A friction-assisted composite anodic jet-electrodeposition device and method for large end face workpieces
By combining composite anode components with flexible friction-assisted technology, the uniformity and efficiency of bronze coating deposition on large end face workpieces were solved, achieving self-compensation of ions in the plating solution and stability of the electric field, thereby improving coating quality and production efficiency.
Patent Information
- Application Number
- CN202610036621.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-01-12
- Publication Date
- 2026-07-03
AI Technical Summary
Existing technologies make it difficult to achieve efficient deposition of bronze coatings and coordinated control of thickness/structure uniformity on large end face workpieces. Traditional electrodeposition suffers from problems such as difficulty in mass transfer of plating solution, uneven electric field distribution, and low deposition efficiency. Jet electrodeposition is prone to defects such as porosity and nodules, and the single anode design leads to uneven ion supply.
By employing a composite anode assembly that combines inert and active anodes and utilizing flexible friction-assisted technology to achieve self-compensation of ions in the plating solution and stability of the electric/flow field, a friction-assisted composite anode jet electrodeposition device for large end-face workpieces is designed. The device includes a motion control device, a plating solution purification and circulation system, a composite anode assembly, and a cathode rotation device.
It improves the uniformity and density of the coating, extends the service life of the plating solution, enhances deposition efficiency and coating quality, adapts to the needs of preparing coatings with diverse compositions, and broadens the process adaptability boundaries of the equipment.
Smart Images

Figure HSA0000302639890000011 
Figure HSA0000302639890000012 
Figure HSA0000302639890000021
Abstract
Description
Technical Field
[0001] This invention belongs to the field of jet electrodeposition, specifically relating to a friction-assisted composite anodic jet electrodeposition device for large end-face workpieces, and is suitable for depositing coatings on the surface of large end-face workpieces with diameters of 50 to 150 mm. Background Technology
[0002] With the continuous improvement of the performance requirements for key components in high-end equipment fields that rely on hydraulic transmission systems, such as aerospace, engineering machinery, rail transportation, marine power, and high-end automobile manufacturing, the demand for high-performance surface functional coatings for large end-face workpieces with diameters of 50-150mm (such as plunger pump distribution plates and diesel engine tappet end faces) is becoming increasingly urgent. Among many candidate coating systems, bronze coatings are widely used on friction pair surfaces under high load and low lubrication conditions due to their excellent wear resistance, friction reduction, and good conformability and embedding properties. However, how to achieve efficient deposition and synergistic control of thickness / structure uniformity of bronze coatings on large-size end faces remains a core technical bottleneck for current electroplating processes and a key scientific problem restricting its engineering application. Currently common coating preparation technologies struggle to balance efficiency and uniformity: hot / cold spraying is prone to uneven coating due to airflow vortices; arc spraying exhibits significant thickness polarization; laser cladding and welding have wide heat-affected zones and high deformation risks; chemical vapor deposition and physical vapor deposition (CVD / PVD) have low deposition rates and high costs. While traditional electrodeposition has the advantages of low cost and controllable composition, it has prominent bottlenecks when adapted to large end faces: on the one hand, the large area makes it difficult for the plating solution to transfer mass, the supply of cations on the cathode surface is uneven, and the limiting current density during the electrodeposition process is generally low, resulting in low deposition efficiency and difficulty in meeting the needs of mass production; on the other hand, the uneven distribution of electric field directly leads to uneven coating thickness and rough and porous surface, which seriously affects the performance.
[0003] Jet electrodeposition technology, with its unique mechanism of enhanced mass transfer through high-speed jets, significantly improves the limiting current density, effectively overcoming the bottleneck of low deposition efficiency on large-face workpieces (50-150mm in diameter) by traditional electrodeposition. It has become an important development direction for the efficient preparation of high-performance coatings. However, traditional jet electrodeposition is still prone to defects such as porosity, nodules, surface protrusions, and the "tip charging" effect, limiting its application in scenarios requiring high uniformity. Therefore, flexible friction-assisted technology has been introduced as a key optimization path: this method utilizes flexible media such as bio-bristles (e.g., horsehair, pig bristles), synthetic polymers (e.g., polyamide PA, polypropylene PP), or natural fibers (e.g., palm fiber) to achieve multiple synergistic effects through the dynamic relative movement of a brush and the cathode surface. On the one hand, it promptly removes adsorbed hydrogen bubbles and suspended impurities from the cathode surface, effectively suppressing the formation of defects such as pores and pinholes; on the other hand, it selectively shields micro-protrusion areas through frictional shear force, inhibiting their preferential growth and promoting the diffusion of metal ions into recessed areas, thereby achieving dynamic leveling of the coating. In addition, this process can refine grains, increase density, and significantly improve surface morphology, wear resistance, and corrosion resistance.
[0004] Nevertheless, the current coupling system of jet electrodeposition and flexible tribology still suffers from two interconnected core defects that severely limit its engineering applicability in multi-component systems such as bronze coatings:
[0005] Firstly, the design of the anode system is too simplistic, making it difficult to balance ion supply stability with electrochemical compatibility. If an active anode (such as a copper-tin alloy anode) is used, non-uniform dissolution inevitably occurs during electrodeposition, leading to dynamic changes in anode geometry and dimensions, which in turn disrupts the stability of the local electric and flow fields. More importantly, the difference in dissolution kinetics between copper and tin can easily cause an imbalance in the cation ratio in the plating bath, potentially resulting in the formation of Cu in localized areas. 2+ or Sn 2+ The enrichment or deficiency of ions. Under these conditions, even with the introduction of flexible friction assistance, the leveling mechanism will still have functional blind spots due to uneven ion supply: the micro-convex areas continue to deposit rapidly due to sufficient ion concentration, while the concave areas may have a lower deposition rate than the friction and wear rate due to insufficient metal ion supply, which will aggravate the uneven thickness and even cause local coating loss.
[0006] Secondly, while inert anodes possess excellent chemical stability, they cannot replenish the continuously consumed metal ions in the plating bath. This not only accelerates the decay of electrolyte components and shortens their service life, but also directly limits the deposition rate and composition controllability. Under conditions of continuously decreasing ion concentration, the dynamic balance of "deposition-leveling" upon which flexible friction relies is difficult to maintain: when the deposition rate is too low, the frictional action may exceed the material accumulation rate, leading to surface mechanical damage; simultaneously, due to limited metal nucleation and growth, the grain refinement effect is weakened, and the improvement in coating hardness and density is limited, making it difficult to meet the comprehensive performance requirements of high-end equipment coatings.
[0007] In summary, how to construct a composite anode system that combines compositional self-compensation capability with electrical / fluid field stability, and achieve synergistic optimization with a flexible friction-assisted mechanism, is a key scientific problem and technological challenge in overcoming the bottleneck of efficient and highly uniform preparation of large-face bronze coatings. The composite anode assembly in this invention employs a combination of active and inert anodes. The active anode maintains the ion balance of the plating solution through electrolytic dissolution, while the inert anode ensures uniform distribution of the electric and flow fields throughout the entire process. The synergy of these two components supports the achievement of the core technological objective. Summary of the Invention
[0008] This invention provides a friction-assisted composite anode jet electrodeposition device and method for large-face workpieces. Addressing the problems of uneven mass transfer in the electroplating solution, uneven electric field distribution, and rapid cation loss in existing jet electrodeposition methods, this invention, based on jet electrodeposition technology, independently develops a composite anode assembly and a cathode rotation device. Simultaneously, it relies on jet and friction assistance to improve the overall mechanical properties and surface quality of the coating, increasing the limiting current density and enabling rapid preparation of high-quality coatings on large-face workpieces. Furthermore, the electrolytic dissolution of bronze beads replenishes metal cations, maintaining a stable metal ion concentration in the plating solution, ensuring a uniform and dense coating, extending the service life of the plating solution, and improving production efficiency.
[0009] A flexible friction-coupled composite anodic jet electrodeposition apparatus and method for surface modification of large-end-face workpieces, the specific implementation steps of which are as follows:
[0010] S1: A friction-assisted composite anode jet electrodeposition device for large end face workpieces, including a motion control device, a plating solution purification and circulation system, a composite anode assembly, a cathode rotation device, a cathode clamp, and a plating solution constant temperature control device, etc.
[0011] S1-1: Motion Control Device: The core components include a cross slide table capable of bidirectional translation along the Y / Z axes, a drive motor, and matching transmission components. Automated control is achieved using a Leadshine Intelligent DMC1000 series multi-axis motion controller. Precise translation of the cross slide table enables alignment and calibration between the composite anode and the large-face workpiece; X-axis position adjustment is achieved through manual fine-tuning of the plating solution storage tank position.
[0012] S1-2: Plating Solution Purification and Circulation System: The core consists of a plating solution storage tank, submersible pump, filtration device, plating solution delivery pipeline, and flow meter with regulating valve. The plating solution storage tank has a water bath insulation structure nested on its outer side, which works in conjunction with the plating solution constant temperature control system to ensure the plating solution is always maintained within the set process temperature range. The flow meter with regulating valve integrates real-time flow monitoring and precise adjustment, dynamically matching the process parameters required for jet electrodeposition. The outer wall of the plating solution delivery pipeline is covered with a high-efficiency heat insulation layer, significantly reducing temperature loss of the plating solution during transportation. The end of the plating solution delivery pipeline is sealed and fixedly connected to the composite anode, ensuring a continuous and stable supply of plating solution after the anode is positioned and installed, thus guaranteeing the smooth operation of the jet electrodeposition process.
[0013] S1-3: Cathode Rotation Device: As the core mechanism driving the large-end-face workpiece to achieve stable rotational motion, it is mainly composed of a high-precision stepper motor, a high-efficiency worm gear transmission mechanism, a high-coaxiality deep groove ball bearing, and a rotating disk (501). The stepper motor outputs power at a rated speed of 900 r / min, which is reduced and increased in torque through the worm gear transmission mechanism (with a transmission ratio precisely set to 1:30 to 1:90), smoothly transmitting the power to the rotating disk. The positioning holes on the rotating disk drive the cathode fixture to rotate. The deep groove ball bearing has both radial support and axial positioning functions, effectively counteracting radial runout and axial movement during rotation, ensuring rotational accuracy, and preventing workpiece sway from affecting the uniformity of the coating. Through precise matching of the transmission ratio and motor speed, the large-end-face workpiece clamped on the cathode fixture is finally driven to rotate stably at a uniform speed of 10–30 r / min, providing a uniform relative motion basis for flexible friction assistance and enhancing the convection mass transfer effect of the plating solution.
[0014] S1-4: Cathode clamp: It is connected to the cathode rotation device for transmission. The clamp uses conductive set screws on both sides to fix the large end face workpiece. The part of the conductive set screw that contacts the clamp is made of insulating material. At the same time, the surface of the clamp is sprayed with a layer of insulating material to prevent the clamp from being corroded or damaged or having a coating deposited during the processing.
[0015] S1-5: Plating solution constant temperature control device: including heating rod and temperature controller, wherein the heating rod is connected to the temperature controller switch, the temperature controller is set to the target control temperature, and the temperature sensor of the temperature controller is placed in the plating solution storage tank to monitor the plating solution temperature and maintain the plating solution temperature at 40-50℃.
[0016] S2: Prepare the required electroplating solution in advance, put it into the plating solution storage tank, and control the temperature of the plating solution to 40-50℃ by heating rod and temperature controller. Wrap the outside of the plating solution delivery pipe with heat insulation cotton and adjust the pH of the plating solution to 10-11.
[0017] S3: A flexible friction pair is installed at the bottom of the inert anode, and bronze beads are filled into the annular cavity of the anode. A bronze rod is inserted into the bronze beads to ensure electrical conductivity.
[0018] S4: For the cathode substrate surface of large end face workpieces, gradient grinding and fine polishing are first performed to remove surface oxide scale, scratches and micro protrusions to ensure that the surface roughness of the substrate meets the standard. Subsequently, acetone, anhydrous ethanol and deionized water are used in stages for ultrasonic cleaning to dissolve oil stains, remove residual impurities and improve surface cleanliness, respectively. Finally, cold air drying is performed to remove the moisture and residual reagents adsorbed on the substrate surface and store it for later use.
[0019] S5: Before starting the coating deposition operation, start the submersible pump and connect its power circuit. With the help of a flow meter with adjustment function, adjust the flow rate of the plating solution jet to the preset process parameter range (6-15L / min). Then, turn on the cathode rotation mechanism to drive the clamped workpiece to gradually reach the target rotation speed of 10-30r / min. After maintaining the entire system in continuous and stable operation for a preset time, stop the machine. Through this pretreatment and debugging process, fully verify and ensure the operational coordination, parameter stability and process adaptability of each component of the equipment.
[0020] S6: Place the pretreated cathode workpiece in the cathode fixture to complete the positioning and fastening. Then connect the positive terminal of the electrodeposition power supply to the composite anode and the negative terminal to the conductive brush to ensure good electrode contact and stable conduction. Then drive the composite anode to the preset process position through the motion control device so that the distance between the inert anode and the workpiece processing end face is precisely controlled at 1.5 to 2 mm.
[0021] S7: Start the submersible pump and cathode rotation mechanism and put them into operation. After the system has been running stably for 2-4 minutes and the plating solution flow field and workpiece rotation state have met the process requirements, close the electrodeposition power supply circuit (set the current density to 8-12 A / dm²). 2 The electrodeposition process officially commences. During deposition, copper-tin alloy microspheres achieve controllable electrolytic dissolution through the conductivity of the bronze rod, dynamically replenishing the copper and tin cations lost in the plating solution and maintaining a stable ion concentration. Simultaneously, the flexible friction pair dynamically frictionally smooths the deposited coating as the workpiece rotates, achieving grain refinement and surface defect elimination. After the electrodeposition process is completed, the electrodeposition power supply is first turned off, then the cathode rotation mechanism is turned off, followed by the submersible pump. Finally, the workpiece is removed for cleaning and drying.
[0022] The friction-assisted composite anode jet electrodeposition device for large-end-face workpieces used in the above method includes: 1-Y and Z-axis transmission device, 2-aluminum profile frame, 3-cathode clamp, 4-conductive brush, 5-cathode rotation device, 6-power supply, 7-heating rod, 8-water bath, 9-submersible pump, 10-plating solution storage tank, 11-flow meter with regulating valve, 12-filtration device, 13-plating solution circulation pipe, 14-temperature controller, 15-composite anode assembly; 501-rotating disk, 502-waterproof bearing, 503-worm gear, 504-bearing, 505-turbine, 506-coupling, 507-housing, 508-stepper motor; 1501-bronze rod, 1502-bronze bead, 1503-guide element, 1504-inert contour anode, 1505-conductive set screw, 1506-anode cavity, 1507-anode cover.
[0023] The overall frame of the above device is constructed with aluminum profiles. The cathode clamp (3) is installed on the cathode rotating device and together with it on the plating solution storage tank (10). The plating solution storage tank can collect and store the electroplating solution flowing out of the large end face workpiece. Then, the plating solution is filtered by the filtration device and flows back to the plating solution storage tank. The plating solution storage tank has a built-in submersible pump (9) for transmitting the plating solution to the composite anode assembly (15) through the pipeline. The pipeline is equipped with a flow meter (11) with a regulating valve, which can regulate and monitor the flow rate of the plating solution in the pipeline.
[0024] Composite anode assembly: This is the core component of this design, and its specific structure and functions are as follows: 1. Sealing connection mechanism: The inert anode (1504) and the flow guide (1503) are fastened together, and a sealing gasket is installed at the joint surface of the two. The flow guide and the anode cavity (1506) are connected by threads, and a threaded sealing waterproof tape is installed in the middle, which can effectively block the penetration path of the electroplating solution and ensure the sealing of the device. 2. Conductive conduction mechanism: The anode wire is connected to the bronze rod (1501), which is located in the middle of the anode cavity. The anode cavity is filled with bronze beads. The bottom of the bronze rod is connected to the inert anode, realizing the conductive conduction between the anode and the bronze beads, and ensuring that the bronze beads dissolve slowly under the action of the electric field. 3. Integrated liquid supply and adaptation system: The bottom of the inert anode (1504) is equipped with an annular array flow channel (orifice diameter 3-5mm) to ensure uniform spraying of plating solution; by replacing bronze beads with different tin contents, it can adapt to the processing requirements of different plating layers. 4. Friction-assisted mechanism: including flexible friction pairs installed at the bottom of the inert anode, made of polytetrafluoroethylene, with 1 to 4 sets evenly arranged along the edge and radial direction of the anode; the workpiece is driven to rotate by the cathode rotation device to achieve dynamic relative friction between the friction pairs and the coating, which plays the role of hydrogen removal, impurity removal and coating leveling.
[0025] Beneficial effects: This invention provides a friction-assisted composite anodic jet electrodeposition apparatus and method for large-end-face workpieces, which has the following advantages compared with the prior art: 1. Based on existing jet electrodeposition technology, this invention independently designed a composite anode integrated structure, which specifically solves the problems of low mass transfer efficiency and uneven spatial distribution of plating solution that are common in the preparation of coatings on large end faces in traditional electrodeposition processes, and greatly improves the uniformity and timeliness of ion transport; at the same time, the inert anode adopts a static fixed arrangement to ensure the stability of the uniform distribution of electric field / flow field across the large end face. 2. This invention employs a composite configuration of copper-tin alloy microspheres (sacrificial active anode units) and an inert anode, overcoming the design limitations of traditional single anodes. During deposition, the copper-tin alloy microspheres achieve controllable dissolution through electrolysis, with their dissolution rate dynamically matching the consumption rate of metal ions in the plating solution, forming a self-replenishing ion system that continuously replenishes the plating solution with copper and tin cations, ensuring that the ion concentration remains stable over a long period. This design not only fundamentally avoids performance degradation caused by ion deficiency in the plating solution, significantly extending its service life, but also improves the uniformity and density of the coating composition through the balanced ion supply. Furthermore, it eliminates the need for additional ion concentration monitoring equipment and forced replenishment devices, simplifying the process and significantly enhancing process stability and reliability in mass production scenarios. 3. The cathode rotation device designed in this invention, in conjunction with the friction pair in the composite anode assembly, achieves dynamic friction without dead angles in the large end face plating, which can level the plating, remove hydrogen impurities, and refine grains. In addition, the composite anode assembly has the characteristics of quick disassembly and assembly, and can easily replace copper-tin alloy microspheres with different tin contents and adaptable friction pairs. It can accurately match the preparation requirements of diverse plating compositions and the processing scenarios of large end face workpieces with different structural types, significantly expanding the process adaptability boundary and application range of the device. Attached Figure Description
[0026] Figure 1 A schematic diagram of the assembly of a friction-assisted composite anode jet electrodeposition device for large end face workpieces;
[0027] Figure 2 A schematic diagram of the cathode rotation device in a friction-assisted composite anode jet electrodeposition apparatus for large-end-face workpieces;
[0028] Figure 3 A schematic diagram of the anode main assembly of a friction-assisted composite anode jet electrodeposition device for large end face workpieces;
[0029] In the diagram, 1-Y and Z-axis transmission device, 2-aluminum profile frame, 3-cathode clamp, 4-conductive brush, 5-cathode rotation device, 6-power supply, 7-heating rod, 8-water bath, 9-submersible pump, 10-plating solution storage tank, 11-flow meter with regulating valve, 12-filtration device, 13-plating solution circulation pipe, 14-temperature controller, 15-composite anode assembly; 501-rotating disk, 502-waterproof bearing, 503-worm gear, 504-bearing, 505-turbine, 506-coupling, 507-housing, 508-stepper motor; 1501-bronze rod, 1502-bronze bead, 1503-flow guide, 1504-inert contour anode, 1505-conductive set screw, 1506-anode cavity, 1507-anode cover. Detailed Implementation
[0030] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments, but it is not limited to the specific structure described in this embodiment.
[0031] like Figure 1 , Figure 2 and Figure 3 As shown, Figure 1 This is a 3D model assembly drawing of a friction-assisted composite anode jet electrodeposition device for large-end-face workpieces. Figure 2 This is a structural diagram of the cathode rotation device. Figure 3 This is a schematic diagram of the composite anode assembly; the following is an implementation description of the preparation of a copper-tin alloy coating on the surface of a large-end workpiece:
[0032] The first step is to prepare the required copper-tin alloy plating solution in advance and pour it into the plating solution storage tank; adjust the temperature of the plating solution to 40°C using a heater and temperature controller, and adjust the pH value of the plating solution to 10-11, then set it aside for use.
[0033] The second step is to pre-treat the large end face workpiece (73mm in diameter, made of 45 steel): first, grind and polish it with 400#→800#→1200#→1500# louvered grinding discs, then clean it and degrease it with alkaline cleaning solution (50g / L sodium hydroxide, 30g / L sodium carbonate) at 50℃ for 10 minutes. Then, clean the workpiece with acetone, alcohol and deionized water in sequence to remove surface oil and impurities. Finally, dry the workpiece for later use.
[0034] Third, start the submersible pump and cathode rotation device, adjust the flow meter valve to make the plating solution flow rate in the circulation pipe reach 10L / min, set the workpiece rotation speed to 15r / min and keep the device running for 4 minutes to ensure system stability, and then shut down the above equipment.
[0035] The fourth step is to clamp the workpiece on the cathode fixture, and then, in conjunction with the control system and manual adjustment, correctly position the composite anode to maintain a gap of 1.8mm between the inert anode and the end face of the workpiece.
[0036] Finally, connect the positive terminal of the electroplating power supply to the composite anode and the negative terminal to the conductive brush on the outside of the fixture. Start the submersible pump and cathode rotation device, and wait for the device to run stably for 3 minutes to ensure uniform distribution of the plating solution in the pipeline before turning on the electroplating power supply (current density 10A / dm³). 2 The plating process is then carried out. After the plating is completed, the electroplating power supply is turned off first, followed by the cathode rotation device and submersible pump. Finally, the main power supply of the device is cut off, and the workpiece is removed for subsequent processing and performance evaluation.
[0037] It should be noted in the description of this invention that the above description using a large-end-face workpiece as an example is intended to illustrate the implementation process of the device in detail and does not constitute a limitation on the scope of application of this invention. Specifically: regarding the anode configuration, the device can flexibly replace bronze beads with different tin contents to adapt to different plating compositions; regarding the type of plating, this device is not limited to preparing copper-tin alloy coatings, but can also adapt to the preparation of nickel and other metal or alloy platings by replacing the active anode beads with corresponding compositions (such as nickel beads); regarding the processing object, the shape of the large end face is not limited to a circle, and other regular large end face structures can also be adapted; regarding the friction form, the number and arrangement of friction pairs can be adjusted according to the end face size. All of the above adjustments are within the scope of the technical concept of this invention and are intended to reflect the adaptability and flexibility of the device and method.
Claims
1. A friction-assisted composite anode jet electrodeposition apparatus and method for large-end-face workpieces, comprising the following specific steps: First, a plating solution is prepared and adjusted to a set constant temperature; after the large-end-face workpiece to be processed undergoes grinding, polishing, degreasing, and cleaning pretreatment in sequence, it is clamped in a cathode fixture; the composite anode and the workpiece are aligned and calibrated; then, the cathode rotation device is started to drive the workpiece to rotate, the jet electrodeposition power supply is turned on, and the bronze beads replenish the metal cations in the plating solution through electrolytic dissolution, while the friction pair of the composite anode assembly synchronously performs dynamic friction on the deposited coating; after the processing is completed, the workpiece is cleaned and dried.
2. The apparatus and method according to claim 1, characterized in that, The pretreatment steps for large end face workpieces include: grinding and polishing with flap wheel grinding discs in sequence from small grit to large grit (400#→800#→1200#→1500#), cleaning and degreasing with alkaline washing solution, then cleaning with acetone, alcohol and deionized water in sequence, and finally drying for later use.
3. The apparatus and method according to claim 1, characterized in that, The device mainly includes: a motion control device, a plating solution purification and circulation system, a composite anode assembly, a cathode rotation device, a cathode clamp, and a plating solution constant temperature control device; wherein: the motion control system achieves precise positioning of the composite anode and the large-end-face workpiece through the movement of the cross slide; the plating solution constant temperature control device maintains the temperature of the plating solution; the plating solution circulation and filtration device controls the jet flow with filters, regulating valves, and flow meters to filter impurities simultaneously; the composite anode assembly is a combination of an inert anode and a copper-tin alloy active anode (soluble anode), and is equipped with a friction pair to cooperate with the cathode rotation to achieve dynamic friction of the plating layer; the cathode rotation device has the functions of clamping, positioning, and rotating the large-end-face workpiece.
4. The apparatus and method according to claim 3, characterized in that, The composite anode assembly (15) can be adapted to the electrodeposition requirements of different plating layers by replacing copper-tin alloy beads (1502) with different tin contents; at the same time, by designing various internal flow channel structures of the inert anode (1504) and installing different forms of friction pairs at its bottom, the flow field, mass transfer field, electric field and friction external force field can be coordinated and controlled, thereby improving the processing quality and deposition efficiency.
5. The apparatus and method according to claims 3 and 4, characterized in that, The composite anode assembly (15) is installed on the cross slide (1). The anode cavity (1506) in the composite anode assembly (15) is filled with bronze beads (1502). The bronze rod (1501) is located in the middle of the anode cavity and is surrounded by bronze beads (1502). The bottom is fixed to the inert anode (1504) to achieve electrical conductivity. The height of the anode cavity (1506) is 80-120 mm, and the filling density of the bronze beads (1502) is 80%-90% of the volume of the anode cavity (1506).
6. The apparatus and method according to claim 3, characterized in that, The cathode rotation device includes a stepper motor (508), a worm gear (503), a worm (505) transmission mechanism, and a deep groove ball bearing (504). The stepper motor (508) drives the cathode fixture (3) to rotate through the worm gear (503) and the worm (505). The bearing (504) ensures the rotation accuracy, and the workpiece rotation speed is controlled between 10 and 30 r / min.
7. The apparatus and method according to claim 3, characterized in that, The inert anode (1504) maintains a gap of 1.5-2mm with the end face of the large end face workpiece. The flow channels at the bottom of the inert anode (1504) are distributed in a ring array with a flow channel diameter of 3-5mm. The bronze beads (1502) have a diameter of 2-4mm and a tin content that matches the target plating layer (7-20wt.%).
8. The apparatus and method according to claim 3, characterized in that, The flow rate of the plating solution in the circulating filtration device is adjusted to 6-15 L / min, the temperature control device controls the temperature of the plating solution to 40-50℃, and the pH value of the plating solution is adjusted to 10-11.
9. The apparatus and method according to claims 1 to 8, characterized in that, Improve processing performance through the following methods: Design and fix the composite anode assembly, and ensure that the inert anode ensures uniform flow field and electric field distribution on the large end face; The mass transfer of the plating solution is enhanced by rotating the cathode, which increases the current density to accelerate the deposition rate, while ensuring uniform distribution of the plating solution on the large end face. By rotating the workpiece and using friction assistance, the deposited layer is dynamically rubbed to achieve grain refinement, hydrogen removal and impurity removal, and coating leveling. The copper-tin alloy beads are designed as active anodes, and the copper rod conducts electricity to replenish metal ions through electrolytic dissolution, thereby extending the life of the plating solution and improving the quality of the plating layer.