Composite MOF (Metal Organic Framework) membrane for gas separation and preparation method of composite MOF membrane
By introducing modified chitosan and modified multi-walled carbon nanotubes, the problems of insufficient compatibility and mechanical strength of composite MOF membranes in the separation of carbon dioxide and nitrogen were solved, thereby improving separation performance and mechanical strength.
Patent Information
- Application Number
- CN202610511189.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-04-17
- Publication Date
- 2026-05-15
AI Technical Summary
Existing composite MOF membranes suffer from insufficient compatibility, easy aggregation, and the formation of micro-voids or pinholes at the interface during the separation of carbon dioxide and nitrogen, resulting in poor separation performance and insufficient mechanical strength.
An interfacial transition layer is formed by the interaction between modified chitosan and the surface of MOF particles, and modified multi-walled carbon nanotubes are introduced to enhance the compatibility and mechanical strength of MOF particles with the PEBAX matrix. The phenolic hydroxyl groups and Fe3+ coordination centers of modified chitosan are used to improve the affinity adsorption of CO2. Combined with the π-π interaction and electrostatic repulsion of multi-walled carbon nanotubes, the separation performance is improved.
It improves the separation performance of composite MOF membranes for CO2 and N2, enhances mechanical strength, reduces non-selective leakage channels, and extends membrane lifespan.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of gas separation technology, and more specifically to a composite MOF membrane for gas separation and its preparation method. Background Technology
[0002] Carbon dioxide and nitrogen separation is applied in scenarios such as flue gas treatment, carbon capture and resource utilization. Membrane separation technology is considered a potentially efficient solution for carbon dioxide and nitrogen separation due to its advantages such as simple process, low energy consumption, compact equipment, and ease of continuous operation.
[0003] To improve the separation performance of carbon dioxide and nitrogen, researchers have proposed introducing porous fillers such as metal-organic frameworks (MOFs) into a polymer matrix to prepare a hybrid matrix membrane. The pore sieving and adsorption selectivity of MOFs enhances the separation of carbon dioxide and nitrogen. However, in actual preparation, insufficient compatibility between MOF particles and the polymer, easy particle agglomeration, and the formation of non-selective leakage channels such as micropores or pinholes at the interface all affect the separation efficiency of carbon dioxide and nitrogen. Secondly, to improve the pressure resistance and operability of the separation membrane under industrial conditions, it is usually necessary to introduce a porous support or improve the strength of the selective layer. However, the mechanical differences between different components in the composite membrane system and insufficient interfacial bonding can still easily cause defects such as microcracks or delamination, shortening the service life of the separation membrane.
[0004] For example, patent application CN111111464A discloses a structural design and preparation method for an ultra-high carbon dioxide gas selective separation composite membrane. This separation composite membrane has a three-layer structure, from bottom to top: an electrospun polyacrylonitrile (PAN) fiber film layer, a cyclodextrin-based metal-organic framework (MOF) layer with high gas selectivity, and a polymer layer. The three layers are tightly connected by intermolecular hydrogen bonds. The cyclodextrin-based MOF layer in the middle is uniformly dispersed and tightly bonded to the upper and lower layers. Although this scheme uses PAN support and MOF layers to improve separation performance, voids and pinholes are still easily generated at the MOF / polymer interface, making it difficult for the separation composite membrane to simultaneously achieve good carbon dioxide and nitrogen separation performance and mechanical strength.
[0005] In summary, there is a need to provide a composite MOF membrane for gas separation and its preparation method to solve the problems existing in the prior art. Summary of the Invention
[0006] In view of this, the present invention provides a composite MOF membrane for gas separation and a method for preparing the same, which can improve the carbon dioxide and nitrogen separation performance and mechanical strength of the composite MOF membrane.
[0007] To achieve the above objectives, the present invention provides a composite MOF membrane for gas separation and a method for preparing the same, comprising the following steps: S1. Dissolve zinc nitrate hexahydrate in methanol to obtain solution A, and dissolve 2-methylimidazole in methanol to obtain solution B; stir solution A and add solution B, seal and heat, cool, centrifuge, wash and dry to obtain MOF particles; S2. Dissolve propyl gallate in eucalyptol, add ferric chloride hexahydrate and anhydrous ethanol, heat and stir, ultrasonically disperse, add chitosan / acetic acid solution, adjust pH to acidic, heat to react, cool, and rotary evaporate to obtain modified chitosan slurry. S3. Mix and stir polyethersulfone, polyvinylpyrrolidone and N-methylpyrrolidone, add fly ash and alumina, heat to react, let stand to degas, coat with film to obtain green body; after solvent removal, drying, two-stage heating and hydroxylation treatment, ceramic substrate film is obtained. S4. Mix PEBAX particles and ethanol solution, heat to reflux, add 3-glycidyl etheroxypropyltrimethoxysilane, stir, add acetic acid solution, MOF particles and modified chitosan slurry, and ultrasonically disperse to obtain casting solution; drop the casting solution onto ceramic substrate membrane, spin-coat in two stages, let stand, dry, and obtain composite MOF membrane.
[0008] In this invention, propyl gallate is reacted with Fe... 3+ Chitosan was pre-complexed before being reacted with it to obtain modified chitosan, which was then introduced into a composite MOF membrane to improve the separation performance of CO2 and N2. The modified chitosan was fully swollen and dispersed in the casting solution by adjusting the amount of acetic acid, allowing it to fully contact the MOF particles and spontaneously adsorb and accumulate on their surface. During subsequent drying, it precipitated with solvent evaporation, forming an interfacial transition layer. This transition layer anchors the modified chitosan to the MOF particle surface through coordination or hydrogen bonding between the amino and phenolic hydroxyl groups on the modified chitosan molecular chain and the zinc ions of the MOF particles. The modified chitosan molecular chain and the PEBAX matrix have good compatibility due to their similar polarity, acting as a "bridge" at the interface between the MOF particles and PEBAX, filling the tiny gaps between the two phases and reducing non-selective interfacial defects. Simultaneously, the phenolic hydroxyl groups and Fe2+ introduced into the modified chitosan... 3+ The coordination center has a strong reversible affinity adsorption effect on CO2 molecules, making CO2 easier to dissolve and accumulate in the composite MOF membrane. It forms a local "transfer-promoting" micro-region around the MOF particles, giving CO2 a more significant transfer advantage over N2 and improving the separation performance of CO2 and N2.
[0009] Furthermore, the introduction of modified chitosan improves the mechanical strength of the composite MOF membrane. The continuous interfacial transition layer formed by modified chitosan between the MOF particles and PEBAX connects the rigid MOF particles and the flexible PEBAX matrix through chemical and hydrogen bonds. This interfacial bonding allows stress under external force to be more evenly transferred and dispersed from the PEBAX matrix to the MOF particles, avoiding stress concentration around the MOF particles due to weak interfacial bonding and thus preventing microcracks, thereby improving the tensile strength of the composite MOF membrane.
[0010] Optionally, in step S4, before ultrasonic dispersion, modified multi-walled carbon nanotubes are added, which are prepared by surface adsorption of multi-walled carbon nanotubes with sodium pyrene-1-sulfonate.
[0011] In this invention, modified multi-walled carbon nanotubes (MWCNTs) are prepared by surface adsorption modification with sodium pyrene-1-sulfonate, and then introduced into a composite MOF membrane to improve the separation performance of the composite MOF membrane for CO2 and N2. The pyrene group can be adsorbed onto the surface of the MMCNTs via π-π interactions, and the sulfonic acid groups of the sodium pyrene-1-sulfonate molecules extend outwards, preventing the aggregation of MMCNTs through electrostatic repulsion, thus improving the dispersion uniformity of the modified MMCNTs and reducing pinholes, microcracks, and non-selective leakage channels caused by aggregation. Simultaneously, the polar sites such as the sulfonic acid groups are beneficial for improving the solubility and local enrichment of CO2 within the membrane, and synergistically form with the CO2-loving sites provided by the modified chitosan, thereby enhancing the separation performance of the composite MOF membrane for CO2 and N2. In addition, multi-walled carbon nanotubes, as high-modulus fibrous nano-reinforcing phases, play a role in skeletal support and stress dispersion in the film layer, effectively bearing and transmitting external forces, avoiding stress concentration that could lead to microcracks, and further improving the tensile strength of the composite MOF film.
[0012] Optionally, multi-walled carbon nanotubes and hydrogen peroxide solution are mixed, heated to 55-60℃ and stirred for 1.5-2 hours. After centrifugation, the mixture is washed 3-4 times with deionized water and vacuum dried at 40-50℃ for 6-7 hours. The mixture is then poured into an ethanol solution and ultrasonically dispersed for 30-35 minutes. Sodium pyrene-1-sulfonate is added, and ultrasonication is continued for 20-30 minutes. The mixture is stirred at 400-500 rpm for 2-2.5 hours. After centrifugation and filtration, the mixture is washed 2-3 times with ethanol solution and vacuum dried at 40-45℃ for 8-10 hours to obtain modified multi-walled carbon nanotubes.
[0013] Optionally, zinc nitrate hexahydrate is dissolved in methanol to obtain solution A; 2-methylimidazole is dissolved in methanol to obtain solution B; solution A is continuously stirred at 300-400 rpm, solution B is added, and the mixture is heated to 70-75°C for 2-3 hours under sealed conditions. After cooling to room temperature, the mixture is centrifuged, and the resulting solid is washed 2-3 times with methanol and then heated to 40-45°C and vacuum dried for 10-12 hours to obtain MOF particles.
[0014] Optionally, propyl gallate is dissolved in eucalyptol, ferric chloride hexahydrate and anhydrous ethanol are added, the mixture is heated to 60-65℃ and stirred for 1-1.5 hours, then ultrasonically dispersed for 5-10 minutes. Chitosan / acetic acid solution is added, and 1,1,3,3-tetramethylguanidine is added to adjust the pH to 5-5.5. The mixture is heated to 50-55℃ and stirred for 4-5 hours. After cooling to room temperature, the mixture is rotary evaporated under vacuum for 3-4 hours to obtain modified chitosan slurry.
[0015] Optionally, polyethersulfone, polyvinylpyrrolidone, and N-methylpyrrolidone are mixed and heated to 60-65°C. The mixture is stirred at 300-500 rpm for 30-40 minutes, fly ash and alumina are added, and the mixture is heated for another 8-10 hours. After standing for 1-2 hours to remove bubbles, a green body is obtained by coating. The green body is then soaked in water for 20-24 hours. After removing the green body, it is dried in an air-drying environment for 12-14 hours. After undergoing a two-stage heating treatment, the green body is cooled to room temperature and then soaked in a pretreatment solution for 30-40 minutes. After filtration, it is dried at room temperature for 0.5-1 hour to obtain a ceramic substrate film.
[0016] In this invention, fly ash and alumina are used as raw materials. By adding polyethersulfone (PES) as a binder and polyvinylpyrrolidone (PVP) as a pore-forming agent, a ceramic substrate membrane with good mechanical strength and open pore structure is prepared through coating and molding, solvent displacement to remove organic components, gradient heating densification and surface hydroxylation treatment, providing stable support for composite MOF membranes.
[0017] Optionally, PEBAX particles and ethanol solution are mixed, heated to 80-85℃ and stirred under reflux for 2-3 hours, 3-glycidyl etheroxypropyltrimethoxysilane is added, and stirring is continued for 30-40 minutes. Acetic acid solution, MOF particles and modified chitosan slurry are added, and ultrasonic dispersion is performed for 25-30 minutes to obtain casting solution. The casting solution is dropped onto a ceramic substrate membrane, and after two-stage spin coating, it is allowed to stand under ventilation for 12-15 hours, heated to 30-40℃ and vacuum dried for 45-48 hours to obtain a composite MOF membrane.
[0018] In this invention, PEBAX particles, 3-glycidyl etheroxypropyltrimethoxysilane crosslinking agent, MOF particles, and modified chitosan slurry are uniformly mixed by ultrasonic dispersion, followed by spin coating and vacuum drying to obtain a composite MOF membrane. The epoxy groups of 3-glycidyl etheroxypropyltrimethoxysilane can undergo ring-opening reactions with the amine groups on the PEBAX molecular chain to form a crosslinking network. Simultaneously, its silanol groups condense with the hydroxyl groups on the ceramic substrate membrane surface, forming a strong bond with the ceramic substrate membrane. The interfacial transition layer formed by the modified chitosan around the MOF particles effectively improves the dispersibility of the MOF particles in the casting solution and their compatibility with PEBAX, reduces interfacial defects, and thus improves the uniformity of the composite MOF membrane.
[0019] Optionally, the green body is first heated to 1000~1020℃ at a rate of 5℃ / min for 60~80min; then heated to 1300~1320℃ at a rate of 4℃ / min for 120~140min; the two-stage spin coating process is as follows: spin coating at a speed of 400~500rpm for 10~15s, and then spin coating at a speed of 2000~3000rpm for 30~40s; the pretreatment solution is a mixture of acetone, anhydrous ethanol and deionized water, and the weight ratio of acetone, anhydrous ethanol and deionized water is 1:1:1.
[0020] In this invention, a two-stage heating process, first at low temperature and then at high temperature, is used to fully remove the organic components in the green body during the low-temperature treatment, while avoiding cracking or deformation of the film layer caused by excessively rapid heating. This improves the mechanical strength of the ceramic substrate film and provides a structurally stable support foundation for the subsequent composite MOF film.
[0021] A composite MOF membrane for gas separation is prepared using the above-described method. The casting solution comprises the following raw materials in parts by weight: 10-11 parts of PEBAX particles, 190-200 parts of 70wt% ethanol solution, 0.24-0.26 parts of 3-glycidyl etheroxypropyltrimethoxysilane, 2-3 parts of 2wt% acetic acid solution, 2-4 parts of MOF particles, and 0.5-1.5 parts of modified chitosan slurry; the ceramic substrate membrane comprises the following raw materials in parts by weight: The modified chitosan slurry comprises the following raw materials in parts by weight: 2-2.2 parts polyethersulfone, 0.16-0.18 parts polyvinylpyrrolidone, 11-12 parts N-methylpyrrolidone, 15-16 parts fly ash, and 5-5.5 parts alumina; the modified chitosan slurry comprises the following raw materials in parts by weight: 0.55-0.6 parts propyl gallate, 3.6-4 parts eucalyptol, 0.5-0.55 parts ferric chloride hexahydrate, 2-3 parts anhydrous ethanol, 0.36-0.4 parts chitosan, and 18-20 parts 2wt% acetic acid solution.
[0022] Optionally, modified multi-walled carbon nanotubes are also added to the casting solution. The modified multi-walled carbon nanotubes include the following raw materials in parts by weight: 0.5-0.6 parts of multi-walled carbon nanotubes, 50-55 parts of 30wt% hydrogen peroxide solution, 120-130 parts of 70wt% ethanol solution, and 0.2-0.25 parts of sodium pyrene-1-sulfonate.
[0023] The above-described technical solution of the present invention has at least the following beneficial effects: In this invention, the introduction of modified chitosan into the composite MOF membrane improves the separation performance of the composite MOF membrane for CO2 and N2. After being adjusted with an appropriate amount of acetic acid in the casting solution, the modified chitosan swells and disperses fully, allowing it to fully contact the MOF particles and spontaneously adsorb and accumulate on their surface. As the solvent evaporates, it precipitates out to form an interfacial transition layer. This transition layer is anchored to the MOF surface through coordination or hydrogen bonding between the amino and phenolic hydroxyl groups on the modified chitosan molecular chain and the zinc ions of the MOF particles, while maintaining good compatibility with the PEBAX matrix. This "bridging" effect at the MOF / PEBAX interface fills the tiny interfacial voids and reduces non-selective interfacial defects. Simultaneously, the phenolic hydroxyl groups and Fe2+ introduced into the modified chitosan... 3+ The coordination center has a reversible affinity adsorption effect on CO2, making CO2 easier to dissolve and accumulate in the membrane. It forms a local "promoted transport" micro-region around the MOF particles, giving CO2 a more significant transport advantage over N2, thereby improving the separation performance of CO2 and N2.
[0024] The continuous interfacial transition layer formed by modified chitosan can connect rigid MOF particles and PEBAX through chemical bonds and hydrogen bonds, so that stress is transmitted and dispersed more evenly under external force, avoiding stress concentration around MOF particles and inducing microcracks, thereby improving the tensile strength of the composite MOF film. Detailed Implementation
[0025] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. The described embodiments are some embodiments of the present invention, and all other embodiments obtained by those skilled in the art based on the described embodiments of the present invention are within the scope of protection of the present invention.
[0026] Example 1 12 parts of zinc nitrate hexahydrate were dissolved in 680 parts of methanol to obtain solution A; 27 parts of 2-methylimidazole were dissolved in 680 parts of methanol to obtain solution B; solution A was continuously stirred at 400 rpm, solution B was added, and the mixture was heated to 75°C for 3 h under sealed conditions. After cooling to room temperature, the mixture was centrifuged, and the resulting solid was washed three times with methanol and then heated to 45°C and vacuum dried for 12 h to obtain MOF particles.
[0027] Dissolve 0.6 parts of propyl gallate in 4 parts of eucalyptol, add 0.55 parts of ferric chloride hexahydrate and 3 parts of anhydrous ethanol, heat to 65°C and stir for 1.5 h, then sonicate for 10 min; add a mixed solution of 0.4 parts of chitosan and 20 parts of 2 wt% acetic acid solution, add 1,1,3,3-tetramethylguanidine to adjust the pH to 5.5, heat to 55°C and continue stirring for 5 h, cool to room temperature, and rotary evaporate under vacuum for 4 h to obtain modified chitosan slurry.
[0028] 0.6 parts of multi-walled carbon nanotubes and 55 parts of 30wt% hydrogen peroxide solution were mixed, heated to 60℃ and stirred for 2 hours, centrifuged, washed 4 times with deionized water, and vacuum dried at 50℃ for 7 hours. The mixture was then poured into 130 parts of 70wt% ethanol solution, ultrasonically dispersed for 35 minutes, and 0.25 parts of sodium pyrene-1-sulfonate were added. The mixture was ultrasonically dispersed for another 30 minutes and stirred at 500 rpm for 2.5 hours. After centrifugation and filtration, the mixture was washed 3 times with ethanol solution and vacuum dried at 45℃ for 10 hours to obtain modified multi-walled carbon nanotubes.
[0029] 2.2 parts of polyethersulfone (PES), 0.18 parts of polyvinylpyrrolidone (PVP), and 12 parts of N-methylpyrrolidone were mixed and heated to 65°C. The mixture was stirred at 500 rpm for 40 min. 16 parts of fly ash (particle size 5~10 μm) and 5.5 parts of alumina were added. The mixture was heated and reacted for 10 h. After standing for 2 h to remove bubbles, the resulting material was coated with a coating machine to obtain a green body with a thickness of 500 μm. The green body was soaked in water for 24 h. After removing the green body, it was dried in a ventilated environment at room temperature for 14 h. Then, it was heated to 1020°C at a rate of 5°C / min and kept at that temperature for 80 min. Then, it was heated to 1320°C at a rate of 4°C / min and kept at that temperature for 140 min. After cooling to room temperature, it was soaked in a pretreatment solution (a mixture of acetone, anhydrous ethanol, and deionized water with a weight ratio of 1:1:1) for 40 min. After filtration, it was dried at room temperature for 1 h to obtain a ceramic substrate film.
[0030] Eleven parts of PEBAX particles (Pebax® 1657) and 200 parts of 70 wt% ethanol solution were mixed, heated to 85 °C and stirred under reflux for 3 h. 0.26 parts of 3-glycidyl etheroxypropyltrimethoxysilane were added and stirred for another 40 min. Then, three parts of 2 wt% acetic acid solution, four parts of MOF particles, 1.5 parts of modified chitosan slurry and 0.2 parts of modified multi-walled carbon nanotubes were added and ultrasonically dispersed for 30 min to obtain a casting solution. The casting solution was dropped onto a ceramic substrate membrane, first spin-coated at 500 rpm for 15 s, then spin-coated at 3000 rpm for 40 s. After standing under ventilation for 15 h, the membrane was heated to 40 °C and vacuum dried for 48 h to obtain a composite MOF membrane.
[0031] Example 2 11 parts of zinc nitrate hexahydrate were dissolved in 670 parts of methanol to obtain solution A; 26 parts of 2-methylimidazole were dissolved in 670 parts of methanol to obtain solution B; solution A was continuously stirred at 350 rpm, solution B was added, and the mixture was heated to 72°C for 2.5 h under sealed conditions. After cooling to room temperature, the mixture was centrifuged, and the resulting solid was washed twice with methanol and dried under vacuum at 43°C for 11 h to obtain MOF particles.
[0032] 0.58 parts of propyl gallate were dissolved in 3.8 parts of eucalyptol, 0.53 parts of ferric chloride hexahydrate and 2.5 parts of anhydrous ethanol were added, and the mixture was heated to 62°C and stirred for 1.3 h. Then, it was ultrasonically dispersed for 7 min. A mixed solution of 0.38 parts of chitosan and 19 parts of 2 wt% acetic acid solution was added, and 1,1,3,3-tetramethylguanidine was added to adjust the pH to 5.2. The mixture was heated to 52°C and stirred for 4.8 h. After cooling to room temperature, the mixture was rotary evaporated under vacuum for 3.5 h to obtain a modified chitosan slurry.
[0033] 0.55 parts of multi-walled carbon nanotubes and 53 parts of 30 wt% hydrogen peroxide solution were mixed, heated to 58 °C and stirred for 1.8 h, centrifuged, washed three times with deionized water, and vacuum dried at 43 °C for 6.5 h. The mixture was then poured into 125 parts of 70 wt% ethanol solution, ultrasonically dispersed for 32 min, and 0.22 parts of sodium pyrene-1-sulfonate were added. The mixture was ultrasonically dispersed for another 25 min and stirred at 450 rpm for 2.2 h. After centrifugation and filtration, the mixture was washed twice with ethanol solution and vacuum dried at 43 °C for 9 h to obtain modified multi-walled carbon nanotubes.
[0034] 2.1 parts polyethersulfone (PES), 0.17 parts polyvinylpyrrolidone (PVP), and 11.5 parts N-methylpyrrolidone were mixed and heated to 63°C. The mixture was stirred at 400 rpm for 35 minutes. Then, 15.5 parts fly ash (particle size 5-10 μm) and 5.3 parts alumina were added. The mixture was heated and reacted for another 9 hours, followed by a 1.5-hour settling period for degassing. The resulting material was then coated using a coating machine to obtain a 500 μm thick green body. The green body was then immersed in water for 2 hours. After 2 hours, the green body was removed and dried at room temperature for 13 hours. Then, it was heated to 1010℃ at a rate of 5℃ / min and kept at that temperature for 70 minutes. Next, it was heated to 1310℃ at a rate of 4℃ / min and kept at that temperature for 130 minutes. After cooling to room temperature, it was immersed in a pretreatment solution for 35 minutes. The pretreatment solution was a mixture of acetone, anhydrous ethanol, and deionized water with a weight ratio of 1:1:1. After filtration, it was dried at room temperature for 0.7 hours to obtain the ceramic substrate film.
[0035] 10.5 parts of PEBAX particles (Pebax®1657) and 195 parts of 70wt% ethanol solution were mixed, heated to 82℃ and stirred under reflux for 2.5h. 0.25 parts of 3-glycidyl etheroxypropyltrimethoxysilane were added and stirred for another 35min. 2.5 parts of 2wt% acetic acid solution, 3 parts of MOF particles, 1 part of modified chitosan slurry and 0.15 parts of modified multi-walled carbon nanotubes were added and ultrasonically dispersed for 27min to obtain a casting solution. The casting solution was dropped onto a ceramic substrate membrane, first spin-coated at 450rpm for 12s, then spin-coated at 2500rpm for 35s. After standing under ventilation for 13h, the membrane was heated to 35℃ and vacuum dried for 47h to obtain a composite MOF membrane.
[0036] Example 3 10 parts of zinc nitrate hexahydrate were dissolved in 660 parts of methanol to obtain solution A; 25 parts of 2-methylimidazole were dissolved in 660 parts of methanol to obtain solution B; solution A was continuously stirred at 300 rpm, solution B was added, and the mixture was heated to 70°C for 2 h under sealed conditions. After cooling to room temperature, the mixture was centrifuged, and the resulting solid was washed twice with methanol and dried under vacuum at 40°C for 10 h to obtain MOF particles.
[0037] Dissolve 0.55 parts of propyl gallate in 3.6 parts of eucalyptol, add 0.5 parts of ferric chloride hexahydrate and 2 parts of anhydrous ethanol, heat to 60℃ and stir for 1 h, then sonicate for 5 min; add a mixed solution of 0.36 parts of chitosan and 18 parts of 2 wt% acetic acid solution, add 1,1,3,3-tetramethylguanidine to adjust the pH to 5, heat to 50℃ and continue stirring for 4 h, cool to room temperature, and rotary evaporate under vacuum for 3 h to obtain modified chitosan slurry.
[0038] 0.5 parts of multi-walled carbon nanotubes and 50 parts of 30wt% hydrogen peroxide solution were mixed, heated to 55℃ and stirred for 1.5 h, centrifuged, washed three times with deionized water, and vacuum dried at 40℃ for 6 h. The mixture was then poured into 120 parts of 70wt% ethanol solution, ultrasonically dispersed for 30 min, and 0.2 parts of sodium pyrene-1-sulfonate were added. The mixture was ultrasonically dispersed for another 20 min and stirred at 400 rpm for 2 h. After centrifugation and filtration, the mixture was washed twice with ethanol solution and vacuum dried at 40℃ for 8 h to obtain modified multi-walled carbon nanotubes.
[0039] Two parts of polyethersulfone (PES), 0.16 parts of polyvinylpyrrolidone (PVP), and 11 parts of N-methylpyrrolidone were mixed and heated to 60°C. The mixture was stirred at 300 rpm for 30 min. Then, 15 parts of fly ash (particle size 5-10 μm) and 5 parts of alumina were added. The mixture was heated and reacted for another 8 h. After standing for 1 h to remove bubbles, the resulting material was coated with a film using a coating machine to obtain a green body with a thickness of 500 μm. The green body was soaked in water for 20 h. After removing the green body, it was dried in a ventilated environment at room temperature for 12 h. Then, it was heated to 1000°C at a rate of 5°C / min and kept at that temperature for 60 min. Next, it was heated to 1300°C at a rate of 4°C / min and kept at that temperature for 120 min. After cooling to room temperature, the green body was soaked in a pretreatment solution (a mixture of acetone, anhydrous ethanol, and deionized water in a weight ratio of 1:1:1) for 30 min. After filtration, the mixture was dried at room temperature for 0.5 h to obtain a ceramic substrate film.
[0040] Ten parts of PEBAX particles (Pebax®1657) and 190 parts of 70wt% ethanol solution were mixed, heated to 80℃ and stirred under reflux for 2h. 0.24 parts of 3-glycidyl etheroxypropyltrimethoxysilane were added and stirred for another 30min. Two parts of 2wt% acetic acid solution, two parts of MOF particles, 0.5 parts of modified chitosan slurry and 0.1 parts of modified multi-walled carbon nanotubes were added and ultrasonically dispersed for 25min to obtain a casting solution. The casting solution was dropped onto a ceramic substrate membrane, first spin-coated at 400rpm for 10s, then spin-coated at 2000rpm for 30s. After standing under ventilation for 12h, the membrane was heated to 30℃ and vacuum dried for 45h to obtain a composite MOF membrane.
[0041] Example 4 12 parts of zinc nitrate hexahydrate were dissolved in 680 parts of methanol to obtain solution A; 27 parts of 2-methylimidazole were dissolved in 680 parts of methanol to obtain solution B; solution A was continuously stirred at 400 rpm, solution B was added, and the mixture was heated to 75°C for 3 h under sealed conditions. After cooling to room temperature, the mixture was centrifuged, and the resulting solid was washed three times with methanol and then heated to 45°C and vacuum dried for 12 h to obtain MOF particles.
[0042] Dissolve 0.6 parts of propyl gallate in 4 parts of eucalyptol, add 0.55 parts of ferric chloride hexahydrate and 3 parts of anhydrous ethanol, heat to 65°C and stir for 1.5 h, then sonicate for 10 min; add a mixed solution of 0.4 parts of chitosan and 20 parts of 2 wt% acetic acid solution, add 1,1,3,3-tetramethylguanidine to adjust the pH to 5.5, heat to 55°C and continue stirring for 5 h, cool to room temperature, and rotary evaporate under vacuum for 4 h to obtain modified chitosan slurry.
[0043] 2.2 parts of polyethersulfone (PES), 0.18 parts of polyvinylpyrrolidone (PVP), and 12 parts of N-methylpyrrolidone were mixed and heated to 65°C. The mixture was stirred at 500 rpm for 40 min. 16 parts of fly ash (particle size 5~10 μm) and 5.5 parts of alumina were added. The mixture was heated and reacted for 10 h. After standing for 2 h to remove bubbles, the resulting material was coated with a coating machine to obtain a green body with a thickness of 500 μm. The green body was soaked in water for 24 h. After removing the green body, it was dried in a ventilated environment at room temperature for 14 h. Then, it was heated to 1020°C at a rate of 5°C / min and kept at that temperature for 80 min. Then, it was heated to 1320°C at a rate of 4°C / min and kept at that temperature for 140 min. After cooling to room temperature, it was soaked in a pretreatment solution (a mixture of acetone, anhydrous ethanol, and deionized water with a weight ratio of 1:1:1) for 40 min. After filtration, it was dried at room temperature for 1 h to obtain a ceramic substrate film.
[0044] 11 parts of PEBAX particles (Pebax®1657) and 200 parts of 70wt% ethanol solution were mixed, heated to 85℃ and stirred under reflux for 3h. 0.26 parts of 3-glycidyl etheroxypropyltrimethoxysilane were added and stirred for another 40min. 3 parts of 2wt% acetic acid solution, 4 parts of MOF particles and 1.5 parts of modified chitosan slurry were added and ultrasonically dispersed for 30min to obtain the casting solution. The casting solution was dropped onto a ceramic substrate membrane, first spin-coated at 500rpm for 15s, then spin-coated at 3000rpm for 40s. After standing for 15h under ventilation, the membrane was heated to 40℃ and vacuum dried for 48h to obtain the composite MOF membrane.
[0045] Example 5 11 parts of zinc nitrate hexahydrate were dissolved in 670 parts of methanol to obtain solution A; 26 parts of 2-methylimidazole were dissolved in 670 parts of methanol to obtain solution B; solution A was continuously stirred at 350 rpm, solution B was added, and the mixture was heated to 72°C for 2.5 h under sealed conditions. After cooling to room temperature, the mixture was centrifuged, and the resulting solid was washed twice with methanol and dried under vacuum at 43°C for 11 h to obtain MOF particles.
[0046] 0.58 parts of propyl gallate were dissolved in 3.8 parts of eucalyptol, 0.53 parts of ferric chloride hexahydrate and 2.5 parts of anhydrous ethanol were added, and the mixture was heated to 62°C and stirred for 1.3 h. Then, it was ultrasonically dispersed for 7 min. A mixed solution of 0.38 parts of chitosan and 19 parts of 2 wt% acetic acid solution was added, and 1,1,3,3-tetramethylguanidine was added to adjust the pH to 5.2. The mixture was heated to 52°C and stirred for 4.8 h. After cooling to room temperature, the mixture was rotary evaporated under vacuum for 3.5 h to obtain a modified chitosan slurry.
[0047] 2.1 parts polyethersulfone (PES), 0.17 parts polyvinylpyrrolidone (PVP), and 11.5 parts N-methylpyrrolidone were mixed and heated to 63°C. The mixture was stirred at 400 rpm for 35 minutes. Then, 15.5 parts fly ash (particle size 5-10 μm) and 5.3 parts alumina were added. The mixture was heated and reacted for another 9 hours, followed by a 1.5-hour settling period for degassing. The resulting material was then coated using a coating machine to obtain a 500 μm thick green body. The green body was then immersed in water for 2 hours. After 2 hours, the green body was removed and dried at room temperature for 13 hours. Then, it was heated to 1010℃ at a rate of 5℃ / min and kept at that temperature for 70 minutes. Next, it was heated to 1310℃ at a rate of 4℃ / min and kept at that temperature for 130 minutes. After cooling to room temperature, it was immersed in a pretreatment solution for 35 minutes. The pretreatment solution was a mixture of acetone, anhydrous ethanol, and deionized water with a weight ratio of 1:1:1. After filtration, it was dried at room temperature for 0.7 hours to obtain the ceramic substrate film.
[0048] 10.5 parts of PEBAX particles (Pebax®1657) and 195 parts of 70wt% ethanol solution were mixed and heated to 82℃ and stirred under reflux for 2.5h. 0.25 parts of 3-glycidyl etheroxypropyltrimethoxysilane were added and stirred for another 35min. 2.5 parts of 2wt% acetic acid solution, 3 parts of MOF particles and 1 part of modified chitosan slurry were added and ultrasonically dispersed for 27min to obtain the casting solution. The casting solution was dropped onto a ceramic substrate membrane, first spin-coated at 450rpm for 12s, then spin-coated at 2500rpm for 35s. After standing under ventilation for 13h, the membrane was heated to 35℃ and vacuum dried for 47h to obtain the composite MOF membrane.
[0049] Example 6 10 parts of zinc nitrate hexahydrate were dissolved in 660 parts of methanol to obtain solution A; 25 parts of 2-methylimidazole were dissolved in 660 parts of methanol to obtain solution B; solution A was continuously stirred at 300 rpm, solution B was added, and the mixture was heated to 70°C for 2 h under sealed conditions. After cooling to room temperature, the mixture was centrifuged, and the resulting solid was washed twice with methanol and dried under vacuum at 40°C for 10 h to obtain MOF particles.
[0050] Dissolve 0.55 parts of propyl gallate in 3.6 parts of eucalyptol, add 0.5 parts of ferric chloride hexahydrate and 2 parts of anhydrous ethanol, heat to 60℃ and stir for 1 h, then sonicate for 5 min; add a mixed solution of 0.36 parts of chitosan and 18 parts of 2 wt% acetic acid solution, add 1,1,3,3-tetramethylguanidine to adjust the pH to 5, heat to 50℃ and continue stirring for 4 h, cool to room temperature, and rotary evaporate under vacuum for 3 h to obtain modified chitosan slurry.
[0051] Two parts of polyethersulfone (PES), 0.16 parts of polyvinylpyrrolidone (PVP), and 11 parts of N-methylpyrrolidone were mixed and heated to 60°C. The mixture was stirred at 300 rpm for 30 min. Then, 15 parts of fly ash (particle size 5-10 μm) and 5 parts of alumina were added. The mixture was heated and reacted for another 8 h. After standing for 1 h to remove bubbles, the resulting material was coated with a film using a coating machine to obtain a green body with a thickness of 500 μm. The green body was soaked in water for 20 h. After removing the green body, it was dried in a ventilated environment at room temperature for 12 h. Then, it was heated to 1000°C at a rate of 5°C / min and kept at that temperature for 60 min. Next, it was heated to 1300°C at a rate of 4°C / min and kept at that temperature for 120 min. After cooling to room temperature, the green body was soaked in a pretreatment solution (a mixture of acetone, anhydrous ethanol, and deionized water in a weight ratio of 1:1:1) for 30 min. After filtration, the mixture was dried at room temperature for 0.5 h to obtain a ceramic substrate film.
[0052] Ten parts of PEBAX particles (Pebax®1657) and 190 parts of 70wt% ethanol solution were mixed, heated to 80℃ and stirred under reflux for 2h. 0.24 parts of 3-glycidyl etheroxypropyltrimethoxysilane were added and stirred for another 30min. Two parts of 2wt% acetic acid solution, two parts of MOF particles and 0.5 parts of modified chitosan slurry were added and ultrasonically dispersed for 25min to obtain the casting solution. The casting solution was dropped onto a ceramic substrate membrane, first spin-coated at 400rpm for 10s, then spin-coated at 2000rpm for 30s. After standing for 12h under ventilation, the membrane was heated to 30℃ and vacuum dried for 45h to obtain the composite MOF membrane.
[0053] The present invention also includes comparative examples and related experiments.
[0054] Comparative Example 1 The only difference from Example 1 is that no modified chitosan slurry was added; all other components and preparation steps were exactly the same, resulting in a composite MOF membrane.
[0055] Comparative Example 2 The only difference from Example 1 is that propyl gallate was not added; all other components and preparation steps were exactly the same, resulting in a composite MOF membrane.
[0056] Comparative Example 3 The only difference from Example 1 is that ferric chloride hexahydrate was not added; all other components and preparation steps were exactly the same, resulting in a composite MOF membrane.
[0057] Performance testing: The separation performance of CO2 and N2 of the composite MOF membranes prepared in Examples 1-6 and Comparative Examples 1-3 was tested according to the national standard GB / T40260-2021 "Test Method for Gas Permeability Performance of Polymer Membrane Materials". The permeation coefficients of CO2 and N2 and the selectivity coefficient of CO2 / N2 were tested respectively. The test temperature was 35℃ and the test pressure was 0.1MPa. The test results are shown in Table 1.
[0058] The mechanical strength of the composite MOF films prepared in Examples 1-6 and Comparative Examples 1-3 was tested in accordance with the national standard GB / T1040.1-2025 "Determination of tensile properties of plastics - Part 1: General Rules". The test results are shown in Table 1.
[0059] Table 1
[0060] As shown in Table 1, the selectivity coefficients of the composite MOF membranes prepared in Examples 1-3 for CO2 and N2 range from 85 to 92, and the tensile strength ranges from 17.7 MPa to 18.3 MPa; while the selectivity coefficients of the composite MOF membranes prepared in Examples 4-6 for CO2 and N2 range from 70 to 78, and the tensile strength ranges from 15.2 MPa to 16.2 MPa. It can be seen that the addition of modified multi-walled carbon nanotubes helps to improve the separation performance of composite MOF membranes for CO2 and N2 as well as their mechanical strength.
[0061] As shown in Table 1, compared with Example 1, the composite MOF membrane prepared in Comparative Example 1 showed a significant decrease in the selectivity coefficient for CO2 and N2 and the tensile strength, indicating that the modified chitosan slurry helps to improve the separation performance of the composite MOF membrane for CO2 and N2 as well as its mechanical strength. Compared with Example 1, the tensile strength of the composite MOF membrane prepared in Comparative Example 2 was significantly reduced, indicating that propyl gallate helps to improve the mechanical properties of the composite MOF membrane. Compared with Example 1, the selectivity coefficient for CO2 and N2 of the composite MOF membrane prepared in Comparative Example 3 was reduced, indicating that ferric chloride hexahydrate helps to improve the separation performance of the composite MOF membrane for CO2 and N2.
[0062] The above are preferred embodiments of the present invention. Those skilled in the art can make several improvements and modifications without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a composite MOF membrane for gas separation, characterized in that, Includes the following steps: S1. Dissolve zinc nitrate hexahydrate in methanol to obtain solution A, and dissolve 2-methylimidazole in methanol to obtain solution B; stir solution A and add solution B, seal and heat, cool, centrifuge, wash and dry to obtain MOF particles; S2. Dissolve propyl gallate in eucalyptol, add ferric chloride hexahydrate and anhydrous ethanol, heat and stir, ultrasonically disperse, add chitosan / acetic acid solution, adjust pH to acidic, heat to react, cool, and rotary evaporate to obtain modified chitosan slurry. S3. Mix and stir polyethersulfone, polyvinylpyrrolidone and N-methylpyrrolidone, add fly ash and alumina, heat to react, let stand to degas, coat with film to obtain green body; after solvent removal, drying, two-stage heating and hydroxylation treatment, ceramic substrate film is obtained. S4. Mix PEBAX particles and ethanol solution, heat to reflux, add 3-glycidyl etheroxypropyltrimethoxysilane, stir, add acetic acid solution, MOF particles and modified chitosan slurry, and ultrasonically disperse to obtain casting solution; drop the casting solution onto ceramic substrate membrane, spin-coat in two stages, let stand, dry, and obtain composite MOF membrane.
2. The method for preparing a composite MOF membrane for gas separation according to claim 1, characterized in that, In step S4, before ultrasonic dispersion, modified multi-walled carbon nanotubes are added. The modified multi-walled carbon nanotubes are prepared by surface adsorption of multi-walled carbon nanotubes with sodium pyrene-1-sulfonate.
3. The method for preparing a composite MOF membrane for gas separation according to claim 2, characterized in that, Multi-walled carbon nanotubes were mixed with hydrogen peroxide solution, heated to 55-60℃ and stirred for 1.5-2 hours. After centrifugation, the mixture was washed 3-4 times with deionized water and vacuum dried at 40-50℃ for 6-7 hours. The mixture was then poured into an ethanol solution and ultrasonically dispersed for 30-35 minutes. Sodium pyrene-1-sulfonate was added and ultrasonication was continued for 20-30 minutes. The mixture was stirred at 400-500 rpm for 2-2.5 hours. After centrifugation and filtration, the mixture was washed 2-3 times with ethanol solution and vacuum dried at 40-45℃ for 8-10 hours to obtain modified multi-walled carbon nanotubes.
4. The method for preparing a composite MOF membrane for gas separation according to claim 1, characterized in that, Zinc nitrate hexahydrate was dissolved in methanol to obtain solution A; 2-methylimidazole was dissolved in methanol to obtain solution B; solution A was continuously stirred at 300-400 rpm, solution B was added, and the mixture was heated to 70-75°C for 2-3 hours under sealed conditions. After cooling to room temperature, the mixture was centrifuged, and the resulting solid was washed 2-3 times with methanol and then heated to 40-45°C and vacuum dried for 10-12 hours to obtain MOF particles.
5. The method for preparing a composite MOF membrane for gas separation according to claim 1, characterized in that, Propyl gallate was dissolved in eucalyptol, ferric chloride hexahydrate and anhydrous ethanol were added, and the mixture was heated to 60-65℃ and stirred for 1-1.5 h. After ultrasonic dispersion for 5-10 min, chitosan / acetic acid solution was added, and 1,1,3,3-tetramethylguanidine was added to adjust the pH to 5-5.
5. The mixture was heated to 50-55℃ and stirred for 4-5 h. After cooling to room temperature, the mixture was rotary evaporated under vacuum for 3-4 h to obtain modified chitosan slurry.
6. The method for preparing a composite MOF membrane for gas separation according to claim 1, characterized in that, Polyethersulfone, polyvinylpyrrolidone, and N-methylpyrrolidone are mixed and heated to 60-65°C. The mixture is stirred at 300-500 rpm for 30-40 minutes. Fly ash and alumina are added, and the mixture is heated for another 8-10 hours. After standing for 1-2 hours to remove bubbles, a green body is obtained by coating. The green body is then soaked in water for 20-24 hours. After removing the green body, it is dried in an air-conditioned environment for 12-14 hours. After undergoing a two-stage heating treatment, the green body is cooled to room temperature and then soaked in a pretreatment solution for 30-40 minutes. After filtration, the green body is dried at room temperature for 0.5-1 hour to obtain a ceramic substrate film.
7. The method for preparing a composite MOF membrane for gas separation according to claim 1, characterized in that, PEBAX particles and ethanol solution are mixed, heated to 80-85℃ and stirred under reflux for 2-3 hours. 3-glycidyl etheroxypropyltrimethoxysilane is added and stirred for another 30-40 minutes. Acetic acid solution, MOF particles and modified chitosan slurry are added and ultrasonically dispersed for 25-30 minutes to obtain casting solution. The casting solution is dropped onto a ceramic substrate membrane, and after two-stage spin coating, it is allowed to stand under ventilation for 12-15 hours. It is then heated to 30-40℃ and vacuum dried for 45-48 hours to obtain a composite MOF membrane.
8. A method for preparing a composite MOF membrane for gas separation according to claim 6, characterized in that, The two-stage heating treatment is as follows: first, the green blank is heated to 1000~1020℃ at a speed of 5℃ / min for 60~80min; then, the green blank is heated to 1300~1320℃ at a speed of 4℃ / min for 120~140min; the two-stage spin coating treatment is as follows: spin coating at a speed of 400~500rpm for 10~15s, then spin coating at a speed of 2000~3000rpm for 30~40s; The pretreatment solution is a mixture of acetone, anhydrous ethanol and deionized water, and the weight ratio of acetone, anhydrous ethanol and deionized water is 1:1:
1.
9. A composite MOF membrane for gas separation, prepared by the method for preparing a composite MOF membrane for gas separation according to any one of claims 1 to 8, characterized in that, The casting solution comprises the following raw materials in parts by weight: 10-11 parts PEBAX particles, 190-200 parts 70wt% ethanol solution, 0.24-0.26 parts 3-glycidyl etheroxypropyltrimethoxysilane, 2-3 parts 2wt% acetic acid solution, 2-4 parts MOF particles, and 0.5-1.5 parts modified chitosan slurry; the ceramic substrate film comprises the following raw materials in parts by weight: 2-2.2 parts polyethersulfone, polyvinylpyrrolidone... The modified chitosan slurry comprises the following raw materials in parts by weight: 0.16-0.18 parts of pyrrolidone, 11-12 parts of N-methylpyrrolidone, 15-16 parts of fly ash, and 5-5.5 parts of alumina; and 0.55-0.6 parts of propyl gallate, 3.6-4 parts of eucalyptol, 0.5-0.55 parts of ferric chloride hexahydrate, 2-3 parts of anhydrous ethanol, 0.36-0.4 parts of chitosan, and 18-20 parts of 2wt% acetic acid solution.
10. A composite MOF membrane for gas separation according to claim 9, characterized in that, The casting solution also contains modified multi-walled carbon nanotubes, which include the following raw materials in parts by weight: 0.5-0.6 parts multi-walled carbon nanotubes, 50-55 parts 30wt% hydrogen peroxide solution, 120-130 parts 70wt% ethanol solution, and 0.2-0.25 parts sodium pyrene-1-sulfonate.