Preparation method of zinc selenide 3-12 [mu] m antireflection film system
By depositing an eight-layer film system of four types of film materials, namely YbF3, ZnSe, Y2O3 and ZnS, on a zinc selenide substrate, the problem of low transmittance of zinc selenide material in the 3-12μm band was solved, achieving high transmittance and stable anti-reflection effect.
Patent Information
- Application Number
- CN202511768665.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-28
- Publication Date
- 2026-02-10
AI Technical Summary
Existing zinc selenide materials have low transmittance in the 3-12μm wavelength range, making it difficult to further improve them through antireflection coating treatment.
An eight-layer membrane system composed of four materials, YbF3, ZnSe, Y2O3 and ZnS, was used to deposit two antireflection films on a zinc selenide substrate using vacuum deposition technology. The process involved steps such as surface cleaning, baking, temperature control of the vacuum deposition machine and ion source cleaning to prepare a 3-12μm zinc selenide antireflection membrane system.
The transmittance of the zinc selenide substrate in the 2-12μm band at a 0° test angle was increased to over 94.5%, enhancing the bonding performance between the film and the substrate. The stability and durability of the film were verified through various tests.
Smart Images

Figure CN121496327A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present disclosure relates to the field of optical coating, and more particularly to a preparation method of a zinc selenide 3-12 μm antireflection film system. BACKGROUND
[0002] Zinc selenide (ZnSe) is an important infrared optical material with low absorption coefficient and high thermal shock resistance, making it an ideal choice for high-power CO2 laser systems and various infrared applications. In the field of infrared optics, zinc selenide is widely used in the manufacture of optical elements such as window materials, focusing lenses, beam splitters, and prisms due to its wide wavelength range (0.5-19 μm) of light transmission performance. Especially in the 3-12 μm mid-infrared band, which covers the atmospheric window and many molecular characteristic absorption peaks, it has irreplaceable application value in the fields of military, medical, industrial detection, etc. The uncoated zinc selenide has a transmittance of about 70% in the 3-12 μm band, and the transmittance can be further improved by antireflection film processing. SUMMARY
[0003] In view of the problems in the background art, an object of the present disclosure is to provide a preparation method of a zinc selenide 3-12 μm antireflection film system, which has an average transmittance of 94.5% or more in the 2-12 μm band at a 0° test angle for the accompanying plated sheet of the zinc selenide substrate together with the film system on both sides.
[0004] Therefore, a preparation method of a zinc selenide 3-12 μm antireflection film system includes the following steps: S0, cleaning the surface of the accompanying plated sheet and the product, wherein the accompanying plated sheet and the product are both lenses and are both zinc selenide substrates, and the accompanying plated sheet is an equal-thickness sheet; S1, placing the cleaned lenses into an oven, setting the temperature of the oven to 150℃, and baking for 2h; S2, loading the baked lenses into a tool clamp, and hanging the tool clamp loaded with the lenses into a vacuum coating machine cavity, setting the temperature of the cavity to 150℃; S3, starting vacuum pumping of the vacuum coating machine, and when the vacuum degree reaches 1.5×10 -3 Pa, opening the Hall ion source of the vacuum coating machine for cleaning, and setting the cleaning time to 6min, the parameters of the Hall ion source to anode voltage of 220V, anode current of 1.2A, neutralization current of 1.5A, neutralization gas flow of 10sccm, and argon flow ratio of 100%; S4, on the first surface of the lenses, depositing an eight-layer film system composed of YbF3, ZnSe, Y2O3, and ZnS four kinds of film materials
[0005] Sub / 100 nm YbF3 / 380.9 nm ZnSe / 270.4 nm YbF3 / 194.8 nm ZnSe / 333 nm YbF3 / 10 nm Y2O3 / 335 nm YbF3 / 60 nm ZnS / Air, each film layer is sequentially coated, wherein Sub is a zinc selenide substrate, Air is air, the numbers with nm before YbF3, ZnSe, Y2O3 and ZnS are the film thicknesses of the corresponding film layers, the YbF3 film layer, the ZnSe film layer and the ZnS film layer are coated by resistance heating evaporation, the Y2O3 film layer is coated by electron beam heating evaporation, the deposition rate of the YbF3 film layer is 0.5 nm / s, the deposition rate of the ZnSe film layer is 0.6 nm / s, the deposition rate of the Y2O3 film layer is 0.3 nm / s, and the deposition rate of the ZnS film layer is 0.4 nm / s, each film layer is deposited by ion source assisted deposition, and each film layer is deposited at a temperature of 150°C in the cavity; S5, after the film system is coated on the first surface of the lens, the cavity is naturally cooled to below 70°C, and the jig is taken out together with the lens; S6, repeating steps S0 to S5, the same film system is coated on the second surface of the lens.
[0006] The beneficial effects of the present disclosure are as follows: in the zinc selenide 3-12 μm antireflection film system preparation method according to the present disclosure, the eight-layer film system (two-surface film system constituting an antireflection film system) composed of YbF3, ZnSe, Y2O3 and ZnS four film materials on both surfaces of the lens is coated by repeating step S4 in step S4 and step S6, and combined with step S0 and repeated step S0 of step S6, step S1 and repeated step S1 of step S6, step S2 and repeated step S2 of step S6, step S3 and repeated step S3 of step S6, and step S5 and repeated step S5 of step S6, as verified by the test process described below, the average transmittance of the accompanying coating piece together with the film system on the corresponding two surfaces in the 2-12 μm wave band at a 0° test angle is above 94.5% (specifically 94.52%). BRIEF DESCRIPTION OF DRAWINGS
[0007] Figure 1 is a schematic structural diagram of a zinc selenide substrate together with the film system on both surfaces prepared according to the zinc selenide 3-12 μm antireflection film system preparation method of the present disclosure.
[0008] Figure 2 is a transmittance curve diagram of the accompanying coating piece together with the film system on both surfaces of Example 1 in the 3-12 μm wave band. DETAILED DESCRIPTION
[0009] It will be understood that the disclosed embodiments are merely examples of this disclosure, which can be implemented in various forms. Therefore, the specific details disclosed herein should not be construed as limiting, but are intended only as the basis for the claims and as an illustrative basis to teach those skilled in the art how to implement this disclosure in various ways.
[0010] [Preparation method of zinc selenide 3-12μm antireflection membrane system]
[0011] Reference Figure 1 The method for preparing the zinc selenide 3-12μm antireflection membrane system according to this disclosure includes the following steps:
[0012] S0, the surfaces of the coating sheet and the product are cleaned. The coating sheet and the product are both lenses and are zinc selenide substrates. The coating sheet is a sheet of equal thickness.
[0013] S1. Place the cleaned lenses into the oven, set the oven temperature to 150℃, and bake for 2 hours.
[0014] S2, load the baked lens into the tooling fixture, hang the tooling fixture with the lens loaded into the vacuum coating machine cavity, and set the temperature of the cavity to 150℃.
[0015] S3, the vacuum coating machine starts vacuuming, and the vacuum level reaches 1.5×10⁻⁶. -3 Pa, turn on the Hall ion source of the vacuum coating machine for cleaning. The cleaning time is 6 minutes. The parameters of the Hall ion source are: anode voltage of 220V, anode current of 1.2A, neutralization current of 1.5A, neutralization gas flow rate of 10sccm, and argon flow rate of 100%.
[0016] S4, on the first surface of the lens, is an eight-layer film system composed of four types of film materials: YbF3, ZnSe, Y2O3, and ZnS.
[0017] Sub / 100nm YbF3 / 380.9nm ZnSe / 270.4nm YbF3 / 194.8nm ZnSe / 333nm YbF3 / 10nm Y2O3 / 335nm YbF3 / 60nm ZnS / Air, each film layer was deposited sequentially.
[0018] Wherein, Sub represents the zinc selenide substrate, Air represents air, and the nm numbers preceding YbF3, ZnSe, Y2O3, and ZnS indicate the film thickness of the corresponding layer. The YbF3, ZnSe, and ZnS layers were deposited using resistance heating evaporation, while the Y2O3 layer was deposited using electron beam heating evaporation. The deposition rate of the YbF3 layer was 0.5 nm / s, the ZnSe layer was 0.6 nm / s, the Y2O3 layer was 0.3 nm / s, and the ZnS layer was 0.4 nm / s. All layers were deposited using ion source-assisted deposition, and the deposition of each layer was completed at a chamber temperature of 150°C.
[0019] S5. After the first surface of the lens is coated, the cavity is naturally cooled to below 70°C, and the tooling fixture and the lens are removed.
[0020] S6. Repeat steps S0 to S5 to deposit the same film system on the second side of the lens.
[0021] In the method for preparing the zinc selenide 3-12μm antireflection film system according to this disclosure, by repeating step S4 in steps S4 and S6, an eight-layer film system composed of four film materials, namely YbF3, ZnSe, Y2O3 and ZnS, is deposited on both sides of the lens (the two-sided film system constitutes the antireflection film system). Combined with the repeated steps S0 and S6 of surface cleaning, the repeated steps S1 of baking, the repeated steps S2 of chamber temperature, the repeated steps S3 of ion source cleaning, and the repeated steps S5 of cooling, as verified in Example 1 of the test process described later, the transmittance of the coated film together with the corresponding two-sided film system in the 2-12μm band at a 0° test angle is 94.5% or more (specifically 94.52%).
[0022] Repeating steps S0 and S6, the surface cleaning in step S0 helps improve the surface condition of each surface of the lens and improves the adhesion between the coating system on each surface and the corresponding surface of the lens. For example, in step S0, the surface of the lens is cleaned using ultrasound or by hand. Further, for example, in step S0, the surface cleaning of the lens using ultrasound involves polishing with an alumina polishing slurry followed by ultrasonic rinsing with pure water. For example, the alumina polishing slurry used is a 0.1μm polycrystalline diamond slurry from Nanjing Hengrui Precision Optics Co., Ltd.
[0023] In step S0, for example, the product is a lens or a flat sheet.
[0024] In step S0, for example, the thickness of the substrate is 1 mm. For example, the substrate is a disc.
[0025] The baking process in step S1 helps to remove stress from the lens.
[0026] The temperature setting of the vacuum coating machine in step S2 heats the lens through the cavity of the coating machine, which helps the film to grow from the lens and reduces the stress of film growth.
[0027] Step S3 uses a Hall ion source for cleaning, which removes impurities and oil molecules adsorbed on the surface of each surface of the lens, significantly improving the interface state and enhancing the adhesion between the film and the corresponding surfaces of the lens. Simultaneously, cleaning with a Hall ion source heats the corresponding surfaces of the lens, aiding in film growth and reducing growth stress. For example, the vacuum coating machine is a Hall ion source with a neutralizer manufactured and sold by Chengdu Xiwoke Vacuum Technology Co., Ltd., and the Hall ion source with the neutralizer was purchased from Boton Optoelectronics Technology Co., Ltd.
[0028] In step S4, in one example, a Hall ion source is used. When depositing the YbF3 film, the ion source parameters are: neutralization current of 0.6A, neutralization gas flow rate of 8sccm, anode voltage of 130V, anode current of 1.3A, argon flow rate ratio of 30%, and oxygen flow rate ratio of 70%. When depositing the ZnSe and ZnS films, the ion source parameters are: neutralization current of 0.5A, neutralization gas flow rate of 8sccm, anode voltage of 90V, anode current of 1.0A, and argon flow rate ratio of 100%. When depositing the Y2O3 film, the ion source parameters are: neutralization current of 0.5A, neutralization gas flow rate of 8sccm, anode voltage of 100V, anode current of 1.2A, and argon flow rate ratio of 100%.
[0029] In step S4, in one example, argon gas is introduced and a vacuum is drawn during the deposition of each film layer to maintain a flow-through constant vacuum. The flow-through constant vacuum setting is not lower than 5.0 × 10⁻⁶. -3 Pa; The crystal oscillator method is used to monitor the film thickness by using the corresponding crystal oscillators of multiple crystal oscillators in the crystal controller. After cleaning with the ion source, the crystal controller controls the new crystal oscillator in the multiple crystal oscillators to work accordingly. The crystal oscillator frequency is not less than 5.99MHz.
[0030] In one example, after step S6, the average transmittance of the substrate and the corresponding films on both sides in the 0° test angle 2-12μm band is above 94.5%; after step S6, the substrate and the films on both sides pass the water immersion test, salt spray test, adhesion test, thermal shock test, constant temperature and humidity test, abrasion resistance test, low temperature test, and high temperature test.
[0031] [test]
[0032] Example 1
[0033] Example 1 uses the following steps:
[0034] S0, the surfaces of the coating sheet and the product are cleaned. The coating sheet and the product are both zinc selenide substrates. The product is a lens. The coating sheet is a sheet of equal thickness with a thickness of 2mm and is a circular sheet. The surface of the lens is cleaned by ultrasonic cleaning. The ultrasonic cleaning process involves polishing with an alumina polishing solution followed by ultrasonic cleaning with pure water. The alumina polishing solution used is 0.1μm polycrystalline diamond solution from Nanjing Hengrui Precision Optics Co., Ltd.
[0035] S1. Place the cleaned lenses into the oven, set the oven temperature to 150℃, and bake for 2 hours.
[0036] S2, load the baked lens into the tooling fixture, hang the tooling fixture with the lens loaded into the vacuum coating machine cavity, and set the temperature of the cavity to 150℃. The vacuum coating machine is a vacuum coating machine with a Hall ion source equipped with a neutralizer manufactured and sold by Chengdu Xiwoke Vacuum Technology Co., Ltd. The Hall ion source equipped with a neutralizer was purchased from Boton Optoelectronics Technology Co., Ltd.
[0037] S3, the vacuum coating machine starts vacuuming, and the vacuum level reaches 1.5×10⁻⁶. -3 Pa, turn on the Hall ion source of the vacuum coating machine for cleaning. The cleaning time is 6 minutes. The parameters of the Hall ion source are: anode voltage of 220V, anode current of 1.2A, neutralization current of 1.5A, neutralization gas flow rate of 10sccm, and argon flow rate of 100%.
[0038] S4, on the first surface of the lens, is an eight-layer film system composed of four types of film materials: YbF3, ZnSe, Y2O3, and ZnS.
[0039] Sub / 100nm YbF3 / 380.9nm ZnSe / 270.4nm YbF3 / 194.8nm ZnSe / 333nm YbF3 / 10nm Y2O3 / 335nm YbF3 / 60nm ZnS / Air, each film layer was deposited sequentially.
[0040] Wherein, Sub represents the zinc selenide substrate, Air represents air, and the nm numbers preceding YbF3, ZnSe, Y2O3, and ZnS indicate the film thickness of the corresponding layer. The YbF3, ZnSe, and ZnS layers were deposited using resistance heating evaporation, while the Y2O3 layer was deposited using electron beam heating evaporation. The deposition rate of the YbF3 layer was 0.5 nm / s, the ZnSe layer was 0.6 nm / s, the Y2O3 layer was 0.3 nm / s, and the ZnS layer was 0.4 nm / s. All layers were deposited using ion source-assisted deposition, and the deposition of each layer was completed at a chamber temperature of 150°C.
[0041] S5. After the first surface of the lens is coated, the cavity is naturally cooled to 70°C, and the tooling fixture and the lens are removed.
[0042] S6. Repeat steps S0 to S5 to deposit the same film system on the second side of the lens.
[0043] In step S4,
[0044] The ion source used is a Hall ion source.
[0045] When depositing the YbF3 film, the ion source parameters are as follows: neutralization current is 0.6A, neutralization gas flow rate is 8sccm, anode voltage is 130V, anode current is 1.3A, argon flow rate accounts for 30%, and oxygen flow rate accounts for 70%.
[0046] When depositing ZnSe and ZnS films, the ion source parameters are as follows: neutralization current is 0.5A, neutralization gas flow rate is 8sccm, anode voltage is 90V, anode current is 1.0A, and argon flow rate is 100%.
[0047] When depositing the Y₂O₃ film, the ion source parameters were as follows: neutralization current 0.5 A, neutralization gas flow rate 8 sccm, anode voltage 100 V, anode current 1.2 A, and argon flow rate percentage 100%. During the deposition of each film layer, argon gas was introduced and a vacuum was evacuated to maintain a constant flow vacuum, set to 5.0 × 10⁻⁶. -3 Pa;
[0048] The crystal oscillator method is used to monitor the film thickness by using the corresponding crystal oscillators of multiple crystal oscillators in the crystal controller. After cleaning with the ion source, the crystal controller controls the new crystal oscillator in the multiple crystal oscillators to work accordingly, and the crystal oscillator frequency is not less than 5.99MHz.
[0049] Figure 2 This is a transmittance curve of the substrate and the films on both sides of Example 1 in the 3-12 μm wavelength range. From... Figure 2It can be seen that after step S6 is completed, the average transmittance of the substrate and the corresponding film system on both sides in the 0° test angle 2-12μm band is 94.52% (i.e. above 94.5%).
[0050] The following tests were performed on both sides of the substrate in Example 1 after it was coated.
[0051] Water immersion test: Take tap water and conduct a water immersion test for 2 hours. Observe whether the film layer on each surface of the substrate is peeled off from the substrate and whether the film layer on each surface of the substrate is cracked.
[0052] Salt spray test: Neutral salt spray test for 48 hours, observe whether the film layer on each surface of the substrate peels off, and observe whether the film layer on each surface of the substrate cracks.
[0053] Adhesion test: Apply 3M tape to each side of the coated sheet by hand and pull the tape in the opposite direction to the adhesive end. Observe whether the film layer is pulled up.
[0054] Thermal shock test: The film is subjected to thermal shock in the range of -40℃ to 85℃ for 24 hours in a high and low temperature chamber. Observe whether the film layer on each surface of the substrate is peeled off and whether the film layer on each surface of the substrate is cracked.
[0055] Constant temperature and humidity test: In a constant temperature and humidity chamber, at 50℃ and 95% relative humidity for 48 hours, observe whether the film layer on each surface of the substrate peels off and whether the film layer on each surface of the substrate cracks.
[0056] Friction resistance test (medium friction test): Wrap the rubber friction head of the rubber with degreased cloth and apply a pressure of 4.9N to the film surface of the coated sheet for 50 cycles (25 back and forth). Observe whether there are scratches or signs of damage on the film surface.
[0057] Low temperature test: In a low temperature chamber, at -40℃ for 48 hours, observe whether the film layer on each surface of the substrate peels off and whether the film layer on each surface of the substrate cracks.
[0058] High temperature test: In a high temperature chamber, at 85℃ for 48 hours, observe whether the film layer on each surface of the substrate peels off and whether the film layer on each surface of the substrate cracks.
[0059] In the water immersion test, salt spray test, thermal shock test, constant temperature and humidity test, low temperature test, and high temperature test, the film layer did not peel off or crack; in the adhesion test, the film layer was not pulled up; in the abrasion resistance test, there were no signs of scratch damage on the film layer surface, i.e., it can withstand moderate abrasion. In other words, the substrate of Example 1, together with the film system on both sides, passed a total of eight tests, including the water immersion test, salt spray test, adhesion test, thermal shock test, constant temperature and humidity test, abrasion resistance test, low temperature test, and high temperature test.
[0060] Several exemplary embodiments have been described in detail above, but this document is not intended to limit itself to the explicitly disclosed combinations. Therefore, unless otherwise stated, the various features disclosed herein can be combined to form several other combinations, which are not shown for simplicity.
Claims
1. A method for preparing a zinc selenide 3-12μm antireflection membrane system, characterized in that, Including the following steps: S0, the surfaces of the coating sheet and the product are cleaned. The coating sheet and the product are both lenses and are zinc selenide substrates. The coating sheet is a sheet of equal thickness. S1. Place the cleaned lenses into the oven, set the oven temperature to 150℃, and bake for 2 hours. S2, load the baked lens into the tooling fixture, hang the tooling fixture with the lens loaded into the vacuum coating machine cavity, and set the temperature of the cavity to 150℃. S3, the vacuum coating machine starts pumping vacuum, and the vacuum level reaches 1.5×10. -3 Pa, turn on the Hall ion source of the vacuum coating machine for cleaning. The cleaning time is 6 minutes. The parameters of the Hall ion source are: anode voltage of 220V, anode current of 1.2A, neutralization current of 1.5A, neutralization gas flow rate of 10sccm, and argon flow rate of 100%. S4, on the first surface of the lens, is an eight-layer film system composed of four types of film materials: YbF3, ZnSe, Y2O3, and ZnS. Sub / 100nm YbF3 / 380.9nm ZnSe / 270.4nm YbF3 / 194.8nm ZnSe / 333nm YbF3 / 10nm Y2O3 / 335nm YbF3 / 60nm ZnS / Air, each film layer was deposited sequentially. Wherein, Sub represents the zinc selenide substrate, Air represents air, and the nm numbers preceding YbF3, ZnSe, Y2O3, and ZnS indicate the film thickness of the corresponding layer. The YbF3, ZnSe, and ZnS layers were deposited using resistance heating evaporation, while the Y2O3 layer was deposited using electron beam heating evaporation. The deposition rate of the YbF3 layer was 0.5 nm / s, the ZnSe layer was 0.6 nm / s, the Y2O3 layer was 0.3 nm / s, and the ZnS layer was 0.4 nm / s. All layers were deposited using ion source-assisted deposition, and the deposition of each layer was completed at a chamber temperature of 150°C. S5. After the coating system is applied to the first surface of the lens, the cavity is naturally cooled to below 70°C, and the tooling fixture is removed along with the lens. S6. Repeat steps S0 to S5 to deposit the same film system on the second side of the lens.
2. The method for preparing the zinc selenide 3-12μm antireflection membrane system according to claim 1, characterized in that, In step S0, the surface of the lens is cleaned using ultrasound or by hand.
3. The method for preparing the zinc selenide 3-12μm antireflection membrane system according to claim 2, characterized in that, In step S0, the surface cleaning treatment of the lens is performed by polishing with an alumina polishing liquid followed by ultrasonic cleaning with pure water.
4. The method for preparing the zinc selenide 3-12μm antireflection membrane system according to claim 3, characterized in that, In step S0, the alumina polishing slurry is a 0.1μm polycrystalline diamond slurry.
5. The method for preparing the zinc selenide 3-12μm antireflection membrane system according to claim 1, characterized in that, In step S0, the product is a lens or a flat sheet.
6. The method for preparing the zinc selenide 3-12μm antireflection membrane system according to claim 1, characterized in that, In step S0, the thickness of the substrate is 2 mm.
7. The method for preparing the zinc selenide 3-12μm antireflection membrane system according to claim 1, characterized in that, In step S4, The ion source used is a Hall ion source. When depositing the YbF3 film, the ion source parameters are as follows: neutralization current is 0.6A, neutralization gas flow rate is 8sccm, anode voltage is 130V, anode current is 1.3A, argon flow rate accounts for 30%, and oxygen flow rate accounts for 70%. When depositing ZnSe and ZnS films, the ion source parameters are as follows: neutralization current is 0.5A, neutralization gas flow rate is 8sccm, anode voltage is 90V, anode current is 1.0A, and argon flow rate is 100%. When depositing the Y2O3 film, the ion source parameters are as follows: neutralization current is 0.5A, neutralization gas flow rate is 8sccm, anode voltage is 100V, anode current is 1.2A, and argon flow rate is 100%.
8. The method for preparing the zinc selenide 3-12μm antireflection membrane system according to claim 1, characterized in that, In step S4, Argon gas is introduced and a vacuum is drawn during the deposition of each film layer to maintain a constant flow vacuum. The constant flow vacuum setting is not lower than 5.0 × 10⁻⁶. -3 Pa; The crystal oscillator method is used to monitor the film thickness by using the corresponding crystal oscillators of multiple crystal oscillators in the crystal controller. After cleaning with the ion source, the crystal controller controls the new crystal oscillator in the multiple crystal oscillators to work accordingly, and the crystal oscillator frequency is not less than 5.99MHz.
9. The method for preparing the zinc selenide 3-12μm antireflection membrane system according to claim 1, characterized in that, After step S6 is completed, the average transmittance of the substrate and the corresponding film system on both sides in the 0° test angle 2-12μm band is above 94.5%. After step S6 is completed, the substrate and the film system on both sides are subjected to water immersion test, salt spray test, adhesion test, thermal shock test, constant temperature and humidity test, abrasion resistance test, low temperature test and high temperature test.