Electrolyte additive as well as preparation method and application thereof

By using compounded electrolyte additives to form a highly ionicly conductive and mechanically stable interface film, the problem of instability of existing additives under high temperature and high rate conditions is solved, improving the fast charging performance and battery life of lithium-ion batteries, and enhancing the chemical stability and safety of the electrolyte.

CN122025813APending Publication Date: 2026-05-12XIAOGAN CORNEX NEW ENERGY INNOVATION TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610227623.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-02-26
Publication Date
2026-05-12

AI Technical Summary

Technical Problem

Existing lithium-ion battery additives are unstable under high temperature and high rate conditions, and are prone to hydrolysis, which leads to an increase in electrolyte acidity and color changes, affecting battery performance and safety, and failing to meet the requirements of fast charging.

Method used

By using a compound of vinylene carbonate, fluoroethylene carbonate, 1,3-propanesulfonate lactone and thiophosphate silane additives, active elements such as silicon, phosphorus and sulfur are introduced through molecular design to form an interface film with high ionic conductivity and mechanical stability, which captures moisture and fluoride ions and inhibits the increase of acidity and color change.

Benefits of technology

It improves the fast-charging performance and lifespan of lithium-ion batteries, forms a dense interface film, suppresses side reactions, enhances the chemical stability and safety of the battery, and extends battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_8
    Figure SMS_8
  • Figure SMS_9
    Figure SMS_9
  • Figure SMS_10
    Figure SMS_10
Patent Text Reader

Abstract

The invention relates to the technical field of battery materials, in particular to an electrolyte additive and a preparation method and application thereof. And the electrolyte additive comprises vinylene carbonate, fluoroethylene carbonate, 1, 3-propane sultone and a sulfur phosphoric acid silane additive. The sulfur-phosphoric acid silane additive is prepared by reacting hexamethyldisilazane with ammonium dihydrogen phosphate and then condensing with a sulfonyl chloride intermediate containing an R group at a low temperature, and the sulfur-phosphoric acid silane additive is compounded with other components according to a specific mass ratio and then is used in the lithium ion battery electrolyte. The electrolyte additive can form a high-conductivity lithium protective film rich in LiF and LiSxOy on an electrode interface, so that the ion transmission capability and stability of the interface are remarkably improved; and meanwhile, the P-O-Si structure can capture trace water, inhibit the generation of HF and effectively control the acidity and chromaticity change of the electrolyte. The additive disclosed by the invention is particularly suitable for a fast-charging type lithium ion battery, and ensures the long-acting stability of the electrolyte while prolonging the cycle life, improving the high-temperature storage performance and improving the rate characteristic.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery materials technology, specifically to an electrolyte additive, its preparation method, and its application. Background Technology

[0002] With the global energy structure transformation and the rapid development of the electric vehicle industry, lithium-ion batteries, as a core power source, directly affect the vehicle's range, safety, reliability, and lifespan. Among various cathode materials, lithium iron phosphate (LFP) has become one of the most widely used material systems in the new energy vehicle field due to its excellent thermal stability, cycle life, and cost advantages. Especially in passenger vehicles and energy storage scenarios where safety requirements are extremely high, LFP batteries have shown significant advantages. However, in contrast to its excellent safety performance, the mass energy density and volumetric energy density of LFP batteries are lower than those of high-nickel ternary systems, resulting in a bottleneck in improving the overall vehicle range. Range anxiety has become one of the key factors restricting its further market expansion.

[0003] To alleviate range anxiety, the industry is focusing on improving charging efficiency and driving the development of fast charging technology. Fast charging not only requires batteries to support high-rate charging and discharging, but also places more stringent demands on the stability and interface control of the electrolyte system. As the medium for lithium ion transport between the positive and negative electrodes, the composition of the electrolyte directly affects the battery's high-rate performance, cycle life, and storage stability. In practical applications, various functional additives are often introduced to optimize the electrode / electrolyte interface, forming a stable solid electrolyte interphase (SEI) film, suppressing side reactions, improving ionic conductivity, and enhancing the thermal and chemical stability of the electrolyte itself.

[0004] Currently, additives commonly used to improve fast-charging performance mainly include sulfate-containing compounds, such as vinyl sulfate (DTD) and methylene disulfonate (MMDS). These additives can participate in interfacial film formation during battery cycling, improving lithium-ion migration kinetics. However, the sulfur-oxygen-carbon bonds in their molecular structure are highly polar, easily reacting with trace amounts of residual moisture in the electrolyte. This not only leads to the additive's own decomposition and inactivation but also continuously releases acidic substances, causing the electrolyte acidity to gradually increase. After long-term storage, the electrolyte often changes from its initial clear and transparent state to brownish-yellow, which is not only an appearance issue but also indicates that the electrolyte system has undergone irreversible chemical changes. Increased acidity accelerates the corrosion of electrode active materials, damages the integrity of the SEI film, increases battery internal resistance, reduces capacity retention and cycle life, and in severe cases, may even lead to battery performance degradation or even safety hazards.

[0005] Furthermore, the stability of existing additives under high-temperature and high-rate conditions is insufficient. During fast charging, batteries experience significant localized heat generation. If the decomposition products of the additives cannot form a dense interfacial film with excellent lithium conductivity, it will exacerbate problems such as uneven lithium deposition and dendrite growth, affecting battery safety and long-term cycle life. Therefore, developing a novel additive that can adapt to fast-charging systems while maintaining the long-term chemical stability and interfacial compatibility of the electrolyte has become an important research direction for improving the overall performance of LFP batteries. Summary of the Invention

[0006] Against this backdrop, the present invention aims to provide an electrolyte additive, its preparation method, and its application. By introducing multiple active elements such as silicon, phosphorus, and sulfur into the molecular design, it enables the additive to perform multiple functions inside the battery: it can participate in the construction of an inorganic interface film with high ionic conductivity and high mechanical stability, thereby improving lithium-ion migration efficiency; and it can effectively suppress the rise in electrolyte acidity and color changes through the capture mechanism of water and fluoride ions, thereby enhancing the chemical stability of the system during storage and cycling. Thus, it provides a high-performance, long-life electrolyte solution for high-rate fast-charging lithium-ion batteries.

[0007] To achieve the above objectives, the present invention is implemented through the following technical solution: In a first aspect, the present invention provides an electrolyte additive comprising vinylene carbonate, fluorovinyl carbonate, 1,3-propanesulfonate lactone, and a thiophosphate silane additive, wherein the thiophosphate silane additive comprises compounds having the structure shown in the following formula: ; R is selected from one of C1 to C6 alkyl, nitrile, or benzene ring.

[0008] In a preferred embodiment of the present invention, R in the structure of the thiophosphate silane additive is a nitrile group. Functionally, the nitrile group is more effective, as it can complex with metal ions, prevent metal ion leakage, reduce SEI side reactions on the negative electrode surface, and improve the loss of active material.

[0009] As a preferred embodiment of the present invention, the thiophosphate silane additive includes at least one of additive A, additive B, or additive C having the structure shown in the following formula: Additive A: ; Additive B: ; Additive C: .

[0010] As a preferred embodiment of the present invention, the mass ratio of vinylene carbonate, fluorovinyl carbonate, 1,3-propanesulfonate lactone and thiophosphate silane additive is (3-5):(0.5-2):(0.1-0.8):(0.1-3).

[0011] Secondly, the present invention provides a method for preparing the electrolyte additive, comprising the following steps: S1: Under an inert atmosphere, hexamethyldisilazane reacts with ammonium dihydrogen phosphate to generate intermediate I; S2: Under low temperature conditions, an alcohol or phenolic compound containing the target R group is reacted with chlorosulfonic acid to generate intermediate II; S3: Under inert atmosphere and low temperature conditions, intermediate II is added dropwise to the solution of intermediate I and reacted, and then post-processed to obtain thiophosphate silane additives. S4: The electrolyte additive is obtained by mixing vinylene carbonate, fluorovinyl carbonate, 1,3-propanesulfonate lactone and thiophosphate silane additives in a preset ratio.

[0012] As a preferred embodiment of the present invention, in step S1, the molar ratio of hexamethyldisilazane to ammonium dihydrogen phosphate is 1:(2-4), the reaction temperature is 90-150°C, and the reaction time is 3-8h; And / or, in step S2, the alcohol or phenolic compound containing the target R group is n-butanol, ethylene nitrile, or phenol, and the molar ratio of the alcohol or phenolic compound containing the target R group to chlorosulfonic acid is 1:(0.8-1.3). And / or, in step S3, the molar ratio of intermediate II to intermediate I is (0.8-1.2):1, the low temperature is an ice bath condition, and the reaction time is 3-6 hours.

[0013] Thirdly, the present invention provides a lithium-ion battery electrolyte, comprising, by mass fraction of 100%, the following components by mass fraction: 11-15% lithium salt, 80-85% organic solvent and 2-9% electrolyte additive; wherein the electrolyte additive is the electrolyte additive described above.

[0014] As a preferred embodiment of the present invention, the lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, and lithium difluorooxalate borate.

[0015] As a preferred embodiment of the present invention, the organic solvent includes at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, and ethyl acetate.

[0016] Fourthly, the present invention provides a lithium-ion battery comprising the aforementioned lithium-ion battery electrolyte.

[0017] Compared with the prior art, the beneficial effects of the present invention include: 1. The thiophosphate silane additive synthesized in this invention contains both phosphosilane groups and sulfonic acid groups in its molecule, and is modified by optional functional R groups such as nitrile groups. This structural design allows the additive to simultaneously perform the following functions in the battery: the sulfonic acid groups participate in the formation of a dense and LiSxOy-rich inorganic interface film on the negative electrode surface. This film has excellent lithium-ion conductivity and electrochemical stability, which is beneficial for high-speed lithium-ion transport and meets the requirements of fast charging. Compared with the SOP bond structure, the PO-Si bond has high polarity and is more sensitive to polar H2O molecules. It can actively capture trace amounts of water in the electrolyte and convert them into stable silanols and phosphoric acid substances, thereby effectively suppressing the problem of electrolyte acidity increase and discoloration caused by hydrolysis and improving the storage stability of the electrolyte. The silicon group has a good affinity for fluoride ions and can bind free F in the electrolyte. - This reduces the formation of corrosive HF and promotes the formation of a LiF protective layer at the interface, further enhancing the ionic conductivity and mechanical stability of the interfacial film. When the R group is a nitrile group, its strong metal ion complexing ability can further stabilize the interface, reduce metal ion dissolution, and protect the SEI film structure of the negative electrode.

[0018] 2. The electrolyte additive of this invention is not a single component, but is a compound of vinylene carbonate (VC), fluoroethylene carbonate (FEC), 1,3-propanesulfonate lactone (PS), and the aforementioned thiophosphate silane additives in a specific mass ratio. This combination exerts a synergistic effect: VC and FEC are recognized as excellent film-forming agents, which can preferentially form the basic framework of the organic-inorganic composite SEI film at the negative electrode. The thiophosphate silane additives further modify and strengthen the interfacial film on the basis of the already formed film, injecting highly lithium-conducting inorganic components (such as LiF, LiSxOy), and removing harmful factors (H2O, HF) in the system. The specific ratio (e.g., (3~5):(0.5~2):(0.1~0.8):(0.1~3)) ensures the effective functioning and balance of each component, avoiding the increase in impedance or side reactions that may be caused by an excess of a certain component. Detailed Implementation

[0019] To enable those skilled in the art to better understand the technical solutions of the present invention, the preferred embodiments of the present invention are described below in conjunction with specific examples. However, these should not be construed as limiting the present invention and are merely examples.

[0020] Unless otherwise specified, the test methods or experimental methods described in the following examples are conventional methods; unless otherwise specified, the reagents and materials are obtained from conventional commercial sources or prepared by conventional methods.

[0021] This invention provides an electrolyte additive comprising vinylene carbonate, fluoroethylene carbonate, 1,3-propanesulfonate lactone, and thiophosphate silane additives, wherein the thiophosphate silane additives comprise compounds having the structure shown in the following formula: ; R is selected from one of C1 to C6 alkyl, nitrile, or benzene ring.

[0022] In a preferred embodiment of the present invention, the thiophosphate silane additive includes at least one of additive A, additive B, and additive C having the following structures: Additive A: ; Additive B: ; Additive C: The preparation methods for additives A, B, and C can be further specified.

[0023] As an optional embodiment of the present invention, additive A can be prepared by the following method: Under nitrogen protection, 0.1 mol of hexamethyldisilazane and 0.3 mol of ammonium dihydrogen phosphate were added to toluene solvent and heated to 120 °C. The mixture was kept at this temperature for 5 h to obtain the intermediate bis(trimethyl)silyl phosphate. Under ice bath conditions, 0.1 mol of n-butanol was dissolved in dichloromethane, and 0.1 mol of chlorosulfonic acid was slowly added to the mixed solvent and stirred for 3 h to obtain the intermediate n-butylsulfonyl chloride. Under nitrogen protection and ice bath conditions, 0.1 mol of n-butylsulfonyl chloride was slowly added dropwise to a 0.1 mol bis(trimethyl)silyl phosphate-tetrahydrofuran solution and the reaction was continued for 4 h. After filtration and purification, additive A was obtained.

[0024] As an optional embodiment of the present invention, additive B can be prepared by the following method: Under nitrogen protection, 0.1 mol of hexamethyldisilazane and 0.3 mol of ammonium dihydrogen phosphate were added to toluene solvent and heated to 120 °C. The mixture was kept at this temperature for 5 h to obtain the intermediate bis(trimethyl)silyl phosphate. Under ice bath conditions, 0.1 mol of oxonium was dissolved in dichloromethane, and 0.1 mol of chlorosulfonic acid was slowly added to the mixed solvent and stirred for 3 h to obtain the intermediate nitrile methanesulfonyl chloride. Under nitrogen protection and ice bath conditions, 0.1 mol of nitrile methanesulfonyl chloride was slowly added dropwise to a 0.1 mol bis(trimethyl)silyl phosphate-tetrahydrofuran solution and the reaction was continued for 4 h. After filtration and purification, additive B was obtained.

[0025] As an optional embodiment of the present invention, additive C can be prepared by the following method: Under nitrogen protection, 0.1 mol of hexamethyldisilazane and 0.3 mol of ammonium dihydrogen phosphate were added to toluene solvent and heated to 120 °C. The mixture was kept at this temperature for 5 h to obtain the intermediate bis(trimethyl)silyl phosphate. Under ice bath conditions, 0.1 mol of phenol was dissolved in dichloromethane, and 0.13 mol of chlorosulfonic acid was slowly added to the mixed solvent and stirred for 3 h to obtain the intermediate benzenesulfonyl chloride. Under nitrogen protection and ice bath conditions, 0.1 mol of benzenesulfonyl chloride was slowly added dropwise to a 0.1 mol bis(trimethyl)silyl phosphate-tetrahydrofuran solution and the reaction was continued for 4 h. After filtration and purification, additive C was obtained.

[0026] In addition to optimizing the specific types of thiophosphate silane additives mentioned above, there are also certain limitations on the dosage of each component of the electrolyte additive.

[0027] As an optional embodiment of the present invention, the mass ratio of vinylene carbonate, fluorovinyl carbonate, 1,3-propanesulfonate lactone and thiophosphate silane additive is (3-5):(0.5-2):(0.1-0.8):(0.1-3).

[0028] The present invention will now be described in further detail with reference to specific embodiments and comparative examples.

[0029] Example 1 This embodiment provides a lithium-ion battery electrolyte: It consists of organic solvents, lithium salts, and electrolyte additives. The organic solvents comprise 78% and are composed of ethylene carbonate, propylene carbonate, dimethyl carbonate, methyl ethyl carbonate, and ethyl acetate, with ethyl acetate accounting for over 30%. The lithium salts comprise 13.5% and are composed of lithium hexafluorophosphate, lithium difluorosulfonylimide, and lithium difluorooxalate borate, with lithium hexafluorophosphate accounting for over 70%. The electrolyte additives comprise 8.5% and are composed of 4.5% vinylene carbonate, 2% fluoroethylene carbonate, 0.5% 1,3-propanesulfonate lactone, and additive A, with additive A comprising 1.5%.

[0030] Example 2 This embodiment provides a lithium-ion battery electrolyte: The electrolyte additive A in Example 1 was replaced with electrolyte additive B, and all other conditions were the same as in Example 1.

[0031] Example 3 This embodiment provides a lithium-ion battery electrolyte: Electrolyte additive A in Example 1 was replaced with electrolyte additive C, and all other conditions were the same as in Example 1.

[0032] Example 4 This embodiment provides a lithium-ion battery electrolyte: The content of electrolyte additive B in Example 2 was increased by 0.5%, and all other conditions were the same as in Example 2.

[0033] Example 5 This embodiment provides a lithium-ion battery electrolyte: The content of electrolyte additive B in Example 2 was reduced by 0.5%, while all other conditions remained the same as in Example 2.

[0034] Comparative Example 1 This comparative example provides a lithium-ion battery electrolyte, in which the electrolyte additive of Example 2 is replaced with DTD, and all other conditions are the same as in Example 2.

[0035] Comparative Example 2 This comparative example provides a lithium-ion battery electrolyte, in which the electrolyte additive of Example 2 is replaced with MMDS, and all other conditions are the same as in Example 2.

[0036] Comparative Example 3 This comparative example provides a lithium-ion battery electrolyte, in which the electrolyte additives of Example 2 are replaced with DTD+TMSP, and the mass ratio of DTD to TMSP (tris(trimethylsilane)phosphate) is 2:1. All other conditions are the same as in Example 2.

[0037] Comparative Example 4 This comparative example provides a lithium-ion battery electrolyte, in which the electrolyte additives of Example 2 are replaced with MMDS+TMSP, the mass ratio of MMDS to TMSP is 2:1, and all other conditions are the same as in Example 2.

[0038] Experimental Example The lithium-ion battery electrolytes prepared in the above embodiments and comparative examples were used to fabricate soft-pack lithium-ion batteries using a pouch stacking process. The specific assembly and testing methods are as follows: The LFP positive electrode, graphite negative electrode and polyethylene separator are stacked and assembled, and then baked until the moisture content is qualified. The electrolyte of the example or comparative example is injected, and after hot pressing formation, high temperature standing and encapsulation, after capacity testing and standing at room temperature, the soft pack finished battery is obtained.

[0039] The test method for 4SC 1000cls@25℃ is as follows: at 25℃, charge at an average of 4C, discharge at a constant current of 1C, and cycle for 1000cls. The test method for 2SC 1000cls@45℃ is as follows: at 45℃, charge at an average of 2C, discharge at a constant current of 1C, and cycle for 1000cls. The test method for 65℃ 30D retention rate is as follows: at 65℃, after the battery is stored at 100% SOC for 30D, the first full discharge capacity is divided by the full discharge capacity before storage. The test method for 65℃ 30D recovery rate is as follows: at 65℃, after the battery is stored at 100% SOC for 30D, the first full charge and discharge capacity is divided by the full discharge capacity before storage. The test method for 25℃ 2C 30s DCR@50% SOC is as follows: at 25℃, with the battery at 50% SOC, perform a 2C rate constant current discharge for 30 seconds. The test method for initial efficiency is: first discharge capacity divided by first charge capacity. The test method for acidity (ppm) at 25℃ storage is: titration to determine HF content. The test method for color change at 25℃ storage is: visual inspection.

[0040] Table 1 Table 2 Based on the performance test data from Examples 1-5, Comparative Examples 1-4, and Tables 1 and 2, the following conclusions can be drawn: In the tests of 1000 cycles at 4SC@25℃ and 1000 cycles at 2SC@45℃, the capacity retention rates (≥94.1%) of all Examples 1-5 using the thiophosphate silane additive of this invention were significantly higher than those of Comparative Examples 1-4 using conventional additives (≤93.7%). Example 2 (containing additive B, where R is a nitrile group) showed the best performance, indicating that the nitrile structure has an advantage in improving high-rate cycling stability, with stronger complexation ability with metal ions, which helps stabilize the interface and reduce side reactions. Furthermore, the amount of additive B in Example 2 was optimal compared to Examples 4 and 5.

[0041] In a 30-day storage test at 65°C, the capacity retention rate (86.4%~87.0%) and recovery rate (88.6%~89.1%) of the example group were superior to or equivalent to those of the comparative group. This indicates that the additive can effectively maintain electrode interface stability and suppress capacity decay even at high temperatures. In a DC internal resistance test at 25°C, 50% SOC, and 30 seconds of 2C discharge, the DCR value of the example group (30.6~31.5) was significantly lower than that of comparative example 1 (35.6) and comparative example 2 (36.1). This demonstrates that the additive of the present invention helps to form an interface film with high ionic conductivity and improves lithium-ion transport kinetics.

[0042] As shown in Table 2, after storage at 25°C for 30 days, the acidity of the example group only increased slightly (e.g., from 50 ppm to 59 ppm in Example 2), and the electrolyte remained clear and transparent throughout. Compared with traditional sulfate ester additives (which are easily hydrolyzed, leading to increased acidity and yellowing of the liquid), the additive of the present invention exhibits excellent hydrolytic stability and chemical inertness.

[0043] Comparative Examples 1-2 (pure DTD or MMDS) showed poor performance in terms of cycle life, internal resistance, and acidity control. Comparative Examples 3-4 (DTD / MMDS+TMSPS) showed some improvement, but still lagged behind the additives of this invention (such as in Example 2), indicating that intramolecular synergistic design is more advantageous than physical mixing. The initial charge-discharge efficiency of all examples was between 90.1% and 90.5%, indicating that this type of additive does not affect the initial film formation and lithium loss of the battery, demonstrating good compatibility.

[0044] In summary, the thiophosphate silane additives described in this invention, especially those with R being a nitrile group, have significant advantages in improving the fast-charging performance, high-temperature stability, and interfacial kinetics of lithium-ion batteries (especially LFP systems). Simultaneously, they effectively suppress the increase in acidity and color changes of the electrolyte during storage, solving the problems of easy hydrolysis and instability associated with traditional sulfate ester additives, and possess promising prospects for industrial application.

[0045] The above are merely preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be considered as limitations on the present invention, and the scope of protection of the present invention should be determined by the scope defined in the claims. For those skilled in the art, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. An electrolyte additive, characterized in that, This includes vinylene carbonate, fluorovinyl carbonate, 1,3-propanesulfonate lactone, and thiophosphate silane additives, wherein the thiophosphate silane additives include compounds having the structure shown below: ; R is selected from one of C1 to C6 alkyl, nitrile, or benzene ring.

2. The electrolyte additive according to claim 1, characterized in that, In the structure of the thiophosphate silane additive, R is a nitrile group.

3. The electrolyte additive according to claim 1, characterized in that, The thiophosphate silane additives include at least one of additive A, additive B, or additive C having the structure shown in the following formula: Additive A: ; Additive B: ; Additive C: 。 4. The electrolyte additive according to claim 1, characterized in that, The mass ratio of the vinylene carbonate, fluorovinyl carbonate, 1,3-propanesulfonate lactone, and thiophosphate silane additives is (3-5):(0.5-2):(0.1-0.8):(0.1-3).

5. A method for preparing an electrolyte additive as described in any one of claims 1 to 4, characterized in that, Includes the following steps: S1: Under an inert atmosphere, hexamethyldisilazane reacts with ammonium dihydrogen phosphate to generate intermediate I; S2: Under low temperature conditions, an alcohol or phenolic compound containing the target R group is reacted with chlorosulfonic acid to generate intermediate II; S3: Under inert atmosphere and low temperature conditions, intermediate II is added dropwise to the solution of intermediate I and reacted, and then post-processed to obtain thiophosphate silane additives. S4: The electrolyte additive is obtained by mixing vinylene carbonate, fluorovinyl carbonate, 1,3-propanesulfonate lactone and thiophosphate silane additives in a preset ratio.

6. The preparation method according to claim 5, characterized in that, In step S1, the molar ratio of hexamethyldisilazane to ammonium dihydrogen phosphate is 1:(2-4), the reaction temperature is 90-150℃, and the reaction time is 3-8h; And / or, in step S2, the alcohol or phenolic compound containing the target R group is n-butanol, ethylene nitrile, or phenol, and the molar ratio of the alcohol or phenolic compound containing the target R group to chlorosulfonic acid is 1:(0.8-1.3). And / or, in step S3, the molar ratio of intermediate II to intermediate I is (0.8-1.2):1, the low temperature is an ice bath condition, and the reaction time is 3-6 hours.

7. A lithium-ion battery electrolyte, characterized in that, The electrolyte comprises, by mass fraction of 100%, the following components by mass fraction: 11-15% lithium salt, 80-85% organic solvent and 2-9% electrolyte additive; wherein the electrolyte additive is the electrolyte additive according to any one of claims 1-6.

8. The lithium-ion battery electrolyte according to claim 7, characterized in that, The lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, and lithium difluorooxalate borate.

9. The lithium-ion battery electrolyte according to claim 7, characterized in that, The organic solvent includes at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, and ethyl acetate.

10. A lithium-ion battery, characterized in that, It comprises the lithium-ion battery electrolyte according to any one of claims 7 to 9.