strength was replaced with 6T, all other steps and process conditions were the same as in Example 1, and ordered oriented short fiber molded carbon / carbon board was obtained accordingly.
[0082] According to GB / T 41501-2022 standard, samples were prepared using the ordered oriented short fiber molded carbon / carbon sheet prepared in Example 5, and the interlaminar shear strength was measured to be 11.5 MPa.
[0083] According to the Q / G260-2012 standard, samples were prepared using the ordered oriented short fiber molded carbon / carbon sheet prepared in Example 5, and the thermal conductivity in the thickness direction of the sheet was measured to be 31 W / (mK).
[0084] Example 6
[0085] Based on Example 1, except that the amount of modified Fe3O4 added to the aqueous solution of modified Fe3O4 was replaced with 50g, all other steps and process conditions were the same as in Example 1, and ordered oriented short fiber molded carbon / carbon board was obtained accordingly.
[0086] According to GB / T 41501-2022 standard, samples were prepared using the ordered oriented short fiber molded carbon / carbon sheet prepared in Example 6, and the interlaminar shear properties were measured to be 9.1 MPa.
[0087] Samples were prepared using the ordered oriented short fiber molded carbon / carbon sheet prepared in Example 6 according to the Q / G260-2012 standard, and the thermal conductivity in the thickness direction of the sheet was measured to be 27 W / (mK).
[0088] Example 7
[0089] Based on Example 1, except that the length of the chopped carbon fiber is replaced with 4 mm and the mass ratio of modified chopped carbon fiber to long carbon fiber is replaced with 10:90, all other steps and process conditions are the same as in Example 1, and ordered oriented short fiber molded carbon / carbon board is obtained accordingly.
[0090] According to GB / T 41501-2022 standard, samples were prepared using the ordered oriented short fiber molded carbon / carbon sheet prepared in Example 7, and the interlaminar shear strength was measured to be 9.5 MPa.
[0091] According to the Q / G260-2012 standard, samples were prepared using the ordered oriented short fiber molded carbon / carbon sheet prepared in Example 7, and the thermal conductivity in the thickness direction of the sheet was measured to be 28.3 W / (mK).
[0092] Example 8
[0093] Based on Example 1, except that the length of the chopped carbon fiber is replaced with 5 mm and the mass ratio of modified chopped carbon fiber to long carbon fiber is replaced with 10:90, all other steps and process conditions are the same as in Example 1, and ordered oriented short fiber molded carbon / carbon board is obtained accordingly.
[0094] According to GB / T 41501-2022 standard, samples were prepared using the ordered oriented short fiber molded carbon / carbon sheet prepared in Example 8, and the interlaminar shear strength was measured to be 9.7 MPa.
[0095] According to the Q / G260-2012 standard, samples were prepared using the ordered oriented short fiber molded carbon / carbon sheet prepared in Example 8, and the thermal conductivity in the thickness direction of the sheet was measured to be 27.9 W / (mK).
[0096] Comparative Example 3
[0097] Based on Example 1, except that the length of the chopped carbon fiber is replaced with 2 mm and the mass ratio of modified chopped carbon fiber to long carbon fiber is replaced with 50:50, all other steps and process conditions are the same as in Example 1, and ordered oriented short fiber molded carbon / carbon board is obtained accordingly.
[0098] According to GB / T 41501-2022 standard, samples were prepared using the ordered oriented short fiber molded carbon / carbon sheet prepared in Comparative Example 3, and the interlaminar shear properties were measured to be 7.1 MPa.
[0099] According to the Q / G260-2012 standard, samples were prepared using the ordered oriented short fiber molded carbon / carbon sheet prepared in Comparative Example 3. The thermal conductivity in the thickness direction of the sheet was measured to be 18.4 W / (mK).
[0100] In summary, the above are merely preferred embodiments of the present invention and are not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for preparing ordered oriented short fiber molded carbon / carbon board, characterized in that, Includes the following steps: Nano-Fe3O4 is loaded onto the surface of chopped carbon fibers to form modified chopped carbon fibers; Modified short-cut carbon fibers, long carbon fibers, dispersant, and resin are mixed evenly to obtain a resin mixture solution; When a directional magnetic field is applied to a resin mixture, the modified short-cut carbon fibers in the resin mixture are oriented along the direction of the magnetic field. During the magnetic field application process, excess resin is removed to obtain a prepreg containing ordered oriented short fibers, and the orientation of the modified short carbon fibers is parallel to the thickness direction of the prepreg. The prepreg is laid into a mold and hot-pressed to obtain a molded preform; The molded preform is carbonized to obtain a carbonized preform; The carbonized preform is densified to obtain carbon / carbon preform; The carbon / carbon preform is graphitized to obtain ordered oriented short fiber molded carbon / carbon board. In the resin mixture, the mass ratio of modified short-cut carbon fibers to long carbon fibers is 10:90 to 20:80, the length of the short-cut carbon fibers is 1 to 8 mm, and the length of the long carbon fibers is 2 to 10 cm.
2. The method for preparing an ordered oriented short fiber molded carbon / carbon board according to claim 1, characterized in that, Modified short-cut carbon fibers were prepared using the following method: Short-cut carbon fibers are immersed in a first acidic solution with oxidizing properties for oxidation treatment, and then removed from the first acidic solution and washed to obtain oxidized short-cut carbon fibers. Nano Fe3O4, a silane coupling agent containing amino and siloxy groups, and a solvent were mixed evenly and stirred at 60–80 °C for 6–12 h under a protective atmosphere. The solvent was then removed and the mixture was washed to obtain modified Fe3O4. An aqueous solution of oxidized short-cut carbon fibers was mixed with an aqueous solution of modified Fe3O4, and the pH of the mixed solution was adjusted to 4.5-5.5 using a second acidic solution. The mixture was then stirred at 30-50°C for 30-60 minutes to allow the modified Fe3O4 to be electrostatically adsorbed onto the surface of the oxidized short-cut carbon fibers. After removing the water, the mixture was washed and dried to obtain the modified short-cut carbon fibers.
3. The method for preparing an ordered oriented short fiber molded carbon / carbon board according to claim 2, characterized in that, In a mixed solution of aqueous solution of oxidized short-cut carbon fiber and aqueous solution of modified Fe3O4, the mass ratio of modified Fe3O4 to oxidized short-cut carbon fiber is (1.5~2.5):
1.
4. The method for preparing an ordered oriented short fiber molded carbon / carbon board according to claim 2, characterized in that, The silane coupling agents containing amino and siloxy groups are (3-aminopropyl)triethoxysilane or (3-aminopropyl)trimethoxysilane; And / or, The pH of the aqueous solution of oxidized short-cut carbon fibers was adjusted to 4.5–5.5 using a second acidic solution; then, the aqueous solution of modified Fe3O4 was added dropwise to the aqueous solution of oxidized short-cut carbon fibers with pH = 4.5–5.5, and the pH of the mixed solution of the aqueous solution of oxidized short-cut carbon fibers and the aqueous solution of modified Fe3O4 was adjusted to 4.5–5.5 using the second acidic solution.
5. The method for preparing an ordered oriented short fiber molded carbon / carbon board according to claim 1, characterized in that, Short-cut carbon fibers and long carbon fibers are each independently at least one of PAN-based carbon fibers, pitch-based carbon fibers, and rayon carbon fibers; And / or, The resin in the resin solution includes phenolic resin, furan resin, or polyimide resin; And / or, The dispersant in the resin solution is polyether-modified siloxane, polyvinylpyrrolidone, or sodium dodecylbenzenesulfonate; And / or, The mass ratio of the sum of the modified short-cut carbon fibers and long fibers in the resin solution to the mass of the resin is 1:(15-20); And / or, The mass fraction of the dispersant is 0.2%–0.7%; And / or, The resin mass percentage in the prepreg is 75-85%.
6. A method for preparing an ordered oriented short fiber molded carbon / carbon sheet according to any one of claims 1 to 5, characterized in that, The strength of the directional magnetic field applied to the resin mixture is 2 to 6 T.
7. A method for preparing an ordered oriented short fiber molded carbon / carbon board according to any one of claims 1 to 5, characterized in that, The length of short-cut carbon fiber is 1-3 mm, and the length of long carbon fiber is 3-5 cm; And / or, The strength of the directional magnetic field applied to the resin mixture is 2 to 6 T.
8. The method for preparing an ordered oriented short fiber molded carbon / carbon board according to claim 6, characterized in that, The molding ratio of the prepreg during the hot pressing process is 1:2 to 1:5; And / or, The thickness of ordered oriented short fiber molded carbon / carbon board is 2-5 mm.
9. The method for preparing an ordered oriented short fiber molded carbon / carbon board according to claim 8, characterized in that, During the hot pressing process, the following heating procedure is adopted: first, the temperature is raised to 80-90℃ at a heating rate of 50-60℃ / h and held for 1-2 hours; then, the pressure is increased to 10-15MPa; after pressurization, the temperature is raised to 120-130℃ at a heating rate of 20-30℃ / h and held for 1-2 hours; finally, the temperature is raised to 180-200℃ at a heating rate of 20-30℃ / h and held for 1-2 hours. And / or, During the carbonization process, the following heating procedure is adopted: first, the temperature is raised to 120-130℃ at a heating rate of 80-90℃ / h and held for 1-2 hours; then, the temperature is raised to 200-220℃ at a heating rate of 20-30℃ / h and held for 1-2 hours; then, the temperature is raised to 890-930℃ at a heating rate of 5-15℃ / h and held for 4-6 hours. The carbonization process must be carried out under a nitrogen or inert gas protective atmosphere. And / or, The carbonized preform is subjected to multiple cycles of treatment in the order of resin impregnation followed by carbonization until it is densified to the required density. And / or, The graphitization temperature is 2000–2200℃, and the graphitization time is 4–6 hours.
10. The method for preparing an ordered oriented short fiber molded carbon / carbon board according to claim 9, characterized in that, When the carbonized preform is subjected to multiple cycles of treatment in the order of resin impregnation followed by carbonization, the resin impregnation pressure is 0.1-0.2 MPa, the resin impregnation time is 4-6 h, the carbonization temperature is 890-930℃, and the carbonization time is 4-6 h in each cycle. And / or, When the carbonized preform is subjected to multiple cycles of treatment in the order of resin impregnation followed by carbonization, the resin used for resin impregnation includes furan resin, phenolic resin or asphalt. And / or, After densification treatment, the density of the char / char preform increases by 0.5–0.8 g / cm³ compared to the density of the carbonized preform. 3 .
Citation Information
Patent Citations
Highly-oriented and densely-arranged carbon fiber heat-conducting composite material and preparation method thereof
CN117447844A
Carbon paper for gas diffusion layer of fuel cell and preparation method of carbon paper
CN119221325A