Production method of environment-friendly pigment red 170

By improving the production process of Pigment Red 170, using acetic acid and alkali to adjust the pH value, and adding kaolin and additives, the problem of excessive toxic substances in the pigment has been solved, resulting in a high-performance environmentally friendly pigment suitable for multiple environmental protection fields, especially the food industry.

CN121495375APending Publication Date: 2026-02-10JIANGSU CAIRUI IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510679464.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-21
Filing Date
2025-05-26
Publication Date
2026-02-10

AI Technical Summary

Technical Problem

Existing Pigment Red 170 products contain high levels of toxic aromatic amines, heavy metals, and salts, failing to meet European and American export standards and domestic requirements for use in food packaging, home decoration, and other fields. Furthermore, traditional production methods cause environmental pollution.

Method used

The process involves steps such as diazotization, coupling, pressure filtration, washing, and post-treatment. Acetic acid and alkali are used to adjust the pH value, and kaolin and additives are added. Through high-speed pulping and high-temperature pressure treatment, organic impurities and salts are removed, improving the stability and dispersibility of pigment particles. A unique post-treatment process is used to obtain high-performance pigments.

Benefits of technology

We have produced Pigment Red 170, which is free of heavy metals and banned aromatic amines. It has a bright color, is light and heat resistant, and is suitable for environmentally friendly water-based pigments, inkjet printing, powder coatings, high-end automotive anti-corrosion paints, and other fields. It is especially suitable for the food industry, where it is environmentally safe and friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121495375A_ABST
    Figure CN121495375A_ABST
Patent Text Reader

Abstract

According to the brand-new environment-friendly pigment red 170 production method, on the basis of a traditional production process, the materials obtained after coupling reaction are subjected to filter pressing and washing, organic impurities and salt are removed, by adding acetic acid, DB-70 can be dissolved more completely, sodium acetate generated through acetic acid and alkali in the subsequent coupling reaction can be used for preparing the pigment red 170, and the pigment red 170 can be obtained. The effect of stabilizing the pH value is achieved; according to the process, pigment particles are subjected to crystal transformation more sufficiently, the crystal form is more stable, the particle size distribution is narrower, the chemical resistance, light resistance, heat resistance and the like of the obtained pigment red 170 are all higher than the industrial standard, and the pigment red 170 is suitable for industrial production. And no forbidden aromatic amine or toxic substance is contained.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application belongs to the field of chemical industry, and relates to a single azo dye in organic pigments, in particular to a production method of an environment-friendly pigment red 170. BACKGROUND

[0002] Pigment red 170, also known as permanent red F5RK or permanent red F3RK, F2RK, etc., is a common organic pigment, and its chemical formula is C 26 H 22 N4O4, and its chemical formula is shown as formula (I):

[0003]

[0004] The preparation of pigment red 170 mainly includes the following steps: diazotization, coupling, powder preparation and drying. The crude product of red 170 is formed after coupling, and the performance of the crude product is unstable and the quality is poor. The existing pigment red 170 product contains toxic aromatic amines, heavy metals and high salt content in the material, and cannot meet the export standards of Europe and the United States and the use requirements in the fields of domestic food packaging, home decoration and the like; in addition, the existing pigment red 170 product is mainly applied to the traditional ink and paint industry, and will cause certain pollution to the environment, and has many adverse effects such as lack of safety and environmental protection.

[0005] With the gradual attention to environmental protection and safety, in the application field of pigments in contact with human body, for the pigments used in plastic and food packaging ink, the AP (89) 1 regulation resolution in EU 1935 / 2004 / EC has strict regulations on the limit of harmful substance residues in pigments, and the limit ranges are as follows: lead ≤100 ppm; antimony ≤100 ppm; arsenic ≤100 ppm; barium ≤100 ppm; cadmium ≤100 ppm; chromium ≤1000 ppm; mercury ≤50 ppm; and aromatic amine ≤500 ppm. The control of aromatic amine is the key. In recent years, several advanced pigment manufacturing enterprises in the European Union and the United States have reported that the content of harmful aromatic amines in azo pigments is reduced from an average level of 1000-5000 ppm to 500 ppm of the corresponding specification pigment varieties, which are pushed to the market.

[0006] On August 1, 2008, the EU formally implemented the REACH regulation for the purpose of protecting human health and the environment, maintaining and improving the competitiveness of the EU chemical industry, increasing the transparency of chemical information, etc. The regulation requires registration of all chemical substances entering the EU market with an output or import volume of more than 1 ton, and a series of technical documents such as chemical safety data table, safety assessment report, risk assessment, etc. are required for chemical substances with an annual output or import volume of more than 10 tons. Subsequently, a safety regulation AP(89)1 was specially introduced in the field of pigments: the residual heavy metals and aromatic amine in pigments in the field of plastic and food packaging ink have clear limiting requirements, and those that do not meet the requirements cannot be applied in this field. China is the world's largest producer of pigments, with an annual output of about 70% of the world's total output. The regulatory requirements of AP(89)1 have become a trade barrier for entering the EU market. Therefore, on the basis of the existing production method of pigment red 170, improvement and upgrading are carried out to realize no heavy metals and banned aromatic amines, environment-friendly, bright color, light and heat resistance, colorless and persistent, and good natural degradation, which can greatly promote the production and manufacturing of domestic environmental-friendly pigments, and help to break the trade barriers. SUMMARY

[0007] In view of the problems existing in the prior art, the purpose of the present application is to provide a production method of environment-friendly pigment red 170, wherein the method comprises the following steps:

[0008] S1, diazotization reaction

[0009] After diluting 30% hydrochloric acid and acetic acid with water, 4-aminobenzamide, i.e. red base DB-70, is added, and after complete dissolution by stirring, ice is added to cool to 3-6℃, and then 20-30% sodium nitrite aqueous solution is added to carry out diazotization reaction for 1-3 hours; the gas generated during the reaction is treated as waste gas, and after the reaction is completed, ice and water are added to maintain the temperature at 3-8℃, and then used;

[0010] S2, coupling reaction

[0011] After diluting the base with water, color phenol AS-PH is added, and heated to 75-80℃ by high-temperature steam, and stirred and dissolved to be transparent, and then 5000kg of crushed ice and 5000L of water are added through the feeding port to cool to 30℃, and a coupling liquid is prepared for use;

[0012] The obtained coupling liquid is added to the diazotization liquid obtained in step S1 to carry out coupling reaction for 0.5-1.0 hours, and the reaction temperature is maintained at 10-25℃, the pH is controlled between pH=5-5.5, and stirring is carried out for 1 hour;

[0013] Kaolin is further added, and the temperature is raised to 95-98℃, and maintained for 1 hour, and then used;

[0014] S3, pressure filtration and washing

[0015] The coupling product obtained in S2 is filtered by a filter press to separate the water from the obtained pigment. The wastewater generated by the filter press is sent to the sewage treatment plant for treatment. Water is added to the filter press to rinse the material until it is neutral. The wastewater generated after rinsing is sent to the sewage treatment plant for treatment. The filter cake is ready for use.

[0016] S4, Post-processing

[0017] Add the filter cake obtained from S3 to the reactor, add water to make up to 70-80% of the reactor volume, and pulverize for 30 minutes at a pulverizing speed of 1000-1500 rpm. Adjust the temperature according to the product color requirements, seal the reactor, raise the temperature to 110-150℃, keep it at that temperature for 2 hours, and cool it down to 60-80℃ with jacketed cooling water.

[0018] S5, pressure filtration, fine washing

[0019] The product obtained from S4 is filtered again by a filter press. The wastewater generated by the filter press is sent to the sewage treatment plant for treatment. Water is added to the filter press to rinse the material until it is neutral. After rinsing, the material is blown off and set aside for use. The wastewater generated after rinsing and blowing off is sent to the sewage treatment plant for treatment.

[0020] S6. Drying and pulverizing

[0021] The filter cake obtained from S5 is dried at a temperature of 80-85℃ for 12 hours. The gas generated during drying is treated by dust removal. The collected dust is mixed with the filter cake and then dried. The moisture content is controlled at 0.5-1.5% before drying is stopped. The collected gas is treated as waste gas. After drying, the finished pigment red 170 is obtained.

[0022] Preferably, the molar ratio of 4-aminobenzamide, sodium nitrite and hydrochloric acid in S1 is 1:1 to 1.1:2 to 3, more preferably 1:1.05:2.8, and most preferably 1:1.03:2.65.

[0023] Preferably, an emulsifier is added to the diazo solution in S1; the emulsifier is preferably fatty alcohol polyoxyethylene ether.

[0024] Preferably, the molar ratio of naphthol AS-PH to sodium hydroxide in S2 is 1:1 to 2, more preferably 1:1.5 to 2, and most preferably 1:1.8.

[0025] Preferably, liquid alkali or soda ash is used in S2, and liquid alkali 546 is preferred.

[0026] Preferably, in S2, the pH is adjusted by hydrochloric acid and liquid alkali, and the pH is stabilized by acetic acid.

[0027] Preferably, in step S5, the material is rinsed until the conductivity is ≤100μs / cm.

[0028] Preferably, in step S6, the filter cake is dried to a moisture content of ≤1.0%.

[0029] Preferably, the dried material obtained in S6 is further subjected to ultrafine pulverization.

[0030] Preferably, Huntsman L-207 and acetoacetanilide are heated at 85-90 degrees Celsius for 6 hours to prepare an auxiliary agent, which is added before the S2 coupling reaction; wherein the molar ratio of the auxiliary agent is 0.051.

[0031] Preferably, after the pigment synthesis is completed and the filter cake is washed, the filter cake is re-pulped at high speed. In the S4 post-treatment process, stearic acid and superdispersant are used to make an emulsion to coat the pigment surface; wherein the ratio of stearic acid to superdispersant is 1:1.

[0032] More preferably, the superdispersant is selected from sodium acrylate, acrylic acid-(meth)acrylic acid copolymer, and nonionic superdispersant.

[0033] Compared with existing technologies, this invention provides a novel environmentally friendly production method for Pigment Red 170. This method, based on traditional production processes, involves pressure filtration and washing of the material after the coupling reaction to remove organic impurities and salts. The addition of acetic acid not only ensures more complete dissolution of DB-70 but also, through the sodium acetate produced by acetic acid and alkali in subsequent coupling reactions, stabilizes the pH value, overcoming the shortcomings of traditional processes that rely solely on hydrochloric acid and alkali for significant pH fluctuations. The filter cake is then rapidly pulped using a specialized high-speed pulper, subjected to high-temperature and pressure treatment in a pressure vessel, and further washed with pure water. This process results in more complete crystallization of pigment particles, more stable crystal forms, and a narrower particle size distribution. The resulting Pigment Red 170 exhibits chemical resistance, lightfastness, and heat resistance exceeding industry standards and does not contain prohibited aromatic amines or toxic substances. The first pressure filtration and washing removes salts and unreacted impurities generated during the reaction, while the second washing further improves product purity. Furthermore, the unique additives of this invention can increase the tinting strength of Pigment Red 170 in the NC system by more than 20%; and the unique post-processing technology can achieve excellent dispersibility and a 1500-mesh pressure filtration value of less than 1 without air jet milling. Performance test data also show that kaolin can significantly improve the dispersibility and heat resistance of the pigment. The Pigment Red 170 produced by the method provided by this invention has a bright color, good light and heat resistance, and does not change color over time. Moreover, the pigment does not contain heavy metals or banned aromatic amines, has good natural degradation properties, and can be widely used in new fields such as environmentally friendly water-based pigments, inkjet printing, powder coatings, and high-end automotive (ship) anti-corrosion paints, especially in the food industry, where it is environmentally safe and friendly.

[0034] Terminology Explanation

[0035] When the term "about" is applied to parameters such as pH, concentration, temperature, etc., it indicates that the parameter can vary by ±10%, and sometimes more preferably within ±5%. As those skilled in the art will understand, when a parameter is not critical, figures are generally given for illustrative purposes only, not as limitations. Attached Figure Description

[0036] Figure 1 Flowchart of the production method of environmentally friendly pigment Red 170 provided by the present invention;

[0037] Figure 2 Photograph of the environmentally friendly pigment Red 170 obtained in the example. Detailed Implementation

[0038] The present invention will be further described in detail and completely below with reference to embodiments. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0039] Unless otherwise specified, the experimental methods described in the following embodiments shall be performed according to the manufacturer's recommended conditions. Unless otherwise specified, all reagents involved in the embodiments of this invention are commercially available products and can be purchased through commercial channels.

[0040] The main materials involved in the embodiments of this invention are as follows:

[0041] Experimental reagents

[0042]

[0043] Example 1

[0044] ① Diazotization reaction

[0045] 20,000L of tap water was added to the diazo tank via pipeline. 1084kg of 30% hydrochloric acid and 50kg of 80% acetic acid were added through the metering tank. 600kg of DB-70 was added to the diazo tank through the feed port and stirred until completely dissolved. Then, 3000kg of crushed ice was added through the feed port to cool the mixture to 3-6℃. 318kg of 98% sodium nitrite was prepared into a 20-30% aqueous solution (dissolved in 1000L of water in a sodium nitrite dissolving tank) and added to the diazo tank through the feed port. The diazotization reaction was carried out for 1.5 hours. The gas generated during the reaction was treated as waste gas. After the reaction, the diazo liquid was placed in a coupling tank, and 2000kg of crushed ice and 5000L of water were added. The temperature was maintained at 3-8℃. 50kg of emulsifier fatty alcohol polyoxyethylene ether was added and the mixture was ready for use.

[0046] ② Coupling reaction

[0047] An auxiliary agent was prepared by heating 10 kg of Huntsman L-207 and 10 kg of acetoacetanilide at 85-90 degrees Celsius for 6 hours, and then set aside for later use.

[0048] Add 15,000 L of tap water to the dissolving tank through a pipeline, then add 546 kg of 32% liquid alkali. Heat the tank with high-temperature steam to 75-80°C. Add 1,340 kg of naphthol AS-PH powder to the dissolving tank through the feeding port, along with the above-mentioned additives. Stir and dissolve until transparent. Add 5,000 kg of crushed ice and 5,000 L of water through the feeding port to cool the tank to 30°C. The prepared coupling solution is ready for use.

[0049] The prepared coupling solution is added to the coupling tank through the liquid level difference, and the reverse coupling reaction is carried out for 0.5 hours. Crushed ice is added through the feeding port to maintain the temperature of the coupling reaction at 10-25℃ and the pH is controlled between pH=5-5.5. Stir for 1 hour, add 100kg of kaolin, raise the temperature to 95-98℃, keep it at the temperature for 1 hour, and then enter the pressure filter washing section.

[0050] ③ Filter press and washing section

[0051] The product from the coupling section is pumped into a filter press for filtration. The wastewater generated from filtration is treated at a wastewater treatment plant. 43,000L of tap water is added through a pipeline to the plate and frame filter press to wash the material until it is neutral. The wastewater generated after rinsing is treated at the wastewater treatment plant, and the filter cake is sent to the post-processing section.

[0052] ④ Post-processing section

[0053] Add the filter cake to the reactor, add 10,000L of water, 100Kg of stearic acid and 50Kg of liquid alkali, heat and dissolve to form a transparent emulsion to coat the pigment surface, slurry for 30 minutes, seal the reactor, heat to 130℃, keep warm for 2 hours, cool down to 80℃ with jacket cooling water, and enter the pressure filtration and washing section.

[0054] ⑤ Filter press and washing section

[0055] The product from the coupling section is pumped into a filter press for filtration. The wastewater generated from filtration is treated at a wastewater treatment plant. 25,000L of tap water is added through a pipeline to the plate and frame filter press to rinse the material until it is neutral. Then, an air compressor blows the material off the plate and frame filter press through a pipeline. The wastewater generated after rinsing and blowing off is treated at a wastewater treatment plant.

[0056] ⑥ Drying section

[0057] The filter cake from the filter press is conveyed to a belt dryer for drying at 80-85℃ for 12 hours. The gas generated during drying is filtered by a two-stage wet packed tower. The collected dust is mixed with the filter cake and then fed into the dryer. The uncollected gas is treated as waste gas. After drying, the finished pigment Red 170 is obtained. (See finished product photo.)Figure 2 .

[0058] Performance testing

[0059] 1. The obtained finished product Pigment Red 170 was tested according to the industry standard HG / T 5371-2018, and the test results are as follows:

[0060]

[0061] 2. Heavy metal and aromatic amine testing

[0062] The obtained finished product was sent to SGS for testing, and the test results are as follows.

[0063] (1) The heavy metal testing method refers to the harmonized standard EN 71-3:2013+A1:2014 - Element migration of the EU Toy Directive 2009 / 48 / EC (for Category 3: Toy materials that can be scraped).

[0064]

[0065] Note: "ND" = Not detected (< MDL method detection limit), "-" = Not specified

[0066] (2) The azo dye detection reference is EN 14362-1:2012 - Analyzed by GC-MS / HPLC-DAD.

[0067]

[0068] (3) Polycyclic aromatic hydrocarbons (PAHs) are tested according to the AfPS GS 2014:01 PAK method and analyzed by GC-MS.

[0069]

[0070] Example 2

[0071] The difference between this example and Example 1 is that kaolin is not added in the coupling reaction.

[0072] Example 3

[0073] The difference between this example and Example 1 is that no additives are added in the coupling reaction.

[0074] Example 4

[0075] The difference between this example and Example 1 is that no stearic acid and hyperdispersant are added in the S4 post-treatment to form an emulsion for coating the pigment surface.

[0076] Comparative example

[0077] The difference between this comparative example and Example 1 is that the coupling reaction does not involve the addition of kaolin and additives, and the post-processing operation of S4 is not performed; instead, a conventional pigment preparation process is used.

[0078] Pigment performance testing experiment

[0079] Color strength Particle size D50 (nm) Solvent migration resistance Heat resistance Light resistance Example 1 120 51 5 levels 200 degrees 7 levels Example 2 120 51 4 levels 200 degrees 6 levels Example 3 100 75 4 levels 180 degrees 6 levels Example 4 110 65 4 levels 200 degrees 6 levels Comparative example 88 80 3 levels 180 degrees 6 levels

[0080] It is easy to see from the above data that the pigment properties obtained in each embodiment of the present invention are significantly better than those of the comparative example. In particular, the pigment obtained in Example 1 with the help of the pre-prepared additive has the best performance. The present invention can increase the tinting strength of Pigment Red 170 in the NC system by more than 20%. In addition, it has been tested that Pigment Red 170 in each embodiment can achieve good dispersibility and a 1500-mesh pressure filtration value of less than 1 without air jet milling.

[0081] Finally, it is necessary to state that the above embodiments are only used to further illustrate the technical solution of the present invention in detail, and should not be construed as limiting the scope of protection of the present invention. Any changes, modifications, substitutions, combinations, or simplifications made by those skilled in the art without departing from the scope of the technical solution of this application using the above-disclosed technical content should be considered as equivalent substitutions and are included within the scope of protection of the present invention.

Claims

1. A method for producing an environmentally friendly pigment, Red 170, characterized in that: The method includes the following steps: S1, Diazotization reaction After diluting hydrochloric acid and acetic acid with water, add 4-aminobenzamide, i.e., red base DB-70, stir until completely dissolved, then add ice to cool to 3-6℃, and then add 20-30% sodium nitrite aqueous solution to carry out a medium diazotization reaction for 1-3 hours; the gas generated during the reaction is treated as waste gas. After the reaction is completed, add ice and water to maintain the temperature at 3-8℃ for later use. S2, Coupling reaction After diluting the alkali with water, add naphthol AS-PH, heat to 75-80℃ with high-temperature steam, stir until dissolved and transparent, add 5000kg of crushed ice and 5000L of water through the feeding port to cool to 30℃, and prepare the coupling solution for later use; Add the obtained coupling solution to the diazonium solution obtained in step S1 and carry out the coupling reaction for 0.5 to 1.0 hours. During the reaction, maintain the reaction temperature at 10-25℃ and control the pH between pH=5-5.5, and stir for 1 hour. Add kaolin, heat to 95-98℃, keep warm for 1 hour, and set aside for use; S3, Filtration, Washing The coupling product obtained in S2 is filtered by a filter press to separate the water from the obtained pigment. The wastewater generated by the filter press is sent to the sewage treatment plant for treatment. Water is added to the filter press to rinse the material until it is neutral. The wastewater generated after rinsing is sent to the sewage treatment plant for treatment. The filter cake is ready for use. S4, Post-processing Add the filter cake obtained from S3 to the reactor, add water to make up to 70-80% of the reactor volume, and pulverize for 30 minutes at a pulverizing speed of 1000-1500 rpm. Adjust the temperature according to the product color requirements, seal the reactor, raise the temperature to 110-150℃, keep it at that temperature for 2 hours, and cool it down to 60-80℃ with jacketed cooling water. S5, pressure filtration, fine washing The product obtained from S4 is filtered again by a filter press. The wastewater generated by the filter press is sent to the sewage treatment plant for treatment. Water is added to the filter press to rinse the material until it is neutral. After rinsing, the material is blown off and set aside for use. The wastewater generated after rinsing and blowing off is sent to the sewage treatment plant for treatment. S6. Drying and pulverizing The filter cake obtained from S5 is dried at a temperature of 80-85℃ for 12 hours. The gas generated during drying is treated by dust removal. The collected dust is mixed with the filter cake and then dried. The moisture content is controlled at 0.5-1.5% before drying is stopped. The collected gas is treated as waste gas. After drying, the finished pigment red 170 is obtained.

2. The production method according to claim 1, characterized in that, In step S1 of the method, 4-amino The molar ratio of benzamide, sodium nitrite and hydrochloric acid is 1:1 to 1.1:2 to 3.

3. The production method according to claim 1, characterized in that, In step S1 of the method, an emulsifier is added to the diazo solution.

4. The production method according to claim 1, characterized in that, In step S2 of the method, the molar ratio of naphthol AS-PH to sodium hydroxide is 1:1 to 2.

5. The production method according to claim 1, characterized in that, In step S2 of the method, liquid alkali or soda ash is used.

6. The production method according to claim 1, characterized in that, In step S2 of the method, the pH is adjusted by hydrochloric acid and liquid alkali, and the pH is stabilized by acetic acid.

7. The production method according to claim 1, characterized in that, In step S5 of the method, the material is rinsed until the conductivity is ≤100μs / cm.

8. The production method according to claim 1, characterized in that, In step S6 of the method, the filter cake is dried to a moisture content of ≤1.0%.

9. The production method according to claim 1, characterized in that, The dried material obtained in step S6 of the method is then subjected to ultrafine pulverization.

10. The production method according to claim 1, characterized in that, In the method, Huntsman L-207 and acetoacetanilide are kept at 85-90 degrees Celsius for 6 hours to prepare an auxiliary agent, which is added before the coupling reaction in step S2.

11. The production method according to claim 1, characterized in that, In the method described above, after the pigment is synthesized and filtered and rinsed, the filter cake is re-pulped at high speed. That is, in the post-treatment process of step S4, stearic acid and superdispersant are used to make an emulsion to coat the pigment surface.

12. The production method according to claim 11, characterized in that, The superdispersant is selected from sodium acrylate, acrylic acid-(meth)acrylic acid copolymer, and nonionic superdispersant.