Polyester filaments, process for their production and use thereof
By adding specific components to the polyester filament copolymer system, the regularity of the polyester molecular chain is disrupted, forming a microstructure that is conducive to the retention and transport of water molecules. This solves the problem of insufficient moisture absorption and wicking properties of polyester filament, and improves the moisture absorption and wicking properties and wearing comfort of the fiber.
Patent Information
- Application Number
- CN202610626401.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-05-08
- Publication Date
- 2026-07-03
AI Technical Summary
Existing polyester filaments are difficult to achieve high moisture absorption and wicking properties, resulting in stuffiness and static electricity when worn.
By adding specific amounts of 1,4-cyclohexanediol, neopentyl glycol, and 2-methyl-2-propyl-1,3-propanediol to the copolymerization system of polyester filament, combined with sodium diethylene glycol isophthalate-5-sulfonate and bi-amino-terminated polyethylene glycol, the regularity of the polyester molecular chain is disrupted, forming a microstructure that is conducive to the retention and transport of water molecules.
It significantly improves the moisture absorption and wicking properties of polyester fibers, enhancing wearing comfort.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This application relates to the field of polyester textiles, and in particular to a polyester filament, its preparation method, and its application. Background Technology
[0002] Polyester (polyethylene terephthalate, PET) fiber is widely used in clothing fabrics due to its high strength, abrasion resistance, and wrinkle resistance. However, ordinary polyester has a compact molecular structure, high crystallinity, and lacks hydrophilic groups, resulting in poor moisture absorption and low moisture regain (only about 0.4%). This makes it prone to causing stuffiness and static electricity when worn, greatly affecting wearing comfort. Therefore, endowing polyester with excellent moisture absorption and wicking properties while maintaining its original excellent physical properties has always been a research hotspot in this field.
[0003] Currently, the main methods for improving the moisture absorption and wicking properties of polyester include physical modification and chemical modification. Physical modification methods, such as fiber shaping (cross-shaped, Y-shaped cross-sections, etc.), can increase wicking through capillary effect, but they can only solve the problem of moisture "conduction" and cannot solve the defect of insufficient moisture "absorption" capacity of the fiber itself, thus having limited improvement on moisture absorption and wicking properties.
[0004] Copolymerization modification in chemical modification methods introduces hydrophilic groups into the polyester macromolecular chain to improve the moisture absorption and wicking properties of the fiber. Existing chemical modification methods often focus on single-dimensional hydrophilic modification such as surface moisture absorption or wicking, making it difficult to achieve high moisture absorption and wicking effects, thus limiting their application scenarios. Summary of the Invention
[0005] The main purpose of this application is to propose a polyester filament, its preparation method and application, aiming to solve the problem that existing polyester filaments are difficult to achieve high moisture absorption and wicking.
[0006] In a first aspect, this application provides a polyester filament comprising the following components in parts by weight: 30-40 parts purified terephthalic acid, 15-20 parts ethylene glycol, 1.83-2.39 parts 1,4-cyclohexanediol, 0.39-0.51 parts neopentyl glycol, 0.62-1.06 parts 2-methyl-2-propyl-1,3-propanediol, 0.4-1.3 parts sodium diethylene glycol isophthalate-5-sulfonate, 1.9-2.8 parts diamino-terminated polyethylene glycol, 0.011-0.018 parts catalyst, and 0.011-0.018 parts additives.
[0007] By employing the above technical solution, adding specific amounts of 1,4-cyclohexanediol and neopentyl glycol to the copolymer system effectively disrupts the regularity of the polyester molecular chain, creating ample space for the residence of hydrophilic segments and water molecules. Combined with the addition of diethylene glycol isophthalate-5-sulfonate and diamino-terminated polyethylene glycol, the rapid moisture absorption and wicking effects are significantly enhanced. Furthermore, the sterically hindered side groups of 2-methyl-2-propyl-1,3-propanediol further disrupt the regularity of the molecular chain and may form microstructures in the fiber that facilitate moisture transport, increasing the contact and evaporation area for water molecules and contributing to improved rapid moisture absorption and surface drying. The synergistic effect of these components significantly enhances the moisture absorption and wicking properties of polyester fibers. It is understood that, under polycondensation conditions, the terminal amino groups can react with the carboxyl groups at the polyester chain ends to form amide bonds, thereby covalently integrating PEG segments into the polyester backbone.
[0008] Preferably, the polyester filament provided in this application comprises the following components in parts by weight: 35 parts purified terephthalic acid, 18 parts ethylene glycol, 1.83~2.39 parts 1,4-cyclohexanediol, 0.39~0.51 parts neopentyl glycol, 0.62~1.06 parts 2-methyl-2-propyl-1,3-propanediol, 0.4~1.3 parts sodium diethylene glycol isophthalate-5-sulfonate, 1.9~2.8 parts diamino-terminated polyethylene glycol, 0.015 parts catalyst, and 0.015 parts additive.
[0009] Optionally, the weight ratio of the 1,4-cyclohexanediol, the neopentyl glycol, and the 2-methyl-2-propyl-1,3-propanediol is (1.93~2.10):(0.45~0.49):(0.85~0.98).
[0010] Preferably, the weight ratio of the 1,4-cyclohexanediol, the neopentyl glycol, and the 2-methyl-2-propyl-1,3-propanediol is 2.1:0.45:0.85.
[0011] By adopting the above technical solution and controlling the ratio of 1,4-cyclohexanediol, neopentyl glycol and 2-methyl-2-propyl-1,3-propanediol, the moisture absorption and wicking properties of polyester fibers can be further improved.
[0012] Optionally, the weight ratio of the sodium diethylene glycol isophthalate-5-sulfonate to the biamino-terminated polyethylene glycol is (0.7~0.9):(2.3~2.5).
[0013] Preferably, the weight ratio of sodium diethylene glycol isophthalate-5-sulfonate to the diamino-terminated polyethylene glycol is 0.7:2.5.
[0014] By adopting the above technical solution and further optimizing the ratio of sodium diethylene glycol 5-sulfonate and bi-amino polyethylene glycol, the moisture absorption and wicking properties of polyester fibers can be effectively improved.
[0015] Optionally, the weight-average molecular weight of the diamino-terminated polyethylene glycol is 1000-4000.
[0016] Optionally, the diamino-terminated polyethylene glycol includes diamino-terminated polyethylene glycol with a weight average molecular weight of 1000, diamino-terminated polyethylene glycol with a weight average molecular weight of 2000, and diamino-terminated polyethylene glycol with a weight average molecular weight of 3400, and the weight ratio of the diamino-terminated polyethylene glycol with a weight average molecular weight of 1000, the diamino-terminated polyethylene glycol with a weight average molecular weight of 2000, and the diamino-terminated polyethylene glycol with a weight average molecular weight of 3400 is (1.5~2.0):(6~7):(1.5~2.0).
[0017] By adopting the above technical solution and compounding polyethylene glycol with different molecular weights and double-terminated amino groups, a gradient moisture-wicking network is formed inside the fiber, which not only improves the moisture wicking rate but also enhances the uniformity of moisture absorption.
[0018] Optionally, the additive includes a heat stabilizer.
[0019] Preferably, the heat stabilizer is triphenyl phosphate.
[0020] Optionally, the catalyst is selected from at least one of antimony glycolate and antimony trioxide.
[0021] Secondly, this application provides a method for preparing polyester filament as described in any of the above claims, comprising the following steps: S1. Mix purified terephthalic acid, ethylene glycol, catalyst and additives, and under a nitrogen protective atmosphere, control the temperature at 220~230℃ and the pressure at 0.2~0.4MPa, and stir the reaction for 1.5~2.5h to obtain the esterification reaction product. S2. Under normal pressure, add sodium diethylene isophthalate-5-sulfonate, bi-amino-terminated polyethylene glycol, 1,4-cyclohexanediol, neopentyl glycol and 2-methyl-2-propyl-1,3-propanediol, stir, and carry out polycondensation reaction under vacuum at 270~280℃. Discharge, cool, and granulate to obtain PET chips. S3. The PET chips obtained in step S2 are pre-crystallized, dried, melt-extruded, spun, stretched and shaped, and wound to obtain the polyester filament.
[0022] Optionally, in step S2, after adding sodium diethylene glycol isophthalate-5-sulfonate and bi-amino-terminated polyethylene glycol, the mixture is stirred for 10-30 min; after adding 1,4-cyclohexanediol and neopentyl glycol, the mixture is stirred for 10-30 min; and after adding 2-methyl-2-propyl-1,3-propanediol, the mixture is stirred for 20-40 min.
[0023] By adopting the above technical solution, sodium diethylene glycol isophthalate-5-sulfonate, biamino-terminated polyethylene glycol, 1,4-cyclohexanediol, neopentyl glycol and 2-methyl-2-propyl-1,3-propanediol are fed in a distributed manner. This timing control ensures the uniformity and stability of the copolymer product.
[0024] Thirdly, this application provides an application of polyester filament as described in any of the above claims in clothing fabrics.
[0025] By adopting the above technical solution, the polyester filament provided in this application is woven into clothing fabric, which has excellent moisture absorption and wicking properties, and improves the comfort of wearing.
[0026] In summary, this application includes at least the following beneficial technical effects: Adding specific amounts of 1,4-cyclohexanediol and neopentyl glycol to the copolymer system effectively disrupts the regularity of the polyester molecular chain, creating ample space for the retention of hydrophilic segments and water molecules. Combined with the addition of diethylene glycol 5-sulfonate and diamino-terminated polyethylene glycol, the rapid moisture absorption and wicking effects are significantly enhanced. Furthermore, the sterically hindered side groups of 2-methyl-2-propyl-1,3-propanediol further disrupt the molecular chain regularity and may form microstructures in the fiber that facilitate moisture transport, increasing the contact and evaporation area for water molecules and contributing to improved rapid moisture absorption and surface drying. The synergistic effect of these components significantly enhances the moisture absorption and wicking properties of polyester fibers. Detailed Implementation
[0027] The present application will be further described in detail below with reference to the embodiments. Examples 1-4
[0028] Examples 1-4 provide a method for preparing polyester filament, wherein the components and contents of the polyester filament are shown in Table 1 below, and the specific preparation method includes the following steps: S1. Mix purified terephthalic acid, ethylene glycol, antimony trioxide and triphenyl phosphate, and stir at 100 rpm for 20 min to obtain a mixture. Add the mixture to a reaction vessel and stir at 60 rpm. Under a nitrogen protective atmosphere, control the temperature inside the vessel at 230℃ and the pressure at 0.3 MPa to carry out the esterification reaction. Stir at 60 rpm for 2 h to complete the esterification reaction. S2. Control the pressure inside the reactor to atmospheric pressure and the temperature to 210℃. Maintain a stirring speed of 60 rpm. Add sodium diethylene glycol isophthalate-5-sulfonate and bi-amino-terminated polyethylene glycol to the reactor over a period of 30 minutes. After adding the materials, stir at 60 rpm for 20 minutes. Add 1,4-cyclohexanediol and neopentyl glycol over a period of 30 minutes. After adding the materials, stir at 60 rpm for 20 minutes. Add 2-methyl-2-propyl-1,3-propanediol over a period of 30 minutes. After adding the materials, stir at 60 rpm for 30 minutes. After about 50 minutes, reduce the pressure inside the reactor to 1.8 kPa. Continue to reduce the pressure inside the reactor to 50 Pa over about 50 minutes. At the same time, raise the temperature inside the reactor to 275℃ and stir at 50 rpm for 2.5 hours. Use nitrogen to break the vacuum, discharge the material, cast into strips, cool, and granulate to obtain PET chips. S3. The PET chips obtained in step S2 are kept at 100℃ for 2 hours, pre-crystallized at 130℃ for 4 hours, dried at 150℃ for 24 hours, and then naturally cooled to 25℃. The cooled PET chips are then added to a twin-screw extruder for melting. The operating conditions of the twin-screw extruder are: zone 1 temperature 270℃, zone 2 temperature 277℃, zone 3 temperature 283℃, zone 4 temperature 283℃, and screw speed 300 rpm. The melt extruded from the twin-screw extruder is fed into a metering pump, and the temperature inside the metering pump is controlled at 278℃. The metering pump then feeds the melt into the spinning box, and the temperature inside the spinning box is controlled. The temperature inside the spinning chamber is 275℃. After the melt flows out of the spinning box, it is spun through a spinneret with a spinneret orifice diameter of 0.3mm. The spinning temperature is controlled at 275℃. The spun fibers are cooled with a cooling air temperature of 20℃ and a wind speed of 0.8m / s. The cooled nascent fibers are then stretched with a hot plate temperature controlled at 95℃ and a stretch ratio of 4. After that, they are heat-set at a temperature of 140℃ for 45s with a setting tension of 7cN / dtex. Finally, they are wound into shape by a winding machine at a winding speed of 900m / min to obtain polyester filament.
[0029] Table 1. Raw materials and usage of polyester filament (unit: parts by weight)
[0030] Among them, purified terephthalic acid in Table 1 is from Nantong Zhonghe Chemical New Materials Co., Ltd., item number 1005814; and diamino-terminated polyethylene glycol is from Henan Yinuokai New Materials Co., Ltd., with a weight-average molecular weight of 2000. Examples 5-7
[0031] Examples 5-7 are based on Example 3, the difference being that in step S2, the total weight parts of 1,4-cyclohexanediol, neopentyl glycol, and 2-methyl-2-propyl-1,3-propanediol are kept constant at 3.4 parts by weight, while the proportions of the three components are adjusted; the other steps remain the same as in Example 3. Specifically, In Example 5, 2.39 parts by weight of 1,4-cyclohexanediol, 0.39 parts by weight of neopentyl glycol, and 0.62 parts by weight of 2-methyl-2-propyl-1,3-propanediol were used.
[0032] In Example 6, 1.93 parts by weight of 1,4-cyclohexanediol, 0.49 parts by weight of neopentyl glycol, and 0.98 parts by weight of 2-methyl-2-propyl-1,3-propanediol were used.
[0033] In Example 7, 1.83 parts by weight of 1,4-cyclohexanediol, 0.51 parts by weight of neopentyl glycol, and 1.06 parts by weight of 2-methyl-2-propyl-1,3-propanediol were used. Examples 8-9
[0034] Examples 8 and 9 are based on Example 6, with the difference being that in step S2, a mixture of bi-amino-terminated polyethylene glycol with a weight average molecular weight of 1000, bi-amino-terminated polyethylene glycol with a weight average molecular weight of 2000, and bi-amino-terminated polyethylene glycol with a weight average molecular weight of 3400 is used to replace the bi-amino-terminated polyethylene glycol with a weight average molecular weight of 2000. The total weight percentages of the bi-amino-terminated polyethylene glycol with a weight average molecular weight of 1000, 2000, and 3400 are kept constant at 2.5 parts by weight. The weight ratios of the three are adjusted, while the other steps remain the same as in Example 6. Specifically, In Example 8, the weight ratio of biamino polyethylene glycol with a weight average molecular weight of 1000, biamino polyethylene glycol with a weight average molecular weight of 2000, and biamino polyethylene glycol with a weight average molecular weight of 3400 is 1.5:7:1.5.
[0035] In Example 9, the weight ratio of biamino-terminated polyethylene glycol with a weight average molecular weight of 1000, biamino-terminated polyethylene glycol with a weight average molecular weight of 2000, and biamino-terminated polyethylene glycol with a weight average molecular weight of 3400 is 2:6:2.
[0036] Among them, the double-amino-terminated polyethylene glycol with a weight average molecular weight of 1000 and the double-amino-terminated polyethylene glycol with a weight average molecular weight of 3400 were both purchased from Henan Inokai New Materials Co., Ltd. Comparative Examples 1-6
[0037] Comparative Examples 1-6 are based on Example 2, except that the raw materials or amounts used in step S2 have changed, while the other steps remain the same as in Example 2. Specifically, In Comparative Example 1, polyethylene glycol (PEG2000, Shanghai Maclean Biochemical Technology Co., Ltd.) was used in equal parts by weight to replace the diamino-terminated polyethylene glycol.
[0038] In Comparative Example 2, the amount of diamino-terminated polyethylene glycol used was 1.3 parts by weight.
[0039] In Comparative Example 3, sodium diethylene isophthalate-5-sulfonate was used in equal parts by weight to replace the amino-terminated polyethylene glycol.
[0040] In Comparative Example 4, neopentyl glycol was used to replace 2-methyl-2-propyl-1,3-propanediol in equal parts by weight.
[0041] In Comparative Example 5, neopentyl glycol was used in place of 1,4-cyclohexanediethanol in equal parts by weight.
[0042] In Comparative Example 6, neopentyl glycol was replaced with an equal part by weight of 1,4-cyclohexanediethanol. Performance testing
[0043] The moisture regain and surface contact angle of the polyester filaments obtained in Examples 1-9 and Comparative Examples 1-6 were tested, and the test results are shown in Table 2 below.
[0044] The surface contact angle test involved tightly winding polyester filaments onto a glass slide in a 250mm × 150mm configuration to obtain a test sample. Under conditions of 20℃ and 65% relative humidity, 2μL of water was added to the test sample at a rate of 1μL / s. The static contact angle was measured within 10 seconds of contact with the polyester filaments, with an average deviation not exceeding ±2°. This process was repeated 10 times, and the average value was taken.
[0045] Moisture regain test: Weigh 50g of polyester filament, wash the polyester filament with surfactant, and dry it in an oven to constant weight. Place the constant-weight polyester filament under conditions of 20℃ and 65% relative humidity for 48 hours to absorb moisture and reach equilibrium. Weigh the polyester filament after moisture absorption to obtain the initial weight W0. Then place it in an oven at 110℃ to dry to constant weight and weigh it again to obtain the dried weight W1. Calculate the moisture regain (%) of the polyester filament using the following formula. Take three samples from each test group, and take the average value of the test results. Moisture regain = [(W0-W1) / W1]×100%.
[0046] Table 2. Test results of surface contact angle and moisture regain
[0047] As shown in Table 2, the experimental results indicate that adding specific amounts of 1,4-cyclohexanediol and neopentyl glycol to the copolymer system effectively disrupts the regularity of the polyester molecular chain, creating ample space for the retention of hydrophilic segments and water molecules. The addition of diethylene glycol isophthalate-5-sulfonate and diamino-terminated polyethylene glycol significantly enhances the rapid moisture absorption and wicking properties. Furthermore, the sterically hindered side groups of 2-methyl-2-propyl-1,3-propanediol further disrupt the molecular chain regularity and may form microstructures in the fiber that facilitate moisture transport, increasing the contact and evaporation area for water molecules and contributing to improved rapid moisture absorption and surface drying. The synergistic effect of these components significantly enhances the moisture absorption and wicking properties of polyester fibers.
[0048] Examples 1-4 investigated the effect of the ratio of sodium diethylene glycol isophthalate-5-sulfonate and diamino-terminated polyethylene glycol on the moisture absorption and wicking properties of the material. When the weight ratio of sodium diethylene glycol isophthalate-5-sulfonate to diamino-terminated polyethylene glycol was (0.7-0.9):(2.3-2.5), the material exhibited superior moisture absorption and wicking properties. Examples 5-7, based on Example 3, investigated the effect of the ratio of 1,4-cyclohexanediol, neopentyl glycol, and 2-methyl-2-propyl-1,3-propanediol on the moisture absorption and wicking properties of the material. When the weight ratio of 1,4-cyclohexanediol, neopentyl glycol, and 2-methyl-2-propyl-1,3-propanediol was (1.93-2.10):(0.45-0.49):(0.85-0.98), the material exhibited superior moisture absorption and wicking properties. Examples 8 and 9, based on Example 6, investigated the effect of compounding diamino-terminated polyethylene glycols of different molecular weights on the moisture absorption and wicking properties of the material.
[0049] Comparative Examples 1-3, based on Example 2, investigated the effects of replacing the diamino-terminated polyethylene glycol (DPP) with polyethylene glycol, using a small amount of DPP, and lacking DPP on the moisture absorption and wicking properties of the materials. When polyethylene glycol replaced the DPP, the moisture absorption and wicking properties of the material were affected. This may be because the lack of terminal amino groups in polyethylene glycol affects its bonding relationship with the polyester matrix, thus affecting the final moisture absorption and wicking properties of the material. Both using a small amount of DPP and lacking DPP affected the hydrophilicity of the material, thereby affecting its moisture absorption and wicking properties. Comparative Examples 4-6, based on Example 2, investigated the effects of the absence of 1,4-cyclohexanediol, neopentyl glycol, and 2-methyl-2-propyl-1,3-propanediol on the moisture absorption and wicking properties of the materials.
[0050] The embodiments described in this specific implementation are preferred embodiments of this application and are not intended to limit the scope of protection of this application. Therefore, all equivalent changes made in accordance with the principles of this application should be covered within the scope of protection of this application.
Claims
1. A polyester filament, characterized in that, The product comprises the following components in parts by weight: 30-40 parts purified terephthalic acid, 15-20 parts ethylene glycol, 1.83-2.39 parts 1,4-cyclohexanediol, 0.39-0.51 parts neopentyl glycol, 0.62-1.06 parts 2-methyl-2-propyl-1,3-propanediol, 0.4-1.3 parts sodium diethylene glycol isophthalate-5-sulfonate, 1.9-2.8 parts diamino-terminated polyethylene glycol, 0.011-0.018 parts catalyst, and 0.011-0.018 parts additives.
2. The polyester filament according to claim 1, characterized in that, The weight ratio of the 1,4-cyclohexanediol, the neopentyl glycol, and the 2-methyl-2-propyl-1,3-propanediol is (1.93~2.10):(0.45~0.49):(0.85~0.98).
3. The polyester filament according to claim 1, characterized in that, The weight ratio of the sodium diethylene glycol isophthalate-5-sulfonate to the diamino-terminated polyethylene glycol is (0.7~0.9):(2.3~2.5).
4. The polyester filament according to claim 1, characterized in that, The weight-average molecular weight of the diamino-terminated polyethylene glycol is 1000-4000.
5. The polyester filament according to claim 4, characterized in that, The diamine-terminated polyethylene glycol includes diamine-terminated polyethylene glycol with a weight average molecular weight of 1000, diamine-terminated polyethylene glycol with a weight average molecular weight of 2000, and diamine-terminated polyethylene glycol with a weight average molecular weight of 3400, and the weight ratio of the diamine-terminated polyethylene glycol with a weight average molecular weight of 1000, the diamine-terminated polyethylene glycol with a weight average molecular weight of 2000, and the diamine-terminated polyethylene glycol with a weight average molecular weight of 3400 is (1.5~2.0):(6~7):(1.5~2.0).
6. The polyester filament according to claim 1, characterized in that, The additives include heat stabilizers.
7. The polyester filament according to claim 1, characterized in that, The catalyst is selected from at least one of antimony glycol and antimony trioxide.
8. A method for preparing polyester filament as described in any one of claims 1 to 7, characterized in that, Includes the following steps: S1. Mix purified terephthalic acid, ethylene glycol, catalyst and additives, and under a nitrogen protective atmosphere, control the temperature at 220~230℃ and the pressure at 0.2~0.4MPa, and stir the reaction for 1.5~2.5h to obtain the esterification reaction product. S2. Under normal pressure, add sodium diethylene isophthalate-5-sulfonate, bi-amino-terminated polyethylene glycol, 1,4-cyclohexanediol, neopentyl glycol and 2-methyl-2-propyl-1,3-propanediol, stir, and carry out polycondensation reaction under vacuum at 270~280℃. Discharge, cool, and granulate to obtain PET chips. S3. The PET chips obtained in step S2 are pre-crystallized, dried, melt-extruded, spun, stretched and shaped, and wound to obtain the polyester filament.
9. The method for preparing polyester filament according to claim 8, characterized in that, In step S2, after adding sodium diethylene glycol isophthalate-5-sulfonate and bi-amino-terminated polyethylene glycol, the mixture is stirred for 10-30 min. After adding 1,4-cyclohexanediol and neopentyl glycol, the mixture is stirred for 10-30 min. After adding 2-methyl-2-propyl-1,3-propanediol, the mixture is stirred for 20-40 min.
10. The application of polyester filament as described in any one of claims 1 to 7 in clothing fabrics.