Vanadium-bromine flow battery based on dual solid-phase energy storage mechanism

By introducing Bi4[Fe(CN)6]3 solid-phase energy storage material into the vanadium bromine flow battery, a dual-target solid-phase energy storage pathway is formed, which solves the problems of energy density improvement and bromine vapor escape, and achieves high energy density and improved stability.

CN122511944BActive Publication Date: 2026-11-10DALIAN RONGKE POWER
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202611002745.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-07-07
Publication Date
2026-11-10
Estimated Expiration
2046-07-07

AI Technical Summary

Technical Problem

The energy density of solid-phase energy storage materials in existing vanadium-bromine flow batteries has limited improvement, and bromine vapor can easily escape during charging, corroding battery components and affecting the long-term operational stability and safety of the battery.

Method used

A dual solid-phase energy storage mechanism is adopted, using Bi4[Fe(CN)6]3 as a solid-phase energy storage material. It combines with tetravalent vanadium ions and bromide ions in the positive electrode electrolyte to form a bromide-containing intercalated compound. During the charging and discharging process, the reversible conversion of ferrous and iron is achieved, capturing polybrominated ions and preventing their free diffusion in the electrolyte.

Benefits of technology

It significantly improves the energy density of the battery, suppresses the escape of bromine vapor, extends the battery's lifespan and operational stability, and reduces chemical corrosion of battery components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_9
    Figure SMS_9
  • Figure SMS_10
    Figure SMS_10
Patent Text Reader

Abstract

The application belongs to the field of liquid flow batteries, and particularly relates to a vanadium-bromine liquid flow battery based on a double solid-phase energy storage mechanism, which comprises a positive electrode, a positive electrolyte, an ion exchange membrane, a negative electrolyte, a negative electrode and a solid-phase energy storage material in contact with the positive electrolyte. The general formula of the solid-phase energy storage material is Bi4[Fe(CN)6]3. The positive electrolyte contains tetravalent vanadium ions and bromide ions, and the negative electrolyte contains trivalent vanadium ions. The application realizes the synergistic effect of iron / ferrous redox and bromine intercalation / deintercalation through the solid-phase energy storage material, forms a double solid-phase energy storage mechanism, can improve the energy density of the battery, effectively fixes polybromide ions, inhibits bromine escape, reduces corrosion on the battery components, and improves the safety and cycle stability of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of flow battery technology, and specifically to a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism. Background Technology

[0002] As the global energy structure accelerates its transformation towards cleaner and lower-carbon energy sources, large-scale electrochemical energy storage technology plays an increasingly crucial role in renewable energy grid integration, grid peak shaving and frequency regulation, and distributed energy systems. Flow batteries, due to their advantages such as power-capacity decoupling, high safety, and long cycle life, are considered one of the most promising large-scale energy storage solutions. Among them, vanadium redox flow batteries (VRFBs), which use vanadium ions as active materials in both the positive and negative electrodes, avoiding cross-contamination issues, have become the most commercially viable flow battery system. However, the energy density of traditional vanadium redox flow batteries is limited by the solubility of vanadium electrolyte in the electrolyte, and the high cost of vanadium resources restricts their further large-scale commercial application.

[0003] To overcome the aforementioned bottlenecks, existing technologies have begun to explore the introduction of solid-phase energy storage materials to construct solid-liquid composite energy storage systems, thereby improving energy density and reducing costs. For example, invention patent CN118645668A discloses a vanadium redox flow battery based on solid energy storage materials and its preparation method. This method involves introducing Prussian blue analogues, such as vanadium ferrocyanide particles or supported carbon felt, into the positive electrode electrolyte, and then assembling it with electrodes, a proton exchange membrane, etc., to form a battery. This approach not only significantly improves the battery's energy density and operating temperature range, overcoming the solubility limitations of vanadium electrolytes, but also effectively reduces the overall system cost thanks to the low-cost and high-efficiency preparation process of the materials, achieving a dual optimization of solid-phase material utilization and vanadium electrolyte efficiency.

[0004] Chinese patent application CN118299630B discloses a high-capacity vanadium redox flow battery positive electrode electrolyte, which includes a solid-phase energy storage material whose main component is ammonium-rich iron / copper ferrocyanide. This material reacts with VOCs in an ammonium-containing supporting electrolyte. 2+ / VO2 + With similar equilibrium potentials, reversible redox reactions can occur during charging and discharging, thereby extending the battery's charge and discharge time. This scheme utilizes low-cost solid-phase materials as auxiliary energy storage media, achieving higher capacity output while reducing pentavalent vanadium concentration. This not only helps improve the system's temperature adaptability but also further reduces electrolyte costs.

[0005] However, the existing technologies for introducing solid-phase energy storage materials still have significant drawbacks and cannot meet the needs of further development. First, their core energy storage mechanism relies on the valence state changes of single metal ions such as ferric and ferrous ions in the solid-phase material, which is a single targeted solid-phase energy storage pathway. This mechanism fails to fully utilize the energy storage potential of other active components in the electrolyte system, resulting in the intrinsic capacity of the solid-phase material not being fully released, and the increase in energy density has an upper limit.

[0006] Secondly, when applied to the more cost-effective vanadium-bromine redox flow battery system, the above single mechanism also has serious compatibility issues: due to the lack of effective fixation of polybromine ions by solid materials, the polybromine ions generated during charging are easily ionized in the electrolyte, which not only cannot contribute to the capacity, but are also more likely to overflow in the form of bromine vapor, and seriously corrode key components such as the graphite plate of the battery, thereby threatening the long-term operational stability and safety of the battery.

[0007] Therefore, there is a need for a vanadium-bromine flow battery that can further improve energy density while effectively suppressing the escape of bromine vapor during charging and its corrosion of battery components. Summary of the Invention

[0008] (a) Technical problems to be solved

[0009] In view of the above-mentioned technical problems, in order to solve the problems that the existing technology has limited ability to improve energy density through solid phase energy storage materials, and that bromine vapor is prone to escape and corrode battery components in vanadium bromine flow battery systems, the present invention provides a vanadium bromine flow battery based on a dual solid phase energy storage mechanism.

[0010] (II) Technical Solution

[0011] To achieve the above objectives, the main technical solutions adopted by the present invention include:

[0012] This invention provides a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism, comprising a positive electrode, a positive electrolyte, an ion exchange membrane, a negative electrolyte, and a negative electrode, and further comprising a solid-phase energy storage material in contact with the positive electrolyte;

[0013] The general formula for solid-phase energy storage materials is Bi4[Fe(CN)6]3;

[0014] The positive electrode electrolyte contains tetravalent vanadium ions and bromide ions, and the negative electrode electrolyte contains trivalent vanadium ions.

[0015] In the vanadium-bromine redox flow battery described above, preferably, the solid-phase energy storage material and the binder form a composite film, and the composite film is placed in the positive electrode electrolyte storage tank;

[0016] The binder is a perfluorosulfonic acid resin or a polyvinylidene fluoride resin, and the mass ratio of the solid-phase energy storage material to the binder is 1:5-1:29.

[0017] In the vanadium-bromine flow battery described above, preferably, the composite thin film is prepared by the following method:

[0018] Solid-phase energy storage material is mixed with a binder and then dissolved in a mixture of water and organic solvent. After ultrasonic treatment, a mixed solution is obtained. The mixed solution is then sprayed onto the substrate surface to obtain a composite film.

[0019] In the vanadium-bromine redox flow battery described above, preferably, the solid-phase energy storage material is prepared as follows:

[0020] S1: Dissolve ferrocyanide or ferricyanide in water to obtain a ferrocyanide solution or a ferricyanide solution;

[0021] S2: Obtain a salt solution by dissolving the inorganic salt of Bi in acid;

[0022] S3: Mix the salt solution with the ferrocyanide solution or the ferricyanide solution, stir and react, let stand for treatment, and then perform post-treatment to obtain the solid-phase energy storage material.

[0023] In the vanadium-bromine flow battery described above, preferably, when ferrocyanide is used in step S1, after the settling treatment in step S3, centrifugation, washing, and drying are performed to obtain a solid-phase energy storage material.

[0024] When ferricyanide is used in step S1, after settling in step S3, the solid is centrifuged and washed, then soaked and washed in a solution containing tetravalent vanadium. After the solution containing tetravalent vanadium turns blue, it is dried to obtain a solid-phase energy storage material.

[0025] In the vanadium-bromine flow battery described above, preferably, in step S1, the ferrocyanide is potassium ferrocyanide, sodium ferrocyanide, or ammonium ferrocyanide; and the ferricyanide is potassium ferricyanide, sodium ferricyanide, or ammonium ferricyanide.

[0026] The concentration of the ferrocyanide solution or ferricyanide solution is 0.1-2 mol / L.

[0027] In the vanadium-bromine flow battery described above, preferably, in step S2, the inorganic salt of Bi is dissolved by dilute sulfuric acid, dilute hydrochloric acid, or dilute hydrobromic acid.

[0028] The inorganic salts of Bi are Bi sulfates, chlorides, or bromides, and the concentration of the salt solution is 0.1-1 mol / L.

[0029] In the vanadium-bromine flow battery described above, preferably, in step S3, the reaction time is 20-40 min and the settling time is 12-24 h.

[0030] In the vanadium-bromine flow battery described above, preferably, the positive electrode includes a current collector and a porous electrode disposed on its surface, wherein the current collector is a graphite plate and the porous electrode is carbon cloth, carbon felt or graphite felt.

[0031] The ion exchange membrane is a proton exchange membrane;

[0032] In the positive electrode electrolyte, the concentration of tetravalent vanadium ions is 1.8-2.2 mol / L, and the concentration of bromide ions is 0.6-1.0 mol / L.

[0033] In the vanadium-bromine flow battery described above, preferably, the mass of solid-phase energy storage material corresponding to each milliliter of positive electrode electrolyte is 0.15-0.3g.

[0034] (III) Beneficial Effects

[0035] First, the solid-phase energy storage material of this invention not only achieves solid-phase energy storage through the reversible transformation between ferrous and iron during charging and discharging, but also creatively incorporates bromine into the solid-phase conversion process. This mechanism changes the traditional energy storage mode of vanadium ferrocyanide or vanadium ferrocyanide materials, which relies solely on a single-target redox reaction, forming a novel dual-target solid-phase energy storage pathway. Specifically, during charging, when ferrocyanide is oxidized to ferrocyanide, the polybromine ions generated in the positive electrode electrolyte can be simultaneously intercalated into the ferrocyanide lattice structure, forming a bromine-containing intercalation compound Bi4[Fe(CN)6]3[Br5]3. During discharging, the iron ions in the bromine-containing intercalation compound can synergistically work with the polybromine ions to continuously oxidize tetravalent vanadium to pentavalent vanadium, while reducing itself back to the ferrocyanide state, thus completing a reversible cycle of dual energy storage. In this invention, the dual-target solid-phase energy storage mechanism of the solid-phase energy storage material significantly improves energy storage capacity, breaks through the limitation of single redox reactions on capacity growth, and greatly improves the overall energy density of the battery.

[0036] Secondly, the solid-phase energy storage material of this invention possesses excellent polybrominated ion capture and stabilization capabilities. Polybrominated ions generated during the charging phase can be effectively stored within the solid-phase material, preventing their free diffusion and volatilization loss in the electrolyte, thereby fundamentally suppressing the escape of bromine vapor. Therefore, this invention not only improves the safety of battery operation but also significantly reduces chemical corrosion to other battery structures, extending battery life and operational stability. Detailed Implementation

[0037] To better explain and facilitate understanding of the present invention, the present invention will be described in detail below in conjunction with specific embodiments.

[0038] This invention provides a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism, comprising a positive electrode, a positive electrolyte, an ion exchange membrane, a negative electrolyte, a negative electrode, and a solid-phase energy storage material in contact with the positive electrolyte. The general formula of the solid-phase energy storage material is Bi₄[Fe(CN)₆]₃. The positive electrolyte contains tetravalent vanadium ions such as VO₄²⁻. 2+ And bromide ions, the negative electrode electrolyte contains trivalent vanadium ions such as VO₃. + .

[0039] The solid-phase energy storage material of this invention not only achieves solid-phase energy storage through the reversible transformation between ferrous and iron during charging and discharging, but also creatively incorporates bromine into the solid-phase conversion process. This mechanism changes the traditional energy storage mode of vanadium ferrocyanide or vanadium ferrocyanide materials, which rely solely on single-target redox reactions, forming a novel dual-target solid-phase energy storage pathway. Specifically, during charging, when ferrocyanide is oxidized to ferrocyanide, polybromine ions generated in the positive electrode electrolyte can be simultaneously intercalated into the ferrocyanide lattice structure, forming a bromine-containing intercalation compound Bi4[Fe(CN)6]3[Br5]3. During discharging, the iron ions in the bromine-containing intercalation compound can synergistically work with the polybromine ions to continuously oxidize tetravalent vanadium to pentavalent vanadium, while reducing itself back to the ferrocyanide state, thus completing a reversible cycle of dual energy storage. In this invention, the dual-target solid-phase energy storage mechanism of the solid-phase energy storage material significantly improves energy storage capacity, breaks through the limitation of single redox reactions on capacity growth, and greatly improves the overall energy density of the battery.

[0040] The solid-phase energy storage material of this invention possesses excellent polybrominated ion capture and stabilization capabilities. Polybrominated ions generated during the charging phase can be effectively stored within the solid-phase material, preventing their free diffusion and volatilization loss in the electrolyte, thereby fundamentally suppressing the escape of bromine vapor. Therefore, this invention not only improves the safety of battery operation but also significantly reduces chemical corrosion to other battery structures, extending battery life and operational stability.

[0041] In this invention, the chemical changes during the charging process on the positive electrode side are as follows:

[0042] ;

[0043] ;

[0044] ;

[0045] ;

[0046] ;

[0047] The chemical changes during the discharge process on the positive electrode side are as follows:

[0048] ;

[0049] ;

[0050] .

[0051] If bismuth is replaced with chromium, the dual solid-state energy storage mechanism is lost.

[0052] Preferably, the solid-phase energy storage material can form a composite film with a binder, which can be placed in the positive electrode electrolyte storage tank to achieve stable interfacial contact and efficient charge transfer. By uniformly dispersing the solid-phase energy storage material in the binder matrix and forming a film, it is possible to effectively prevent material detachment or agglomeration, thereby improving its structural integrity during long-term cycling.

[0053] Preferably, the binder can be perfluorosulfonic acid resin or polyvinylidene fluoride resin. Perfluorosulfonic acid resin and / or polyvinylidene fluoride have excellent proton conductivity, chemical stability, and film-forming properties, and can maintain functional stability for a long time in an acidic electrolyte environment. They can also promote the rapid migration of hydrogen ions at the reaction interface. The mass ratio of solid-phase energy storage material to binder can be 1:5 to 1:29. Within this range, sufficient active material loading can be ensured to contribute to the capacity, while maintaining good mechanical strength and conductive network connectivity.

[0054] More preferably, the preparation method of the above-mentioned composite film is as follows: A solid-phase energy storage material is mixed with a binder, then dissolved in a mixed solvent of water and an organic solvent. After ultrasonic treatment, a mixed solution is obtained. The mixed solution is sprayed onto the surface of a substrate, such as a glass plate. After separation from the substrate, a composite film with a thickness of 20-50 μm is obtained. The organic solvent can be selected from isopropanol, ethanol, etc., which helps to improve the dispersion uniformity. The volume ratio of water to organic solvent can be 1:1.

[0055] Preferably, the preparation method of solid-phase energy storage material is as follows:

[0056] S1: Dissolve ferrocyanide or ferricyanide in water to obtain a ferrocyanide solution or ferricyanide solution with a concentration of 0.1-2 mol / L. The ferrocyanide used can be selected from potassium ferrocyanide, sodium ferrocyanide or ammonium ferrocyanide, and the ferricyanide can be selected from potassium ferricyanide, sodium ferricyanide or ammonium ferricyanide.

[0057] S2: Dissolve the inorganic salt of Bi in dilute sulfuric acid, dilute hydrochloric acid, or dilute hydrobromic acid to obtain a salt solution with a concentration of 0.1-1 mol / L. The inorganic salt of Bi is its sulfate, chloride, or bromide, such as bismuth nitrate or bismuth chloride.

[0058] S3: Mix the salt solution with the ferrocyanide solution or the ferrocyanide solution, stir vigorously for 20-40 minutes, let stand for 12-24 hours to achieve aging, and then perform post-processing to obtain the solid-phase energy storage material.

[0059] More preferably, in step S3, a salt solution is added in excess of the reactants.

[0060] The post-processing method in step S3 varies depending on the precursor:

[0061] When ferrocyanide is used in step S1, step S3 involves centrifugation, washing, and drying after settling to obtain a solid-phase energy storage material. When ferrocyanide is used in step S1, because free ferricyanide ions may be present in the product, step S3 involves centrifugation and washing after settling, followed by soaking and washing the solid in a solution containing tetravalent vanadium. After the solution turns blue, drying is performed to obtain the solid-phase energy storage material. 2+ It will react with residual [Fe(CN)6] 3- The reaction produces a blue Prussian blue precipitate. When the washing solution no longer turns blue, it indicates that the impurities have been basically removed. After drying, a high-purity product can be obtained.

[0062] Preferably, the positive electrode of the present invention includes a current collector and a porous electrode disposed on its surface, wherein the current collector may be a hard graphite plate and the porous electrode may be carbon cloth, carbon felt or graphite felt.

[0063] Ion exchange membranes are proton exchange membranes, such as the Nafion series membranes, for example, Nafion 212. They possess high proton selective permeability and good chemical stability, effectively blocking cross-contamination of vanadium species between the positive and negative electrodes, while allowing H2O to pass through. + Rapid migration to maintain charge balance.

[0064] In the above positive electrode electrolyte, the concentration of tetravalent vanadium ions is 1.8-2.2 mol / L, and the concentration of bromide ions is 0.6-1.0 mol / L.

[0065] More preferably, the mass of solid-phase energy storage material corresponding to each milliliter of positive electrode electrolyte is 0.15-0.3g.

[0066] To further clarify the present invention and its technological advancements, the following description is provided in conjunction with specific embodiments and technical effects.

[0067] Example 1:

[0068] This embodiment provides a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism, including a positive electrode, a positive electrolyte, an ion exchange membrane, a negative electrolyte, a negative electrode, and a solid-phase energy storage material in contact with the positive electrolyte.

[0069] This embodiment constructs and tests a vanadium-bromine flow battery as follows:

[0070] The solid-phase energy storage material in this embodiment has the general formula Bi4[Fe(CN)6]3. The preparation method of Bi4[Fe(CN)6]3 is as follows: Potassium ferrocyanide K4[Fe(CN)6] is added to deionized water and stirred to dissolve, resulting in a 0.1 mol / L potassium ferrocyanide solution. Bismuth chloride is then added to deionized water, and the pH is adjusted using 0.5 mol / L hydrochloric acid to obtain a 0.1 mol / L acidic bismuth chloride solution. Under continuous vigorous stirring, an acidic bismuth chloride solution was slowly poured into a potassium ferrocyanide solution at a volume ratio of 400:300. The reaction was maintained with stirring for 30 min, followed by standing and aging for 12 h. Then, the mixture was centrifuged at 8000 rpm for 10 min. The obtained solid was washed three times with deionized water and anhydrous ethanol. The obtained solid was then dried in a vacuum drying oven at 60 °C for 12 h to obtain a black powdery solid-phase energy storage material Bi4[Fe(CN)6]3.

[0071] Weigh out the Bi4[Fe(CN)6]3 powder prepared above and mix it with perfluorosulfonic acid resin at a mass ratio of 1:5. Add a mixed solvent composed of deionized water and isopropanol at a volume ratio of 1:1. Sonicate for 60 min to obtain a mixed solution. Spray the mixed solution onto the surface of a substrate, such as a glass plate. After separating it from the substrate, a composite film with a thickness of 30 μm is obtained. Place it in a positive electrode electrolyte storage tank.

[0072] A porous positive electrode is constructed using hard graphite plates as both positive and negative current collectors. This porous positive electrode is placed inside the positive current collector, and a Nafion 212 ion exchange membrane is used. The positive electrolyte contains 2.0 mol / L tetravalent vanadium ions (VO₄²⁻). 2+ The negative electrode electrolyte contains 0.8 mol / L bromide ions and 15 g Bi4[Fe(CN)6]3, and trivalent vanadium ions (VO3) in the electrolyte. + Assemble the above components to form an effective area of ​​48 cm². 2 The initial setup for the single-cell flow battery is a positive electrode electrolyte volume of 70 mL and a negative electrode electrolyte volume of 110 mL, thus obtaining the vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism in this embodiment.

[0073] Example 2:

[0074] This embodiment provides a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism. The difference from Embodiment 1 is that, in the preparation process of the composite thin film, the mass ratio of Bi4[Fe(CN)6]3 powder to perfluorosulfonic acid resin is 1:9.

[0075] In this embodiment, a hard graphite plate is used as the current collector for both the positive and negative electrodes. The positive electrode electrolyte contains 1.8 mol / L tetravalent vanadium ions (VO₄²⁻). 2+ 0.6 mol / L of bromide ions and 10.5 g of Bi4[Fe(CN)6]3.

[0076] Example 3:

[0077] This embodiment provides a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism. The difference from Embodiment 1 is that, in the preparation process of the composite thin film, the mass ratio of Bi4[Fe(CN)6]3 powder to perfluorosulfonic acid resin is 1:14.

[0078] In this embodiment, a hard graphite plate is used as the current collector for both the positive and negative electrodes. The positive electrode electrolyte contains 2.2 mol / L tetravalent vanadium ions (VO₄²⁻). 2+ 1 mol / L of bromide ions and 21 g of Bi4[Fe(CN)6]3.

[0079] Example 4:

[0080] This embodiment provides a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism. The difference from Embodiment 1 is that, in the preparation process of the composite thin film, the mass ratio of Bi4[Fe(CN)6]3 powder to perfluorosulfonic acid resin is 1:19.

[0081] Example 5:

[0082] This embodiment provides a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism. The difference from Embodiment 1 is that, in the preparation process of the composite thin film, the mass ratio of Bi4[Fe(CN)6]3 powder to perfluorosulfonic acid resin is 1:29.

[0083] Example 6:

[0084] This embodiment provides a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism. The difference from Embodiment 1 lies in the preparation method of Bi₄[Fe(CN)₆]₃: Potassium ferrocyanide K₄[Fe(CN)₆] is added to deionized water and stirred to dissolve, resulting in a 0.2 mol / L potassium ferrocyanide solution. BiCl₃ is then added to deionized water, and the pH is adjusted using 0.5 mol / L hydrochloric acid to obtain a 0.4 mol / L acidic bismuth chloride solution. Under continuous vigorous stirring, an acidic bismuth chloride solution was slowly poured into a potassium ferrocyanide solution at a volume ratio of 100:150. The mixture was stirred for 20 minutes, then allowed to stand for 24 hours. The mixture was then centrifuged at 8000 rpm for 10 minutes. The resulting solid was washed three times with deionized water and anhydrous ethanol. The solid was then dried in a vacuum drying oven at 60°C for 12 hours to obtain a black powdery solid-phase energy storage material Bi4[Fe(CN)6]3.

[0085] In addition, in this embodiment, the binder used in the composite film is PVDF, and the mass ratio of Bi4[Fe(CN)6]3 powder to PVDF is 1:9 during the preparation of the composite film.

[0086] Example 7:

[0087] This embodiment provides a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism. The difference from Embodiment 1 lies in the preparation method of Bi₄[Fe(CN)₆]₃: Potassium ferrocyanide K₄[Fe(CN)₆] is added to deionized water and stirred to dissolve, resulting in a 0.5 mol / L potassium ferrocyanide solution. BiCl₃ is then added to deionized water, and the pH is adjusted using 0.5 mol / L hydrochloric acid to obtain a 0.5 mol / L acidic bismuth chloride solution. Under continuous vigorous stirring, an acidic bismuth chloride solution was slowly poured into a potassium ferrocyanide solution at a volume ratio of 160:60. The reaction was maintained with stirring for 40 min, followed by standing and aging for 18 h. Then, the mixture was centrifuged at 8000 rpm for 10 min. The obtained solid was washed three times with deionized water and anhydrous ethanol. The obtained solid was then dried in a vacuum drying oven at 60 °C for 12 h to obtain a black powdery solid-phase energy storage material Bi4[Fe(CN)6]3.

[0088] In addition, in this embodiment, during the preparation of the composite film, the mass ratio of Bi4[Fe(CN)6]3 powder to perfluorosulfonic acid resin is 1:9.

[0089] Example 8:

[0090] This embodiment provides a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism. The difference from Embodiment 1 lies in the preparation method of Bi₄[Fe(CN)₆]₃: Potassium ferrocyanide K₄[Fe(CN)₆] is added to deionized water and stirred to dissolve, resulting in a 1 mol / L potassium ferrocyanide solution. BiCl₃ is then added to deionized water, and the pH is adjusted using 0.5 mol / L hydrochloric acid to obtain a 1 mol / L acidic bismuth chloride solution. Under continuous vigorous stirring, an acidic bismuth chloride solution was slowly poured into a potassium ferrocyanide solution at a volume ratio of 80:30. The reaction was maintained with stirring for 30 min, followed by standing and aging for 12 h. Then, the mixture was centrifuged at 8000 rpm for 10 min. The obtained solid was washed three times with deionized water and anhydrous ethanol. The obtained solid was then dried in a vacuum drying oven at 60 °C for 12 h to obtain a black powdery solid-phase energy storage material Bi4[Fe(CN)6]3.

[0091] In addition, in this embodiment, during the preparation of the composite film, the mass ratio of Bi4[Fe(CN)6]3 powder to perfluorosulfonic acid resin is 1:9.

[0092] Example 9:

[0093] This embodiment provides a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism. The difference from Embodiment 1 lies in the preparation method of Bi₄[Fe(CN)₆]₃: Potassium ferrocyanide K₄[Fe(CN)₆]₆ is added to deionized water and stirred to dissolve, resulting in a 2 mol / L potassium ferrocyanide solution. BiCl₃ is then added to the deionized water, and the pH is adjusted using 0.5 mol / L hydrochloric acid to obtain a 1 mol / L acidic bismuth chloride solution. Under continuous vigorous stirring, an acidic bismuth chloride solution was slowly poured into a potassium ferrocyanide solution at a volume ratio of 40:15. The reaction was maintained with stirring for 30 min, followed by standing and aging for 12 h. Then, the mixture was centrifuged at 8000 rpm for 10 min. The obtained solid was washed three times with deionized water and anhydrous ethanol. The obtained solid was then dried in a vacuum drying oven at 60 °C for 12 h to obtain a black powdery solid-phase energy storage material Bi4[Fe(CN)6]3.

[0094] In addition, in this embodiment, during the preparation of the composite film, the mass ratio of Bi4[Fe(CN)6]3 powder to perfluorosulfonic acid resin is 1:9.

[0095] Example 10:

[0096] This embodiment provides a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism. The difference from Embodiment 1 lies in the preparation method of Bi4[Fe(CN)6]3: Sodium ferrocyanide is added to deionized water and stirred until dissolved to obtain a 0.5 mol / L sodium ferrocyanide solution. Bismuth sulfate is added to deionized water, and the pH is adjusted with 0.5 mol / L sulfuric acid to obtain a 0.25 mol / L bismuth sulfate acidic solution. Under continuous vigorous stirring, the bismuth sulfate acidic solution is slowly poured into the sodium ferrocyanide solution at a volume ratio of 160:60. The reaction is maintained with stirring for 30 min, followed by standing and aging for 12 h. The mixture is then centrifuged at 8000 rpm for 10 min. The resulting solid is washed three times with deionized water and anhydrous ethanol, and then dried in a 60℃ vacuum drying oven for 12 h to obtain a black powdery solid-phase energy storage material, Bi4[Fe(CN)6]3.

[0097] In addition, in this embodiment, during the preparation of the composite film, the mass ratio of Bi4[Fe(CN)6]3 powder to perfluorosulfonic acid resin is 1:9.

[0098] Example 11:

[0099] This embodiment provides a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism. The difference from Embodiment 1 lies in the preparation method of Bi₄[Fe(CN)₆]₃: Ammonium ferrocyanide is added to deionized water and stirred to dissolve, resulting in a 0.5 mol / L ammonium ferrocyanide solution. Bismuth bromide is then added to deionized water, and the pH is adjusted using 0.5 mol / L hydrobromic acid to obtain a 0.25 mol / L acidic bismuth bromide solution. Under continuous vigorous stirring, an acidic bismuth bromide solution was slowly poured into an ammonium ferrocyanide solution at a volume ratio of 160:60. The reaction was maintained with stirring for 30 min, followed by standing and aging for 12 h. Then, the mixture was centrifuged at 8000 rpm for 10 min. The obtained solid was washed three times with deionized water and anhydrous ethanol. The obtained solid was then dried in a vacuum drying oven at 60 °C for 12 h to obtain a black powdery solid-phase energy storage material Bi4[Fe(CN)6]3.

[0100] In addition, in this embodiment, during the preparation of the composite film, the mass ratio of Bi4[Fe(CN)6]3 powder to perfluorosulfonic acid resin is 1:9.

[0101] Example 12:

[0102] This embodiment provides a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism. The difference from Embodiment 1 lies in the preparation method of Bi₄[Fe(CN)₆]₃: potassium ferricyanide is added to deionized water and stirred until dissolved to obtain a 2 mol / L potassium ferricyanide solution. BiCl₃ is then added to deionized water, and the pH is adjusted using 0.5 mol / L hydrochloric acid to obtain a 1 mol / L acidic bismuth chloride solution. Under continuous vigorous stirring, an acidic bismuth chloride solution was slowly poured into a potassium ferricyanide solution at a volume ratio of 40:15. The reaction was maintained with stirring for 30 minutes, followed by standing and aging for 12 hours. Then, the mixture was centrifuged at 8000 rpm for 10 minutes. The obtained solid was washed three times with deionized water and anhydrous ethanol, and then soaked in a sufficient amount of vanadium oxysulfate solution and washed again until the color of the vanadium oxysulfate solution showed no significant difference before and after washing. The obtained solid was then dried in a vacuum drying oven at 60°C for 12 hours to obtain a black powdery solid-phase energy storage material Bi4[Fe(CN)6]3.

[0103] In addition, in this embodiment, during the preparation of the composite film, the mass ratio of Bi4[Fe(CN)6]3 powder to perfluorosulfonic acid resin is 1:9.

[0104] Example 13:

[0105] This embodiment provides a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism. The difference from Embodiment 1 is that the preparation method of Bi₄[Fe(CN)₆]₃ is as follows: Sodium ferricyanide is added to deionized water and stirred to dissolve, resulting in a sodium ferricyanide solution with a concentration of 2 mol / L. BiCl₃ is then added to deionized water, and the pH is adjusted using 0.5 mol / L sulfuric acid to obtain an acidic bismuth chloride solution with a concentration of 1 mol / L. Under continuous vigorous stirring, an acidic bismuth chloride solution was slowly poured into a sodium ferricyanide solution at a volume ratio of 160:60. The mixture was stirred for 30 minutes, then allowed to stand for 12 hours. The mixture was then centrifuged at 8000 rpm for 10 minutes. The resulting solid was washed three times with deionized water and anhydrous ethanol, and then soaked in a sufficient amount of vanadium oxysulfate solution and washed again until the color of the vanadium oxysulfate solution showed no significant difference before and after washing. The resulting solid was then dried in a vacuum drying oven at 60°C for 12 hours to obtain a black powdery solid-phase energy storage material Bi4[Fe(CN)6]3.

[0106] In addition, in this embodiment, during the preparation of the composite film, the mass ratio of Bi4[Fe(CN)6]3 powder to perfluorosulfonic acid resin is 1:9.

[0107] Example 14:

[0108] This embodiment provides a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism. The difference from Embodiment 1 lies in the preparation method of Bi₄[Fe(CN)₆]₃: Ammonium ferricyanide is added to deionized water and stirred to dissolve, resulting in a 0.5 mol / L ammonium ferricyanide solution. Bismuth bromide is then added to deionized water, and the pH is adjusted using 0.5 mol / L hydrobromic acid to obtain a 0.25 mol / L acidic bismuth bromide solution. Under continuous vigorous stirring, an acidic bismuth bromide solution was slowly poured into an ammonium ferricyanide solution at a volume ratio of 160:60. The reaction was maintained with stirring for 30 minutes, followed by standing and aging for 12 hours. Then, the mixture was centrifuged at 8000 rpm for 10 minutes. The obtained solid was washed three times with deionized water and anhydrous ethanol, and then soaked in a sufficient amount of vanadium oxyhydrobromide solution and washed again until the color of the vanadium oxyhydrobromide solution showed no significant difference before and after washing. The obtained solid was then dried in a vacuum drying oven at 60°C for 12 hours to obtain a black powdery solid-phase energy storage material Bi4[Fe(CN)6]3.

[0109] In addition, in this embodiment, during the preparation of the composite film, the mass ratio of Bi4[Fe(CN)6]3 powder to perfluorosulfonic acid resin is 1:9.

[0110] Comparative Example 1:

[0111] This comparative example provides a vanadium-bromine flow battery based on a solid-phase energy storage mechanism. The difference from Example 1 is that the solid-phase energy storage material is Cr4[Fe(CN)6]3. The preparation method of Cr4[Fe(CN)6]3 is as follows: Potassium ferrocyanide is added to deionized water and stirred to dissolve, resulting in a 0.1 mol / L potassium ferrocyanide solution. Chromium chloride is then added to deionized water, and the pH is adjusted using 0.5 mol / L hydrochloric acid to obtain a 0.1 mol / L acidic chromium chloride solution. Under continuous vigorous stirring, an acidic chromium chloride solution was slowly poured into a potassium ferrocyanide solution at a volume ratio of 300:150. The mixture was stirred for 30 minutes, then allowed to stand for 12 hours. The mixture was then centrifuged at 8000 rpm for 10 minutes. The resulting solid was washed three times with deionized water and anhydrous ethanol. The solid was then dried in a vacuum drying oven at 60°C for 12 hours to obtain a black powdery solid-phase energy storage material Cr4[Fe(CN)6]3.

[0112] In addition, in this comparative example, the mass ratio of Cr4[Fe(CN)6]3 powder to perfluorosulfonic acid resin was 1:9 during the preparation of the composite film.

[0113] Comparative Example 2:

[0114] This comparative example provides a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism. The difference from Example 1 is that the solid-phase energy storage material is Cr4[Fe(CN)6]3. The preparation method of Cr4[Fe(CN)6]3 is as follows: Potassium ferrocyanide is added to deionized water and stirred to dissolve, resulting in a 0.5 mol / L potassium ferrocyanide solution. Chromium sulfate is then added to deionized water, and the pH is adjusted using 0.5 mol / L sulfuric acid to obtain a 0.25 mol / L acidic chromium sulfate solution. Under continuous vigorous stirring, a chromium sulfate acidic solution was slowly poured into a potassium ferrocyanide solution at a volume ratio of 160:60. The reaction was maintained with stirring for 30 min, followed by standing and aging for 12 h. Then, the mixture was centrifuged at 8000 rpm for 10 min. The obtained solid was washed three times with deionized water and anhydrous ethanol. The obtained solid was then dried in a vacuum drying oven at 60 °C for 12 h to obtain a black powdery solid-phase energy storage material Cr4[Fe(CN)6]3.

[0115] In addition, in this comparative example, the mass ratio of Cr4[Fe(CN)6]3 powder to perfluorosulfonic acid resin was 1:9 during the preparation of the composite film.

[0116] Comparative Example 3:

[0117] This comparative example provides a vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism. The difference from Example 1 is that the solid-phase energy storage material is Cr4[Fe(CN)6]3. The preparation method of Cr4[Fe(CN)6]3 is as follows: Potassium ferrocyanide is added to deionized water and stirred to dissolve, resulting in a 0.5 mol / L potassium ferrocyanide solution. Chromium bromide is then added to deionized water, and the pH is adjusted using 0.5 mol / L hydrobromic acid to obtain a 0.25 mol / L chromium bromide acidic solution. Under continuous vigorous stirring, an acidic solution of chromium bromide was slowly poured into a potassium ferrocyanide solution at a volume ratio of 160:60. The mixture was stirred for 30 minutes, then allowed to stand for 12 hours. The mixture was then centrifuged at 8000 rpm for 10 minutes. The resulting solid was washed three times with deionized water and anhydrous ethanol. The solid was then dried in a vacuum drying oven at 60°C for 12 hours to obtain a black powdery solid-phase energy storage material Cr4[Fe(CN)6]3.

[0118] In addition, in this comparative example, the mass ratio of Cr4[Fe(CN)6]3 powder to perfluorosulfonic acid resin was 1:9 during the preparation of the composite film.

[0119] Comparative Example 4:

[0120] This comparative example provides a vanadium-bromine flow battery, which differs from Example 1 in that the vanadium-bromine flow battery is constructed and tested in the following manner:

[0121] Potassium ferrocyanide was completely dissolved in deionized water to obtain a 0.1 M potassium ferrocyanide solution. Vanadium oxysulfate was dissolved in 0.5 M hydrochloric acid to obtain a 0.1 M vanadium oxysulfate solution. The vanadium oxysulfate solution was poured into the potassium ferrocyanide solution under rapid stirring, and the stirring was maintained for 30 min. After standing for 12 h for aging, the powder was centrifuged, washed, and vacuum dried at 60 °C to obtain VO6[Fe(CN)6]3 solid-phase energy storage material.

[0122] VO6[Fe(CN)6]3 and perfluorosulfonic acid resin were mixed and dispersed in a 1:9 mass ratio in a 1:1 volume mixture of water and isopropanol, and the mixture was thoroughly ultrasonicated to homogenize it. The mixture was then sprayed onto the surface of a glass plate using a spraying machine to prepare a composite film.

[0123] Hard graphite plates were used as current collectors for both the positive and negative electrodes. A composite membrane was placed in the positive electrode electrolyte storage tank, and Nafion 212 was used as the ion exchange membrane. The positive electrode electrolyte contained 2.0 mol / L tetravalent vanadium ions (VO₄²⁻). 2+ The negative electrode electrolyte contains 0.8 mol / L bromide ions and 15 g VO₆[Fe(CN)₆]₃, and trivalent vanadium ions VO₆. + Assemble the above components to form an effective area of ​​48 cm². 2 The initial setup for the single-cell flow battery was a positive electrode electrolyte volume of 70 mL and a negative electrode electrolyte volume of 110 mL, thus obtaining the vanadium-bromine flow battery of this comparative example.

[0124] Using 100mA / cm 2 The batteries prepared in Examples 1-14 and Comparative Examples 1-4 were subjected to charge-discharge cycle tests at a constant current density to observe the capacity increase of the batteries and the corrosion status of the graphite plate on the positive electrode side. Tables 1 and 2 were obtained.

[0125] Table 1. Battery performance statistics for Examples 1-14

[0126] Table 2. Battery performance statistics for Comparative Examples 1-4

[0127] A comparison of the results in Tables 1 and 2 for Examples 1-5 shows that none of the examples using Bi4[Fe(CN)6]3 exhibited severe corrosion phenomena such as graphite plate pulverization and detachment, and the capacity increase was significantly higher than that of Comparative Examples 1-4. This indicates that the solid-phase energy storage material of the present invention can effectively exert a dual solid-phase energy storage mechanism under different ratios, solving the problems of polybrominated ion escape and module corrosion. Among them, the membrane powder prepared by mixing Bi4[Fe(CN)6]3 with perfluorosulfonic acid / PVDF resin at a mass ratio of 1:9 has the best utilization rate, with no battery blockage, no bromine vapor escape, no graphite plate corrosion, and the largest capacity increase. Example 1, with a lower solid-phase material ratio, still suppressed bromine escape and corrosion, with only slight blockage. Examples 3-5, with a higher binder ratio, showed a capacity increase close to that of Example 2. Although slight bromine vapor and color changes on the graphite plate surface were observed, their degree was much less than that of the comparative examples, still achieving effective fixation of polybrominated ions and protection of the battery module. Statistical results from Examples 2 and Comparative Examples 1-4 show that batteries using Cr4[Fe(CN)6]3 or VO6[Fe(CN)6]3 exhibited severe bromine vapor overflow and graphite plate pulverization and detachment, with relatively low capacity increases. This demonstrates that chromium-based and vanadium-based Prussian blue analogues cannot intercalate and stabilize polybromine ions, and therefore lack dual solid-phase energy storage capabilities. In contrast, the unique structure of Bi4[Fe(CN)6]3 enables synergistic energy storage through iron / ferrous redox reactions and bromine intercalation / deintercalation, thus exhibiting significant advantages in capacity, safety, and stability.

[0128] The experimental results of Examples 2 and 6-9 show that the performance of Bi4[Fe(CN)6]3 synthesized under different precursor solution concentrations fluctuates slightly, but all exhibit excellent dual solid-phase energy storage performance, with no significant bromine vapor overflow or graphite plate pulverization.

[0129] The experimental results of Examples 10-14 show that Bi4[Fe(CN)6]3 prepared by using different bismuth salts, acids and ferrocyanide / ferrocyanide raw materials and adjusting the corresponding valence states exhibit similar performance in energy storage and inhibition of bromine corrosion. This indicates that the preparation method of the present invention has good applicability to various related reagents and derivatives, and the products all have dual solid-phase energy storage characteristics.

[0130] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A vanadium-bromine flow battery based on a dual solid-phase energy storage mechanism, comprising a positive electrode, a positive electrolyte, an ion exchange membrane, a negative electrolyte, and a negative electrode, characterized in that, It also includes solid-phase energy storage materials that come into contact with the positive electrode electrolyte; The general formula for solid-phase energy storage materials is Bi4[Fe(CN)6]3; The positive electrode electrolyte contains tetravalent vanadium ions and bromide ions, and the negative electrode electrolyte contains trivalent vanadium ions.

2. The vanadium-bromine redox flow battery according to claim 1, characterized in that, The solid-phase energy storage material and the binder form a composite film, and the composite film is placed in the positive electrode electrolyte storage tank; The binder is a perfluorosulfonic acid resin or a polyvinylidene fluoride resin, and the mass ratio of the solid-phase energy storage material to the binder is 1:5-1:

29.

3. The vanadium-bromine redox flow battery according to claim 2, characterized in that, The method for preparing the composite film is as follows: Solid-phase energy storage material is mixed with a binder and then dissolved in a mixture of water and organic solvent. After ultrasonic treatment, a mixed solution is obtained. The mixed solution is then sprayed onto the substrate surface to obtain a composite film.

4. The vanadium-bromine redox flow battery according to claim 1, characterized in that, The preparation methods for solid-phase energy storage materials are as follows: S1: Dissolve ferrocyanide or ferricyanide in water to obtain a ferrocyanide solution or a ferricyanide solution; S2: Obtain a salt solution by dissolving the inorganic salt of Bi in acid; S3: Mix the salt solution with the ferrocyanide solution or the ferricyanide solution, stir and react, let stand for treatment, and then perform post-treatment to obtain the solid-phase energy storage material.

5. The vanadium-bromine redox flow battery according to claim 4, characterized in that, When ferrocyanide is used in step S1, after settling in step S3, centrifugation, washing, and drying are performed to obtain solid-phase energy storage material. When ferricyanide is used in step S1, after settling in step S3, the solid is centrifuged and washed, then soaked and washed in a solution containing tetravalent vanadium. After the solution containing tetravalent vanadium turns blue, it is dried to obtain a solid-phase energy storage material.

6. The vanadium-bromine redox flow battery according to claim 4, characterized in that, In step S1, the ferrocyanide is potassium ferrocyanide, sodium ferrocyanide, or ammonium ferrocyanide; the ferricyanide is potassium ferricyanide, sodium ferricyanide, or ammonium ferricyanide. The concentration of the ferrocyanide solution or ferricyanide solution is 0.1-2 mol / L.

7. The vanadium-bromine redox flow battery according to claim 4, characterized in that, In step S2, the inorganic salts of Bi are dissolved using dilute sulfuric acid, dilute hydrochloric acid, or dilute hydrobromic acid. The inorganic salts of Bi are Bi sulfates, chlorides, or bromides, and the concentration of the salt solution is 0.1-1 mol / L.

8. The vanadium-bromine redox flow battery according to claim 4, characterized in that, In step S3, the reaction time is 20-40 min and the standing time is 12-24 h.

9. The vanadium-bromine redox flow battery according to claim 2, characterized in that, The positive electrode includes a current collector and a porous electrode disposed on its surface. The current collector is a graphite plate, and the porous electrode is carbon cloth, carbon felt, or graphite felt. The ion exchange membrane is a proton exchange membrane; In the positive electrode electrolyte, the concentration of tetravalent vanadium ions is 1.8-2.2 mol / L, and the concentration of bromide ions is 0.6-1.0 mol / L.

10. The vanadium-bromine redox flow battery according to claim 1, characterized in that, The mass of solid-phase energy storage material corresponding to each milliliter of positive electrode electrolyte is 0.15-0.3g.

Citation Information

Patent Citations

  • A high-capacity cathode electrolyte for all-vanadium redox flow batteries

    CN118299630B

  • Vanadium redox flow battery based on solid energy storage material and preparation method of vanadium redox flow battery

    CN118645668A

  • Double-function negative electrode and applications of double-function negative electrode as all-vanadium flow battery negative electrode

    CN104518221A

  • Electrochemical storage devices comprising chelated metals

    CN113853523A