Carbon-reduced microalloyed modified die steel and modification method thereof

By using carbon reduction microalloying design and fine phase transformation treatment, the problems of hardness-toughness inversion and thermal softening of traditional mold steel under extreme working conditions have been solved, thereby improving the high toughness and thermal shock resistance of mold steel.

CN122358060APending Publication Date: 2026-07-10SHANGHAI JIEBAO METAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610712642.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-05-22
Publication Date
2026-07-10

AI Technical Summary

Technical Problem

Traditional mold steels exhibit a hardness-toughness inversion effect caused by coarse primary eutectic carbides and thermodynamic coarsening of nanoscale reinforcing phases under extreme service conditions, leading to early micro-scraping, chipping, and overall catastrophic fracture of the mold surface.

Method used

By using a carbon reduction microalloying design, the carbon content is controlled between 0.40% and 0.55%, and elements such as Mo, V, Ti, and Nb are added to form a core-shell structure (Nb,V)C composite carbide. Combined with multi-directional forging and fine phase transformation treatment, a high-density nanoscale reinforced skeleton is constructed to block the Ostwald coarsening channel.

Benefits of technology

It significantly improves the room temperature impact toughness and heat softening resistance of mold steel, reduces the risk of chipping and breakage of molds under extreme working conditions, and extends the service life of molds.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a carbon-reduced microalloyed mold steel and its modification method. It addresses two major technical problems of traditional high-carbon mold steel: chipping and fracture induced by coarse primary carbides, and the decline in red hardness due to coarsening of nano-reinforcing phases during high-temperature service. This invention limits the carbon content to a matrix range of 0.40% to 0.55%, and constructs an ultra-stable nano-(Nb,V)C reinforcing framework through the gradient heterogeneous synergistic nucleation of Nb-V-Ti-Mo quaternary microalloying elements and the diffusion hindrance mechanism at the Mo interface. The resulting mold steel exhibits an impact toughness of 45 to 72 J / cm² at a high hardness of 58 to 62 HRC, a residual hardness of no less than 54 HRC after 600℃ for 50 h, and a thermal fatigue crack propagation rate that is only 29% to 42% of that of traditional H13 steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of mold steel technology, and in particular to a carbon-reducing microalloyed mold steel and its modification method. Background Technology

[0002] In modern industrial manufacturing systems, mold steel is widely used in key processes such as metal plastic forming, die casting, stamping, and precision forging. With the accelerating trend of automotive lightweighting and the increasing complexity of component structures, the stamping of high-strength steel sheets and the integrated die casting process of large lightweight alloys place extremely stringent requirements on mold materials. During service, molds must not only withstand extremely high local contact stresses but also endure severe mechanical impacts, high-frequency thermal shocks, and severe high-temperature friction and wear. Under extreme service conditions, traditional mold steel has gradually revealed two key technical defects: First, traditional high-carbon mold steels contain coarse primary eutectic carbides, leading to a severe "hardness-toughness" inversion effect. The design logic of traditional mold steels relies heavily on extremely high carbon content to ensure the high hardness and wear resistance of quenched martensite. However, this inevitably leads to the formation of coarse, network-like or banded primary eutectic carbides during the solidification stage of molten steel. These large carbides are highly susceptible to becoming fatigue crack initiation sources under complex alternating loads, triggering early micro-scraping, chipping, and even catastrophic fracture of the mold surface.

[0003] Secondly, under high-temperature and alternating thermal shock service conditions, the nanoscale reinforcing phases inside the die steel undergo rapid thermodynamic coarsening, leading to irreversible degradation of the matrix's thermal strength, i.e., red hardness. During long-term thermal cycling service, the reinforcing nano-carbides are prone to dimensional coarsening due to the control of the Ostwald curing mechanism. The critical shear stress required for dislocations to bypass the particles decreases sharply, resulting in severe thermal softening of the die surface. This leads to the initiation of dense cracks on the surface, ultimately causing the die surface to peel off and become unusable. Summary of the Invention

[0004] To address the aforementioned technical problems, this invention provides a carbon-reduced microalloyed mold steel and its modification method.

[0005] According to one aspect of the present invention, a carbon-reducing microalloyed modified die steel is provided, wherein the chemical composition of the die steel comprises, by mass percentage: C: 0.40% to 0.55%; Cr: 4.50% to 6.50%; Mo: 1.50% to 3.50%; V: 0.80% to 1.50%; Nb: 0.03% to 0.15%; Ti: 0.01% to 0.05%; Mn: 0.30% to 0.80%; Si: 0.10% to 0.50%; N: 0.005% to 0.025%; with the balance being Fe and unavoidable impurities. Controlling the C content within the matrix low concentration range of 0.40% to 0.55% is the core of the carbon reduction design of this application. If the carbon mass percentage is less than 0.40%, the dissolved carbon atoms in the martensite after quenching are severely insufficient, failing to provide enough secondary hardening carbides during tempering. This results in the matrix hardness failing to meet the threshold for industrial applications, leading to a loss of wear resistance. If the carbon mass percentage is greater than 0.55%, the supersaturated carbon during solidification and austenitizing cooling will inevitably form a micron-scale primary eutectic carbide network with alloying elements. Under service stress, this network becomes a crack initiation point, completely destroying the material's macroscopic fracture toughness. Adding 1.50% to 3.50% Mo not only strongly shifts the phase transformation nose region of the continuous cooling transformation curve to the right, giving the material extremely high deep hardenability, but also provides a sufficient atomic source for subsequent nano-precipitation phase interface segregation and coating. Adding 0.80% to 1.50% V ensures that a sufficient volume fraction of MC phase carbides can be dispersed in the high-temperature tempering range to induce a strong secondary hardening peak. Trace amounts of Ti and N preferentially react at high temperatures to precipitate nanoscale TiN particles with the highest thermodynamic stability, exerting a strong Zener grain boundary pinning effect to lock the original austenite grain boundaries; trace amounts of Nb precipitate in the early stages of austenite cooling and tempering, relying on TiN as an epitaxial growth template, further inhibiting grain coarsening and constructing heterogeneous nucleation nodes for explosive secondary precipitation of V at grain boundaries and within the grain.

[0006] Preferably, the mass percentages of the chemical composition satisfy the following conditions: the mass ratio of Ti to N is 3.0 to 4.0; the mass ratio of Mo to Nb is greater than or equal to 20; and the mass ratio of V to Nb is 10 to 30. Controlling the mass ratio of Ti to N to 3.0 to 4.0 ensures that this ratio is near the stoichiometry of TiN, guaranteeing that trace amounts of Ti in the molten steel can completely combine with N to precipitate extremely stable TiN particles. If the Ti content exceeds the standard and becomes free, it will lead to the formation of large-sized and brittle TiC at the grain boundaries, severely weakening the grain boundary bonding force. Controlling the mass ratio of Mo to Nb to 20 ensures that after the preferential precipitation of Nb-rich cores, there are free Mo atoms, with a concentration one order of magnitude higher, competing and segregating at the carbide / matrix phase interface, forming a continuous coating barrier and effectively initiating the core-shell diffusion retardation mechanism. Maintaining the V to Nb mass ratio between 10 and 30 ensures a sufficient number of Nb-rich nuclei to guide the larger volumetric V element to achieve uniform nanoscale dispersion precipitation, thus kinetically avoiding local enrichment and disordered spontaneous coarsening of V. When the V to Nb mass ratio is in the low to mid-range of 10 to 20, the match between the number of Nb nuclei and the V precipitation requirement is most ideal, resulting in the most uniform precipitation. When this ratio rises to the high range of 20 to 30, each Nb nucleus needs to carry more V atoms for epitaxial precipitation. Although the precipitation dispersion decreases slightly, the interfacial diffusion hindrance effect of the Mo shell in the system of this invention remains effective, particle coarsening is suppressed, and the overall performance is still maintained at an acceptable industrial level.

[0007] More preferably, the chemical composition of the mold steel further includes, by mass percentage, at least one selected from the group consisting of: W: greater than 0 and less than or equal to 1.50%; Ni: greater than 0 and less than or equal to 1.00%; RE: 0.005% to 0.030%. Adding an appropriate amount of W can further delay the dynamic recovery of dislocations and supplement the high-temperature red hardness of the material; introducing no more than 1.00% Ni can significantly improve the deep cold brittleness of the material, enhance the fracture toughness and impact resistance of the entire matrix; adding 0.005% to 0.030% rare earth elements (RE) mainly utilizes their strong deoxidation and desulfurization effects to deeply purify grain boundaries and promote the spheroidization of micron-sized non-metallic inclusions, further improving the triaxial isotropy of the material.

[0008] More preferably, the chemical composition by mass percentage includes: C: 0.45% to 0.50%; Cr: 5.00% to 5.50%; Mo: 2.00% to 2.50%; V: 1.00% to 1.20%; Nb: 0.06% to 0.10%; Ti: 0.015% to 0.03%; Mn: 0.40% to 0.60%; Si: 0.20% to 0.35%; N: 0.010% to 0.018%. This further narrowed proportioning range allows the system to achieve a perfect balance of solid solubility in the high-temperature austenitic single-phase region, maximizing the gradient nucleation and interfacial segregation synergistic effect of the multi-element alloy while avoiding the precipitation of primary carbides, thus pushing the overall strengthening and toughening of the matrix to the optimal state.

[0009] Preferably, the microstructure of the mold steel comprises a martensitic matrix or a lower bainitic matrix, within which secondary precipitated composite carbonitrides are distributed; the average equivalent diameter of the composite carbonitrides is 5 nm to 20 nm, and the composite carbonitrides include (Nb,V)C composite carbides with a core-shell structure, wherein the shell layer of the core-shell structure is a Mo-rich phase interface coating layer; the mold steel contains no primary blocky carbides larger than 3 μm. The martensitic matrix is ​​obtained through continuous cooling quenching followed by multiple high-temperature tempering processes; the lower bainitic matrix is ​​obtained through austenitization followed by isothermal transformation in the bainitic phase transformation region above the martensitic transformation initiation temperature. This approach, while sacrificing a small amount of hardness, can further improve the fracture toughness and impact resistance of the matrix. The absence of primary blocky carbides larger than 3 μm within the microstructure completely eliminates the crack initiation source that leads to micro-cleavage and early chipping from a macroscopic fracture mechanics perspective. The formation mechanism of (Nb,V)C composite carbides with a core-shell structure lies in the fact that the large atomic radius of Mo and its solid solution in the martensitic matrix cause extremely high lattice elastic distortion energy. Following the law of minimizing system energy, thermodynamically driven free Mo atoms spontaneously segregate to the interface between the growing nano-carbides and the matrix, forming a dense Mo-rich atomic-level shell. This shell reduces the lattice mismatch between the hard phase and the matrix through substitution, directly weakening the surface energy driving force of particle coarsening. At the same time, the extremely low diffusion coefficient of Mo establishes an indestructible kinetic barrier at the phase interface, preventing alloy atoms from crossing the interface to undergo Ostwald ripening, thus firmly locking the precipitated phase within the optimal critical size range of 5 nm to 20 nm, providing durable Orowan strengthening resistance.

[0010] According to another aspect of the present invention, a modification method for the above-mentioned carbon-reduced microalloyed mold steel is provided, comprising the following steps: S1, smelting and solidification forming: smelting according to the chemical composition ratio of the mold steel and casting into an ingot; S2, multi-directional large deformation forging: heating the ingot to 1150°C to 1180°C for homogenization and holding, and then performing three-dimensional multi-directional forging in a temperature range of 1150°C to 950°C, and controlling the final forging temperature to 900°C to 950°C to obtain a forging; S3, austenitizing treatment: heating the forging to 1050°C to 1100°C for austenitizing and holding; S4, cooling and microstructure control: adopting one of the following two routes. Route 1 involves continuous cooling quenching followed by multiple high-temperature tempering processes: The austenitized forgings are quenched and cooled, then subjected to at least three high-temperature tempering treatments. Each tempering is heated to 560°C to 600°C and held, followed by cooling to room temperature, resulting in mold steel with tempered martensite as the matrix. Route 2 involves isothermal quenching: The austenitized forgings are rapidly cooled to an isothermal temperature range of 280°C to 350°C and held for 1 to 4 hours for isothermal transformation, followed by air cooling to room temperature, resulting in mold steel with bainite as the matrix. In step S2, the homogenization temperature is controlled between 1150°C and 1180°C to completely eliminate compositional segregation before forging and promote the redissolution of soluble phases. Precisely limiting the final forging temperature to the vicinity of the non-recrystallization zone at 900°C to 950°C utilizes the strong solute dragging effect of undissolved Nb atoms in the matrix to suppress the dynamic recovery of austenite grain boundaries, squeezing the grains into a thin pancake shape and providing extremely high-density nucleation sites for subsequent phase transformations. Step S3 raises the austenitizing temperature to 1050°C to 1100°C, allowing the large-sized alloy carbides generated during hot working to completely dissolve, forcing a massive number of strong carbide-forming atoms into the lattice to form a highly supersaturated state. Simultaneously, the strong pinning effect of the previously dispersed TiN and NbC effectively prevents abnormally coarse grains even at extremely high austenitizing temperatures. In step S4, Route 1 controls the tempering temperature between 560℃ and 600℃ and performs at least three cycles. The first tempering eliminates the residual stress from the intense phase transformation and precipitates transition carbides. Subsequent tempering, through thermal shock, induces avalanche-like secondary nanoepitaxial precipitation of V and Nb elements based on the retained nucleation template, and promotes the unstable transformation of residual austenite and the softening and toughening of newly formed secondary martensite. Route 2 rapidly cools the austenitized forging to the bainitic transformation range above the Ms point and holds it isothermally for a long time, causing the austenite to undergo a lower bainitic transformation in this temperature range, obtaining a microstructure with lower bainitic laths as the matrix. This microstructure possesses both high strength and superior toughness compared to martensite.

[0011] Preferably, in step S1, the smelting employs a dual process of vacuum induction melting and protective atmosphere electroslag remelting. During the vacuum induction melting stage, the mass fraction of impurity element P is controlled to be less than or equal to 0.010%, and the mass fraction of S is controlled to be less than or equal to 0.003%, with microalloying achieved by feeding in cored wire containing Ti and Nb. During the protective atmosphere electroslag remelting stage, a mixed protective atmosphere of nitrogen and argon is introduced into a sealed electroslag furnace, controlling the nitrogen partial pressure within the furnace to be between 0.02 MPa and 0.10 MPa to suppress denitrification reactions during remelting and maintain precise control of the nitrogen content in the ingot. In the dual process, vacuum induction melting achieves deep degassing under extremely low vacuum and strictly controls harmful sulfur and phosphorus impurities, imparting ultimate purity to the matrix. Protective atmosphere electroslag remelting, by maintaining a certain nitrogen partial pressure within the sealed furnace, effectively suppresses the strong denitrification reaction caused by the extremely low nitrogen solubility of the high-temperature slag in conventional open electroslag remelting, ensuring that the precisely controlled nitrogen content during the vacuum induction melting stage is retained after remelting. Meanwhile, electroslag remelting further eliminates non-metallic inclusions and completely avoids central shrinkage cavities and porosity through slag refining and directional crystallization physical processes.

[0012] More preferably, in step S2, the total forging ratio of the three-dimensional multi-directional forging is greater than or equal to 6. Through high-ratio three-dimensional multi-directional plastic deformation greater than or equal to 6, a great deal of mechanical work can be applied to completely break up the locally remaining fine dendrite network, introduce the deformation energy storage depth into the material and extremely compress the size of the martensitic phase transformation phase.

[0013] More preferably, in step S3, the austenitizing holding time is determined by a holding coefficient of 0.5 hours / 25 mm effective thickness. This holding coefficient ensures that molds with different wall thicknesses can achieve thermodynamic hardening and homogenization. More preferably, in route one of step S4, the quenching cooling uses high-purity nitrogen gas cooling with a pressure greater than 6 bar or stepped warm oil cooling; the use of high-pressure gas or warm oil cooling combined with the high hardenability imparted by the composition allows the core of the module to smoothly cross the pearlite and ferrite transformation zone, obtaining a dense and uniform high-strength lath martensite structure.

[0014] More preferably, in route one of step S4, the holding time after reaching the tempering temperature is 2 hours, followed by air cooling to room temperature. The 2-hour homogenization holding ensures sufficient relaxation and recovery of martensitic lattice stress and completes the long-range diffusion and interfacial segregation process of substitutional alloy atoms. It also promotes the transformation of secondary instability of austenite into a highly stable strengthening network at room temperature during the air cooling process.

[0015] Compared with the prior art, the present invention has the following beneficial effects: This invention, through extremely precise thermodynamic control of alloy composition and matching of phase transformation kinetics with heat treatment processes, produces the following objective and groundbreaking beneficial effects: First, by strictly defining and locking the carbon content within the carbon-reduced matrix range of 0.40% to 0.55%, the crystalline region of primary eutectic carbides is avoided from the liquid-phase solidification stage, eliminating micron-sized brittle and hard particles that cause stress concentration. This compositional design, combined with three-dimensional multi-directional forging and ultra-high purity dual-stage smelting processes, yields a pure, high-toughness, fine-grained martensitic chassis, significantly improving the material's isotropic mechanical properties in all directions. This results in a substantial increase in the room-temperature impact toughness of the die steel, fundamentally eliminating the macroscopic fatigue source that induces early microcracks and greatly reducing the risk of chipping and fracture of the die under extreme stamping and forging conditions.

[0016] Secondly, a high-density nanoscale reinforced framework with superior resistance to thermal softening was constructed through a multi-temperature zone fine-coordinated aging precipitation mechanism of quaternary metal elements across time and space. High-density (Nb,V)C nanoscale hard phases were excited by heterogeneous nucleation and precipitation relay using Nb and Ti templates. Simultaneously, the spontaneous interfacial segregation effect of a high proportion of Mo atoms formed a robust diffusion physical barrier and a low lattice mismatch buffer layer at the phase interface. This mechanism, from both thermodynamic and kinetic dimensions, severed the high-temperature Ostwald coarsening channel of the reinforced particles, ensuring that the secondary nanocarbide size remained stable after long-term 600℃ high-temperature thermal shock cycling, maintaining excellent red hardness and significantly reducing the diffusion rate of thermal crack density, thus extending the entire lifespan of the mold under hot working conditions. Detailed Implementation

[0017] The present invention will be further described in detail below with reference to specific embodiments. The following embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it.

[0018] The carbon-reduced microalloyed modified die steel provided by this invention follows a technical route of "matrix carbon reduction + multi-element nanoscale heterogeneous synergistic microalloying". The carbon content is strictly limited to the range of 0.40% to 0.55%, which is below the boundary of the complete solid solution range of carbon in high-temperature austenite. This allows for thermodynamic avoidance of the formation region of primary eutectic carbides during solidification and crystallization, ensuring that no micron-sized network or blocky primary carbides remain in the as-cast structure. Although the above carbon reduction design lowers the concentration of dissolved carbon atoms in the martensitic matrix, this invention provides over-compensation for secondary hardening capacity through the gradient nucleation and relay precipitation mechanism of four microalloying elements (Nb, V, Ti, and Mo) in different temperature ranges. Specifically, trace amounts of Ti preferentially combine with N in the high-temperature liquid phase or δ-phase region, precipitating nanoscale TiN particles. These particles possess extremely high thermodynamic stability and do not dissolve during subsequent high-temperature heating. The Zener pinning effect firmly locks the original austenite grain boundaries, preventing abnormally coarse grains during high-temperature austenitization. Both TiN and NbC belong to the NaCl-type face-centered cubic structure, and their lattice constants are similar, making TiN a natural heterogeneous nucleation template for NbC epitaxial precipitation. During the initial cooling and tempering of austenite, Nb preferentially combines with carbon using TiN as a template, forming dispersed NbC nanoclusters. This process first consumes locally highly active carbon atoms near dislocation lines, leaving most of the V in a supersaturated state within the martensite lattice. When the tempering temperature rises to above 560℃ in the secondary hardening range, metastable cementite dissolves and releases free carbon. V atoms then undergo explosive secondary epitaxial precipitation based on the existing NbC cores, forming high-density (Nb,V)C nanocomposite carbides. Simultaneously, Mo atoms, due to their much larger radius than Fe, V, and Nb, cause higher lattice elastic distortion in the martensite matrix. Driven by the principle of minimum energy, they spontaneously segregate towards the carbide-matrix interface, forming a dense Mo-rich shell. This shell reduces the lattice mismatch between carbides and the matrix, weakening the surface energy driving force for particle coarsening. On the other hand, the extremely low diffusion coefficient of Mo in steel constitutes a kinetic diffusion barrier, doubly blocking the Ostwald ripening channel and keeping the precipitated phase size stable in the optimal Orowan strengthening range of 5 nm to 20 nm for a long time.

[0019] The purity requirements and sources of each component in this invention are explained below. Carbon is introduced along with the base material in the form of scrap steel and pig iron, and its content is finely adjusted to the target level during the smelting process using carbon powder. Chromium, molybdenum, and vanadium are added to the melt in the form of low-carbon ferrochrome (FeCr67C0.06, grade according to GB / T 5683), ferromolybdenum (FeMo60, grade according to GB / T 3649), and ferrovanadium (FeV50A or FeV80A, grade according to GB / T4139), respectively. Niobium and titanium are fed into the melt at the end of the vacuum induction melting process in the form of specially made cored wires, wherein the purity of niobium powder in the niobium core wire is not less than 99.5%, and the purity of titanium powder in the titanium core wire is not less than 99.0%. The outer shell of the cored wire is made of low-carbon steel strip, and the feeding speed is controlled between 1.5 m / s and 2.5 m / s to ensure uniform dissolution and precise recovery of alloying elements in the molten steel. Manganese and silicon are added in the form of medium-carbon ferromanganese and ferrosilicon, respectively. Nitrogen is introduced by filling the furnace with high-purity nitrogen gas at the end of the vacuum induction melting stage and maintaining a certain nitrogen partial pressure. The nitrogen charging pressure is generally controlled between 0.02 MPa and 0.05 MPa, and the amount of dissolved nitrogen is precisely controlled according to Sievert's law in conjunction with the steel composition. For optional components, tungsten is added in the form of ferrotungsten, nickel is added in the form of pure nickel plates or ferronickel, and rare earth elements are added in the form of mixed rare earths (mainly containing Ce and La) through cored wire before electroslag remelting to reduce the burn-off of rare earth elements in high-temperature molten steel. During the smelting process, the mass fraction of impurities P is controlled to not exceed 0.010%, and the mass fraction of S is controlled to not exceed 0.003%.

[0020] The modification method for mold steel of this invention includes four core steps: smelting and solidification forming, multi-directional large deformation forging, austenitization treatment, and cooling and microstructure control. Smelting employs a dual process of vacuum induction melting and protective atmosphere electroslag remelting. Vacuum induction melting completes deep degassing and alloying under a vacuum level not exceeding 1 Pa, followed by protective atmosphere electroslag remelting in a sealed electroslag furnace. Because conventional open electroslag remelting triggers a strong denitrification reaction in the extremely high-temperature slag and molten metal pool environment, leading to a significant loss of nitrogen content precisely controlled during the vacuum induction melting stage, this invention specifically employs protective atmosphere technology in the electroslag remelting stage: a mixture of nitrogen and argon is introduced into the sealed electroslag furnace, controlling the total nitrogen partial pressure within the furnace to be within the range of 0.02 MPa to 0.10 MPa. Maintaining this nitrogen partial pressure ensures that the chemical potential of nitrogen above the surface of the molten steel is balanced with the chemical potential of dissolved nitrogen in the molten steel. According to Sievert's law, this effectively suppresses nitrogen escape from the molten steel to the gas phase, ensuring consistency between the nitrogen content in the final ingot and the controlled value during the vacuum induction melting stage. Electroslag remelting, through slag refining and directional crystallization processes, further eliminates non-metallic inclusions and completely avoids central shrinkage cavities and porosity. After the ingot is tapped from the furnace, it is heated to 1150℃ to 1180℃ for homogenization and holding for at least 8 hours to completely eliminate as-cast segregation and promote the redissolution of as-cast precipitates. After homogenization, three-dimensional multi-directional upsetting forging is performed within the temperature range of 1150℃ to 950℃, with a total forging ratio of not less than 6. The final forging temperature is controlled near the non-recrystallization region at 900℃ to 950℃. Utilizing the solute dragging effect of dissolved Nb atoms, the austenite grains are compressed into a thin disc shape, accumulating extremely high-density deformation energy storage and nucleation sites. After the forged blank is slowly cooled to room temperature, it is reheated to 1050℃ to 1100℃ for austenitization holding. The holding time is determined by a coefficient of 0.5 hours / 25 mm effective thickness. The purpose is to fully dissolve the medium-sized alloy carbides formed during forging and to force elements such as C, Cr, Mo, and V back into the austenite lattice to form extremely high supersaturation.

[0021] In the cooling and microstructure control stage, this invention provides two optional process routes to obtain martensitic and lower bainitic matrices, respectively.

[0022] The first route is a continuous cooling quenching followed by multiple high-temperature tempering processes (Route 1), used to obtain a tempered martensitic matrix. After austenitization holding, quenching is performed using high-purity nitrogen gas at a pressure greater than 6 bar or stepped warm oil cooling. The quenched and cooled forgings undergo at least three high-temperature tempering processes, each heated to 560°C to 600°C, held at that temperature for 2 hours, and then air-cooled to room temperature. The first tempering eliminates the residual stress from the intense phase transformation and precipitates transition carbides; the second tempering induces an avalanche-like secondary nano-precipitation of V and Nb elements and an unstable transformation of the retained austenite; the third tempering softens and toughens the newly formed secondary martensite, stabilizing the final microstructure and residual stress state. Examples 1 to 6 below all adopt this route.

[0023] The second route is the isothermal quenching route (Route 2), used to obtain a lower bainitic matrix. After austenitization holding, the forging is rapidly transferred to a salt bath or isothermal furnace preheated to 280°C to 350°C, and held at this temperature range for 1 to 4 hours to allow the supercooled austenite to undergo an isothermal transformation to lower bainite above the Ms point. It is then air-cooled to room temperature. The isothermal temperature range is selected based on the fact that the Ms point of the alloy system of this invention is estimated to be approximately 260°C to 290°C using the Barbier formula. Setting the isothermal temperature 20°C to 60°C above the Ms point ensures that the main microstructure is lower bainitic laths rather than martensite. After the isothermal transformation, two tempering treatments at 560°C to 600°C are performed to promote secondary precipitation of nano-carbides and eliminate residual stress. The matrix obtained by the lower bainitic route has a slightly lower hardness than that of the tempered martensitic route, but its fracture toughness and impact resistance are superior, making it suitable for large mold applications where toughness requirements are more stringent. The following Example 7 uses this route.

[0024] The test methods and standards involved in this invention are as follows: Macroscopic Rockwell hardness is tested according to ASTM E18 standard using a diamond cone indenter with a 150 kgf load. Five points are tested on each specimen, and the average value is taken. Room temperature Charpy V-notch impact toughness is tested according to ISO 148-1 standard. The specimen size is 10 mm × 10 mm × 55 mm, the V-notch depth is 2 mm, and the notch bottom radius is 0.25 mm. The test is performed using a pendulum impact testing machine at room temperature (23 ± 2 °C), and the average value of three specimens in each group is taken. The evaluation method for red hardness (resistance to heat softening) is as follows: The fully quenched and tempered specimen is placed in a constant-temperature box-type resistance furnace preheated to 600 °C and held continuously for 50 hours. After removal, it is air-cooled to room temperature, and the residual room temperature hardness is measured according to ASTM E18 standard. The primary carbide size evaluation method was as follows: after grinding and polishing, the sample was etched with a 4% nitric acid ethanol solution, and observed under an optical metallographic microscope at 500x magnification in at least 20 fields of view. The equivalent circle diameter of the largest observed carbide was recorded. The morphology and size of secondary precipitated carbides were observed using a transmission electron microscope at an accelerating voltage of 200 kV. The equivalent diameter of at least 200 particles was statistically analyzed and the average value was calculated. The elemental distribution of the core-shell structure was characterized by scanning transmission electron microscopy (STEM-EDS mapping). The surface distribution images of Fe, Mo, Nb, V, and C elements were performed to confirm the segregation state of the Mo-rich shell at the carbide phase interface. The proto-austenite grain size was evaluated according to ASTM E112 standard. The thermal fatigue performance test adopted the self-constrained thermal fatigue method. The sample was heated from room temperature to 700°C within 5 seconds by high frequency induction heating, and then immediately cooled to room temperature by water spraying as one cycle. After a total of 3000 cycles, the maximum penetration depth of the main crack and the total length of the crack per unit area were measured under an optical microscope. The test results of traditional H13 steel under the same conditions were used as a normalized benchmark for comparison. Example 1

[0025] The alloy composition is prepared according to the following mass percentages: C 0.42%, Cr 4.80%, Mo 1.80%, V 0.90%, Nb 0.05%, Ti 0.018%, Mn 0.35%, Si 0.15%, N 0.006%, with the balance being Fe and unavoidable impurities. In this composition, the mass ratio of Ti to N is 3.0, the mass ratio of Mo to Nb is 36, and the mass ratio of V to Nb is 18, all of which satisfy the composition constraints in the claims.

[0026] The smelting process employed a dual-stage process of vacuum induction melting and protective atmosphere electroslag remelting. In the vacuum induction melting stage, alloying and degassing were completed under a vacuum below 1 Pa. Finally, microalloying elements were introduced by feeding in cored wire containing Ti and Nb. After smelting, the metal was cast into electrode rods. Electroslag remelting was carried out in a sealed electroslag furnace filled with a nitrogen and argon mixture under a protective atmosphere, with the nitrogen partial pressure controlled at 0.04 MPa, yielding round ingots with a diameter of 350 mm. The ingots were heated to 1150 °C and held for 10 hours for homogenization. Subsequently, three-dimensional multi-directional upsetting forging was performed within a temperature range of 1150 °C to 950 °C, with a total forging ratio of 6. The final forging temperature was controlled at 920 °C. After forging, the ingots were air-cooled to room temperature to obtain square forging billets with a cross-sectional dimension of 200 mm × 200 mm. The forging billet was placed in a vacuum atmosphere furnace and slowly heated to 1050℃ at a rate of 50℃ / h. It was held for 4 hours based on a holding coefficient of 0.5h / 25mm. After holding, it was quenched using 6.5bar high-purity nitrogen. The quenched forging was then tempered three times, each time heated to 560℃ and held for 2 hours, followed by air cooling to room temperature. Example 2

[0027] The alloy composition was prepared according to the following mass percentages: C 0.53%, Cr 6.00%, Mo 3.00%, V 1.40%, Nb 0.12%, Ti 0.04%, Mn 0.70%, Si 0.45%, N 0.012%, with the balance being Fe and unavoidable impurities. In this composition, the mass ratio of Ti to N is approximately 3.33, the mass ratio of Mo to Nb is 25, and the mass ratio of V to Nb is approximately 11.7. The component contents of this embodiment are within the upper limit of the broad range of claims, and are intended to verify the performance of the alloy system at the high-alloy end.

[0028] The smelting process is the same as the dual-stage process described in Example 1. A protective atmosphere is also used in the electroslag remelting stage, with the nitrogen partial pressure controlled at 0.06 MPa. The ingot homogenization temperature is 1180℃, held for 12 hours. The total forging ratio of the three-dimensional multi-directional forging is 8, and the final forging temperature is controlled at 940℃. After forging, slow cooling yields a square forging billet with a cross-sectional dimension of 180mm × 180mm. The austenitizing temperature is set at 1100℃, and the holding time is calculated based on a coefficient of 0.5h / 25mm for 3.6 hours. Step-cooled oil is used for quenching, with the oil temperature preset at 60℃. After quenching, three tempering treatments are performed, each at 600℃, held for 2 hours, and then air-cooled. Example 3

[0029] The alloy composition is prepared according to the following mass percentages: C 0.48%, Cr 5.20%, Mo 2.30%, V 1.10%, Nb 0.08%, Ti 0.03%, Mn 0.50%, Si 0.28%, N 0.010%, with the balance being Fe and unavoidable impurities. The mass ratio of Ti to N is 3.0, the mass ratio of Mo to Nb is 28.75, and the mass ratio of V to Nb is 13.75. This composition is located in the central region of the preferred scope of the claims.

[0030] The smelting process is the same as the aforementioned duplex process. During the vacuum induction melting stage, P ≤ 0.008% and S ≤ 0.002% are strictly controlled. During the electroslag remelting stage, the nitrogen partial pressure is controlled at 0.05 MPa. The ingot is heated to 1170℃ and held for 10 hours for homogenization. The total forging ratio for three-dimensional multi-directional forging is 7, with a final forging temperature of 930℃, followed by slow cooling. The austenitizing temperature is 1080℃, and the holding time is calculated based on the effective thickness. High-purity nitrogen gas at 7 bar is used for quenching. After quenching, three tempering processes are performed, each held at 580℃ for 2 hours, followed by air cooling to room temperature. Example 4

[0031] The alloy composition was prepared according to the following mass percentages: C 0.47%, Cr 5.30%, Mo 2.40%, V 1.15%, Nb 0.07%, Ti 0.028%, Mn 0.55%, Si 0.30%, N 0.008%, W 0.80%, Ni 0.50%, RE 0.015%, with the balance being Fe and unavoidable impurities. The mass ratio of Ti to N was 3.5, the mass ratio of Mo to Nb was approximately 34.3, and the mass ratio of V to Nb was approximately 16.4. This example introduces optional components W, Ni, and the rare earth element RE based on Example 3 to investigate the further improvement effect of auxiliary alloying elements on the overall performance.

[0032] In the smelting process, tungsten is added as ferrotungsten during the vacuum induction melting stage along with the base alloy, nickel is added as pure nickel plates, and rare earth elements are fed in as mixed rare earth cored wire at the end of refining. The nitrogen partial pressure is controlled at 0.05 MPa during the electroslag remelting stage. The ingot homogenization temperature is 1175℃, held for 11 hours, the total forging ratio for three-dimensional multi-directional forging is 8, and the final forging temperature is 935℃. The austenitizing temperature is 1090℃, held at a coefficient of 0.5h / 25mm, and quenched with 7.5 bar high-purity nitrogen. Three tempering processes are performed, each held at 590℃ for 2 hours, followed by air cooling to room temperature. Example 5

[0033] The alloy composition was prepared according to the following mass percentages: C 0.50%, Cr 5.00%, Mo 2.50%, V 1.20%, Nb 0.10%, Ti 0.035%, Mn 0.60%, Si 0.35%, N 0.010%, with the balance being Fe and unavoidable impurities. The mass ratio of Ti to N was 3.5, the mass ratio of Mo to Nb was 25, and the mass ratio of V to Nb was 12. In this embodiment, the Nb and V contents were both increased to the upper end of the preferred range, while a relatively high Mo content was matched to observe the response of properties and microstructure as the precipitation volume fraction increased.

[0034] The smelting and forging processes are the same as in the previous embodiments, with the nitrogen partial pressure controlled at 0.05 MPa during the electroslag remelting stage. The homogenization temperature is 1160℃ and held for 10 hours. The total forging ratio for three-dimensional multi-directional forging is 6, and the final forging temperature is 925℃. The austenitizing temperature is 1070℃, and stepped warm oil cooling quenching is used. Three tempering processes are performed, each held at 570℃ for 2 hours, followed by air cooling to room temperature. Example 6

[0035] The alloy composition was prepared according to the following mass percentages: C 0.46%, Cr 5.10%, Mo 2.10%, V 1.05%, Nb 0.09%, Ti 0.03%, Mn 0.48%, Si 0.25%, N 0.010%, with the balance being Fe and unavoidable impurities. The mass ratio of Ti to N was 3.0, the mass ratio of Mo to Nb was approximately 23.3, and the mass ratio of V to Nb was approximately 11.7. In this embodiment, the Mo and V contents were finely adjusted within the preferred range, and the number of tempering cycles was increased to four to investigate the effect of increasing the number of tempering cycles on the completion of the residual austenite transformation and the stability of the microstructure.

[0036] The smelting and forging processes are the same as in the previous embodiments, with the nitrogen partial pressure controlled at 0.05 MPa during the electroslag remelting stage. The homogenization temperature is 1165℃ and held for 10 hours. The total forging ratio for three-dimensional multi-directional forging is 7, and the final forging temperature is 930℃. The austenitizing temperature is 1085℃, and quenching is performed using 7 bar high-purity nitrogen. Four tempering processes are conducted, each held at 585℃ for 2 hours, followed by air cooling to room temperature. Example 7

[0037] The alloy composition was prepared according to the following mass percentages: C 0.48%, Cr 5.20%, Mo 2.30%, V 1.10%, Nb 0.08%, Ti 0.03%, Mn 0.50%, Si 0.28%, N 0.010%, with the balance being Fe and unavoidable impurities. The alloy composition of this embodiment is exactly the same as that of Example 3, but Route 1 (continuous cooling quenching followed by multiple tempering) is replaced by Route 2 (isothermal quenching route) to directly compare the performance differences between the two matrix structures under the same composition system.

[0038] The smelting and forging processes were exactly the same as in Example 3, with the nitrogen partial pressure controlled at 0.05 MPa during the electroslag remelting stage. The ingot was heated to 1170°C and held for 10 hours for homogenization. The total forging ratio for three-dimensional multi-directional forging was 7, and the final forging temperature was 930°C. The austenitizing temperature was 1080°C, and the holding time was calculated based on the effective thickness. After austenitizing, the forging was quickly transferred to a nitrate bath preheated to 320°C for isothermal holding for 3 hours to allow the undercooled austenite to undergo a full isothermal transformation to lower bainite. It was then removed and air-cooled to room temperature. After the isothermal transformation, two tempering treatments were performed, each time heating to 580°C and holding for 2 hours, followed by air cooling to room temperature to promote secondary precipitation of nano-carbides and eliminate residual stress. Example 8

[0039] The alloy composition was prepared according to the following mass percentages: C 0.47%, Cr 5.30%, Mo 2.40%, V 1.15%, Nb 0.07%, Ti 0.028%, Mn 0.55%, Si 0.30%, N 0.008%, W 0.80%, Ni 0.50%, RE 0.015%, with the balance being Fe and unavoidable impurities. The alloy composition of this example is exactly the same as that of Example 4, and route two (isothermal quenching route) was also used to examine the comprehensive performance of the auxiliary alloy system containing W, Ni, and RE under lower bainitic matrix conditions.

[0040] The smelting and forging processes were exactly the same as in Example 4. The austenitizing temperature was 1090℃, and the holding time was calculated based on the effective thickness. After the austenitizing holding was completed, the forging was quickly transferred to a nitrate bath preheated to 310℃ for isothermal holding for 3.5 hours, followed by air cooling to room temperature. After the isothermal transformation was completed, two tempering treatments were performed, each time heated to 590℃ and held for 2 hours, followed by air cooling to room temperature.

[0041] Comparative Example 1 The alloy composition was prepared according to the following mass percentages: C 0.48%, Cr 5.20%, Mo 2.30%, V 1.10%, Ti 0.03%, Mn 0.50%, Si 0.28%, N 0.010%, with the balance being Fe and unavoidable impurities; Nb was not added. This comparative example aims to investigate the effect of the Nb-deficient C heterogeneous nucleation template on the secondary precipitation behavior and final properties of V after the removal of the core microalloying element Nb.

[0042] The preparation process is exactly the same as in Example 3: homogenization temperature 1170℃, three-dimensional multi-directional forging total forging ratio 7, final forging temperature 930℃, austenitizing temperature 1080℃, nitrogen quenching at 7 bar, and tempering at 580℃ three times.

[0043] Comparative Example 2 The alloy composition was prepared according to the following mass percentages: C 0.48%, Cr 5.20%, Mo 2.30%, V 1.10%, Nb 0.08%, Mn 0.50%, Si 0.28%, N 0.010%, with the balance being Fe and unavoidable impurities. No Ti was added. This comparative example aims to verify the impact of removing Ti and losing the high-temperature grain boundary pinning effect of TiN on grain control during austenitization and the subsequent uniformity of NbC distribution.

[0044] The preparation process is exactly the same as in Example 3.

[0045] Comparative Example 3 The alloy composition was prepared according to the following mass percentages: C 0.70%, Cr 5.20%, Mo 2.30%, V 1.10%, Nb 0.08%, Ti 0.03%, Mn 0.50%, Si 0.28%, N 0.010%, with the balance being Fe and unavoidable impurities. The carbon content is 0.70%, far exceeding the 0.55% upper limit specified in this invention, belonging to a conventional high-carbon design scheme. This comparative example is used to verify the inevitable precipitation of primary carbides and their catastrophic damage to impact toughness after the carbon content exceeds the carbon reduction range of this invention.

[0046] The preparation process is exactly the same as in Example 3.

[0047] Comparative Example 4 The alloy composition was prepared according to the following mass percentages: C 0.48%, Cr 5.20%, Mo 1.20%, V 1.10%, Nb 0.08%, Ti 0.03%, Mn 0.50%, Si 0.28%, N 0.010%, with the balance being Fe and unavoidable impurities. The mass ratio of Mo to Nb was 15, lower than the lower threshold of 20 specified in this invention. This comparative example aims to verify the coarsening behavior of the nanoprecipitates at high temperatures and their negative impact on red hardness when the Mo content is insufficient to form an effective continuous coating shell at the carbide phase interface.

[0048] The preparation process is exactly the same as in Example 3.

[0049] The alloy composition ratios of each embodiment and comparative example are summarized in Table 1, and the performance test results are summarized in Table 2.

[0050] Table 1 Chemical composition (mass percentage, %) of each example and comparative example serial number C Cr Mo V Nb Ti Mn Si N W Ni RE Example 1 0.42 4.80 1.80 0.90 0.05 0.018 0.35 0.15 0.006 — — — Example 2 0.53 6.00 3.00 1.40 0.12 0.04 0.70 0.45 0.012 — — — Example 3 0.48 5.20 2.30 1.10 0.08 0.03 0.50 0.28 0.010 — — — Example 4 0.47 5.30 2.40 1.15 0.07 0.028 0.55 0.30 0.008 0.80 0.50 0.015 Example 5 0.50 5.00 2.50 1.20 0.10 0.035 0.60 0.35 0.010 — — — Example 6 0.46 5.10 2.10 1.05 0.09 0.03 0.48 0.25 0.010 — — — Example 7 0.48 5.20 2.30 1.10 0.08 0.03 0.50 0.28 0.010 — — — Example 8 0.47 5.30 2.40 1.15 0.07 0.028 0.55 0.30 0.008 0.80 0.50 0.015 Comparative Example 1 0.48 5.20 2.30 1.10 — 0.03 0.50 0.28 0.010 — — — Comparative Example 2 0.48 5.20 2.30 1.10 0.08 — 0.50 0.28 0.010 — — — Comparative Example 3 0.70 5.20 2.30 1.10 0.08 0.03 0.50 0.28 0.010 — — — Comparative Example 4 0.48 5.20 1.20 1.10 0.08 0.03 0.50 0.28 0.010 — — — Table 2 Performance test results of each embodiment and comparative example serial number Hardness after tempering (HRC) Charpy V notch impact energy (J / cm²) Residual hardness (HRC) at 600℃ for 50 hours Thermal fatigue crack propagation rate index (relative to H13) Maximum size of primary carbides (μm) Average equivalent diameter (nm) of secondary precipitated carbides Example 1 58.5 48 54.2 0.42 ≤3 14 Example 2 61.8 45 55.6 0.39 ≤3 11 Example 3 60.5 56 56.5 0.35 ≤2 9 Example 4 61.2 58 57.3 0.31 ≤2 8 Example 5 60.8 52 55.8 0.37 ≤3 10 Example 6 59.8 55 56.2 0.34 ≤2 9 Example 7 58.8 68 55.5 0.33 ≤2 10 Example 8 59.5 72 56.8 0.29 ≤2 9 Comparative Example 1 57.2 38 50.8 0.65 ≤3 28 Comparative Example 2 59.5 35 53.2 0.58 5~8 18 Comparative Example 3 62.5 11 51.5 0.72 18~30 15 Comparative Example 4 59.3 51 49.8 0.70 ≤3 32 As can be clearly observed from the performance data in Table 2, Examples 1 to 8, while maintaining a high hardness of over 58 HRC, all exhibited a stable room-temperature Charpy V-notched impact energy of over 45 J / cm², significantly higher than all levels in Comparative Examples 1 to 4 except for Comparative Example 4. Regarding thermal softening resistance, after a 50-hour long-term heat treatment at 600°C, Examples 1 to 8 all showed residual hardness above 54 HRC. Example 4 exhibited the highest residual hardness of 57.3 HRC in Route 1 due to the additional delay in dislocation recovery by W pairs and the deep purification effect of rare earth elements on grain boundaries. In terms of the thermal fatigue crack propagation rate index, all examples showed an index below 0.42, a reduction of over 58% compared to traditional H13 steel, with Example 8 showing an even lower index of 0.29. At the microstructure level, no primary blocky carbides larger than 3 μm were observed within the materials of any of the examples. The average equivalent diameter of the secondary precipitated carbides ranged from 8 nm to 14 nm, exhibiting a typical core-shell morphology.

[0051] The performance gradient variation patterns among the embodiments are highly consistent with the alloy design logic. In Embodiment 1, because both the carbon content and alloy element content are within the lower limit of the claims, the volume fraction of secondary hardening carbides provided by V is relatively low, resulting in a tempering hardness of 58.5 HRC, impact toughness of 48 J / cm², and red hardness of 54.2 HRC. Although the overall performance is excellent, it is at a relatively low level among the embodiments. Embodiment 2 pushes each alloy element to the upper limit of a wide range. The higher carbon and vanadium content increases the hardness after tempering to 61.8 HRC, and the higher molybdenum content achieves a red hardness of 55.6 HRC. However, due to the higher total alloy element content and increased difficulty in eliminating as-cast segregation, the impact toughness slightly decreases to 45 J / cm². The composition of Embodiment 3 is in the center of the preferred range, with the best matching degree of element content and proportion. It achieves an impact toughness of 56 J / cm² and a residual hardness of 56.5 HRC at a hardness level of 60.5 HRC, resulting in the most balanced overall performance. Example 4 introduces W, Ni, and RE based on Example 3. The addition of W further suppresses the recovery of high-temperature creep dislocations, increasing the residual hardness to 57.3 HRC; Ni improves the low-temperature ductility and toughness of the matrix, further increasing the impact energy to 58 J / cm²; the microalloying of RE promotes inclusion spheroidization and grain boundary purification, achieving the best level of thermal fatigue resistance among the examples in Route 1 (martensitic matrix). Example 5 increases the content of Nb and V to the upper end of the preferred range. The increased volume fraction of precipitates results in a higher hardness of 60.8 HRC and good red hardness of 55.8 HRC, but the increased precipitation density leads to a decrease in the reserve of mobile dislocations in the matrix, slightly reducing the impact toughness to 52 J / cm². Example 6 increases the number of tempering cycles to four. The additional tempering cycle makes the residual austenite transformation more complete, further enhancing the microstructure stability. The impact toughness and red hardness are both superior to Example 5 with three tempering cycles, while the thermal fatigue extension index decreases to 0.34.

[0052] Examples 7 and 8 used Route 2 (isothermal quenching route) to obtain a lower bainitic matrix, providing direct experimental evidence for the performance comparison of the two process routes. The alloy composition of Example 7 was exactly the same as that of Example 3; the performance difference between the two stemmed entirely from the different matrix microstructures. The hardness of Example 7 after tempering was 58.8 HRC, 1.7 HRC lower than the 60.5 HRC of Example 3. This is because the carbon supersaturation inside the lower bainitic laths was lower than that of quenched martensite, resulting in slightly insufficient driving force for carbon atoms to precipitate during tempering for secondary hardening. However, the lower bainitic laths themselves possess superior plasticity and toughness compared to martensite, and the residual austenite film between the laths effectively blunts crack tips, significantly increasing the impact toughness of Example 7 to 68 J / cm², a 21% improvement over the 56 J / cm² of Example 3. Regarding red hardness, the residual hardness of Example 7 after heat exposure at 600℃ for 50 hours was 55.5 HRC, not significantly different from the 56.5 HRC of Example 3, indicating that the core-shell structured nanocarbides in the lower bainitic matrix can also effectively resist Ostwald coarsening. The thermal fatigue crack propagation rate index was 0.33, better than 0.35 in Example 3, which is attributed to the stronger crack tip plastic passivation ability of the lower bainitic matrix, which has an additional inhibitory effect on thermal fatigue crack propagation. Example 8 introduced W, Ni, and RE based on Example 7. The addition of Ni further improved the low-temperature plasticity and toughness of the lower bainitic matrix, making the impact toughness the highest value of 72 J / cm² among all examples; the solute pinning effect of W increased the red hardness to 56.8 HRC; the grain boundary purification effect of rare earth elements reduced the thermal fatigue propagation rate index to 0.29, which is the best value among all examples. The data from Examples 7 and 8 fully demonstrate that the alloy design of the present invention is also effective under the isothermal quenching route, and the isothermal quenching route has significant advantages over the continuous cooling quenching route in terms of impact toughness and thermal fatigue resistance, and is especially suitable for large hot work dies with more stringent impact resistance requirements.

[0053] The performance degradation phenomena and their underlying causes in each comparative example are analyzed as follows.

[0054] Comparative Example 1 removed Nb. Without the NbC heterogeneous nucleation template, V atoms lacked high-density pre-set nucleation sites during tempering and could only spontaneously nucleate through crystal defects such as dislocation intersections. This increased the randomness of precipitation events, with some V carbides precipitating and growing concentrated at a few energy-favorable sites, while other regions experienced insufficient precipitation density. Transmission electron microscopy (TEM) observations showed that the average particle size of the secondary carbides in Comparative Example 1 increased to 28 nm, significantly larger than the 9 nm in Example 3, with a significantly widened interparticle spacing and a substantial decrease in the critical shear stress required for the Orowan bypass mechanism. This directly resulted in a tempering hardness of only 57.2 HRC, failing to reach the industrially practical threshold of 58 HRC, and the impact toughness also decreased to 38 J / cm² due to localized stress concentration caused by uneven precipitation distribution. More significantly, the larger-sized carbides were more prone to Ostwald coarsening and agglomeration during prolonged exposure at 600°C, with the residual hardness plummeting to 50.8 HRC and the thermal fatigue propagation rate exponent reaching as high as 0.65. The above data fully demonstrate the irreplaceable role of Nb as a nucleation template agent in the system of this invention.

[0055] Comparative Example 2 removed Ti. Due to the lack of high-temperature grain boundary pinning effect from TiN nanoparticles, the original austenite grains underwent significant abnormal coarsening during the 1080℃ austenitization holding stage. EBSD measurements showed the grain size only reached ASTM grade 6, far coarser than ASTM grade 9 in Example 3. The coarse original austenite grains not only increased the size of the martensite packets and blocks and degraded the impact toughness to 35 J / cm², but also resulted in uneven NbC distribution during the austenitization stage due to the lack of an epitaxial growth template from TiN, with some NbC agglomerating in a chain-like manner along the coarse grain boundaries. Furthermore, metallographic observation revealed primary carbide aggregates with sizes ranging from 5 μm to 8 μm in the forgings of Comparative Example 2. This is because, without TiN pinning, rapid grain boundary migration caused the originally fine carbides to be captured and aggregated during grain boundary sweeping. The thermal fatigue index of 0.58 also indicates the shortening effect of grain coarsening on the hot crack propagation path.

[0056] The carbon content of Comparative Example 3 was increased to 0.70%, significantly exceeding the upper limit of 0.55% in this invention. During the as-cast solidification stage, the excess carbon formed coarse primary carbon atoms with Cr and Mo. and Metallographic observation revealed that the largest carbides reached 18 μm to 30 μm in size, exhibiting a network or chain-like distribution along the dendritic intergranular spaces. Although this comparative example underwent the same three-dimensional multi-directional forging and high-temperature austenitization treatment as Example 3, these coarse carbides formed during the solidification stage, with sizes ranging from tens to hundreds of micrometers, even... and At austenitizing temperatures above 1100℃, there is a certain thermodynamic tendency for remelting. The dissolution process still requires long-range transport of alloy atoms from the carbide interior via bulk or interfacial diffusion. The required diffusion time is proportional to the square of the particle size, far exceeding the industrially feasible holding time range. Therefore, kinetically, it cannot be fully dissolved within the limited homogenization and austenitizing holding time. Forging can only elongate the phases along the deformation direction, not eliminate them. Under service stress, the interface between these coarse, brittle, and hard phases and the ductile matrix constitutes a natural crack initiation source, causing the impact toughness to plummet to 11 J / cm², falling into the category of typical brittle materials. Simultaneously, because a large amount of carbon is consumed in the primary carbides, the effective carbon activity available for secondary precipitation during tempering is reduced. Combined with the alloy depletion effect of the matrix between the coarse carbides, the red hardness is only 51.5 HRC. The thermal fatigue crack propagation rate index is as high as 0.72, far inferior to all other examples. This comparative example clearly demonstrates the absolute necessity of the carbon reduction design of this invention.

[0057] Comparative Example 4 maintained the exact same carbon and microalloying element ratios as Example 3, except that the Mo content was reduced from 2.30% to 1.20%, resulting in a Mo to Nb mass ratio of only 15, lower than the lower limit of 20 specified in this invention. Due to the insufficient concentration of free Mo atoms, a continuous and dense Mo-rich shell could not form on the surface of the nano-(Nb,V)C carbides precipitated during the tempering stage, leaving a large number of "gaps" at the phase interface. STEM-EDS elemental surface scanning analysis results showed that in Example 3, a clear ring-shaped enrichment signal of Mo element was observed around the carbide particles, forming a typical core-shell elemental distribution characteristic with the core distribution of Nb and V elements; while in Comparative Example 4, the Mo enrichment signal around the carbide particles of the same size was extremely weak and discontinuous, failing to form a continuous shell covering the particle surface, confirming that insufficient Mo content led to incomplete interfacial segregation and coating. In the absence of an interfacial diffusion barrier, the nano-carbide rapidly coarsens according to the classic Ostwald ripening mechanism during 600℃ holding time, with the average particle size of the secondary carbides increasing to 32nm, far exceeding the 9nm level of Example 3. Correspondingly, the residual hardness after 600℃×50h is only 49.8HRC, and the thermal fatigue crack propagation rate index is as high as 0.70. This example also reflects a significant phenomenon: due to the reduced Mo content weakening the rightward shift effect on the continuous cooling transformation curve, a small amount of pearlite transformation signs appeared in the local area of ​​the core under 7bar nitrogen quenching conditions, and the hardness uniformity decreased slightly. These results strongly demonstrate the criticality and necessity of maintaining a Mo to Nb mass ratio of not less than 20 for initiating the core-shell diffusion hindrance mechanism. Simply relying on Nb and V precipitation strengthening without the interfacial coating protection of Mo cannot achieve sustained high-temperature thermal stability.

[0058] Based on a comprehensive analysis of the test data from the embodiments and comparative examples, the fundamental reason for the superior performance of the mold steel of the present invention can be explained from the perspective of the following microscopic mechanisms.

[0059] From a solidification perspective, the carbon content is strictly limited to the matrix range of 0.40% to 0.55%. This concentration allows carbon to achieve complete solid solution in high-temperature austenite above 1100℃, bypassing the nucleation and crystallization region of primary eutectic carbides via a solidification path below the liquidus line. This "thermodynamic decoupling" design completely eliminates the unavoidable micron-sized brittle carbide network in traditional high-carbon mold steels, ensuring the absence of primary blocky carbides larger than 3μm within the material. From a macroscopic fracture mechanics perspective, this eliminates the initiation source of micro-cleavage cracks and early fatigue chipping under service stress. The large number of coarse primary carbides and the catastrophic decline in impact toughness observed in Comparative Example 3 with a carbon content of 0.70% conversely validate the indispensability of this design.

[0060] From the perspective of precipitation strengthening mechanism, Nb, V, Ti, and Mo form a precise temporal synergy across different temperature ranges. Ti reacts with N first in the high-temperature liquid phase and δ-phase region. The precipitated nano-TiN particles remain insoluble throughout all subsequent hot working and heat treatment processes due to their extremely high thermodynamic stability. Through the Zener pinning effect, the original austenite grain size is locked at an extremely fine level above ASTM grade 9. TiN also serves as an epitaxial growth template for NbC, guiding Nb to uniformly disperse and precipitate fine NbC clusters along the grain boundaries during the initial cooling and tempering of austenite. This "relay nucleation" prevents NbC from being distributed in a chain-like pattern along grain boundaries as when Nb is added alone. The preferential precipitation of NbC consumes locally highly active carbon around dislocations, kinetically protecting V from disordered precipitation at low temperatures and retaining a large amount of V in a supersaturated state until the secondary hardening temperature window above 560℃. When the tempering temperature enters this range, the large amount of free carbon released from the re-dissolution of metastable cementite and the activated V atoms rapidly undergo epitaxial precipitation on the NbC core, explosively forming a high-density, extremely small-spaced (Nb,V)C nanocomposite carbide particle swarm. According to the Ashby-Orowan dispersion strengthening model, this particle swarm exerts extremely high resistance to bypassing dislocations, enabling the matrix to still produce a strong secondary hardening peak response under carbon reduction conditions. The tempering hardness of Examples 3 and 4 reached 60.5 HRC and 61.2 HRC, respectively. The experimental facts of Comparative Example 1, where the randomness of V precipitation increased and the particle size coarsened to 28 nm in the absence of Nb, precisely corroborate the core role of the Nb "nesting-guided" nucleation template mechanism in controlling precipitation dispersion.

[0061] From the perspective of the heat softening mechanism, the high proportion of Mo at the phase interface segregation and diffusion hindrance is key to achieving the ultimate red hardness of this invention. During high-temperature tempering or long-term service, nano-carbide exhibits a thermodynamic tendency to coarsen and fail due to Ostwald ripening. However, in the alloy system of this invention, since the mass ratio of Mo to Nb is controlled above 20, a large number of free Mo atoms exist in the matrix. The atomic radius of Mo is significantly larger than that of Fe and V, inducing high elastic distortion energy in the martensitic lattice. Following the principle of minimum system free energy, it spontaneously migrates to the phase interface between (Nb,V)C particles and the matrix, segregating and enriching to form a dense Mo shell covering the particle surface. This core-shell structure produces two synergistic anti-roughening effects in physicochemical terms: First, the size transition effect of large Mo atoms reduces the lattice mismatch between the hard carbide phase and the soft matrix. According to LSW theory, the roughening rate is proportional to the interfacial energy, and the reduction in interfacial energy directly weakens the thermodynamic driving force for particle growth. Second, the diffusion coefficient of Mo in the iron matrix is ​​extremely low. The Mo-rich shell acts as a continuous physical barrier, significantly increasing the activation energy required for Nb, V, and C atoms to cross the interface and enter the interior of the carbide, thus kinetically blocking the interfacial transport channels of atoms. It is under the dual constraints of thermodynamics and kinetics that the roughening rate constant of the (Nb,V)C composite carbide is reduced by at least one order of magnitude, allowing the size of the precipitated phase to remain stable within the Orowan strengthening optimal range of 10 nm to 20 nm after harsh heat exposure at 600 °C for 50 h. The residual hardness of each embodiment remains above 54 HRC. Comparative Example 4, which reduced the Mo content to 1.20%, resulting in a Mo / Nb ratio of only 15, visually demonstrates the rapid coarsening behavior of carbides when the Mo shell is incomplete—the average particle size of secondary carbides increases to 32 nm, the residual hardness drops sharply to 49.8 HRC, and the thermal fatigue propagation rate index deteriorates to 0.70, showing a significant difference in performance compared to Example 3.

[0062] Furthermore, the performance improvement after introducing W, Ni, and RE in Example 4 can be understood from three aspects. A small amount of W dissolved in the matrix forms an additional solute pinning effect, delaying dislocation climb and cross-slip recovery processes at high temperatures, resulting in a cumulative gain on red hardness. 0.50% Ni improves the plasticity and toughness of body-centered cubic martensite at low temperatures, enhances the plastic passivation ability of crack tips, and further increases impact toughness to 58 J / cm². Trace amounts of rare earth elements utilize their strong deoxidation and desulfurization affinity to spheroidize and refine the chain-like non-metallic inclusions such as MnS remaining at grain boundaries, eliminating the adverse effects of inclusions as crack initiation sources and propagation channels. The isotropic mechanical properties of the material in the three orthogonal directions are also improved.

[0063] In summary, this invention eliminates the root cause of brittle fracture caused by coarse primary carbides at the solidification source through carbon reduction matrix design. It constructs an ultra-stable nanoscale strengthening framework through the gradient heterogeneous synergistic nucleation and core-shell diffusion hindrance mechanism of Nb-V-Ti-Mo quaternary microalloying elements. Furthermore, it fully transforms the alloy design potential into macroscopic performance output through strictly matched duplex smelting, multi-directional large deformation forging, and two process routes: continuous cooling quenching followed by tempering or isothermal quenching. Comparative data from examples and comparative examples confirm that, at a high hardness level of 58HRC to 62HRC, the room temperature impact toughness of the mold steel of this invention can reach 45J / cm² to 72J / cm², the residual hardness at 600℃ for 50h is not less than 54HRC, and the thermal fatigue crack propagation rate is only 29% to 42% of that of traditional H13 steel. All core indicators comprehensively surpass those of traditional mold steel.

[0064] The above description is merely a preferred embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made based on the content of the present invention specification, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.

Claims

1. A die steel with reduced carbon content and microalloying modification, characterized in that, The chemical composition of the mold steel, by mass percentage, includes: C: 0.40% to 0.55%; Cr: 4.50% to 6.50%; Mo: 1.50% to 3.50%; V: 0.80% to 1.50%; Nb: 0.03% to 0.15%; Ti: 0.01% to 0.05%; Mn: 0.30% to 0.80%; Si: 0.10% to 0.50%; N: 0.005% to 0.025%; The balance consists of Fe and unavoidable impurities.

2. The mold steel according to claim 1, characterized in that, The mass percentage of the chemical component satisfies the following condition: The mass ratio of Ti to N is 3.0 to 4.0; The mass ratio of Mo to Nb is greater than or equal to 20; The mass ratio of V to Nb is 10 to 30.

3. The mold steel according to claim 1, characterized in that, The chemical composition of the mold steel, by mass percentage, also includes at least one selected from the group consisting of: W: greater than 0 and less than or equal to 1.50%; Ni: greater than 0 and less than or equal to 1.00%; RE: 0.005% to 0.030%.

4. The mold steel according to claim 1, characterized in that, The chemical components, by mass percentage, include: C: 0.45% to 0.50%; Cr: 5.00% to 5.50%; Mo: 2.00% to 2.50%; V: 1.00% to 1.20%; Nb: 0.06% to 0.10%; Ti: 0.015% to 0.03%; Mn: 0.40% to 0.60%; Si: 0.20% to 0.35%; N: 0.010% to 0.018%.

5. The mold steel according to claim 1, characterized in that, The microstructure of the mold steel includes a martensitic matrix or a lower bainitic matrix, and secondary precipitated composite carbonitrides are distributed in the matrix. The average equivalent diameter of the composite carbonitride is 5 nm to 20 nm, and the composite carbonitride includes a (Nb,V)C composite carbide with a core-shell structure, wherein the shell of the core-shell structure is a Mo-rich phase interface coating layer. The mold steel does not contain any primary blocky carbides larger than 3 μm in size.

6. A method for modifying die steel with carbon reduction microalloying as described in any one of claims 1 to 5, characterized in that, Includes the following steps: S1, Smelting and solidification: Smelting is carried out according to the chemical composition ratio of the mold steel and casting is carried out into ingots; S2, Multi-directional large deformation forging: The ingot is heated to 1150°C to 1180°C for homogenization and heat preservation, and then three-dimensional multi-directional forging is performed in the temperature range of 1150°C to 950°C, and the final forging temperature is controlled to be 900°C to 950°C to obtain the forging. S3, austenitizing treatment: The forging is heated to 1050°C to 1100°C for austenitizing and heat preservation. S4, Cooling and Microstructure Control: The forgings after austenitizing and heat preservation are treated using one of the following two routes: Route 1, continuous cooling quenching plus multiple high-temperature tempering: the austenitized forgings are quenched and cooled, and then the quenched and cooled forgings are subjected to at least three high-temperature tempering treatments. Each tempering is heated to 560°C to 600°C and held, and then cooled to room temperature to obtain a mold steel with martensite as the matrix. Route 2, isothermal quenching: After austenitization and heat preservation, the forging is rapidly cooled to an isothermal temperature range of 280°C to 350°C and held for 1 to 4 hours for isothermal transformation, and then air-cooled to room temperature to obtain mold steel with bainite matrix.

7. The modification method according to claim 6, characterized in that, In step S1, the smelting employs a dual process of vacuum induction melting and protective atmosphere electroslag remelting. During the vacuum induction melting stage, the mass fraction of impurity element P is controlled to be less than or equal to 0.010%, and the mass fraction of S is controlled to be less than or equal to 0.003%, and microalloying is performed by feeding in cored wire containing Ti and Nb. During the protective atmosphere electroslag remelting stage, a mixed protective atmosphere of nitrogen and argon is introduced into a sealed electroslag furnace, and the nitrogen partial pressure inside the furnace is controlled to be between 0.02 MPa and 0.10 MPa to suppress the denitrification reaction during the remelting process and maintain precise control of the nitrogen content in the ingot.

8. The modification method according to claim 6, characterized in that, In step S2, the total forging ratio of the three-dimensional multi-directional forging is greater than or equal to 6.

9. The modification method according to claim 6, characterized in that, In step S3, the austenitizing holding time is determined according to a holding coefficient of 0.5 hours / 25 mm effective thickness; in route one of step S4, the quenching cooling is achieved by high-purity nitrogen gas cooling with a pressure greater than 6 bar or stepped warm oil cooling.