Preparation method and application of graphene modified super-weatherable nano-coating system
By grafting ultraviolet-absorbing and free radical-capturing groups onto the surface of graphene and constructing a double-layer gradient coating, the problems of dispersion and single function of graphene-modified coatings are solved, achieving multiple protective effects of the coating, which is suitable for outdoor steel structures, bridges and marine engineering equipment.
Patent Information
- Application Number
- CN202610535548.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Filing Date
- 2026-04-22
- Publication Date
- 2026-07-10
AI Technical Summary
Existing graphene-modified coatings exhibit poor dispersion in resin matrices, limited functionalization, and a lack of synergistic design in multilayer coatings. This leads to interface failure and functional degradation during long-term service, making it impossible to simultaneously achieve adhesion, barrier performance, and weather resistance.
By preparing bifunctionalized modified graphene, grafting ultraviolet absorbing groups and free radical scavenging groups, and constructing a two-layer gradient coating system of primer and topcoat, the coating performance is improved by utilizing chemical bonding and synergistic effects.
It significantly improves the weather resistance and adhesion of the coating, achieving multi-level protection against light, oxygen, water, and corrosive media, and is suitable for corrosion and aging prevention in harsh environments such as outdoor steel structures, bridges, and marine engineering equipment.
Smart Images

Figure CN122356956A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of coating materials technology, specifically to a method for preparing a graphene-modified ultra-weather-resistant nano-coating system and its application. Background Technology
[0002] Coating protection is one of the widely used technical means for corrosion prevention of metal materials. By forming a protective layer on the surface of the metal substrate, water, oxygen and corrosive media can be isolated, and the corrosion failure process of the substrate can be delayed. With the development of modern industry, outdoor steel structures, bridges, photovoltaic brackets, marine engineering equipment and other facilities that are exposed to harsh environments for a long time have put forward increasingly higher requirements for the weather resistance, corrosion resistance and service life of coatings.
[0003] Graphene, as a two-dimensional nanomaterial, possesses excellent physical barrier properties, chemical inertness, and high specific surface area, making it an ideal anti-corrosion filler. Introducing graphene or its derivatives, such as graphene oxide, into polymer coatings can extend the diffusion path of corrosive media and improve the barrier properties and anti-corrosion capabilities of the coating. However, existing technologies in the field of graphene-modified coatings still have the following shortcomings:
[0004] First, the problem of graphene dispersion in resin matrix has not been fundamentally solved. Graphene sheets have strong π-π interactions and van der Waals forces, which make them prone to aggregation, resulting in uneven dispersion in coatings and making it difficult to fully utilize their nanoscale effect. At the same time, the surface of graphene oxide contains a large number of oxygen-containing functional groups such as hydroxyl, epoxy, and carboxyl groups. The presence of these polar groups makes graphene oxide highly hydrophilic, which may accelerate the adsorption and diffusion of water molecules in the coating, adversely affecting the long-term barrier performance of the coating.
[0005] Secondly, existing technologies for functionalizing graphene are relatively singular and lack synergistic protective designs. Current research has attempted to modify the surface of graphene using silane coupling agents to improve its compatibility and dispersibility with resin matrices. For example, phenyltrimethoxysilane was used to modify nitrogen- and sulfur-doped graphene for use in powder coatings for marine photovoltaic brackets, improving the dispersibility of graphene and the wear resistance of the coating. Another study used pyrene-containing azo compounds to non-covalently modify graphene and applied it to polyurethane coatings, significantly improving the weather resistance of the coating. However, the above modification strategies usually only endow graphene with a single function, such as improving dispersibility, enhancing adhesion, or improving wear resistance. They fail to synergistically graft multiple protective functions such as ultraviolet absorption and free radical capture onto the graphene surface, making it difficult to actively inhibit the photo-oxidative aging process of the coating from a chemical level.
[0006] Existing coating systems are mostly single-layer structures, lacking systematic and gradient functional synergy. Traditional single-layer coatings cannot simultaneously achieve multiple functions such as adhesion, barrier performance, and weather resistance. Although some studies have attempted to construct multi-layer coating systems, there is often a lack of clear functional division and synergy between the layers. Poor performance matching between the bottom layer and the top layer leads to interface failure or functional degradation of the coating during long-term service. In addition, the choice of topcoat resin is crucial to the weather resistance of the coating. Currently, fluorocarbon resins are mostly used to achieve weather resistance, but their cost is high and the adhesion matching with the primer needs further optimization. Unmodified graphene may produce cathodic corrosion promoting activity in the coating, that is, after the coating is damaged, it will accelerate the local corrosion of the metal substrate, which limits the practical application of graphene anti-corrosion coatings.
[0007] In summary, how to develop a graphene-modified coating system that combines good dispersibility and multiple protective functions, and can achieve synergistic enhancement through multi-layer structural design, has become a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0008] This invention provides a method for preparing a graphene-modified ultra-weather-resistant nano-coating system and its application;
[0009] To achieve the above objectives, the technical solution of the present invention is as follows:
[0010] In a first aspect, a method for preparing a graphene-modified ultra-weather-resistant nanocoating system is provided, comprising the following steps:
[0011] S1. Prepare bifunctionalized modified graphene by dispersing graphene oxide in a solvent, adding a first silane coupling agent containing ultraviolet absorbing functional groups and a second silane coupling agent containing free radical scavenging groups in sequence, and carrying out a reflux reaction to allow the first silane coupling agent and the second silane coupling agent to be chemically bonded to the surface of graphene oxide. After separation, washing and drying, bifunctionalized modified graphene with ultraviolet absorbing groups and free radical scavenging groups grafted on is obtained.
[0012] Bifunctionalized modified graphene is a nanoscale sheet material;
[0013] S2, Prepare primer component: Mix and disperse the bifunctional modified graphene obtained in step S1 with modified epoxy resin, first diluent and first additive to obtain primer component A;
[0014] The epoxy curing agent is mixed with the second diluent to obtain primer component B;
[0015] S3, Prepare the topcoat component by mixing and dispersing the bifunctional modified graphene obtained in step S1 with modified epoxy resin, fourth diluent, ultraviolet absorber, light stabilizer and third additive to obtain the topcoat component.
[0016] S4, Coating application: Mix primer component A and primer component B from step S2, apply the mixture to the substrate surface, and cure to form a primer layer.
[0017] The topcoat component from step S3 is coated onto the primer layer and cured to form the topcoat layer, thus obtaining the graphene-modified ultra-weather-resistant nano-coating system.
[0018] Preferably, in step S1, the first silane coupling agent containing ultraviolet absorbing functional groups is a silane coupling agent containing benzotriazole groups or triazine groups.
[0019] The second silane coupling agent containing a free radical scavenging group is a silane coupling agent containing a hindered amine group;
[0020] The mass ratio of graphene oxide to the first silane coupling agent and the second silane coupling agent is 1:(0.5-2):(0.5-2).
[0021] Preferably, in step S1, the reflux reaction temperature is 60-100℃, and the reaction time decreases as the temperature increases. Specifically, when the reaction temperature is 60-70℃, the reaction time is 36-48 hours; when the reaction temperature is 71-90℃, the reaction time is 18-30 hours; and when the reaction temperature is 91-100℃, the reaction time is 12-18 hours.
[0022] The solvent is one or more of toluene, xylene, or N,N-dimethylformamide.
[0023] Preferably, in step S2, the epoxy resin is bisphenol A type epoxy resin or bisphenol F type epoxy resin;
[0024] The epoxy curing agent is an amine-based curing agent;
[0025] In the primer components, the mass of bifunctionalized modified graphene accounts for 0.5%-5% of the total solid mass of the primer.
[0026] Preferably, in step S3, the modified epoxy resin is bisphenol A type epoxy resin or bisphenol F type epoxy resin.
[0027] The ultraviolet absorber is a benzotriazole or triazine ultraviolet absorber;
[0028] The light stabilizer is a hindered amine light stabilizer;
[0029] In the topcoat components, the mass of bifunctionalized modified graphene accounts for 0.1%-1% of the total solid mass of the topcoat.
[0030] Preferably, in step S4, the dry film thickness of the primer layer is 30-80 μm;
[0031] The dry film thickness of the topcoat layer is 20-50μm.
[0032] Preferably, in step S4, the curing temperature of the primer layer is room temperature or baking at 60-100℃.
[0033] The topcoat layer is cured at room temperature or by baking.
[0034] Preferably, the mixing and dispersion in steps S2 and S3 are carried out by high-speed stirring or sand milling, and the dispersion fineness is ≤30μm.
[0035] On the other hand, a graphene-modified ultra-weather-resistant nano-coating system prepared by the above method is applied in the corrosion and aging prevention of outdoor steel structures, bridges, photovoltaic supports or marine engineering equipment.
[0036] Beneficial effects
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] This invention prepares bifunctionalized graphene by simultaneously grafting ultraviolet absorbing groups and free radical scavenging groups onto the surface of nanoscale graphene through chemical bonding. This bifunctionalized graphene not only solves the dispersion problem of graphene in resin matrices but also endows graphene with the chemical function of actively inhibiting photo-oxidative aging. Specifically, the ultraviolet absorbing groups can efficiently absorb ultraviolet light and convert it into heat energy; the free radical scavenging groups can capture active free radicals generated during photo-oxidation, interrupting the free radical chain reaction. The synergistic effect of these two groups actively delays the photo-oxidative degradation process of the resin matrix from a chemical perspective, significantly improving the weather resistance of the coating.
[0039] This invention constructs a dual-layer gradient coating system consisting of a primer layer and a topcoat layer, achieving synergistic enhancement of adhesion, barrier performance, and weather resistance. The primer layer uses epoxy resin as a matrix, utilizing the active groups on the surface of bifunctionalized modified graphene to react with the metal substrate and epoxy resin, forming chemical bonds and significantly improving the adhesion between the coating and the substrate. The topcoat layer uses modified epoxy resin as a matrix, retaining the good interlayer adhesion between the epoxy resin and the primer. Furthermore, by introducing the UV absorption and free radical scavenging functions of bifunctionalized modified graphene, along with the synergistic effect of UV absorbers and light stabilizers, an active protective layer combining physical barrier and chemical protection is formed. The dual-layer structure works together to compensate for the functional deficiencies of single-layer coatings, achieving multi-level protection against light, oxygen, water, and corrosive media.
[0040] The coating system prepared by this invention has excellent comprehensive performance and wide applicability. By optimizing the amount of nano-scale bifunctional modified graphene added and the dry film thickness in the primer and topcoat, it is possible to balance economy and workability while ensuring coating performance. The coating system prepared by this invention exhibits excellent performance in terms of salt spray resistance, aging resistance, adhesion, and electrochemical impedance. It can be widely used in the field of corrosion and aging prevention in harsh environments such as outdoor steel structures, bridges, photovoltaic brackets, and marine engineering equipment, and has significant economic and social benefits. Attached Figure Description
[0041] Figure 1 This is a process flow diagram of the preparation of a graphene-modified ultra-weather-resistant nano-coating system prepared in Example 1 of the present invention.
[0042] Figure 2 This is a schematic diagram of the structure of the graphene-modified ultra-weather-resistant nano-coating system prepared in this invention;
[0043] Figure 3 This is a curve comparing the aging resistance of the coating system of the present invention with that of the comparative coating. Detailed Implementation
[0044] To further illustrate the technical means and effects adopted by the present invention to achieve its intended purpose, exemplary embodiments will be described in detail below. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with this application. Rather, they are merely examples of methods and systems consistent with some aspects of this application as detailed in the appended claims.
[0045] The terminology used in this application is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. The singular forms “a,” “the,” and “the” used in this application and the appended claims are also intended to include the plural forms unless the context clearly indicates otherwise. It should also be understood that the term “and / or” as used herein refers to and includes any or all possible combinations of one or more of the associated listed items.
[0046] The raw materials used in the embodiments of the present invention are from the following sources, but are not limited thereto:
[0047] Graphene oxide, prepared using a modified Hummers method, consists of 1-5 layers with a sheet diameter of 5-20 μm, and is a nanoscale sheet material.
[0048] Silane coupling agents containing benzotriazole groups, Nanjing Liansilicon Chemical Co., Ltd.
[0049] Silane coupling agents containing triazine groups, Nanjing Liansilicon Chemical Co., Ltd.;
[0050] Silane coupling agents containing hindered amine groups, Nanjing Liansilicon Chemical Co., Ltd.;
[0051] Bisphenol A type epoxy resin, China Petroleum & Chemical Corporation;
[0052] Bisphenol F type epoxy resin, China Petroleum & Chemical Corporation;
[0053] Amine curing agents, Air Products and Chemicals, Inc.
[0054] Benztriazole UV absorbers, BASF AG;
[0055] Triazine UV absorbers, BASF AG;
[0056] Hindered amine light stabilizers, BASF AG;
[0057] The topcoat component of this invention uses modified epoxy resin as the matrix, and by adding bifunctional modified nano-graphene, ultraviolet absorber and light stabilizer, a modified epoxy resin system is formed, which significantly improves weather resistance.
[0058] The following are preferred embodiments, which provide a detailed description of the specific implementation methods, features, and effects of the present invention.
[0059] Example 1
[0060] Please refer to Figure 1 , Figure 2 This embodiment provides a method for preparing a graphene-modified ultra-weather-resistant nanocoating system, including the following steps:
[0061] S1. Preparation of nanoscale bifunctional modified graphene: 10g of graphene oxide, i.e., nanoscale sheet material, was weighed and added to 1000mL of anhydrous toluene. The mixture was ultrasonically dispersed for 30min to obtain a uniform graphene oxide dispersion. 5g of a first silane coupling agent containing benzotriazole groups and 5g of a second silane coupling agent containing hindered amine groups were added sequentially to the dispersion. The mixture was heated to 80℃ under nitrogen protection and refluxed for 24h. After the reaction, the product was centrifuged and washed three times with anhydrous ethanol and deionized water, and then vacuum dried at 60℃ for 12h to obtain bifunctional modified graphene grafted with both ultraviolet absorbing groups and free radical scavenging groups, denoted as G-UV-HALS. Its sheet size remained at the nanoscale. The grafting rate was determined by thermogravimetric analysis (TGA) to be approximately 15.6%.
[0062] S2, Preparation of primer components;
[0063] Primer component A: Weigh 100g of bisphenol A type epoxy resin, add 30g of xylene as the first diluent, add 5g of G-UV-HALS obtained in step S1, 1g of defoamer and 2g of dispersant, disperse in a high-speed disperser at 1500rpm for 30min, the dispersion fineness is ≤30μm, and primer component A is obtained.
[0064] For primer component B, weigh 50g of amine curing agent, add 15g of n-butanol as a second diluent, stir evenly, and you will get primer component B;
[0065] In the primer components, the bifunctionalized modified graphene accounts for 2.3% of the total solids mass of the primer;
[0066] S3, preparation of topcoat components;
[0067] Weigh 100g of bisphenol A type epoxy resin, add 40g of xylene and 10g of butyl acetate as a fourth diluent, add 0.5g of G-UV-HALS prepared in step S1, 1g of benzotriazole UV absorber, 1g of hindered amine light stabilizer, 0.3g of defoamer and 0.5g of leveling agent, disperse in a high-speed disperser at 1000rpm for 20min, with a dispersion fineness ≤30μm, to obtain the topcoat component;
[0068] In the topcoat components, the mass of bifunctionalized modified graphene accounts for 0.2% of the total solid mass of the topcoat;
[0069] S4, Coating application;
[0070] In step S2, primer component A and primer component B are mixed evenly at a mass ratio of 2:1, and then coated onto the surface of a sandblasted Q235 carbon steel substrate using an air spraying method. The dry film thickness is controlled at 50 μm, and the primer layer is cured at room temperature for 24 hours.
[0071] The topcoat component from step S3 is sprayed onto the primer layer, the dry film thickness is controlled at 40 μm, and the topcoat layer is formed by curing at room temperature for 72 h, thus obtaining the graphene-modified ultra-weather-resistant nano-coating system.
[0072] Example 2
[0073] This embodiment is basically the same as Embodiment 1, except that in step S1, the first silane coupling agent is a silane coupling agent containing a triazine group, the second silane coupling agent is a silane coupling agent containing a hindered amine group, and the mass ratio of graphene oxide to the first and second silane coupling agents is 1:1:1. The other steps are the same as in Embodiment 1.
[0074] Example 3
[0075] This embodiment is basically the same as Example 1, except that in step S1, the reflux reaction temperature is 60°C, the reaction time is 48h, and the solvent used is N,N-dimethylformamide. The other steps are the same as in Example 1.
[0076] Example 4
[0077] This embodiment is basically the same as that of Embodiment 1, except that in step S1, the reflux reaction temperature is 100°C and the reaction time is 12h. The other steps are the same as those in Embodiment 1.
[0078] Example 5
[0079] This embodiment is basically the same as Embodiment 1, except that in step S2, the epoxy resin used is bisphenol F type epoxy resin, and the amount of bifunctionalized modified graphene is adjusted to 1g, accounting for 0.5% of the total solid mass of the primer. The other steps are the same as in Embodiment 1.
[0080] Example 6
[0081] This embodiment is basically the same as Embodiment 1, except that in step S2, the amount of bifunctionalized modified graphene is adjusted to 12g, accounting for 5.0% of the total solid mass of the primer. The other steps are the same as in Embodiment 1.
[0082] Example 7
[0083] This embodiment is basically the same as Embodiment 1, except that in step S3, the amount of bifunctional modified graphene is adjusted to 0.2g, accounting for 0.1% of the total solid mass of the topcoat. The other steps are the same as in Embodiment 1.
[0084] Example 8
[0085] This embodiment is basically the same as Embodiment 1, except that in step S3, the amount of bifunctional modified graphene is adjusted to 2.5g, accounting for 1.0% of the total solid mass of the topcoat. The other steps are the same as in Embodiment 1.
[0086] Example 9
[0087] This embodiment is basically the same as that of Embodiment 1, except that in step S3, the ultraviolet absorber is a triazine-based ultraviolet absorber. The other steps are the same as those of Embodiment 1.
[0088] Example 10
[0089] This embodiment is basically the same as Embodiment 1, except that in step S4, the dry film thickness of the primer layer is controlled to be 30μm and the dry film thickness of the topcoat layer is controlled to be 30μm. The other steps are the same as in Embodiment 1.
[0090] Example 11
[0091] This embodiment is basically the same as Embodiment 1, except that in step S4, the dry film thickness of the primer layer is controlled to be 80μm and the dry film thickness of the topcoat layer is controlled to be 50μm. The other steps are the same as in Embodiment 1.
[0092] Example 12
[0093] This embodiment is basically the same as Embodiment 1, except that in step S4, the primer layer is cured by baking at 60°C for 1 hour and the topcoat layer is cured by baking at 80°C for 2 hours. The other steps are the same as in Embodiment 1.
[0094] Comparative Example 1
[0095] This comparative example is basically the same as Example 1, except that in step S1, only the first silane coupling agent is added and the second silane coupling agent is not added to prepare monofunctionalized modified graphene with only ultraviolet absorbing groups grafted on. The other steps are the same as in Example 1.
[0096] Comparative Example 2
[0097] This comparative example is basically the same as Example 1, except that in step S1, only the second silane coupling agent is added and the first silane coupling agent is not added, so as to prepare monofunctionalized modified graphene with only free radical capturing groups grafted on. The other steps are the same as in Example 1.
[0098] Comparative Example 3
[0099] This comparative example is basically the same as Example 1, except that in step S1, unmodified graphene oxide is used instead of bifunctionalized graphene. The other steps are the same as in Example 1.
[0100] Comparative Example 4
[0101] This comparative example uses a commercially available epoxy zinc-rich primer and epoxy topcoat system, AkzoNobel, as a control. The coating was applied according to the product instructions, and the total dry film thickness was comparable to that of Example 1, approximately 90 μm.
[0102] Performance testing
[0103] The coating systems prepared in Examples 1-12 and Comparative Examples 1-4 were subjected to performance tests, and the test methods are as follows:
[0104] The resistance to neutral salt spray was tested according to GB / T 1771-2007 standard for 3000 hours. The coating surface was observed for phenomena such as blistering, rusting, and peeling.
[0105] The artificial weathering resistance was tested according to GB / T 1865-2009 standard, using a xenon lamp aging test chamber for 2000 hours. Considering the weather resistance limit of epoxy topcoat, the test duration was adjusted appropriately to evaluate the chalking, discoloration, and gloss loss of the coating. The gloss retention rate was determined according to GB / T 9754-2007.
[0106] Adhesion was tested according to GB / T 9286-1998 standard, with an evaluation level of 0-5.
[0107] Electrochemical impedance spectroscopy (EIS) was performed after immersion in 3.5% NaCl solution for 30 days, with the impedance modulus measured at a low frequency of 0.01 Hz. To evaluate the barrier performance of the coating;
[0108] Table 1 Performance test results of the examples and comparative examples
[0109] Please refer to Figure 3 The coating systems prepared in Examples 1-12 of this invention all exhibited excellent weather resistance and corrosion resistance. After 2000 hours of neutral salt spray testing, except for slight loss of gloss in Examples 6 and 8, no abnormal phenomena such as blistering, rusting, or peeling were observed on the coating surface. After 2000 hours of artificial climate aging testing, the gloss retention rate remained above 75%, with a maximum of 83.5%. The adhesion was all at grade 0, and the electrochemical impedance values all reached [value missing]. The magnitude indicates that the coating has excellent barrier properties;
[0110] Comparing Examples 1-4, it can be seen that by using different types of ultraviolet absorbing functional groups, namely benzotriazole groups or triazine groups, and different reaction conditions, such as temperatures of 60-100℃ and times of 12-48h, good bifunctional modification effects can be achieved, and the performance of the resulting coatings is comparable, indicating that the technical solution of the present invention has good process adaptability.
[0111] Comparing Examples 1, 5, and 6, it can be seen that the performance of the primer is excellent when the mass ratio of bifunctional modified graphene in the primer is in the range of 0.5%-2.3%. When the amount is increased to 5.0% in Example 6, the gloss retention rate decreases slightly and the adhesion drops to level 1. This may be due to the decrease in dispersibility of excessive graphene in the primer, but it is still better than the comparative example.
[0112] Comparing Example 1 with Comparative Examples 1-3, it can be seen that Example 1, which uses bifunctionalized modified graphene, has significantly improved weather resistance, corrosion resistance and adhesion compared with Comparative Examples 1-2 with monofunctionalized modification or Comparative Example 3 with unmodified graphene. This indicates that the synergistic effect of ultraviolet absorbing groups and free radical scavenging groups is the key to achieving super weather resistance.
[0113] Comparing Example 1 and Comparative Example 4, it can be seen that the coating system prepared by the present invention is significantly better than the commercially available epoxy system in terms of weather resistance and corrosion resistance. After 2000 hours of aging, the gloss retention rate is increased by about 30.2%, and the electrochemical impedance value is increased by about two orders of magnitude.
[0114] In summary, the graphene-modified ultra-weather-resistant nanocoating system provided by this invention achieves excellent weather resistance, corrosion resistance, and adhesion by constructing a bifunctional modified graphene and a bilayer gradient coating structure. It can be widely used in outdoor steel structures, bridges, photovoltaic supports, or marine engineering equipment.
[0115] Finally, it should be noted that the device models used in this embodiment are only for verification and do not limit the scope of this application. The above embodiments are only used to illustrate the technical solutions of this application and are not intended to limit the scope of protection of this application. Although this application has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of this application without departing from the substance and scope of the technical solutions of this application.
Claims
1. A method for preparing a graphene-modified ultra-weather-resistant nanocoating system, characterized in that, Includes the following steps: S1. Prepare bifunctionalized modified graphene by dispersing graphene oxide in a solvent, adding a first silane coupling agent containing ultraviolet absorbing functional groups and a second silane coupling agent containing free radical scavenging groups in sequence, and performing a reflux reaction to allow the first silane coupling agent and the second silane coupling agent to be chemically bonded to the surface of graphene oxide. After separation, washing and drying, bifunctionalized modified graphene with ultraviolet absorbing groups and free radical scavenging groups grafted on is obtained. The bifunctionalized modified graphene is a nanoscale sheet material; S2, Prepare primer component: Mix and disperse the bifunctional modified graphene obtained in step S1 with modified epoxy resin, first diluent and first additive to obtain primer component A; The epoxy curing agent is mixed with the second diluent to obtain primer component B; S3, Prepare the topcoat component by mixing and dispersing the bifunctional modified graphene obtained in step S1 with modified epoxy resin, fourth diluent, ultraviolet absorber, light stabilizer and third additive to obtain the topcoat component. S4, Coating application: Mix primer component A and primer component B from step S2, apply the mixture to the substrate surface, and cure to form a primer layer. The topcoat component from step S3 is coated onto the primer layer and cured to form the topcoat layer, thus obtaining the graphene-modified ultra-weather-resistant nano-coating system.
2. The preparation method according to claim 1, characterized in that, In step S1, the first silane coupling agent containing ultraviolet absorbing functional groups is a silane coupling agent containing benzotriazole groups or triazine groups. The second silane coupling agent containing a free radical scavenging group is a silane coupling agent containing a hindered amine group; The mass ratio of the graphene oxide to the first silane coupling agent and the second silane coupling agent is 1:(0.5-2):(0.5-2).
3. The preparation method according to claim 1, characterized in that, In step S1, the reflux reaction temperature is 60-100℃, and the reaction time decreases as the temperature increases. Specifically, when the reaction temperature is 60-70℃, the reaction time is 36-48 hours; when the reaction temperature is 71-90℃, the reaction time is 18-30 hours; and when the reaction temperature is 91-100℃, the reaction time is 12-18 hours. The solvent is one or more of toluene, xylene, or N,N-dimethylformamide.
4. The preparation method according to claim 1, characterized in that, In step S2, the modified epoxy resin is bisphenol A type epoxy resin or bisphenol F type epoxy resin. The epoxy curing agent is an amine-based curing agent; In the primer component, the mass of bifunctionalized modified graphene accounts for 0.5%-5% of the total solid mass of the primer.
5. The preparation method according to claim 1, characterized in that, In step S3, the modified epoxy resin is bisphenol A type epoxy resin or bisphenol F type epoxy resin. The ultraviolet absorber is a benzotriazole or triazine ultraviolet absorber; The light stabilizer is a hindered amine light stabilizer; In the topcoat components, the mass of bifunctionalized modified graphene accounts for 0.1%-1% of the total solid mass of the topcoat.
6. The preparation method according to claim 1, characterized in that, In step S4, the dry film thickness of the primer layer is 30-80 μm; The dry film thickness of the topcoat layer is 20-50 μm.
7. The preparation method according to claim 1, characterized in that, In step S4, the curing temperature of the primer layer is room temperature or baking at 60-100℃. The topcoat layer is cured at room temperature or by baking.
8. The preparation method according to claim 1, characterized in that, The mixing and dispersion described in steps S2 and S3 are carried out by high-speed stirring or sand milling, and the dispersion fineness is ≤30μm.
9. The application of a graphene-modified ultra-weather-resistant nanocoating system prepared by the method of any one of claims 1-8 in the corrosion and aging prevention of outdoor steel structures, bridges, photovoltaic supports or marine engineering equipment.