Preparation method of polyphenylene sulfide / aramid nanofiber composite film

By developing a method for preparing composite films of polyphenylene sulfide and aramid nanofibers, the problems of easy degradation and insufficient chemical stability of the composite current collector support layer at high temperatures have been solved, resulting in a high-strength, corrosion-resistant composite film suitable for lithium batteries used in new energy vehicles and energy storage.

CN122232223APending Publication Date: 2026-06-19DALIAN POLYTECHNIC UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610340881.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-03-19
Publication Date
2026-06-19

AI Technical Summary

Technical Problem

Existing composite current collector support layer materials such as PET and PP are prone to degradation at high temperatures and have insufficient chemical stability, making it difficult to meet the stability requirements under high voltage and long cycle conditions. Pure polyphenylene sulfide films have poor thermal stability and insufficient toughness, making them brittle and limiting their application in complex stress environments.

Method used

A polyphenylene sulfide (PPS)/aramid nanofiber composite system was adopted to prepare PPS/aramid nanofiber composite films through wet papermaking, coating, hot pressing and other processes. The high strength and π-π conjugation of aramid nanofibers were used to improve interfacial compatibility and construct a multi-scale reinforced structure.

Benefits of technology

It significantly improves the mechanical properties and high-temperature dimensional stability of the composite film, solves the problems of easy degradation at high temperatures and poor chemical stability of traditional support layers, and provides a high-strength, corrosion-resistant composite current collector suitable for lithium batteries used in new energy vehicles and energy storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
Patent Text Reader

Abstract

This invention discloses a method for preparing a polyphenylene sulfide (PPS) / aramid nanofiber composite film, belonging to the field of high-temperature resistant, high-strength, and high-toughness composite film preparation. The preparation method includes the following steps: 1) preparing PPS fiber paper using a wet-process papermaking method, and then coating the surface with aramid nanofibers using a coating process; 2) attaching an adhesive to the surface of the composite film using a spreading process, and obtaining the composite film through a series of hot-pressing processes and oxidation treatment. The composite film prepared by this invention exhibits strong high-temperature dimensional stability, high insulation, and strong mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of high-temperature resistant, high-strength, and high-toughness composite film preparation, specifically a method for preparing a polyphenylene sulfide / aramid nanofiber composite film. Background Technology

[0002] With the surge in demand for high-energy-density and high-safety lithium batteries from new energy vehicles and energy storage systems, composite current collector technology has become the focus of the industry due to its lightweight, high safety, and cost advantages. Traditional metal current collectors (such as copper foil and aluminum foil) face problems such as insufficient mechanical strength and the risk of lithium dendrite puncture during the thinning process. While existing polymer support layer materials such as polyethylene terephthalate (PET) and polypropylene (PP) can reduce weight, they are difficult to meet the stability requirements under high voltage and long-cycle conditions due to defects such as poor high-temperature resistance and insufficient chemical stability.

[0003] Current research on composite current collector support layers mainly focuses on single polymer materials or inorganic filler composite systems, but this faces significant bottlenecks. For example, PET-based materials are prone to degradation during high-temperature cycling, leading to increased interfacial impedance; while PP-based materials are inexpensive, their thermal stability is insufficient, and they are prone to softening and deformation after long-term use. In recent years, the industry has attempted to improve performance through base film modification (such as surface roughening and doping with toughening agents), but the inherent defects of the materials are difficult to eliminate.

[0004] Polyphenylene sulfide (PPS), a semi-crystalline special engineering plastic, features alternating rigid benzene rings and flexible sulfide bonds in its molecular chain, giving it excellent high-temperature resistance (melting point 280-300℃, long-term service temperature 200-240℃), chemical inertness (resistance to acids, alkalis, and organic solvents), and high mechanical strength. However, pure PPS films suffer from poor thermal stability, insufficient toughness, and are prone to brittleness, limiting their application in complex stress environments. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention provides a method for preparing a polyphenylene sulfide (PPS) / aramid nanofiber composite film. The composite system of PPS and aramid nanofibers, with its synergistic reinforcing effect, offers an innovative solution for a new generation of composite current collector support layers. The introduction of aramid nanofibers effectively compensates for the poor thermal stability and insufficient toughness of PPS films. Their high strength, high aspect ratio, and high-temperature resistance not only improve the mechanical properties of the composite film but also enhance the interfacial compatibility with the PPS matrix through intermolecular π-π conjugation, forming a multi-scale reinforced structure. The combination of the two retains the chemical corrosion resistance and dimensional stability of PPS while improving the toughness of the composite film through the toughening effect of aramid fibers.

[0006] The technical solution adopted in this invention is as follows:

[0007] A method for preparing a polyphenylene sulfide / aramid nanofiber composite film, the method comprising the following steps: (1) Preparation of polyphenylene sulfide fiber / aramid nanofiber composite membrane: Polyphenylene sulfide short fibers are used to prepare polyphenylene sulfide fiber paper by wet papermaking process. After drying, aramid nanofiber / dimethyl sulfoxide (DMSO) dispersion is coated on its surface, and it is soaked in water to solidify. After drying, polyphenylene sulfide fiber / aramid nanofiber composite membrane is obtained for later use.

[0008] (2) Preparation of adhesive: Using a good solvent and a bad solvent as a composite solvent, the polyphenylene sulfide powder polymer (resin), the good solvent and the bad solvent are mixed, nitrogen is passed through to remove oxygen, the temperature is raised to 250-257 ℃, and the mixture is stirred for 5-10 min to completely dissolve and form a homogeneous solution. After cooling and curing, the adhesive powder is obtained by mechanical crushing.

[0009] (3) Preparation of polyphenylene sulfide / aramid nanofiber composite film: Using polyimide (PI) film as base film, the composite film prepared in step (1) is attached to the surface of the base film, and the adhesive powder prepared in step (2) is evenly spread on the surface of the composite film. Then, a polyphenylene sulfide / aramid nanofiber wet film is prepared by hot pressing. The obtained wet film is soaked and washed in an extractant to remove the solvent and remove the PI base film. After drying, it is hot-pressed and shaped a second time to obtain the nascent composite film. Then, it is oxidized and washed thoroughly with water and dried completely to obtain the polyphenylene sulfide / aramid nanofiber composite film.

[0010] This invention also relates to protecting the polyphenylene sulfide / aramid nanofiber composite film prepared by the above-described preparation method, with a basis weight of 15-100 g / m³. 2 The thickness is 10-80μm.

[0011] This invention utilizes polyphenylene sulfide (PPS) fibers, aramid nanofibers, and PPS / solvent solid powder as raw materials to prepare PPS / aramid nanofiber composite films using a wet papermaking process, coating, spreading, hot pressing, and oxidation. Specifically, 1) PPS fiber paper is prepared using a wet papermaking process, and aramid nanofibers are coated onto its surface; 2) an adhesive is attached to the surface of the composite film using a spreading process, and the composite film is obtained through multiple hot pressing processes and oxidation treatment. The composite film prepared by this invention exhibits strong high-temperature dimensional stability, high insulation, and strong mechanical properties.

[0012] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) Using polyphenylene sulfide and aramid as raw materials, it has the characteristics of high mechanical strength, high thermal stability and good toughness, which fundamentally solves the defects of traditional support layers such as PET and PP that are easily degraded at high temperature, have increased interfacial impedance and poor chemical stability, and significantly improves the structural stability and working reliability of composite current collectors under high temperature conditions.

[0013] (2) Aramid nanofibers, with their high aspect ratio and high strength, enhance the compatibility of the composite interface by means of intermolecular π-π conjugation and construct a multi-scale reinforced structure. At the same time, the morphology of the fiber paper produced by wet papermaking greatly improves the folding resistance of polyphenylene sulfide, and significantly improves the mechanical properties and high-temperature dimensional stability of the composite film.

[0014] (3) The process combines wet papermaking, powder spreading, multi-stage hot pressing, and oxidation. The preparation process is simple, the conditions are mild and controllable, and the production cost is low, showing good prospects for industrial mass production. The resulting composite film is thin and uniform, and integrates multiple advantages such as high strength, high temperature resistance, and corrosion resistance. It breaks through the performance bottleneck of single polymers and can be widely used as a high-performance support layer in composite current collectors for new energy vehicles and energy storage lithium batteries, which strongly promotes the development of composite current collectors towards lightweight, high safety, and long life. Attached Figure Description

[0015] Figure 1 This is a photograph of the polyphenylene sulfide / aramid nanofiber composite film prepared in Example 3 of the present invention.

[0016] Figure 2 The image shows a surface electron microscope image of the polyphenylene sulfide / aramid nanofiber composite film prepared in Example 3 of the present invention. As can be seen from the image, the surface is smooth, and the interfaces of polyphenylene sulfide fibers, aramid nanofibers and adhesive are tightly bonded with no obvious defects. Detailed Implementation

[0017] Specific embodiments of the present invention are given below. These specific embodiments are only used to further illustrate the present invention and do not limit the scope of protection of the claims of this application.

[0018] This invention provides a method for preparing a polyphenylene sulfide / aramid nanofiber composite film (hereinafter referred to as the method), which includes the following steps: (1) Preparation of polyphenylene sulfide fiber / aramid nanofiber composite membrane: Take polyphenylene sulfide short fibers and prepare polyphenylene sulfide fiber paper by wet papermaking process. After drying, coat the surface of the paper with aramid nanofiber / DMSO dispersion, immerse it in water to solidify, and dry it to obtain polyphenylene sulfide fiber / aramid nanofiber composite membrane for later use.

[0019] The polyphenylene sulfide (PPS) fibers have a diameter of 8-13 μm and a length of 3-8 mm; the PPS molecular weight is 3.7-5.0 W; the drying temperature of the PPS fiber paper is 50-150℃, preferably 60-80℃, and the drying time is 0.5-24 h, preferably 4-6 h; the PPS fiber paper obtained by wet papermaking has a thickness of 0.2-1.0 mm and a basis weight of 40-120 g / m². 2 The aramid nanofibers have a diameter of 10-30 nm, a length of 30-50 μm, and an aspect ratio of 1000-5000; the concentration of the aramid nanofiber dispersion is 0.5-10 g / L, preferably 2-5 g / L; the coating method is at least one of doctor blade coating, roller coating, and slot extrusion coating, with a speed of 0.3-2 m / min, preferably 0.8-1.2 m / min, and a coating amount of 0.5-3 L / m 2 The soaking time in water is 12-48 hours, and the temperature is 20-35℃; the drying temperature after curing is 20-70℃, preferably 35-50℃, and the drying time is 12-48 hours.

[0020] (2) Preparation of adhesive: Using a good solvent and a bad solvent as a composite solvent, the polyphenylene sulfide powder, the good solvent and the bad solvent are mixed, nitrogen is passed through to remove oxygen, the temperature is raised to 250-257 ℃, and the mixture is stirred for 5-10 min to completely dissolve and form a homogeneous solution. After cooling and curing, the adhesive powder is obtained by mechanical crushing.

[0021] The benign solvent is at least one of N-methylpyrrolidone, benzophenone, benzoin, caprolactam, diphenyl sulfone, 1-chloronaphthalene, and diphenyl ether; the inferior solvent includes at least one of dibutyl phthalate, dibutyl sebacate, dioctyl phthalate, dioctyl sebacate, diethyl isophthalate, dibutyl isophthalate, dioctyl isophthalate, glycerol, and polyethylene glycol. The polyphenylene sulfide powder resin has a molecular weight of 6-8W; the sum of the mass of the benign solvent, the inferior solvent, and the polyphenylene sulfide resin is 100%, the proportion of polyphenylene sulfide powder resin is 5-18%, preferably 12-15%; the proportion of the benign solvent is 60-85%, preferably 70-75%; the proportion of the inferior solvent is 0-20%, preferably 15-20%; the cooling method is at least one of air curing, water bath curing, and liquid nitrogen curing; the mechanical pulverization temperature is 0-25℃, the pulverization time is 0.5-10min, and the pulverization speed is 4000-12000r / min.

[0022] (3) Preparation of polyphenylene sulfide / aramid nanofiber composite film: Using PI film as base film, the composite film prepared in step (1) is attached to the surface of the base film, and the adhesive powder prepared in step (2) is evenly spread on the surface of the composite film. Then, a polyphenylene sulfide / aramid nanofiber wet film is prepared by hot pressing. The obtained wet film is soaked and washed in an extractant to remove the solvent and remove the PI film. After drying, it is hot-pressed and shaped a second time to obtain the nascent composite film. Then, it is oxidized and washed thoroughly with water and dried completely to obtain the polyphenylene sulfide / aramid nanofiber composite film.

[0023] The PI-based film has a thickness of 50-300 μm, preferably 150-250 μm; the spreading method is at least one of screen spreading, roller spreading, metering roller spreading, electrostatic spreading, and airflow spreading; the amount of adhesive powder spread is 50-500 g / m³. 2 Preferably 200-300g / m 2 The hot pressing process includes a primary hot pressing and a secondary hot pressing; the primary hot pressing temperature is 120-240℃, preferably 180-230℃, the pressure is 2-18 MPa, preferably 8-12 MPa, and the hot pressing time is 10-300 s, preferably 60-180 s; the secondary hot pressing temperature is 160-230℃, the pressure is 8-20 MPa, preferably 8-12 MPa, and the hot pressing time is 10-300 s, preferably 60-180 s.

[0024] The solvent used for extraction and washing is at least one selected from water, alcohol solvents, halogenated hydrocarbon solvents, ester solvents, hydrocarbon solvents, and amide solvents; the alcohol solvent is at least one selected from ethanol, propanol, isopropanol, butanol, isobutanol, and benzyl alcohol; the halogenated hydrocarbon solvent is at least one selected from tetrachloromethane, 1,2-dichloroethane, trichloroethane, and tetrahydrofuran; the ester solvent is at least one selected from ethyl acetate, butyl acetate, ethyl benzoate, ethyl formate, dimethyl carbonate, diethyl carbonate, dibutyl carbonate, and dipropyl carbonate; the hydrocarbon solvent is at least one selected from n-hexane, cyclohexane, benzene, and toluene; the amide solvent is at least one selected from dimethylformamide, N,N-dimethylformamide, N,N-diethylacetamide, and N-methylpyrrolidone; and the solvent temperature is 50-70 °C.

[0025] The reagent used in the oxidation process is at least one of potassium permanganate, hydrogen peroxide, sodium hypochlorite, nitric acid, and sodium perchlorate; the temperature in the oxidation process is 30-60℃, and the treatment time is 0.5-24 h; the drying temperature is 50-150℃, preferably 60-80℃, and the drying time is 0.5-24 h, preferably 4-6 h.

[0026] The test methods used in the following embodiments are as follows: [Thickness] GB / T 6672-2001 Mechanical Measurement Method for Determination of Thickness of Plastic Films and Sheets [Basis Weight] GB / T 31729-2015 Test Method for Unit Area Mass of Plastic Film [Tension Strength], [Elongation at Break] GB / T 1040.3-2006 Determination of Tensile Properties of Plastics Part 3: Test Conditions for Films and Sheets [Heat Shrinkage Rate] GB / T 12027-2004 Test Method for Dimensional Change Rate of Plastic Films and Sheets under Heat Example 1 (1) Take short polyphenylene sulfide fibers (diameter 8-13μm, length 3-8mm, polyphenylene sulfide molecular weight 37000) and prepare 50g / m² by wet papermaking process. 2 A 0.4 mm thick polyphenylene sulfide fiber paper was dried in an oven at 70℃ for 6 hours. Then, a 2.0 g / L aramid nanofiber (10-30 nm in diameter, 30-50 μm in length) / DMSO dispersion was coated onto its surface. The coating speed was 0.8 m / min, and the coating amount was 1.5 L / m². 2 The membrane was then soaked in deionized water at 30°C for 24 hours, and then dried at 45°C for 24 hours to obtain a composite membrane for later use.

[0027] (2) Weigh polyphenylene sulfide powder (molecular weight 70000), benzophenone and dibutyl phthalate into a three-necked flask at mass fractions of 12%, 80% and 8% respectively. Turn on the heating to 255°C, turn on the mechanical stirring at 600 r / min and stir for 7 min to obtain a homogeneous solution. Then cool in an ice water bath to completely solidify, and then mechanically crush at 8000 r / min for 2 min to obtain adhesive powder.

[0028] (3) Using a PI film with a thickness of 150 μm as the base film, the composite film prepared in step (1) is attached to the surface of the base film. The prepared adhesive powder is evenly spread on the surface of the composite film using a sieve, with a spreading amount of 200 g / m. 2 Subsequently, a polyphenylene sulfide / aramid nanofiber wet film was prepared by hot pressing at 200℃, 10MPa, and 60s. The obtained wet film was then immersed and washed in ethanol at 50℃ for 12h. After removing the PI film, it was dried and then subjected to a second hot pressing at 200℃, 8MPa, and 120s to obtain the nascent composite film.

[0029] (4) The obtained nascent composite film was soaked in 6% hydrogen peroxide at 50°C for 6 hours, then taken out and thoroughly washed with deionized water, and dried in a forced-air drying oven at 60°C for 6 hours to obtain a polyphenylene sulfide / aramid nanofiber composite film.

[0030] (5) After testing, the thickness of the obtained composite film was 18 μm and the basis weight was 37 g / m. 2 The tensile breaking strength is 42 MPa, the elongation at break is 4.9%, and the surface shows no obvious wrinkles after being treated in an oven at 180℃ for 30 min. The calculated thermal shrinkage rate is 1.7%.

[0031] Example 2 (1) Take short polyphenylene sulfide fibers (diameter 8-13μm, length 3-8mm, polyphenylene sulfide molecular weight 37000) and prepare 50g / m² by wet papermaking process. 2 A 0.4 mm thick polyphenylene sulfide fiber paper was dried in an oven at 70°C for 6 hours. Then, a 2.5 g / L aramid nanofiber (10-30 nm in diameter, 30-50 μm in length) / DMSO dispersion was coated onto its surface. The coating speed was 0.8 m / min, and the coating amount was 1.5 L / m². 2 The membrane was then soaked in deionized water at 30°C for 24 hours, and then dried at 45°C for 24 hours to obtain a composite membrane for later use.

[0032] (2) Weigh polyphenylene sulfide powder (molecular weight 70000), benzophenone and dibutyl phthalate into a three-necked flask at mass fractions of 14%, 78% and 8% respectively. Turn on the heating to 255°C, turn on the mechanical stirring at 600 r / min and stir for 7 min to obtain a homogeneous solution. Then cool in an ice water bath to completely solidify, and then use mechanical pulverization at 8000 r / min for 2 min to obtain adhesive powder.

[0033] (3) Using a PI film with a thickness of 150 μm as the base film, the composite film prepared in step (1) is attached to the surface of the base film. The prepared adhesive powder is evenly spread on the surface of the composite film using a sieve, with a spreading amount of 200 g / m. 2 Subsequently, a polyphenylene sulfide / aramid nanofiber wet film was prepared by hot pressing at 230°C, 10MPa, and 120s. The obtained wet film was then immersed and washed in ethanol at 50°C for 12 hours. After removing the PI film, the film was dried and then subjected to a second hot pressing at 200°C, 8MPa, and 120s to obtain the nascent composite film.

[0034] (4) The nascent composite film was soaked in 6% hydrogen peroxide at 50°C for 8 hours, then washed thoroughly with deionized water and dried in a forced-air drying oven at 60°C for 6 hours to obtain a polyphenylene sulfide / aramid nanofiber composite film.

[0035] (5) After testing, the thickness of the obtained composite film was 24 μm and the basis weight was 39 g / m. 2The tensile breaking strength is 45 MPa, the elongation at break is 4.6%, and the surface shows no obvious wrinkles after being treated in an oven at 180℃ for 30 min. The calculated thermal shrinkage rate is 1.9%.

[0036] Example 3 (1) Take short polyphenylene sulfide fibers (diameter 8-13μm, length 3-8mm, polyphenylene sulfide molecular weight 37000) and prepare 50g / m² by wet papermaking process. 2 A 0.4 mm thick polyphenylene sulfide fiber paper was dried in an oven at 70℃ for 6 hours. Then, a 3.0 g / L aramid nanofiber (10-30 nm in diameter, 30-50 μm in length) / DMSO dispersion was coated onto its surface. The coating speed was 0.8 m / min, and the coating amount was 1.5 L / m². 2 The membrane was then soaked in deionized water at 30°C for 24 hours, and then dried at 45°C for 24 hours to obtain a composite membrane for later use.

[0037] (2) Weigh polyphenylene sulfide powder (molecular weight 70000), benzophenone and dibutyl phthalate into a three-necked flask at mass fractions of 16%, 76% and 8% respectively. Turn on the heating to 255°C, turn on the mechanical stirring at 600 r / min and stir for 7 min to obtain a homogeneous solution. Then cool in an ice water bath to completely solidify, and then mechanically crush at 8000 r / min for 2 min to obtain adhesive powder.

[0038] (3) Using a PI film with a thickness of 150 μm as the base film, the composite film prepared in step (1) is attached to the surface of the base film. The prepared adhesive powder is evenly spread on the surface of the composite film using a sieve, with a spreading amount of 200 g / m. 2 Subsequently, a polyphenylene sulfide / aramid nanofiber wet film was prepared by hot pressing at 230°C, 10MPa, and 120s. The obtained wet film was then immersed and washed in ethanol at 50°C for 12 hours. After removing the PI film, the film was dried and then subjected to a second hot pressing at 220°C, 10MPa, and 120s to obtain the nascent composite film.

[0039] (4) The nascent composite film was soaked in 6% hydrogen peroxide at 50°C for 12 hours, then washed thoroughly with deionized water and dried in a forced-air drying oven at 60°C for 6 hours to obtain a polyphenylene sulfide / aramid nanofiber composite film.

[0040] (5) After testing, the thickness of the obtained composite film was 25 μm and the basis weight was 42 g / m. 2 The tensile breaking strength is 48 MPa, the elongation at break is 6.4%, and the surface shows no obvious wrinkles after being treated in an oven at 180℃ for 30 min. The calculated thermal shrinkage rate is 2.2%.

[0041] Example 4 (1) Take short polyphenylene sulfide fibers (diameter 8-13μm, length 3-8mm, polyphenylene sulfide molecular weight 37000) and prepare a basis weight of 70g / m² by wet papermaking process. 2 A 0.5 mm thick polyphenylene sulfide fiber paper was dried in an oven at 70°C for 6 hours. Then, a 3.0 g / L aramid nanofiber (10-30 nm in diameter, 30-50 μm in length) / DMSO dispersion was coated onto its surface. The coating speed was 0.8 m / min, and the coating amount was 1.5 L / m². 2 The membrane was then soaked in deionized water at 30°C for 24 hours, and then dried at 45°C for 24 hours to obtain a composite membrane for later use.

[0042] (2) Weigh polyphenylene sulfide powder (molecular weight 70000), benzophenone and dibutyl phthalate into a three-necked flask at mass fractions of 16%, 76% and 8% respectively. Turn on the heating to 255°C, turn on the mechanical stirring at 600 r / min and stir for 7 min to obtain a homogeneous solution. Then cool in an ice water bath to completely solidify, and then mechanically crush at 8000 r / min for 2 min to obtain adhesive powder.

[0043] (3) Using a PI film with a thickness of 150 μm as the base film, the composite film prepared in step (1) is attached to the surface of the base film. The prepared adhesive powder is evenly spread on the surface of the composite film using a sieve, with a spreading amount of 220 g / m. 2 Subsequently, a polyphenylene sulfide / aramid nanofiber wet film was prepared by hot pressing at 230°C, 10MPa, and 120s. The obtained wet film was then immersed and washed in ethanol at 50°C for 12 hours. After removing the PI film, the film was dried and then subjected to a second hot pressing at 230°C, 10MPa, and 120s to obtain the nascent composite film.

[0044] (4) The obtained nascent composite film was soaked in 6% hydrogen peroxide at 50°C for 6 hours, then taken out and thoroughly washed with deionized water, and dried in a forced-air drying oven at 60°C for 6 hours to obtain a polyphenylene sulfide / aramid nanofiber composite film.

[0045] (5) After testing, the thickness of the obtained composite film was 32 μm and the basis weight was 51 g / m. 2 The tensile breaking strength is 39 MPa, the elongation at break is 2.9%, and the surface shows no obvious wrinkles after being treated in an oven at 180℃ for 30 min. The calculated thermal shrinkage rate is 5.2%.

[0046] Example 5 (1) Take short polyphenylene sulfide fibers (diameter 8-13μm, length 3-8mm, polyphenylene sulfide molecular weight 37000) and prepare 80g / m² fibers by wet papermaking process. 2A 0.5 mm thick polyphenylene sulfide fiber paper was dried in an oven at 70°C for 6 hours. Then, a 3.0 g / L aramid nanofiber (10-30 nm in diameter, 30-50 μm in length) / DMSO dispersion was coated onto its surface. The coating speed was 0.8 m / min, and the coating amount was 1.5 L / m². 2 The membrane was then soaked in deionized water at 30°C for 24 hours, and then dried at 45°C for 24 hours to obtain a composite membrane for later use.

[0047] (2) Weigh polyphenylene sulfide powder (molecular weight 70000), caprolactam and dibutyl phthalate into a three-necked flask at mass fractions of 16%, 76% and 8% respectively. Turn on the heating to 255°C and turn on the mechanical stirring at 600 r / min for 7 min to obtain a homogeneous solution. Then, cool it in an ice water bath to completely solidify it. Finally, use mechanical pulverization at 8000 r / min for 2 min to obtain the adhesive powder.

[0048] (3) Using a PI film with a thickness of 150 μm as the base film, the composite film prepared in step (1) is attached to the surface of the base film. The prepared adhesive powder is evenly spread on the surface of the composite film using a sieve, with a spreading amount of 220 g / m. 2 Subsequently, a polyphenylene sulfide / aramid nanofiber wet film was prepared by hot pressing at 220°C, 10MPa, and 120s. The obtained wet film was then immersed and washed in deionized water at 50°C for 12 hours. After removing the PI film, the film was dried and then subjected to a second hot pressing at 220°C, 12MPa, and 60s to obtain the nascent composite film.

[0049] (4) The nascent composite film was soaked in a 15% sodium hypochlorite solution at 50°C for 6 hours, then removed and thoroughly washed with deionized water, and dried in a forced-air drying oven at 60°C for 6 hours to obtain a polyphenylene sulfide / aramid nanofiber composite film.

[0050] (5) After testing, the thickness of the obtained composite film was 35 μm and the basis weight was 48 g / m. 2 The tensile breaking strength is 39 MPa, the elongation at break is 5.1%, and the surface wrinkles slightly after being treated in an oven at 180℃ for 30 min. The calculated thermal shrinkage rate is 3.9%.

[0051] Example 6 (1) Take short polyphenylene sulfide fibers (diameter 8-13μm, length 3-8mm, polyphenylene sulfide molecular weight 37000) and prepare 50g / m² by wet papermaking process. 2A 0.4 mm thick polyphenylene sulfide fiber paper was dried in an oven at 70°C for 6 hours. Then, a 2.5 g / L aramid nanofiber (10-30 nm in diameter, 30-50 μm in length) / DMSO dispersion was coated onto its surface. The coating speed was 1.2 m / min, and the coating amount was 1.5 L / m². 2 The membrane was then soaked in deionized water at 30°C for 24 hours, and then dried at 45°C for 24 hours to obtain a composite membrane for later use.

[0052] (2) Weigh polyphenylene sulfide powder (molecular weight 70000), benzophenone and dibutyl sebacate into a three-necked flask with mass fractions of 14%, 78% and 8% respectively. Turn on the heating to 255°C and turn on the mechanical stirring at 600 r / min for 7 min to obtain a homogeneous solution. Then, cool it in an ice water bath to completely solidify it. Finally, use mechanical pulverization at 8000 r / min for 2 min to obtain the adhesive powder.

[0053] (3) Using a PI film with a thickness of 150 μm as the base film, the composite film prepared in step (1) is attached to the surface of the base film. The prepared adhesive powder is evenly spread on the surface of the composite film using a sieve, with a spreading amount of 240 g / m. 2 Subsequently, a polyphenylene sulfide / aramid nanofiber wet film was prepared by hot pressing at 220°C, 12MPa, and 120s. The obtained wet film was then immersed and washed in ethanol at 50°C for 12 hours, dried, and subjected to a second hot pressing at 220°C, 12MPa, and 120s to obtain a nascent composite film.

[0054] (4) The obtained nascent composite film was soaked in 12% hydrogen peroxide at 60°C for 6 hours, then taken out and thoroughly washed with deionized water, and dried in a forced-air drying oven at 60°C for 6 hours to obtain a polyphenylene sulfide / aramid nanofiber composite film.

[0055] (5) After testing, the thickness of the obtained composite film was 32 μm and the basis weight was 35 g / m. 2 The tensile breaking strength is 46 MPa, the elongation at break is 3.9%, and the surface shows no obvious wrinkles after being treated in an oven at 180℃ for 30 min. The calculated thermal shrinkage rate is 4.8%.

[0056] Example 7 (1) Take short polyphenylene sulfide fibers (diameter 8-13μm, length 3-8mm, polyphenylene sulfide molecular weight 37000) and prepare 50g / m² by wet papermaking process. 2A 0.4 mm thick polyphenylene sulfide fiber paper was dried in an oven at 70°C for 6 hours. Then, a 2.5 g / L aramid nanofiber (10-30 nm in diameter, 30-50 μm in length) / DMSO dispersion was coated onto its surface. The coating speed was 1.2 m / min, and the coating amount was 1.5 L / m². 2 The membrane was then soaked in deionized water at 30°C for 24 hours, and then dried at 45°C for 24 hours to obtain a composite membrane for later use.

[0057] (2) Weigh polyphenylene sulfide powder (molecular weight 70000), benzophenone and dibutyl sebacate into a three-necked flask with mass fractions of 14%, 78% and 8% respectively. Turn on the heating to 255°C and turn on the mechanical stirring at 600 r / min for 7 min to obtain a homogeneous solution. Then, cool it in an ice water bath to completely solidify it. Finally, use mechanical pulverization at 8000 r / min for 2 min to obtain the adhesive powder.

[0058] (3) Using a PI film with a thickness of 150 μm as the base film, the composite film prepared in step (1) is attached to the surface of the base film. The prepared adhesive powder is evenly spread on the surface of the composite film using a sieve, with a spreading amount of 260 g / m. 2 Subsequently, a polyphenylene sulfide / aramid nanofiber wet film was prepared by hot pressing at 200℃, 12MPa, and 120s. The obtained wet film was then immersed and washed in ethanol at 50℃ for 12h. After removing the PI film, it was dried and then subjected to a second hot pressing at 220℃, 12MPa, and 180s to obtain the nascent composite film.

[0059] (4) The obtained nascent composite film was soaked in 18% hydrogen peroxide at 60°C for 6 hours, then taken out and thoroughly washed with deionized water, and dried in a forced-air drying oven at 60°C for 6 hours to obtain a polyphenylene sulfide / aramid nanofiber composite film.

[0060] (5) After testing, the thickness of the obtained composite film was 28 μm and the basis weight was 42 g / m. 2 The tensile breaking strength is 32 MPa, the elongation at break is 4.2%, and the surface shows no obvious wrinkles after being treated in an oven at 180℃ for 30 min. The calculated thermal shrinkage rate is 3.1%.

[0061] Any aspects not covered in this invention are applicable to existing technologies.

Claims

1. A method for preparing a polyphenylene sulfide / aramid nanofiber composite film, characterized in that, The preparation method includes the following steps: (1) Preparation of polyphenylene sulfide fiber / aramid nanofiber composite membrane: Polyphenylene sulfide short fibers are used to prepare polyphenylene sulfide fiber paper by wet papermaking process. After drying, aramid nanofiber / DMSO dispersion is coated on its surface, and then it is soaked in water to solidify. After drying, polyphenylene sulfide fiber / aramid nanofiber composite membrane is obtained. (2) Preparation of adhesive: Using a good solvent and a bad solvent as a composite solvent, the polyphenylene sulfide powder polymer, the good solvent and the bad solvent are mixed, and after purging with nitrogen to remove oxygen, the temperature is raised to 250-257 ℃ and stirred continuously for 5-10 min to completely dissolve and form a homogeneous solution. After cooling and curing, the adhesive powder is obtained by mechanical crushing. (3) Preparation of polyphenylene sulfide / aramid nanofiber composite film: Using PI film as base film, the composite film prepared in step (1) is attached to the surface of the base film, and the adhesive powder prepared in step (2) is evenly spread on the surface of the composite film. Then, a polyphenylene sulfide / aramid nanofiber wet film is prepared by hot pressing. The obtained wet film is soaked and washed in the extractant, dried and then hot pressed a second time to obtain the nascent composite film. Then, it is oxidized and washed thoroughly with water and dried to obtain the polyphenylene sulfide / aramid nanofiber composite film.

2. The method for preparing a polyphenylene sulfide / aramid nanofiber composite film according to claim 1, characterized in that, In step (1), the polyphenylene sulfide fiber has a diameter of 8-13 μm, a length of 3-8 mm, and a molecular weight of 3.7-5.0 W for the polyphenylene sulfide powder polymer; the drying temperature of the polyphenylene sulfide fiber paper is 50-150℃, and the drying time is 0.5-24 h; the thickness of the polyphenylene sulfide fiber paper obtained by wet papermaking is 0.2-1.0 mm, and the basis weight is 40-120 g / m². 2 The aramid nanofibers have a diameter of 10-30 nm, a length of 30-50 μm, and an aspect ratio of 1000-5000; the concentration of the aramid nanofiber / DMSO dispersion is 0.5-10 g / L; the coating method is at least one of doctor blade coating, roller coating, and slot extrusion coating, with a speed of 0.3-2 m / min and a coating amount of 0.5-3 L / m 2 The soaking time in water for curing is 12-48 hours, and the temperature is 20-35℃; the drying temperature after curing is 20-70℃, and the drying time is 12-48 hours.

3. The method for preparing a polyphenylene sulfide / aramid nanofiber composite film according to claim 1, characterized in that, In step (2), the benign solvent is at least one of N-methylpyrrolidone, benzophenone, benzoin, caprolactam, diphenyl sulfone, 1-chloronaphthalene, and diphenyl ether; the inferior solvent includes at least one of dibutyl phthalate, dibutyl sebacate, dioctyl phthalate, dioctyl sebacate, diethyl isophthalate, dibutyl isophthalate, dioctyl isophthalate, glycerol, and polyethylene glycol.

4. The method for preparing a polyphenylene sulfide / aramid nanofiber composite film according to claim 1, characterized in that, In step (2), the molecular weight of the polyphenylene sulfide powder polymer is 6-8W; the sum of the mass of the good solvent, the bad solvent, and the polyphenylene sulfide resin is 100%, the proportion of polyphenylene sulfide powder resin is 5-18%, the proportion of the good solvent is 60-85%, and the proportion of the bad solvent is 0-20%; the cooling method is at least one of air curing, water bath curing, and liquid nitrogen curing; the mechanical pulverization temperature is 0-25℃, the pulverization time is 0.5-10min, and the pulverization speed is 4000-12000r / min.

5. The method for preparing a polyphenylene sulfide / aramid nanofiber composite film according to claim 1, characterized in that, In step (3), the thickness of the PI base film is 50-300 μm; the spreading method is at least one of screen spreading, roller spreading, metering roller spreading, electrostatic spreading, and airflow spreading; the amount of adhesive powder spread is 50-500 g / m³. 2 The temperature of the first hot pressing is 120-240 ℃, the pressure is 2-18 MPa, and the hot pressing time is 10-300 s; the temperature of the second hot pressing is 160-230 ℃, the pressure is 8-20 MPa, and the hot pressing time is 10-300 s.

6. The method for preparing a polyphenylene sulfide / aramid nanofiber composite film according to claim 1, characterized in that, In step (3), the solvent used for extraction and washing is at least one of water, alcohol solvents, halogenated hydrocarbon solvents, ester solvents, hydrocarbon solvents, and amide solvents; the alcohol solvent is at least one of ethanol, propanol, isopropanol, butanol, isobutanol, and benzyl alcohol; the halogenated hydrocarbon solvent is at least one of tetrachloromethane, 1,2-dichloroethane, trichloroethane, and tetrahydrofuran; the ester solvent is at least one of ethyl acetate, butyl acetate, ethyl benzoate, ethyl formate, dimethyl carbonate, diethyl carbonate, dibutyl carbonate, and dipropyl carbonate; the hydrocarbon solvent is at least one of n-hexane, cyclohexane, benzene, and toluene; the amide solvent is at least one of dimethylformamide, N,N-dimethylformamide, N,N-diethylacetamide, and N-methylpyrrolidone; and the solvent temperature is 50-70 °C.

7. The method for preparing a polyphenylene sulfide / aramid nanofiber composite film according to claim 1, characterized in that, In step (3), the reagent used in the oxidation process is at least one of potassium permanganate, hydrogen peroxide, sodium hypochlorite, nitric acid, and sodium perchlorate; the temperature in the oxidation process is 30-60℃ and the treatment time is 0.5-24 h; the drying temperature is 50-150℃ and the drying time is 0.5-24 h.

8. The phenyl sulfide / aramid nanofiber composite film prepared by the preparation method according to any one of claims 1-7.