Preparation method of high-purity molybdenum trioxide

By combining multi-stage purification with precise calcination processes, and using quartz boats with complexing impurity removers and composite coatings, the problems of incomplete impurity removal and crystal morphology control in molybdenum trioxide production have been solved, achieving the preparation of high-purity molybdenum trioxide, which is suitable for high-end catalysis and semiconductor industries.

CN122254556APending Publication Date: 2026-06-23ANQING YUETONG MOLYBDENUM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610345499.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-03-20
Publication Date
2026-06-23
Patent Text Reader

Abstract

The application relates to the technical field of molybdenum trioxide production, and particularly discloses a preparation method of high-purity molybdenum trioxide. The method comprises the following steps: preparing a complexing impurity removing agent by taking diatomite, citric acid, ethylenediaminetetraacetic acid disodium and tartaric acid as raw materials; dissolving industrial ammonium dimolybdate to obtain an ammonium molybdate solution, adding the impurity removing agent into the ammonium molybdate solution, complexing impurities under an acidic condition, and deeply removing the impurities through flocculation and precision filtration; adjusting the alkalinity of the filtrate, and cooling and crystallizing the filtrate to obtain high-purity ammonium molybdate; and finally performing program-controlled temperature calcination in an atmosphere with a specific oxygen content by using a quartz boat coated with a composite coating on the inner wall, so as to obtain high-purity molybdenum trioxide. The application combines multi-stage purification with an accurate calcination process, can efficiently remove impurities in raw materials, and has stable process flow; the obtained molybdenum trioxide product has high purity, good crystal morphology, good process stability and good industrialization prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of molybdenum trioxide production technology, and more specifically, to a method for preparing high-purity molybdenum trioxide. Background Technology

[0002] Molybdenum trioxide (Mo) is an important inorganic functional material with wide applications in catalysts, electronic materials, anti-corrosion pigments, and energy storage. Its purity and physicochemical properties directly affect the performance of end products. In particular, the high-end catalysis and semiconductor industries have imposed stringent requirements on the purity, crystal morphology, and impurity content of Mo. trioxide.

[0003] Currently, the mainstream industrial process for producing molybdenum trioxide (MoTrioxide) is still the thermal decomposition method using ammonium molybdate. This process typically starts with molybdenum concentrate, proceeds through pyrometallurgical roasting or wet leaching to obtain crude molybdate, which is then purified and acid-precipitated to convert into ammonium molybdate intermediates, finally yielding MoTrioxide through calcination. However, traditional pyrometallurgical roasting processes generate large amounts of sulfur dioxide gas, causing environmental pollution, and are difficult to process low-grade or complex ores. While hydrometallurgical technologies, such as high-pressure oxygen-alkali leaching or nitric acid oxidation, mitigate gas pollution to some extent, they generally suffer from long process flows, high reagent consumption, and low metal recovery rates. To improve the purity of MoTrioxide, various purification technologies have been developed. For example, ion exchange resins are used for deep purification of molybdate solutions, or high-purity ammonium molybdate is prepared through multiple recrystallizations before calcination. Although ion exchange methods offer good purification results, the resin is expensive, the regeneration process is complex, and it is not suitable for processing initial raw materials with high impurity content. The multiple recrystallization process is cumbersome, resulting in a low direct molybdenum yield and difficulty in completely removing certain impurity ions. Furthermore, while sublimation purification of molybdenum trioxide is available, effectively separating some volatile impurities and obtaining high-purity products, it requires sophisticated equipment, consumes significant energy, and struggles to precisely control the crystal morphology and particle size distribution of the product. In the final thermal decomposition stage, conventional calcination processes are often carried out in a simple air atmosphere; improper temperature control can easily lead to product sintering and agglomeration, uneven particle size distribution, and even the reduction of some molybdenum trioxide to low-valence molybdenum oxide due to localized reducing atmospheres, affecting product purity and color. Therefore, this invention provides a method for preparing high-purity molybdenum trioxide to solve the aforementioned technical problems. Summary of the Invention

[0004] The purpose of this invention is to provide a method for preparing high-purity molybdenum trioxide. By combining multi-stage purification with precise calcination, impurities in the raw materials can be efficiently removed. At the same time, the process is stable, and the resulting molybdenum trioxide product has high purity and good crystal morphology, with good process stability and industrialization prospects.

[0005] This invention provides a method for preparing high-purity molybdenum trioxide, employing the following technical solution:

[0006] S1. Disperse diatomaceous earth in deionized water, add citric acid, adjust the pH to 5-6, and reflux at 85-90℃ and 240-300rpm for 2-4 hours. Then add tartaric acid and react for 30-40 minutes. Add disodium ethylenediaminetetraacetate and continue the reaction for 1-3 hours. After centrifugation, washing, and vacuum drying, obtain the complexing impurity remover.

[0007] S2. Dissolve industrial-grade ammonium dimolybdate in deionized water, heat to 55-60℃, and stir at 280-320 rpm for 45-50 min to obtain an ammonium dimolybdate solution. Add a complexing and impurity-removing agent to the solution, adjust the pH to 4.5-5.0 with 1.5M dilute hydrochloric acid, keep warm and stir for 1-2 h, then add polyacrylamide, stir slowly at 100-110 rpm for 10-15 min, and let it stand for 45-50 min to settle. Use a precision filter press with a filter membrane pore size ≤0.5μm to completely filter the mixture, collect the filtrate, and wash the filter cake with deionized water in small amounts several times. The washing liquid is added to the main filtrate.

[0008] S3. Adjust the pH of the filtrate obtained in S2 to 8-9 with ammonia water, cool it to 8-12℃ at 0.5℃ / min, crystallize at constant temperature for 2-3 hours, then centrifuge, wash, and vacuum dry to obtain high-purity ammonium molybdate crystals.

[0009] S4. The high-purity ammonium molybdate crystals obtained in S3 are loaded into a quartz boat with a composite coating on the inner wall and placed in a tube furnace. First, nitrogen is introduced to purge the air, and then the mixture of oxygen and air with an oxygen volume fraction of 60-65% is switched. The temperature is first raised to 370-380℃ at 5℃ / min and held for 1-2 hours. Then, the temperature is raised to 580-600℃ at 3℃ / min and held for 2-3 hours. Finally, the temperature is lowered to 460-480℃ at 2℃ / min and held for 40-50 minutes to obtain high-purity molybdenum trioxide.

[0010] Preferably, the composite coating preparation step in step S4 is as follows:

[0011] A1. Disperse nano-zirconia and aluminum isopropoxide in anhydrous ethanol, stir and react at 60-65℃ and 400-500rpm for 2-3h, add deionized water dropwise to form aluminum hydroxide colloid, heat to 80-85℃ to evaporate the solvent, calcine at 400-410℃ for 1-1.5h, cool and redisperse in an ethanol aqueous solution, adjust the pH to 4.5-5.5 with acetic acid, add KH560, react at 60-65℃ for 2-3h, centrifuge, wash, vacuum dry, and pulverize by air jet milling to a particle size ≤40nm to obtain modified nano-zirconia;

[0012] A2. Disperse the modified nano-zirconia in deionized water, add sodium hexametaphosphate, and sonicate at 50-60 kHz for 20-30 min. Then add polyethylene glycol 400 and continue sonicating for 15-20 min. Transfer to a ball mill and ball mill at 250-300 rpm for 3-4 h. Take the slurry and centrifuge at 3000-3500 rpm for 15-20 min. Take the supernatant and add hydroxypropyl methylcellulose. Stir at 500-600 rpm for 10-15 min to obtain the nano-zirconia dispersion.

[0013] A3. Add yttrium oxide sol, nano-zirconia dispersion, cerium oxide, ethyl silicate, polydimethylsiloxane, and polyvinyl alcohol to a high-speed mixer and stir at 25-30℃ and 1200-1500rpm for 40-50min to obtain a coating slurry. Apply the slurry to the inner wall of a quartz boat using the dip-coating method, controlling the wet film thickness to 12-18μm. After standing at room temperature for 20-25min, pre-cur it at 80℃ for 30-40min, then dry it at 110-120℃ for 1.5-2h. Finally, raise the temperature to 580-600℃ at 3℃ / min and hold for 1-1.5h, then raise the temperature to 1250-1300℃ at 1℃ / min and hold for 4-5h. Then lower the temperature to 750-800℃ at 2℃ / min and hold for 1-2h. Finally, cool it to room temperature with the furnace to form a composite coating.

[0014] Preferably, in step S1, the ingredients are 10-15 parts by weight of diatomaceous earth, 35-40 parts of deionized water, 0.5-0.8 parts of citric acid, 0.6-0.9 parts of tartaric acid, and 1-3 parts of disodium ethylenediaminetetraacetate.

[0015] Preferably, step S2 comprises, by weight, 8-12 parts of industrial-grade ammonium dimolybdate, 15-20 parts of deionized water, 2-4 parts of complexing impurity remover and 0.04-0.08 parts of polyacrylamide.

[0016] Preferably, in step S2, the dissolution temperature is 55-60℃, the stirring speed is 280-320rpm, the dissolution time is 45-50min, the pH is adjusted to 4.5-5.5, the slow stirring speed is 100-110rpm, and the time is 10-15min, and the filter membrane pore size of the precision filter press is ≤0.5μm.

[0017] Preferably, in step S5, the oxygen volume fraction in the oxygen-air mixture is 60-65%; the programmed temperature calcination includes: heating to 370-380℃ at a rate of 5℃ / min and holding for 1-2 hours, then heating to 580-600℃ at a rate of 3℃ / min and holding for 2-3 hours, and finally cooling to 460-480℃ at a rate of 2℃ / min and holding for 40-50 minutes.

[0018] Preferably, step A1 comprises, by weight, 5-8 parts nano-zirconia, 2-3 parts aluminum isopropoxide, 20-25 parts anhydrous ethanol, 15-20 parts 75-80 wt% aqueous ethanol solution, and 0.4-0.7 parts KH560.

[0019] Preferably, step A2 comprises, by weight, 2-3 parts modified nano-zirconia, 15-20 parts deionized water, 0.05-0.08 parts sodium hexametaphosphate, 0.1-0.2 parts polyethylene glycol 400, and 0.03-0.06 parts hydroxypropyl methylcellulose.

[0020] Preferably, step A3 comprises, by weight, 10-12 parts of yttrium oxide sol, 3-5 parts of nano-zirconia dispersion, 0.8-1.2 parts of cerium oxide, 0.5-0.8 parts of ethyl silicate, 0.03-0.06 parts of polydimethylsiloxane, and 0.1-0.2 parts of polyvinyl alcohol.

[0021] In summary, the present invention has the following beneficial effects:

[0022] 1. This invention constructs a multi-stage purification and precise calcination process route, organically combining complexing impurity removers with stepwise purification and precise pyrolysis processes to form a complete high-purity molybdenum trioxide preparation process. This process addresses the problems of incomplete impurity removal, limited product purity, and difficulty in controlling crystal morphology in traditional methods. By using a complexing impurity remover under acidic conditions to target and bind impurity ions, combined with flocculation sedimentation and precision filtration, deep impurity removal is achieved, effectively solving the deficiency of weak impurity capture ability in conventional purification technologies. The subsequent alkali-adjusting crystallization process ensures the formation of high-purity ammonium molybdate intermediates, while the programmed temperature-controlled calcination under a specific oxygen content atmosphere avoids the risk of product sintering and agglomeration or reduction to low-valence molybdenum oxide at high temperatures, and also regulates the crystal growth environment. The entire process is stable and reliable, reducing uncertainties in the production process.

[0023] 2. The complexing impurity remover of this invention is prepared by synergistic compounding of diatomaceous earth, citric acid, disodium ethylenediaminetetraacetate (EDTA), and tartaric acid, constructing a multi-component synergistic impurity removal system. In this impurity remover, diatomaceous earth serves as a carrier, providing excellent dispersibility and adsorption. Citric acid adjusts the pH of the system to optimize the complexation reaction environment and simultaneously enhances the dissolution of impurity ions. Disodium EDTA and tartaric acid, with their strong complexing abilities, can form stable complexes with various metal impurity ions in the raw materials, effectively disrupting the dissolution balance of impurity ions. This multi-component synergistic system significantly improves the capture efficiency of impurity ions, solves the problem of incomplete impurity removal by traditional methods, and lays the foundation for efficient subsequent purification processes. Furthermore, the preparation process of this impurity remover is simple, cost-controllable, and easy to scale up for production and application.

[0024] 3. The composite coating of this invention is formed by combining various inorganic materials such as modified nano-zirconia, yttrium oxide sol, and cerium oxide with organic components such as ethyl silicate and polydimethylsiloxane through a specific process. This composite coating exhibits excellent thermal stability, chemical inertness, and anti-adhesion properties, significantly reducing the interaction between highly reactive molybdenum oxide and the carrier during calcination, avoiding the introduction of new impurities or product adhesion to the wall, thereby ensuring the high purity and ease of collection of the product. Detailed Implementation

[0025] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0026] Unless otherwise specified, the experimental methods used in the following examples are conventional methods, and the experimental materials used, unless otherwise specified, were all purchased from conventional biochemical reagent stores. All quantitative experiments in the following examples were performed in triplicate, and the data are the average of the three replicates or the average ± standard deviation.

[0027] Polyacrylamide, purchased from Shanghai Yuanye Biotechnology Co., Ltd., product number S31321;

[0028] Nano-zirconia, purchased from Hangzhou Jiupeng New Materials Co., Ltd., CAS No. ;

[0029] Polyethylene glycol 400 was purchased from Nanjing Kerunjiang Chemical Co., Ltd., CAS No. 25322-68-3;

[0030] Yttrium oxide sol, purchased from Hangzhou Jiupeng New Materials Co., Ltd., CAS No. 1314-36-9;

[0031] Ethyl silicate, purchased from Condis Chemical (Hubei) Co., Ltd., CAS No. 78-10-4;

[0032] Polydimethylsiloxane, purchased from Shanghai Yuanye Biotechnology Co., Ltd., product number S26896;

[0033] KH560, purchased from Shanghai Yuanye Biotechnology Co., Ltd., product number S15029;

[0034] Polyvinyl alcohol, purchased from Anhui Longyang Environmental Protection Technology Co., Ltd., CAS No. 9002-85.

[0035] Example 1

[0036] This embodiment provides a method for preparing high-purity molybdenum trioxide, using the following technical solution:

[0037] S1. Disperse 10 parts of diatomaceous earth in 35 parts of deionized water, add 0.5 parts of citric acid, adjust the pH to 6, and reflux at 85℃ and 240rpm for 4h. Then add 0.6 parts of tartaric acid, react for 40min, add 1 part of disodium ethylenediaminetetraacetate, and continue to react for 3h. After centrifugation, washing, and vacuum drying, obtain the complexing impurity removal agent.

[0038] S2. Dissolve 8 parts of industrial grade ammonium dimolybdate in 15 parts of deionized water, heat to 55℃, stir at 280 rpm for 50 min to obtain ammonium dimolybdate solution, add 2 parts of complexing impurity removal agent, adjust pH to 5.0 with 1.5M dilute hydrochloric acid, keep warm and stir for 2 h, then add 0.04 parts of polyacrylamide, stir slowly at 100 rpm for 15 min, let stand and settle for 50 min, use a precision filter press with a filter membrane pore size ≤0.5μm to completely filter the mixture, collect the filtrate, wash the filter cake with deionized water in small amounts and multiple times, and combine the washing liquid into the main filtrate;

[0039] S3. Adjust the pH of the filtrate obtained in S2 to 9 with ammonia water, cool it to 12℃ at 0.5℃ / min, crystallize at constant temperature for 3 hours, then centrifuge, wash, and vacuum dry to obtain high-purity ammonium molybdate crystals.

[0040] S4. The high-purity ammonium molybdate crystals obtained in S3 are loaded into a quartz boat with a composite coating on the inner wall and placed in a tube furnace. First, nitrogen is introduced to purge the air, and then the mixture of oxygen and air with an oxygen volume fraction of 60% is switched. The temperature is first raised to 370°C at 5°C / min and held for 2 hours, then raised to 580°C at 3°C / min and held for 3 hours, and finally lowered to 460°C at 2°C / min and held for 50 minutes to obtain high-purity molybdenum trioxide.

[0041] The preparation step of the composite coating in step S4 is as follows:

[0042] A1. Disperse 5 parts of nano-zirconia and 2 parts of aluminum isopropoxide in 20 parts of anhydrous ethanol, stir at 60℃ and 400 rpm for 3 h, add deionized water dropwise to form aluminum hydroxide colloid, heat to 80℃ to evaporate the solvent, calcine at 400℃ for 1.5 h, cool and redisperse in 15 parts of 80wt% ethanol aqueous solution, adjust pH to 5.5 with acetic acid, add 0.4 parts of KH560, react at 60℃ for 3 h, centrifuge, wash, vacuum dry, and pulverize by air jet to a particle size ≤40 nm to obtain modified nano-zirconia;

[0043] A2. Disperse 2 parts of modified nano-zirconia in 15 parts of deionized water, add 0.05 parts of sodium hexametaphosphate, sonicate at 50 kHz for 30 min, then add 0.1 parts of polyethylene glycol 400 and continue sonicating for 20 min. Transfer to a ball mill and ball mill at 250 rpm for 4 h. Take the slurry and centrifuge at 3000 rpm for 20 min. Take the supernatant and add 0.03 parts of hydroxypropyl methylcellulose. Stir at 500 rpm for 15 min to obtain nano-zirconia dispersion.

[0044] A3. Add 10 parts of yttrium oxide sol, 3 parts of nano-zirconia dispersion, 0.8 parts of cerium oxide, 0.5 parts of ethyl silicate, 0.03 parts of polydimethylsiloxane, and 0.1 parts of polyvinyl alcohol to a high-speed mixer and stir at 25°C and 1200 rpm for 50 min to obtain a coating slurry. Apply the slurry to the inner wall of a quartz boat using the dip coating method, controlling the wet film thickness to 18 μm. After standing at room temperature for 25 min, pre-cur it at 80°C for 40 min, then dry it at 110°C for 2 h. Finally, raise the temperature to 580°C at 3°C / min and hold for 1.5 h, then raise the temperature to 1250°C at 1°C / min and hold for 5 h, then lower the temperature to 750°C at 2°C / min and hold for 1 h. Finally, cool it to room temperature with the furnace to form a composite coating.

[0045] Example 2

[0046] This embodiment provides a method for preparing high-purity molybdenum trioxide, using the following technical solution:

[0047] S1. Disperse 12 parts of diatomaceous earth in 36 parts of deionized water, add 0.6 parts of citric acid, adjust the pH to 5.8, and reflux at 87℃ and 242rpm for 3.8h. Then add 0.7 parts of tartaric acid, react for 38min, add 1.2 parts of disodium ethylenediaminetetraacetate, and continue the reaction for 2.8h. After centrifugation, washing, and vacuum drying, obtain the complexing impurity removal agent.

[0048] S2. Dissolve 9 parts of industrial grade ammonium dimolybdate in 16 parts of deionized water, heat to 59℃, stir at 300 rpm for 48 min to obtain ammonium dimolybdate solution, add 2.5 parts of complexing impurity remover, adjust pH to 4.7 with 1.5M dilute hydrochloric acid, keep warm and stir for 1.8 h, then add 0.05 parts of polyacrylamide, stir slowly at 105 rpm for 13 min, let stand and settle for 48 min, use a precision filter press with a filter membrane pore size ≤0.5μm to completely filter the mixture, collect the filtrate, wash the filter cake with deionized water in small amounts and multiple times, and combine the washing liquid into the main filtrate;

[0049] S3. Adjust the pH of the filtrate obtained in S2 to 8.7 with ammonia water, cool it to 11℃ at 0.5℃ / min, crystallize at constant temperature for 2.8h, then centrifuge, wash, and vacuum dry to obtain high-purity ammonium molybdate crystals.

[0050] S4. The high-purity ammonium molybdate crystals obtained in S3 are loaded into a quartz boat with a composite coating on the inner wall and placed in a tube furnace. Nitrogen gas is first introduced to purge the air, and then the mixture of oxygen and air with an oxygen volume fraction of 62% is switched. The temperature is first raised to 375°C at 5°C / min and held for 1.8 hours, then raised to 582°C at 3°C / min and held for 2.9 hours, and finally lowered to 475°C at 2°C / min and held for 48 minutes to obtain high-purity molybdenum trioxide.

[0051] The preparation step of the composite coating in step S4 is as follows:

[0052] A1. Six parts of nano-zirconia and 2.4 parts of aluminum isopropoxide were dispersed in 22 parts of anhydrous ethanol and stirred at 62℃ and 420rpm for 2.8h. Deionized water was added dropwise to form aluminum hydroxide colloid. The solvent was evaporated at 82℃ and calcined at 402℃ for 1.4h. After cooling, the mixture was redispersed in 16 parts of 78wt% ethanol aqueous solution. The pH was adjusted to 4.8 with acetic acid. 0.5 parts of KH560 were added and reacted at 62℃ for 2.8h. After centrifugation, washing, vacuum drying, and air jet milling to a particle size ≤40nm, modified nano-zirconia was obtained.

[0053] A2. Disperse 2.4 parts of modified nano-zirconia in 16 parts of deionized water, add 0.06 parts of sodium hexametaphosphate, sonicate at 52 kHz for 28 min, then add 0.14 parts of polyethylene glycol 400 and continue sonicating for 18 min. Transfer to a ball mill and ball mill at 260 rpm for 3.8 h. Take the slurry and centrifuge at 3200 rpm for 18 min. Take the supernatant and add 0.04 parts of hydroxypropyl methylcellulose. Stir at 520 rpm for 14 min to obtain nano-zirconia dispersion.

[0054] A3. Add 11 parts of yttrium oxide sol, 4 parts of nano-zirconia dispersion, 0.9 parts of cerium oxide, 0.6 parts of ethyl silicate, 0.04 parts of polydimethylsiloxane, and 0.14 parts of polyvinyl alcohol to a high-speed mixer and stir at 26°C and 1300 rpm for 48 min to obtain a coating slurry. Apply the slurry to the inner wall of a quartz boat using the dip coating method, controlling the wet film thickness to 15 μm. After standing at room temperature for 24 min, pre-cur it at 80°C for 38 min, then dry it at 115°C for 1.7 h. Finally, raise the temperature to 590°C at 3°C / min and hold for 1.4 h, then raise the temperature to 1260°C at 1°C / min and hold for 4.8 h, then lower the temperature to 760°C at 2°C / min and hold for 1.8 h. Finally, cool it to room temperature with the furnace to form a composite coating.

[0055] Example 3

[0056] This embodiment provides a method for preparing high-purity molybdenum trioxide, using the following technical solution:

[0057] S1. Disperse 15 parts of diatomaceous earth in 40 parts of deionized water, add 0.8 parts of citric acid, adjust the pH to 5, and reflux at 90℃ and 300rpm for 2h. Then add 0.9 parts of tartaric acid, react for 30min, add 3 parts of disodium ethylenediaminetetraacetate, and continue to react for 1h. After centrifugation, washing, and vacuum drying, obtain the complexing impurity removal agent.

[0058] S2. Dissolve 12 parts of industrial grade ammonium dimolybdate in 20 parts of deionized water, heat to 60℃, stir at 320 rpm for 45 min to obtain ammonium dimolybdate solution, add 4 parts of complexing and impurity removal agent, adjust pH to 4.5 with 1.5M dilute hydrochloric acid, keep warm and stir for 1 h, then add 0.08 parts of polyacrylamide, stir slowly at 110 rpm for 10 min, let stand and settle for 45 min, use a precision filter press with a filter membrane pore size ≤0.5μm to completely filter the mixture, collect the filtrate, wash the filter cake with deionized water in small amounts and multiple times, and combine the washing liquid into the main filtrate;

[0059] S3. Adjust the pH of the filtrate obtained in S2 to 8 with ammonia water, cool it to 8℃ at 0.5℃ / min, crystallize at constant temperature for 2 hours, then centrifuge, wash, and vacuum dry to obtain high-purity ammonium molybdate crystals.

[0060] S4. The high-purity ammonium molybdate crystals obtained in S3 are loaded into a quartz boat with a composite coating on the inner wall and placed in a tube furnace. First, nitrogen is introduced to purge the air, and then the mixture of oxygen and air with an oxygen volume fraction of 65% is switched. The temperature is first raised to 380°C at 5°C / min and held for 1 hour, then raised to 600°C at 3°C / min and held for 2 hours, and finally lowered to 480°C at 2°C / min and held for 40 minutes to obtain high-purity molybdenum trioxide.

[0061] The preparation step of the composite coating in step S4 is as follows:

[0062] A1. Disperse 8 parts of nano-zirconia and 3 parts of aluminum isopropoxide in 25 parts of anhydrous ethanol, stir at 65℃ and 500 rpm for 2 h, add deionized water dropwise to form aluminum hydroxide colloid, heat to 85℃ to evaporate the solvent, calcine at 410℃ for 1 h, cool and redisperse in 20 parts of 75wt% ethanol aqueous solution, adjust pH to 4.5 with acetic acid, add 0.7 parts of KH560, react at 65℃ for 2 h, centrifuge, wash, vacuum dry, and pulverize by air jet to a particle size ≤40nm to obtain modified nano-zirconia;

[0063] A2. Disperse 3 parts of modified nano-zirconia in 20 parts of deionized water, add 0.08 parts of sodium hexametaphosphate, sonicate at 60 kHz for 20 min, then add 0.2 parts of polyethylene glycol 400 and continue sonicating for 15 min. Transfer to a ball mill and ball mill at 300 rpm for 3 h. Take the slurry and centrifuge at 3500 rpm for 15 min. Take the supernatant and add 0.06 parts of hydroxypropyl methylcellulose. Stir at 600 rpm for 10 min to obtain nano-zirconia dispersion.

[0064] A3. Add 12 parts of yttrium oxide sol, 5 parts of nano-zirconia dispersion, 1.2 parts of cerium oxide, 0.8 parts of ethyl silicate, 0.06 parts of polydimethylsiloxane, and 0.2 parts of polyvinyl alcohol to a high-speed mixer and stir at 30°C and 1500 rpm for 40 min to obtain a coating slurry. Apply the slurry to the inner wall of a quartz boat using the dip coating method, controlling the wet film thickness to 18 μm. After standing at room temperature for 20 min, pre-cur it at 80°C for 30 min, then dry it at 120°C for 1.5 h. Finally, raise the temperature to 600°C at 3°C / min and hold for 1 h, then raise the temperature to 1300°C at 1°C / min and hold for 4 h, then lower the temperature to 800°C at 2°C / min and hold for 1 h. Finally, cool it to room temperature with the furnace to form a composite coating.

[0065] Example 4

[0066] This embodiment provides a method for preparing high-purity molybdenum trioxide, using the following technical solution:

[0067] S1. Disperse 15 parts of diatomaceous earth in 35 parts of deionized water, add 0.8 parts of citric acid, adjust the pH to 5, and reflux at 90℃ and 300rpm for 3h. Then add 0.9 parts of tartaric acid, react for 35min, add 3 parts of disodium ethylenediaminetetraacetate, and continue to react for 1.5h. After centrifugation, washing, and vacuum drying, obtain the complexing impurity removal agent.

[0068] S2. Dissolve 12 parts of industrial-grade ammonium dimolybdate in 20 parts of deionized water, heat to 60℃, and stir at 320 rpm for 45 min to obtain ammonium dimolybdate solution. Add 3 parts of complexing and impurity removal agent to the solution, adjust the pH to 4.8 with 1.5M dilute hydrochloric acid, keep warm and stir for 1.2 h, then add 0.05 parts of polyacrylamide, stir slowly at 110 rpm for 12 min, and let stand for 45 min to settle. Use a precision filter press with a filter membrane pore size ≤0.5μm to completely filter the mixture, collect the filtrate, and wash the filter cake with deionized water in small amounts several times. The washing liquid is added to the main filtrate.

[0069] S3. Adjust the pH of the filtrate obtained in S2 to 8 with ammonia water, cool it to 8℃ at 0.5℃ / min, crystallize at constant temperature for 2.5h, then centrifuge, wash, and vacuum dry to obtain high-purity ammonium molybdate crystals.

[0070] S4. The high-purity ammonium molybdate crystals obtained in S3 are loaded into a quartz boat with a composite coating on the inner wall and placed in a tube furnace. Nitrogen gas is first introduced to purge the air, and then the mixture of oxygen and air with an oxygen volume fraction of 65% is switched. The temperature is first raised to 380°C at 5°C / min and held for 1 hour, then raised to 560°C at 3°C / min and held for 2 hours, and finally lowered to 460°C at 2°C / min and held for 40 minutes to obtain high-purity molybdenum trioxide.

[0071] The preparation step of the composite coating in step S4 is as follows:

[0072] A1. Disperse 8 parts of nano-zirconia and 3 parts of aluminum isopropoxide in 25 parts of anhydrous ethanol, stir at 65℃ and 450 rpm for 2.5 h, add deionized water dropwise to form aluminum hydroxide colloid, heat to 85℃ to evaporate the solvent, calcine at 400℃ for 1 h, cool and redisperse in 20 parts of 75wt% ethanol aqueous solution, adjust pH to 4.5 with acetic acid, add 0.6 parts of KH560, react at 62℃ for 2.2 h, centrifuge, wash, vacuum dry, and pulverize by air jet milling to a particle size ≤40 nm to obtain modified nano-zirconia;

[0073] A2. Disperse 3 parts of modified nano-zirconia in 20 parts of deionized water, add 0.08 parts of sodium hexametaphosphate, sonicate at 60 kHz for 20 min, then add 0.2 parts of polyethylene glycol 400 and continue sonicating for 15 min. Transfer to a ball mill and ball mill at 300 rpm for 3.5 h. Take the slurry and centrifuge at 3500 rpm for 18 min. Take the supernatant and add 0.05 parts of hydroxypropyl methylcellulose. Stir at 600 rpm for 12 min to obtain nano-zirconia dispersion.

[0074] A3. Add 12 parts of yttrium oxide sol, 4 parts of nano-zirconia dispersion, 1 part of cerium oxide, 0.6 parts of ethyl silicate, 0.05 parts of polydimethylsiloxane, and 0.17 parts of polyvinyl alcohol to a high-speed mixer and stir at 30°C and 1500 rpm for 40 min to obtain a coating slurry. Apply the slurry to the inner wall of a quartz boat using the dip coating method, controlling the wet film thickness to 15 μm. After standing at room temperature for 20 min, pre-cur it at 80°C for 30 min, then dry it at 110°C for 1.5 h. Finally, raise the temperature to 580°C at 3°C / min and hold for 1 h, then raise the temperature to 1250°C at 1°C / min and hold for 4 h, then lower the temperature to 750°C at 2°C / min and hold for 1.2 h. Finally, cool it to room temperature with the furnace to form a composite coating.

[0075] Comparative Example 1

[0076] A method for preparing high-purity molybdenum trioxide differs from Example 4 in that: no complexing and impurity-removing agent is prepared or added in step S1, i.e., the entire step S1 is omitted, and in step S2, dilute hydrochloric acid is directly added to the ammonium dimolybdate solution to adjust the pH before subsequent flocculation, filtration and crystallization operations are carried out, with other conditions being the same as in Example 4.

[0077] Comparative Example 2

[0078] A method for preparing high-purity molybdenum trioxide differs from Example 4 in that tartaric acid is omitted in the preparation of the complexing and impurity-removing agent. That is, in step S1, only diatomaceous earth, citric acid, and disodium ethylenediaminetetraacetate are added, without adding tartaric acid. Other conditions are the same as in Example 4.

[0079] Comparative Example 3

[0080] A method for preparing high-purity molybdenum trioxide differs from Example 4 in that diatomaceous earth is not used as a carrier when preparing the complexing impurity remover. That is, diatomaceous earth is not added in step S1. Instead, citric acid, disodium ethylenediaminetetraacetate, and tartaric acid are directly dissolved in deionized water and refluxed under the same pH and temperature conditions. Other conditions are the same as in Example 4.

[0081] Comparative Example 4

[0082] A method for preparing high-purity molybdenum trioxide differs from Example 4 in that the coating on the inner wall of the quartz boat used for calcination in step S4 is a common yttrium oxide coating, rather than a composite coating. That is, the inner wall of the quartz boat is coated with yttrium oxide sol only by immersion, drying, and high-temperature sintering to form the yttrium oxide coating. Other conditions are the same as in Example 4.

[0083] Comparative Example 5

[0084] A method for preparing high-purity molybdenum trioxide differs from Example 4 in that the nano-zirconia dispersion is omitted when preparing the composite coating; that is, the nano-zirconia dispersion is not added in the coating slurry preparation in step A3, while other conditions are the same as in Example 4.

[0085] Performance testing

[0086] The preparation methods of high-purity molybdenum trioxide in Examples 1-4 and Comparative Examples 1-5 were tested for performance, and the test results are shown in Table 1.

[0087] Table 1

[0088] Test Project Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 <![CDATA[MnO3 purity %]]> 99.98 99.99 99.99 99.99 99.85 99.93 99.90 99.96 99.97 Total impurities (ppm) 7.1 6.5 5.4 5.2 41.3 19.1 24.8 9.6 8.7

[0089] The test results show that the molybdenum trioxide products prepared in Examples 1-4 of this invention exhibit significant advantages in core performance indicators. This change fully demonstrates the precise control of each step in the process, including the composition and dosage of the complexing and impurity-removing agent, reaction conditions, and the precise control of the preparation and calcination procedures of the composite coating. These factors play a decisive role in deep purification and perfect crystal growth. The performance indicators of the comparative examples are significantly inferior to those of the examples, mainly due to the absence or simplification of key process steps.

[0090] The above description is merely an example and illustration of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described, or use similar methods to replace them, as long as they do not deviate from the invention or exceed the scope defined in the claims, all of which should fall within the protection scope of the present invention.

Claims

1. A method for preparing high-purity molybdenum trioxide, characterized in that, Includes the following steps: S1. Disperse diatomaceous earth in deionized water, add citric acid to adjust the pH of the system, reflux the reaction, add tartaric acid to react first, then add disodium ethylenediaminetetraacetate to continue the reaction, and obtain the complexing impurity remover by centrifugation, washing and vacuum drying. S2. Dissolve industrial grade ammonium dimolybdate in deionized water, heat and stir to dissolve to obtain ammonium dimolybdate solution, add complexing and impurity removal agent to it, adjust the pH of the system with dilute hydrochloric acid, keep warm and stir the reaction, then add polyacrylamide, stir slowly and let stand to settle, filter precisely to collect the filtrate, wash the filter cake and combine the washing liquid with the main filtrate. S3. Adjust the pH of the filtrate with ammonia water, cool it down and crystallize it at a constant temperature. After centrifugation, washing and vacuum drying, high-purity ammonium molybdate crystals are obtained. S4. Place the high-purity ammonium molybdate crystals in a quartz boat with a composite coating on the inner wall, put it into a tube furnace, first purge the air with nitrogen, then switch to a mixture of oxygen and air, calcine by programmed heating, and then cool down and hold the temperature to obtain high-purity molybdenum trioxide.

2. The method for preparing high-purity molybdenum trioxide according to claim 1, characterized in that, The preparation steps of the composite coating in step S4 are as follows: A1. Disperse nano-zirconia and aluminum isopropoxide in anhydrous ethanol, stir and react, then add deionized water dropwise to form aluminum hydroxide colloid, heat to evaporate the solvent, calcine and cool, redisperse the product in an ethanol-water solution, adjust the pH value with acetic acid, add KH560 to continue the reaction, and after the reaction, centrifuge, wash, vacuum dry, and air jet mill to obtain modified nano-zirconia. A2. Disperse the modified nano-zirconia in deionized water, add sodium hexametaphosphate and sonicate, then add polyethylene glycol 400 and continue sonication. Transfer the product to a ball mill for ball milling. After ball milling, take the slurry and centrifuge. Take the supernatant and add hydroxypropyl methylcellulose. Stir to obtain nano-zirconia dispersion. A3. Yttrium oxide sol, nano-zirconia dispersion, cerium oxide, ethyl silicate, polydimethylsiloxane and polyvinyl alcohol are added to a high-speed mixer and stirred to prepare a coating slurry. The coating slurry is coated onto the inner wall of a quartz boat by dip coating. After standing at room temperature, it is pre-cured and dried in sequence. Then it is heated and kept at room temperature, then heated and kept at room temperature, and finally cooled to room temperature with the furnace to form a composite coating on the inner wall of the quartz boat.

3. The method for preparing high-purity molybdenum trioxide according to claim 1, characterized in that, In step S1, the ingredients are 10-15 parts by weight of diatomaceous earth, 35-40 parts of deionized water, 0.5-0.8 parts of citric acid, 0.6-0.9 parts of tartaric acid, and 1-3 parts of disodium ethylenediaminetetraacetate.

4. The method for preparing high-purity molybdenum trioxide according to claim 1, characterized in that, In step S2, the ingredients are 8-12 parts by weight of industrial grade ammonium dimolybdate, 15-20 parts of deionized water, 2-4 parts of complexing impurity remover, and 0.04-0.08 parts of polyacrylamide.

5. The method for preparing high-purity molybdenum trioxide according to claim 1, characterized in that, In step S2, the dissolution temperature is 55-60℃, the stirring speed is 280-320rpm, the dissolution time is 45-50min, the pH is adjusted to 4.5-5.5, the slow stirring speed is 100-110rpm, and the time is 10-15min. The pore size of the filter membrane of the precision filter press is ≤0.5μm.

6. The method for preparing high-purity molybdenum trioxide according to claim 1, characterized in that, In step S4, the oxygen volume fraction in the oxygen-air mixture is 60-65%. The programmed temperature calcination process includes: heating to 370-380℃ at a rate of 5℃ / min and holding for 1-2 hours, then heating to 580-600℃ at a rate of 3℃ / min and holding for 2-3 hours, and finally cooling to 460-480℃ at a rate of 2℃ / min and holding for 40-50 minutes.

7. The method for preparing high-purity molybdenum trioxide according to claim 2, characterized in that, In step A1, the components by weight are 5-8 parts nano-zirconia, 2-3 parts aluminum isopropoxide, 20-25 parts anhydrous ethanol, 15-20 parts 75-80 wt% aqueous ethanol solution, and 0.4-0.7 parts KH560.

8. The method for preparing high-purity molybdenum trioxide according to claim 2, characterized in that, In step A2, the ingredients are 2-3 parts by weight of modified nano-zirconia, 15-20 parts of deionized water, 0.05-0.08 parts of sodium hexametaphosphate, 0.1-0.2 parts of polyethylene glycol 400, and 0.03-0.06 parts of hydroxypropyl methylcellulose.

9. The method for preparing high-purity molybdenum trioxide according to claim 2, characterized in that, In step A3, the ingredients are, by weight, 10-12 parts yttrium oxide sol, 3-5 parts nano-zirconia dispersion, 0.8-1.2 parts cerium oxide, 0.5-0.8 parts ethyl silicate, 0.03-0.06 parts polydimethylsiloxane, and 0.1-0.2 parts polyvinyl alcohol.