A smoke rod base BCDs / in2se3 / wO 3-x Ternary composite photothermal catalytic material, preparation method and application thereof

CN122644090APending Publication Date: 2026-08-28KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610669494.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-05-15
Publication Date
2026-08-28

AI Technical Summary

Technical Problem

[0007]针对现有技术的不足,本发明的目的在于提供一种烟杆基BCDs/In2Se3/WO3-x三元复合光热催化材料及其制备方法,以解决现有In2Se3基光催化材料电荷分离效率低、氧化能力不足以及光热效应利用不充分的问题,并提供其在有机污染物,尤其是四环素类抗生素降解中的应用

Benefits of technology

(1)本发明通过将In2Se3、WO3-x和烟杆基BCDs进行三元复合,构建出界面耦合紧密的异质结体系,达到了促进光生载流子的分离与迁移、提高复合材料光热响应能力的效果;本发明采用废弃烟杆为碳源制备BCDs,在实现生物质废弃物资源化利用的同时,制得可作为界面电子调控组分和光热响应组分参与三元复合体系构筑的烟杆基BCDs;进一步地,利用WO3-x的氧空位缺陷结构和烟杆基BCDs良好的光吸收与非辐射弛豫能力,与In2Se3协同,使复合材料具有较强的光热响应能力。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122644090A_ABST
    Figure CN122644090A_ABST
Patent Text Reader

Abstract

This invention discloses a tobacco rod-based BCDs / In2Se3 / WO 3‑x This paper describes ternary composite photothermal catalytic materials, their preparation methods, and applications, belonging to the fields of photocatalytic materials and water pollution control technology. The method includes: firstly, cleaning, drying, and crushing waste tobacco stalks, followed by carbonization under an inert atmosphere; then, oxidizing with ammonia / peroxide, filtering, dialysis, and freeze-drying to obtain tobacco stalk-based BCDs; next, preparing WO3 using tungstate as a raw material, and constructing oxygen-rich vacancy WO3 using a microwave method. 3‑x Finally, the base BCDs and WO of the cigarette rod are added. 3‑x Microwave-assisted solvothermal composite with the In2Se3 precursor system yielded tobacco stalk-based BCDs / In2Se3 / WO 3‑x Ternary composite photothermal catalytic material. This material contains In₂Se₃ and WO₃. 3‑x By forming a tight heterogeneous interface, BCDs are distributed on the surface and / or interface of the composite system, enabling double Z-type charge transfer and enhancing photothermal conversion capabilities. This material can be used for the degradation of organic pollutants, especially tetracycline antibiotics, and has the advantages of a wide light absorption range, high charge separation efficiency, good photothermal synergy, and good stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of photocatalytic materials and water pollution control technology, and relates to a tobacco stalk-based BCDs / In2Se3 / WO 3-x Ternary composite photothermal catalytic materials, their preparation methods and their applications in the degradation of organic pollutants. Background Technology

[0002] With the widespread use of antibiotics in the pharmaceutical, aquaculture, and related industrial fields, their residues are constantly entering the aquatic environment, becoming a significant emerging pollutant. Tetracycline antibiotics, in particular, have attracted widespread attention due to their stable chemical structure, difficulty in degradation in the natural environment, and potential risk of spreading drug resistance. Oxytetracycline, as one of the common tetracycline antibiotics, has a certain detection rate in water bodies, making the development of efficient and green removal methods crucial. Photocatalysis technology, which utilizes solar energy to drive reactions, offers advantages such as mild reaction conditions and minimal secondary pollution, showing promising application prospects in antibiotic wastewater treatment. However, during photocatalysis, some light energy is often dissipated as heat and not effectively utilized, thus limiting solar energy utilization efficiency. Therefore, introducing a photothermal synergistic effect, by simultaneously utilizing photogenerated carriers and localized thermal effects to enhance reaction kinetics, has become an important approach to improving photocatalytic performance.

[0003] In₂Se₃, a typical III-VI semiconductor, possesses a narrow direct bandgap, good visible-near-infrared light response, and a relatively negative conduction band potential, providing a strong thermodynamic driving force for reduction reactions. Furthermore, its inherent layered structure endows it with high carrier mobility, which is beneficial for the separation and transport of photogenerated carriers, thus showing great application potential in photocatalysis. However, single In₂Se₃ still suffers from problems such as easy recombination of photogenerated carriers, insufficient oxidation capacity, and inadequate utilization of the photothermal effect, limiting its further application in the degradation of complex organic pollutants.

[0004] WO3 has a high valence band position and strong oxidizing ability. 3-x The abundant oxygen vacancies in the medium can not only serve as active sites, but also induce W 5+ The associated localized surface plasmon resonance effect gives it strong light absorption in the visible-near infrared region and generates a localized thermal effect. Therefore, WO 3-x They can serve as potential components to enhance the oxidation capacity and photothermal response performance of the system. On the other hand, BCDs have good light absorption capacity, interfacial electronic modulation capacity, and certain photothermal conversion capacity. Introducing them into semiconductor composite systems can help promote interfacial charge migration, suppress carrier recombination, and enhance the photothermal utilization efficiency during the reaction process.

[0005] Furthermore, tobacco straw, as a widely available agricultural waste, is rich in nitrogen-containing organic components and can serve as a precursor for the preparation of biochemical carbon compounds (BCDs). Using tobacco straw as a carbon source to prepare BCDs not only improves the material's interfacial electronic modulation capabilities and potential photothermal response, but also facilitates the resource utilization of agricultural waste.

[0006] Although researchers have modified In2Se3-based systems through morphology regulation, heterostructure construction, and multi-component compositing, existing systems still struggle to simultaneously achieve efficient carrier separation, strong oxidation capacity, and rapid interfacial reaction kinetics in the degradation of tetracycline antibiotics, thus limiting the efficient and deep degradation of pollutants. Therefore, developing In2Se3-based composite catalytic systems that combine efficient carrier separation, strong oxidation capacity, and photothermal synergy remains of great significance. Summary of the Invention

[0007] To address the shortcomings of existing technologies, the present invention aims to provide a tobacco rod-based BCDs / In2Se3 / WO 3-x The ternary composite photothermal catalytic material and its preparation method are proposed to solve the problems of low charge separation efficiency, insufficient oxidation capacity and inadequate utilization of photothermal effect of existing In2Se3-based photocatalytic materials, and to provide its application in the degradation of organic pollutants, especially tetracycline antibiotics.

[0008] To achieve the above objectives, the present invention adopts the following technical solution: This invention provides a tobacco rod-based BCDs / In2Se3 / WO 3-x The ternary composite photothermal catalytic material, namely the tobacco rod-based BCDs / In2Se3 / WO 3-x The ternary composite photothermal catalytic material consists of In2Se3 and oxygen-rich vacancy WO3. 3-x It is composed of BCDs and tobacco rod base; the In2Se3 and WO 3-x A heterojunction is formed, and the tobacco stem-based BCDs are distributed in In2Se3 / WO3. 3-x At the surface and / or interface of the composite system; the WO 3-x Containing oxygen vacancy defect structures, the tobacco stem-based BCDs and WO 3-x It forms an interface coupling with In2Se3.

[0009] Preferably, the In2Se3 and WO 3-x The molar ratio is (0.3~3):1; the mass of the tobacco rod-based BCDs accounts for 1%~15% of the mass of In2Se3.

[0010] As a further preferred option, the In2Se3 and WO 3-xThe molar ratio is (0.5~2):1; the mass of the tobacco rod-based BCDs is 1%~10% of the mass of In2Se3.

[0011] This invention also provides a tobacco rod base BCDs / In2Se3 / WO 3-x The preparation method of ternary composite photothermal catalytic materials includes the following steps: (1) Preparation of tobacco rod-based BCDs; (2) Preparation of oxygen-rich vacancy WO3 3-x ; (3) Dissolve the indium source in the reaction medium, sonicate until the solution is clear, and add oxygen-rich vacancy WO3. 3-x The mixture was dissolved by ultrasonication, and then tobacco stalk-based BCDs that had been pre-dispersed with a small amount of deionized water were added. The mixture was then subjected to ultrasonication again to obtain dispersion A. Separately, a selenium source was taken and a reducing agent was added to the mixture to obtain dispersion B. (4) Dispersion B is added to dispersion A to obtain a mixed solution. After pre-reaction, the mixed solution is transferred to a microwave reactor for microwave-assisted solvothermal reaction. After cooling, the reaction solution is filtered, washed alternately, and dried under vacuum to obtain the tobacco stick-based BCDs / In2Se3 / WO 3-x Ternary composite photothermal catalytic materials.

[0012] Preferably, in step (1), the preparation method of the tobacco stem-based BCDs is as follows: it is obtained by carbonization, oxidation, filtration, dialysis and concentration drying of waste tobacco stems. Specifically, the waste tobacco stems are carbonized at 200~500 ℃ for 18~24 min under Ar atmosphere; the carbonized product is dispersed in 0.3 mol / L NH3·H2O solution at a ratio of 0.002~0.008 g / mL to obtain a mixture; H2O2 solution with a mass percentage concentration of 30% is added to the mixture at a volume ratio of NH3·H2O solution to H2O2 solution of (10~25):1; after stirring and reacting at room temperature, it is filtered through a 0.22 μm microporous membrane, dialyzed through a dialysis bag with a molecular weight cutoff of 1000 Da, and concentrated and dried to obtain tobacco stem-based BCDs.

[0013] As a further preferred option, in step (1), the carbonization temperature is 300 °C and the carbonization time is 20 min.

[0014] Preferably, in step (2), the oxygen-rich vacancy WO 3-xThe preparation method is as follows: Tungstate is dissolved in water at a ratio of 0.01–0.05 mol / L, and citric acid and glucose are added sequentially. The mixture is stirred until homogeneous to obtain a mixed solution. The molar ratio of tungstate, citric acid, and glucose in the mixed solution is (1–4):(1–3):(2–6). Concentrated hydrochloric acid is added dropwise to the mixed solution at a ratio of 0.5–3 mL of 12 mol / L concentrated hydrochloric acid per 1 mmol of tungstate. After ultrasonic treatment, the mixed solution undergoes a first microwave reaction to prepare the WO3 precursor. Subsequently, the WO3 precursor is dissolved in an organic solvent to obtain a 0.01–0.025 mol / L precursor solution. 0.0045–0.009 g / mL of CTAB aqueous solution is added dropwise to the precursor solution at a volume ratio of (4–10):1. After ultrasonic treatment, the mixture undergoes a second microwave reaction to obtain oxygen-rich vacancy WO3. 3-x .

[0015] As a further preferred option, in step (2), the tungstate is Na2WO4·2H2O; and the organic solvent is ethylene glycol.

[0016] As a further preferred option, in step (2), the conditions for the first microwave reaction are: temperature of 100~160 ℃, power of 200~800 W, and time of 1~3 h; the conditions for the second microwave reaction are: temperature of 160~200 ℃, power of 200~800 W, and time of 1~3 h.

[0017] Preferably, in step (3), the indium source is selected from one or both of In(NO3)3·xH2O and InCl3; the reaction medium is triethylene glycol; the selenium source is Se powder; and the reducing agent is hydrazine hydrate.

[0018] Preferably, in step (3), the solid-liquid ratio of the selenium source to the reducing agent is 0.009~0.047 g / mL.

[0019] Preferably, in step (4), the pre-reaction is a water bath heating reaction at a temperature of 60~120 ℃ and a time of 15~60 min; the microwave-assisted solvothermal reaction is at a temperature of 160~240 ℃ and a power of 200~800 W; the time is 60~150 min; and the vacuum drying is at a temperature of 40~100 ℃ and a time of 4~24 h.

[0020] As a further preferred option, in step (4), the microwave-assisted solvothermal reaction time is 120 min.

[0021] The present invention also provides a tobacco rod base BCDs / In2Se3 / WO 3-xThe application of ternary composite photothermal catalytic materials in the degradation of organic pollutants, namely the tobacco stalk-based BCDs / In2Se3 / WO 3-x Ternary composite photothermal catalytic materials serve as catalysts for highly efficient photocatalytic reactions driven by visible light, and are used to degrade organic pollutants.

[0022] Preferably, the organic pollutant is an antibiotic pollutant.

[0023] As a further preferred option, the organic pollutant is a tetracycline antibiotic.

[0024] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention uses In2Se3 and WO 3-x Ternary composites were formed with tobacco stalk-based BCDs to construct a tightly coupled heterojunction system, achieving the effects of promoting the separation and migration of photogenerated carriers and improving the photothermal response of the composite material. This invention uses waste tobacco stalks as a carbon source to prepare BCDs, realizing the resource utilization of biomass waste while obtaining tobacco stalk-based BCDs that can participate in the construction of ternary composite systems as interfacial electronic regulation components and photothermal response components. Furthermore, using WO3... 3-x The oxygen vacancy defect structure and the good light absorption and non-radiative relaxation ability of the tobacco stalk-based BCDs, in synergy with In2Se3, give the composite material a strong photothermal response capability.

[0025] (2) This invention uses In2Se3 and WO 3-x By combining In2Se3 and tobacco-based BCDs in a ternary composite, the double Z-type charge transport characteristics of this ternary system are utilized to improve the pollutant degradation efficiency. The ternary composite system of this invention exhibits significant interfacial electronic interactions, with electrons primarily flowing from In2Se3 and tobacco-based BCDs to WO3. 3-x Migration creates a built-in electric field at the interface; under illumination, this system exhibits a double Z-type charge transport characteristic, retaining highly reducing electrons and highly oxidizing holes, achieving spatial separation of oxidation and reduction sites, thereby improving pollutant degradation efficiency; the tobacco stalk-based BCDs / In2Se3 / WO prepared in this invention 3-x The composite material exhibits excellent performance in the degradation of organic pollutants, especially tetracycline antibiotics: taking oxytetracycline as an example, the optimal sample achieved a degradation rate of 93.54% within 120 min, with a pseudo-first-order kinetic rate constant of 0.0224 min. -1 Furthermore, the photothermal synergy factor SF is 2.26.

[0026] (3) The tobacco rod-based BCDs / In2Se3 / WO prepared in this invention 3-xThe composite material exhibits good stability and environmental adaptability, maintaining high degradation capacity in different water matrices, and the degradation rate remains above 80% after five consecutive cycles. Attached Figure Description

[0027] Figure 1 Image a is a transmission electron microscope image of the tobacco stem-based BCDs prepared in Example 1 of the present invention; image b is a particle size distribution diagram of the tobacco stem-based BCDs prepared in Example 1 of the present invention. Figure 2 This is the oxygen-rich vacancy WO prepared in Example 1 of this invention. 3-x Transmission electron microscope image; Figure 3 This is the In2Se3 / WO prepared in Comparative Example 1 of this invention. 3-x Transmission electron microscope image of binary composite material; Figure 4 This is the tobacco stem-based BCDs / In2Se3 / WO prepared in Example 1 of this invention. 3-x Transmission electron microscope image of ternary composite material; Figure 5 The tobacco rod-based BCDs and oxygen-rich vacancy WO3 prepared in Example 1 of this invention are 3-x and cigarette rod base BCDs / In2Se3 / WO 3-x Ternary composite materials, and the In2Se3 / WO prepared in Comparative Example 1 3-x X-ray photoelectron energy full spectrum of binary composite materials; Figure 6 The tobacco rod-based BCDs and oxygen-rich vacancy WO3 prepared in Example 1 of this invention are 3-x and cigarette rod base BCDs / In2Se3 / WO 3-x Ternary composite materials, and the In2Se3 / WO prepared in Comparative Example 1 3-x UV-Vis absorption spectrum of binary composite material; Figure 7 The In2Se3 / WO prepared in Comparative Examples 1 to 4 of this invention 3-x Photothermal degradation performance of binary composite materials on oxytetracycline; Figure 8 The tobacco stem-based BCDs / In2Se3 / WO prepared in Examples 1 to 5 of this invention 3-x Photothermal degradation performance of ternary composite materials on oxytetracycline; Figure 9 The tobacco stem-based BCDs / In2Se3 / WO prepared in Example 4 of this invention 3-x Comparison of the degradation performance of ternary composite materials on oxytetracycline under photothermal synergy, light irradiation alone, and heating alone. Detailed Implementation

[0028] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0029] Example 1 Example 1 provides a tobacco rod base BCDs / In2Se3 / WO 3-x The preparation method of ternary composite materials, wherein the mass ratio of tobacco stalk-based BCDs to In2Se3 is 1%, and the mass ratio of In2Se3 to WO3 is... 3-x The molar ratio is 1:1, as detailed below: (1) Preparation of tobacco stem-based BCDs: Waste tobacco stems were cut into small pieces, repeatedly washed with deionized water to remove surface impurities, and then dried in an oven at 60 ℃ to constant weight; the dried tobacco stems were ground into fine powder with a particle size of less than 1 mm and sealed for later use; the tobacco stem powder was placed in a microwave tube furnace and carbonized at 300 ℃ for 20 min under Ar atmosphere; 0.8 g of carbonized product was weighed and dispersed in 200 mL of 0.3 mol / L NH3·H2O solution, and then 16 mL of H2O2 (30%) was added. The reaction was stirred continuously at room temperature for 48 h to obtain a brown transparent solution; after the reaction was completed, the obtained solution was filtered through a 0.22 μm microporous membrane and dialyzed for 2 days using a dialysis bag with a molecular weight cutoff of 1000 Da; finally, the precipitate in the dialysis bag was concentrated and dried by rotary evaporation to obtain tobacco stem-based BCDs powder.

[0030] (2)WO 3-xPreparation: 2 mmol Na₂WO₄·2H₂O was dissolved in 60 mL of ultrapure water and stirred thoroughly until clear. Then, 3 mmol citric acid and 10 mmol glucose were added sequentially, and stirring was continued for 10 min to obtain a mixture. 3 mL of concentrated hydrochloric acid (12 mol / L) was then added dropwise to the mixture, and the mixture was sonicated for 1 h. The mixture was then transferred to a microwave reactor and reacted at 120 °C and 600 W for 2 h. After the reaction, the mixture was filtered, washed, and vacuum dried at 60 °C for 12 h to obtain the WO₃ precursor. 0.5 mmol of the WO₃ precursor (calculated as WO₃) was weighed and dispersed in 25 mL of ethylene glycol using ultrasonication for 30 min to obtain a precursor solution. Separately, 0.0375 g CTAB was dissolved in 5 mL of deionized water and dispersed using ultrasonication for 30 min to obtain a CTAB aqueous solution. The CTAB aqueous solution was slowly added dropwise to the precursor solution, and ultrasonication was continued for 60 min. The mixture was then transferred to a microwave reactor and reacted at 180 °C and 600 W for 120 min. min; after cooling, the product was filtered, washed alternately, and dried under vacuum at 60 °C for 12 h to obtain oxygen-rich vacancy WO3. 3-x powder.

[0031] (3) Preparation of ternary composite material: In(NO3)3·xH2O (0.1204 g, 0.4 mmol) was dissolved in 28 mL of triethylene glycol and sonicated for 10 min until clear; WO3 was added 3-x After sonicating (0.0464 g, 0.2 mmol) for 20 min, add 0.0009 g of tobacco stalk-based BCDs pre-dispersed with a small amount of deionized water, and continue sonicating for 20 min to obtain dispersion A; separately, take Se powder (0.0474 g, 0.6 mmol), add 2.5 mL of hydrazine hydrate, and stir for 5 min to obtain dispersion B; slowly add dispersion B dropwise to dispersion A, and reflux in a water bath at 80 ℃ for 30 min; then transfer the mixture to a microwave reactor and react at 220 ℃ and 600 W for 120 min; after cooling, filter, wash alternately, and vacuum dry at 60 ℃ for 12 h to obtain tobacco stalk-based BCDs / In2Se3 / WO 3-x Ternary composite photothermal catalytic materials.

[0032] Example 2 Example 2 provides a tobacco rod base BCDs / In2Se3 / WO 3-x The preparation method of ternary composite materials, wherein the mass ratio of tobacco stalk-based BCDs to In2Se3 is 3%, and the mass ratio of In2Se3 to WO3 is... 3-x The molar ratio is 1:1, as detailed below: (1) Preparation of tobacco stem-based BCDs: Waste tobacco stems were cut into small pieces, repeatedly washed with deionized water to remove surface impurities, and then dried in an oven at 60 ℃ to constant weight; the dried tobacco stems were ground into fine powder with a particle size of less than 1 mm and sealed for later use; the tobacco stem powder was placed in a microwave tube furnace and carbonized at 300 ℃ for 20 min under Ar atmosphere; 0.8 g of carbonized product was weighed and dispersed in 200 mL of 0.3 mol / L NH3·H2O solution, and then 16 mL of H2O2 (30%) was added. The reaction was stirred continuously at room temperature for 48 h to obtain a brown transparent solution; after the reaction was completed, the obtained solution was filtered through a 0.22 μm microporous membrane and dialyzed for 2 days using a dialysis bag with a molecular weight cutoff of 1000 Da; finally, the precipitate in the dialysis bag was concentrated and dried by rotary evaporation to obtain tobacco stem-based BCDs powder.

[0033] (2)WO 3-x Preparation: 2 mmol Na₂WO₄·2H₂O was dissolved in 60 mL of ultrapure water and stirred thoroughly until clear. Then, 3 mmol citric acid and 10 mmol glucose were added sequentially, and stirring was continued for 10 min to obtain a mixture. 3 mL of concentrated hydrochloric acid (12 mol / L) was then added dropwise to the mixture, and the mixture was sonicated for 1 h. The mixture was then transferred to a microwave reactor and reacted at 120 °C and 600 W for 2 h. After the reaction, the mixture was filtered, washed, and vacuum dried at 60 °C for 12 h to obtain the WO₃ precursor. 0.5 mmol of the WO₃ precursor (calculated as WO₃) was weighed and dispersed in 25 mL of ethylene glycol using ultrasonication for 30 min to obtain a precursor solution. Separately, 0.0375 g CTAB was dissolved in 5 mL of deionized water and dispersed using ultrasonication for 30 min to obtain a CTAB aqueous solution. The CTAB aqueous solution was slowly added dropwise to the precursor solution, and ultrasonication was continued for 60 min. The mixture was then transferred to a microwave reactor and reacted at 180 °C and 600 W for 120 min. min; after cooling, the product was filtered, washed alternately, and dried under vacuum at 60 °C for 12 h to obtain oxygen-rich vacancy WO3. 3-x powder.

[0034] (3) Preparation of ternary composite material: In(NO3)3·xH2O (0.1204 g, 0.4 mmol) was dissolved in 28 mL of triethylene glycol and sonicated for 10 min until clear; WO3 was added 3-xAfter sonicating (0.0464 g, 0.2 mmol) for 20 min, add 0.0028 g of tobacco stalk-based BCDs pre-dispersed in a small amount of deionized water, and continue sonicating for 20 min to obtain dispersion A; separately, take Se powder (0.0474 g, 0.6 mmol), add 2.5 mL of hydrazine hydrate, and stir for 5 min to obtain dispersion B; slowly add dispersion B dropwise to dispersion A, and reflux in a water bath at 80 ℃ for 30 min; then transfer the mixture to a microwave reactor and react at 220 ℃ and 600 W for 120 min; after cooling, filter, wash alternately, and vacuum dry at 60 ℃ for 12 h to obtain tobacco stalk-based BCDs / In2Se3 / WO 3-x Ternary composite photothermal catalytic materials.

[0035] Example 3 Example 3 provides a tobacco rod base BCDs / In2Se3 / WO 3-x A method for preparing ternary composite materials, wherein the mass ratio of tobacco stalk-based BCDs to In2Se3 is 5%, and the mass ratio of In2Se3 to WO3 is... 3-x The molar ratio is 1:1, as detailed below: (1) Preparation of tobacco stem-based BCDs: Waste tobacco stems were cut into small pieces, repeatedly washed with deionized water to remove surface impurities, and then dried in an oven at 60 ℃ to constant weight; the dried tobacco stems were ground into fine powder with a particle size of less than 1 mm and sealed for later use; the tobacco stem powder was placed in a microwave tube furnace and carbonized at 300 ℃ for 20 min under Ar atmosphere; 0.8 g of carbonized product was weighed and dispersed in 200 mL of 0.3 mol / L NH3·H2O solution, and then 16 mL of H2O2 (30%) was added. The reaction was stirred continuously at room temperature for 48 h to obtain a brown transparent solution; after the reaction was completed, the obtained solution was filtered through a 0.22 μm microporous membrane and dialyzed for 2 days using a dialysis bag with a molecular weight cutoff of 1000 Da; finally, the precipitate in the dialysis bag was concentrated and dried by rotary evaporation to obtain tobacco stem-based BCDs powder.

[0036] (2)WO 3-xPreparation: 2 mmol Na₂WO₄·2H₂O was dissolved in 60 mL of ultrapure water and stirred thoroughly until clear. Then, 3 mmol citric acid and 10 mmol glucose were added sequentially, and stirring was continued for 10 min to obtain a mixture. 3 mL of concentrated hydrochloric acid (12 mol / L) was then added dropwise to the mixture, and the mixture was sonicated for 1 h. The mixture was then transferred to a microwave reactor and reacted at 120 °C and 600 W for 2 h. After the reaction, the mixture was filtered, washed, and vacuum dried at 60 °C for 12 h to obtain the WO₃ precursor. 0.5 mmol of the WO₃ precursor (calculated as WO₃) was weighed and dispersed in 25 mL of ethylene glycol using ultrasonication for 30 min to obtain a precursor solution. Separately, 0.0375 g CTAB was dissolved in 5 mL of deionized water and dispersed using ultrasonication for 30 min to obtain a CTAB aqueous solution. The CTAB aqueous solution was slowly added dropwise to the precursor solution, and ultrasonication was continued for 60 min. The mixture was then transferred to a microwave reactor and reacted at 180 °C and 600 W for 120 min. min; after cooling, the product was filtered, washed alternately, and dried under vacuum at 60 °C for 12 h to obtain oxygen-rich vacancy WO3. 3-x powder.

[0037] (3) Preparation of ternary composite material: In(NO3)3·xH2O (0.1204 g, 0.4 mmol) was dissolved in 28 mL of triethylene glycol and sonicated for 10 min until clear; WO3 was added 3-x After sonicating (0.0464 g, 0.2 mmol) for 20 min, add 0.0046 g of tobacco stalk-based BCDs pre-dispersed in a small amount of deionized water, and continue sonicating for 20 min to obtain dispersion A; separately, take Se powder (0.0474 g, 0.6 mmol), add 2.5 mL of hydrazine hydrate, and stir for 5 min to obtain dispersion B; slowly add dispersion B dropwise to dispersion A, and reflux in a water bath at 80 ℃ for 30 min; then transfer the mixture to a microwave reactor and react at 220 ℃ and 600 W for 120 min; after cooling, filter, wash alternately, and vacuum dry at 60 ℃ for 12 h to obtain tobacco stalk-based BCDs / In2Se3 / WO 3-x Ternary composite photothermal catalytic materials.

[0038] Example 4 Example 4 provides a tobacco rod base BCDs / In2Se3 / WO 3-x The preparation method of ternary composite materials, wherein the mass ratio of tobacco stalk-based BCDs to In2Se3 is 7%, and the mass ratio of In2Se3 to WO3 is... 3-x The molar ratio is 1:1, as detailed below: (1) Preparation of tobacco stem-based BCDs: Waste tobacco stems were cut into small pieces, repeatedly washed with deionized water to remove surface impurities, and then dried in an oven at 60 ℃ to constant weight; the dried tobacco stems were ground into fine powder with a particle size of less than 1 mm and sealed for later use; the tobacco stem powder was placed in a microwave tube furnace and carbonized at 300 ℃ for 20 min under Ar atmosphere; 0.8 g of carbonized product was weighed and dispersed in 200 mL of 0.3 mol / L NH3·H2O solution, and then 16 mL of H2O2 (30%) was added. The reaction was stirred continuously at room temperature for 48 h to obtain a brown transparent solution; after the reaction was completed, the obtained solution was filtered through a 0.22 μm microporous membrane and dialyzed for 2 days using a dialysis bag with a molecular weight cutoff of 1000 Da; finally, the precipitate in the dialysis bag was concentrated and dried by rotary evaporation to obtain tobacco stem-based BCDs powder.

[0039] (2)WO 3-x Preparation: 2 mmol Na₂WO₄·2H₂O was dissolved in 60 mL of ultrapure water and stirred thoroughly until clear. Then, 3 mmol citric acid and 10 mmol glucose were added sequentially, and stirring was continued for 10 min to obtain a mixture. 3 mL of concentrated hydrochloric acid (12 mol / L) was then added dropwise to the mixture, and the mixture was sonicated for 1 h. The mixture was then transferred to a microwave reactor and reacted at 120 °C and 600 W for 2 h. After the reaction, the mixture was filtered, washed, and vacuum dried at 60 °C for 12 h to obtain the WO₃ precursor. 0.5 mmol of the WO₃ precursor (calculated as WO₃) was weighed and dispersed in 25 mL of ethylene glycol using ultrasonication for 30 min to obtain a precursor solution. Separately, 0.0375 g CTAB was dissolved in 5 mL of deionized water and dispersed using ultrasonication for 30 min to obtain a CTAB aqueous solution. The CTAB aqueous solution was slowly added dropwise to the precursor solution, and ultrasonication was continued for 60 min. The mixture was then transferred to a microwave reactor and reacted at 180 °C and 600 W for 120 min. min; after cooling, the product was filtered, washed alternately, and dried under vacuum at 60 °C for 12 h to obtain oxygen-rich vacancy WO3. 3-x powder.

[0040] (3) Preparation of ternary composite material: In(NO3)3·xH2O (0.1204 g, 0.4 mmol) was dissolved in 28 mL of triethylene glycol and sonicated for 10 min until clear; WO3 was added 3-xAfter sonicating (0.0464 g, 0.2 mmol) for 20 min, add 0.0065 g of tobacco stalk-based BCDs pre-dispersed with a small amount of deionized water, and continue sonicating for 20 min to obtain dispersion A; separately, take Se powder (0.0474 g, 0.6 mmol), add 2.5 mL of hydrazine hydrate, and stir for 5 min to obtain dispersion B; slowly add dispersion B dropwise to dispersion A, and reflux in a water bath at 80 ℃ for 30 min; then transfer the mixture to a microwave reactor and react at 220 ℃ and 600 W for 120 min; after cooling, filter, wash alternately, and vacuum dry at 60 ℃ for 12 h to obtain tobacco stalk-based BCDs / In2Se3 / WO 3-x Ternary composite photothermal catalytic materials.

[0041] Example 5 Example 5 provides a tobacco rod base BCDs / In2Se3 / WO 3-x A method for preparing ternary composite materials, wherein the mass ratio of tobacco stalk-based BCDs to In2Se3 is 10%, and the mass ratio of In2Se3 to WO3 is... 3-x The molar ratio is 1:1, as detailed below: (1) Preparation of tobacco stem-based BCDs: Waste tobacco stems were cut into small pieces, repeatedly washed with deionized water to remove surface impurities, and then dried in an oven at 60 ℃ to constant weight; the dried tobacco stems were ground into fine powder with a particle size of less than 1 mm and sealed for later use; the tobacco stem powder was placed in a microwave tube furnace and carbonized at 300 ℃ for 20 min under Ar atmosphere; 0.8 g of carbonized product was weighed and dispersed in 200 mL of 0.3 mol / L NH3·H2O solution, and then 16 mL of H2O2 (30%) was added. The reaction was stirred continuously at room temperature for 48 h to obtain a brown transparent solution; after the reaction was completed, the obtained solution was filtered through a 0.22 μm microporous membrane and dialyzed for 2 days using a dialysis bag with a molecular weight cutoff of 1000 Da; finally, the precipitate in the dialysis bag was concentrated and dried by rotary evaporation to obtain tobacco stem-based BCDs powder.

[0042] (2)WO 3-xPreparation: 2 mmol Na₂WO₄·2H₂O was dissolved in 60 mL of ultrapure water and stirred thoroughly until clear. Then, 3 mmol citric acid and 10 mmol glucose were added sequentially, and stirring was continued for 10 min to obtain a mixture. 3 mL of concentrated hydrochloric acid (12 mol / L) was then added dropwise to the mixture, and the mixture was sonicated for 1 h. The mixture was then transferred to a microwave reactor and reacted at 120 °C and 600 W for 2 h. After the reaction, the mixture was filtered, washed, and vacuum dried at 60 °C for 12 h to obtain the WO₃ precursor. 0.5 mmol of the WO₃ precursor (calculated as WO₃) was weighed and dispersed in 25 mL of ethylene glycol using ultrasonication for 30 min to obtain a precursor solution. Separately, 0.0375 g CTAB was dissolved in 5 mL of deionized water and dispersed using ultrasonication for 30 min to obtain a CTAB aqueous solution. The CTAB aqueous solution was slowly added dropwise to the precursor solution, and ultrasonication was continued for 60 min. The mixture was then transferred to a microwave reactor and reacted at 180 °C and 600 W for 120 min. min; after cooling, the product was filtered, washed alternately, and dried under vacuum at 60 °C for 12 h to obtain oxygen-rich vacancy WO3. 3-x powder.

[0043] (3) Preparation of ternary composite material: In(NO3)3·xH2O (0.1204 g, 0.4 mmol) was dissolved in 28 mL of triethylene glycol and sonicated for 10 min until clear; WO3 was added 3-x After sonicating (0.0464 g, 0.2 mmol) for 20 min, add 0.0093 g of tobacco stalk-based BCDs pre-dispersed with a small amount of deionized water, and continue sonicating for 20 min to obtain dispersion A; separately, take Se powder (0.0474 g, 0.6 mmol), add 2.5 mL of hydrazine hydrate, and stir for 5 min to obtain dispersion B; slowly add dispersion B dropwise to dispersion A, and reflux in a water bath at 80 ℃ for 30 min; then transfer the mixture to a microwave reactor and react at 220 ℃ and 600 W for 120 min; after cooling, filter, wash alternately, and vacuum dry at 60 ℃ for 12 h to obtain tobacco stalk-based BCDs / In2Se3 / WO 3-x Ternary composite photothermal catalytic materials.

[0044] Example 6 Example 6 provides a tobacco rod base BCDs / In2Se3 / WO 3-x A method for preparing ternary composite materials, wherein the mass ratio of tobacco stalk-based BCDs to In2Se3 is 15%, and the mass ratio of In2Se3 to WO3 is... 3-x The molar ratio is 1:1, as detailed below: (1) Preparation of tobacco stem-based BCDs: Waste tobacco stems were cut into small pieces, repeatedly washed with deionized water to remove surface impurities, and then dried in an oven at 60 ℃ to constant weight; the dried tobacco stems were ground into fine powder with a particle size of less than 1 mm and sealed for later use; the tobacco stem powder was placed in a microwave tube furnace and carbonized at 300 ℃ for 20 min under Ar atmosphere; 0.8 g of carbonized product was weighed and dispersed in 200 mL of 0.3 mol / L NH3·H2O solution, and then 16 mL of H2O2 (30%) was added. The reaction was stirred continuously at room temperature for 48 h to obtain a brown transparent solution; after the reaction was completed, the obtained solution was filtered through a 0.22 μm microporous membrane and dialyzed for 2 days using a dialysis bag with a molecular weight cutoff of 1000 Da; finally, the precipitate in the dialysis bag was concentrated and dried by rotary evaporation to obtain tobacco stem-based BCDs powder.

[0045] (2)WO 3-x Preparation: 2 mmol Na₂WO₄·2H₂O was dissolved in 60 mL of ultrapure water and stirred thoroughly until clear. Then, 3 mmol citric acid and 10 mmol glucose were added sequentially, and stirring was continued for 10 min to obtain a mixture. 3 mL of concentrated hydrochloric acid (12 mol / L) was then added dropwise to the mixture, and the mixture was sonicated for 1 h. The mixture was then transferred to a microwave reactor and reacted at 120 °C and 600 W for 2 h. After the reaction, the mixture was filtered, washed, and vacuum dried at 60 °C for 12 h to obtain the WO₃ precursor. 0.5 mmol of the WO₃ precursor (calculated as WO₃) was weighed and dispersed in 25 mL of ethylene glycol using ultrasonication for 30 min to obtain a precursor solution. Separately, 0.0375 g CTAB was dissolved in 5 mL of deionized water and dispersed using ultrasonication for 30 min to obtain a CTAB aqueous solution. The CTAB aqueous solution was slowly added dropwise to the precursor solution, and ultrasonication was continued for 60 min. The mixture was then transferred to a microwave reactor and reacted at 180 °C and 600 W for 120 min. min; after cooling, the product was filtered, washed alternately, and dried under vacuum at 60 °C for 12 h to obtain oxygen-rich vacancy WO3. 3-x powder.

[0046] (3) Preparation of ternary composite material: In(NO3)3·xH2O (0.1204 g, 0.4 mmol) was dissolved in 28 mL of triethylene glycol and sonicated for 10 min until clear; WO3 was added 3-xAfter sonicating (0.0464 g, 0.2 mmol) for 20 min, add 0.0138 g of tobacco stalk-based BCDs pre-dispersed in a small amount of deionized water, and continue sonicating for 20 min to obtain dispersion A; separately, take Se powder (0.0474 g, 0.6 mmol), add 2.5 mL of hydrazine hydrate, and stir for 5 min to obtain dispersion B; slowly add dispersion B dropwise to dispersion A, and reflux in a water bath at 80 ℃ for 30 min; then transfer the mixture to a microwave reactor and react at 220 ℃ and 600 W for 120 min; after cooling, filter, wash alternately, and vacuum dry at 60 ℃ for 12 h to obtain tobacco stalk-based BCDs / In2Se3 / WO 3-x Ternary composite photothermal catalytic materials.

[0047] Example 7 Example 7 provides a tobacco rod base BCDs / In2Se3 / WO 3-x The preparation method of ternary composite materials, wherein the mass ratio of tobacco stalk-based BCDs to In2Se3 is 7%, and the mass ratio of In2Se3 to WO3 is... 3-x The molar ratio is 0.3:1, as detailed below: (1) Preparation of tobacco stem-based BCDs: Waste tobacco stems were cut into small pieces, repeatedly washed with deionized water to remove surface impurities, and then dried in an oven at 60 ℃ to constant weight; the dried tobacco stems were ground into fine powder with a particle size of less than 1 mm and sealed for later use; the tobacco stem powder was placed in a microwave tube furnace and carbonized at 200 ℃ for 24 min under Ar atmosphere; 0.4 g of carbonized product was weighed and dispersed in 200 mL of 0.3 mol / L NH3·H2O solution, and then 20 mL of H2O2 (30%) was added. The reaction was stirred continuously at room temperature for 48 h to obtain a brown transparent solution; after the reaction was completed, the obtained solution was filtered through a 0.22 μm microporous membrane and dialyzed for 2 days using a dialysis bag with a molecular weight cutoff of 1000 Da; finally, the dialysis bag residue was concentrated and dried by rotary evaporation to obtain tobacco stem-based BCDs powder.

[0048] (2)WO 3-xPreparation: 2 mmol Na₂WO₄·2H₂O was dissolved in 60 mL of ultrapure water and stirred thoroughly until clear. Then, 2 mmol citric acid and 12 mmol glucose were added sequentially, and stirring was continued for 10 min to obtain a mixture. 3 mL of concentrated hydrochloric acid (12 mol / L) was then added dropwise to the mixture, and the mixture was sonicated for 1 h. The mixture was then transferred to a microwave reactor and reacted at 120 °C and 600 W for 2 h. After the reaction, the mixture was filtered, washed, and vacuum dried at 60 °C for 12 h to obtain the WO₃ precursor. 0.5 mmol of the WO₃ precursor (calculated as WO₃) was weighed and dispersed in 20 mL of ethylene glycol using ultrasonication for 30 min to obtain a precursor solution. Separately, 0.045 g CTAB was dissolved in 5 mL of deionized water and dispersed using ultrasonication for 30 min to obtain a CTAB aqueous solution. The CTAB aqueous solution was slowly added dropwise to the precursor solution, and ultrasonication was continued for 60 min. The mixture was then transferred to a microwave reactor and reacted at 160 °C and 800 W for 150 min. min; after cooling, the sample was filtered, washed alternately, and dried under vacuum at 100 °C for 4 h to obtain oxygen-rich vacancy WO3. 3-x powder.

[0049] (3) Preparation of ternary composite material: In(NO3)3·xH2O (0.1204 g, 0.4 mmol) was dissolved in 30 mL of triethylene glycol and sonicated for 10 min until clear; WO3 was added 3-x After sonicating (0.0464 g, 0.2 mmol) for 20 min, add 0.0065 g of tobacco stalk-based BCDs pre-dispersed in a small amount of deionized water, and continue sonicating for 20 min to obtain dispersion A; separately, take Se powder (0.0474 g, 0.6 mmol), add 5 mL of hydrazine hydrate, and stir for 5 min to obtain dispersion B; slowly add dispersion B dropwise to dispersion A, and reflux in a water bath at 60 ℃ for 60 min; then transfer the mixture to a microwave reactor and react at 220 ℃ and 600 W for 120 min; after cooling, filter, wash alternately, and vacuum dry at 60 ℃ for 12 h to obtain tobacco stalk-based BCDs / In2Se3 / WO 3-x Ternary composite photothermal catalytic materials.

[0050] Example 8 Example 8 provides a tobacco rod base BCDs / In2Se3 / WO 3-x The preparation method of ternary composite materials, wherein the mass ratio of tobacco stalk-based BCDs to In2Se3 is 7%, and the mass ratio of In2Se3 to WO3 is... 3-x The molar ratio is 3:1, as detailed below: (1) Preparation of tobacco stem-based BCDs: Waste tobacco stems were cut into small pieces, repeatedly washed with deionized water to remove surface impurities, and then dried in an oven at 60 ℃ to constant weight; the dried tobacco stems were ground into fine powder with a particle size of less than 1 mm and sealed for later use; the tobacco stem powder was placed in a microwave tube furnace and carbonized at 500 ℃ for 18 min under Ar atmosphere; 1.6 g of carbonized product was weighed and dispersed in 200 mL of 0.3 mol / L NH3·H2O solution, and then 8 mL of H2O2 (30%) was added. The reaction was stirred continuously at room temperature for 48 h to obtain a brown transparent solution; after the reaction was completed, the obtained solution was filtered through a 0.22 μm microporous membrane and dialyzed for 2 days using a dialysis bag with a molecular weight cutoff of 1000 Da; finally, the precipitate in the dialysis bag was concentrated and dried by rotary evaporation to obtain tobacco stem-based BCDs powder.

[0051] (2)WO 3-x Preparation: 4 mmol Na₂WO₄·2H₂O was dissolved in 60 mL of ultrapure water and stirred thoroughly until clear. Then, 3 mmol citric acid and 2 mmol glucose were added sequentially, and stirring was continued for 10 min to obtain a mixture. 3 mL of concentrated hydrochloric acid (12 mol / L) was then added dropwise to the mixture, and the mixture was sonicated for 1 h. The mixture was then transferred to a microwave reactor and reacted at 120 °C and 600 W for 2 h. After the reaction, the mixture was filtered, washed, and vacuum dried at 60 °C for 12 h to obtain the WO₃ precursor. 0.5 mmol of the WO₃ precursor (calculated as WO₃) was weighed and dispersed in 50 mL of ethylene glycol using ultrasonication for 30 min to obtain a precursor solution. Separately, 0.0225 g CTAB was dissolved in 5 mL of deionized water and dispersed using ultrasonication for 30 min to obtain a CTAB aqueous solution. The CTAB aqueous solution was slowly added dropwise to the precursor solution, and ultrasonication was continued for 60 min. The mixture was then transferred to a microwave reactor and reacted at 180 °C and 600 W for 120 min. min; after cooling, the product was filtered, washed alternately, and dried under vacuum at 60 °C for 12 h to obtain oxygen-rich vacancy WO3. 3-x powder.

[0052] (3) Preparation of ternary composite material: In(NO3)3·xH2O (0.1204 g, 0.4 mmol) was dissolved in 25 mL of triethylene glycol and sonicated for 10 min until clear; 0.06047 g of WO3 was added. 3-xAfter sonication for 20 min, 0.0065 g of tobacco stalk-based BCDs, pre-dispersed in a small amount of deionized water, was added, and sonication continued for another 20 min to obtain dispersion A. Separately, 0.0474 g (0.6 mmol) of Se powder was added to 1 mL of hydrazine hydrate and stirred for 5 min to obtain dispersion B. Dispersion B was slowly added dropwise to dispersion A, and the mixture was refluxed in a water bath at 120 °C for 15 min. The mixture was then transferred to a microwave reactor and reacted at 240 °C and 200 W for 60 min. After cooling, the mixture was filtered, washed alternately, and dried under vacuum at 40 °C for 24 h to obtain tobacco stalk-based BCDs / In2Se3 / WO3. 3-x Ternary composite photothermal catalytic materials.

[0053] Comparative Example 1 Comparative Example 1 provides an In2Se3 / WO 3-x Preparation method of binary composite materials, WO in this comparative example 3-x The preparation method is the same as in Example 1, wherein In2Se3 and WO 3-x The molar ratio is 0.5:1, as detailed below: Dissolve In(NO3)3·xH2O (0.1204 g, 0.4 mmol) in 27.5 mL of triethylene glycol and sonicate for 10 min until completely dissolved; then add WO3. 3-x (0.0927 g, 0.4 mmol) was sonicated for 20 min to obtain solution A; 0.0474 g of Se powder was added to 2.5 mL of hydrazine hydrate and stirred for 5 min to obtain solution B; solution B was added dropwise to solution A to obtain a mixed solution, which was then refluxed and stirred in an 80 ℃ water bath for 30 min; the mixed solution was then transferred to a microwave reactor and reacted at 220 ℃ and 600 W for 120 min; after cooling, it was filtered, washed, and vacuum dried at 60 ℃ for 12 h to obtain In2Se3 / WO 3-x Binary composite materials.

[0054] Comparative Example 2 Comparative Example 2 provides an In2Se3 / WO 3-x Preparation method of binary composite materials, WO in this comparative example 3-x The preparation method is the same as in Example 1, wherein In2Se3 and WO 3-x The molar ratio is 0.67:1, as detailed below: Dissolve In(NO3)3·xH2O (0.1204 g, 0.4 mmol) in 27.5 mL of triethylene glycol and sonicate for 10 min until completely dissolved; then add WO3. 3-x(0.0696 g, 0.3 mmol) was sonicated for 20 min to obtain solution A; 0.0474 g of Se powder was added to 2.5 mL of hydrazine hydrate and stirred for 5 min to obtain solution B; solution B was added dropwise to solution A to obtain a mixed solution, which was then refluxed and stirred in an 80 ℃ water bath for 30 min; the mixed solution was then transferred to a microwave reactor and reacted at 220 ℃ and 600 W for 120 min; after cooling, it was filtered, washed, and vacuum dried at 60 ℃ for 12 h to obtain In2Se3 / WO 3-x Binary composite materials.

[0055] Comparative Example 3 Comparative Example 3 provides an In2Se3 / WO 3-x Preparation method of binary composite materials, WO in this comparative example 3-x The preparation method is the same as in Example 1, wherein In2Se3 and WO 3-x The molar ratio is 1:1, as detailed below: Dissolve In(NO3)3·xH2O (0.1204 g, 0.4 mmol) in 27.5 mL of triethylene glycol and sonicate for 10 min until completely dissolved; then add WO3. 3-x (0.0696 g, 0.3 mmol) was sonicated for 20 min to obtain solution A; 0.0474 g of Se powder was added to 2.5 mL of hydrazine hydrate and stirred for 5 min to obtain solution B; solution B was added dropwise to solution A to obtain a mixed solution, which was then refluxed and stirred in an 80 ℃ water bath for 30 min; the mixed solution was then transferred to a microwave reactor and reacted at 220 ℃ and 600 W for 120 min; after cooling, it was filtered, washed, and vacuum dried at 60 ℃ for 12 h to obtain In2Se3 / WO 3-x Binary composite materials.

[0056] Comparative Example 4 Comparative Example 4 provides an In2Se3 / WO 3-x Preparation method of binary composite materials, WO in this comparative example 3-x The preparation method is the same as in Example 1, wherein In2Se3 and WO 3-x The molar ratio is 1.5:1, as detailed below: Dissolve In(NO3)3·xH2O (0.1204 g, 0.4 mmol) in 27.5 mL of triethylene glycol and sonicate for 10 min until completely dissolved; then add WO3. 3-x(0.0309 g, 0.133 mmol) was sonicated for 20 min to obtain solution A; 0.0474 g of Se powder was added to 2.5 mL of hydrazine hydrate and stirred for 5 min to obtain solution B; solution B was added dropwise to solution A to obtain a mixed solution, which was then refluxed and stirred in an 80 ℃ water bath for 30 min; the mixed solution was then transferred to a microwave reactor and reacted at 220 ℃ and 600 W for 120 min; after cooling, it was filtered, washed, and vacuum dried at 60 ℃ for 12 h to obtain In2Se3 / WO 3-x Binary composite materials.

[0057] The structure and composition of the materials prepared in the examples were analyzed, and the results are as follows: Figure 4 and 5 As shown in the figure: In2Se3, WO 3-x It achieves effective composite with the tobacco rod-based BCDs and forms a relatively tight interfacial contact.

[0058] Using oxytetracycline as the target pollutant, the degradation performance of the material samples prepared in the examples under photothermal synergistic conditions was tested; the results are as follows: Figure 7 and 8 As shown: With WO 3-x Variations in the proportion and amount of tobacco stalk-based BCDs added resulted in different catalytic performances in the samples. Among them, the ternary composite material with 7% tobacco stalk-based BCDs (Example 4) exhibited the best performance, achieving a degradation rate of 93.54% for oxytetracycline within 120 min, corresponding to a pseudo-first-order kinetic rate constant of 0.0224 min. -1 The prepared ternary composite material exhibited superior catalytic activity compared to single-component and binary systems in the degradation of oxytetracycline, and also showed significant photothermal synergistic enhancement and good cycle stability.

[0059] The degradation of oxytetracycline in the optimal ternary composite material (prepared in Example 4) was tested under photocatalytic, thermocatalytic, and photothermal synergistic conditions, respectively. The results are as follows: Figure 8 As shown, under photothermal synergistic conditions, the material exhibits a higher degradation rate, with a synergistic factor SF of 2.26, indicating that the ternary composite system has a significant photothermal synergistic enhancement effect.

[0060] Cyclic experiments were conducted on the optimal ternary composite material (prepared in Example 4), and the results are as follows: Figure 9 As shown, after five consecutive cycles, the degradation rate remained above 80%, demonstrating good reusability. Furthermore, the material maintained high oxytetracycline degradation efficiency in different water matrices, such as deionized water, tap water, river water, and pond water, indicating its good environmental adaptability.

[0061] The band structure test, XPS results, and photoelectrochemical test results show that there are obvious interfacial electronic interactions in the ternary composite system prepared in this invention, with electrons mainly flowing from In2Se3 and tobacco-based BCDs to WO3. 3-x Migration creates a built-in electric field at the interface. Under illumination, this system exhibits a double Z-type charge transport characteristic, retaining highly reducing electrons and highly oxidizing holes, achieving spatial separation of oxidation and reduction sites, thereby improving pollutant degradation efficiency.

[0062] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A type of cigarette rod based on BCDs / In2Se3 / WO 3-x The ternary composite photothermal catalytic material is characterized by... The material consists of In2Se3 and oxygen-rich vacancy WO3. 3-x It is composed of BCDs and tobacco rod base; the In2Se3 and WO 3-x A heterojunction is formed, and the tobacco stem-based BCDs are distributed in In2Se3 / WO3. 3-x At the surface and / or interface of the composite system; the WO 3-x Containing oxygen vacancy defect structures, the tobacco stem-based BCDs and WO 3-x It forms an interface coupling with In2Se3.

2. The tobacco rod base BCDs / In2Se3 / WO according to claim 1 3-x The ternary composite photothermal catalytic material is characterized by: The In2Se3 and WO 3-x The molar ratio is (0.3~3):1; the mass of the tobacco rod-based BCDs accounts for 1%~15% of the mass of In2Se3.

3. The tobacco rod base BCDs / In2Se3 / WO as described in claim 1 or 2 3-x The method for preparing ternary composite photothermal catalytic materials is characterized by... Includes the following steps: (1) Preparation of tobacco rod-based BCDs; (2) Preparation of oxygen-rich vacancy WO3 3-x ; (3) Add indium source and WO 3-x The tobacco stem-based BCDs are dispersed in the reaction medium to form dispersion A, and the selenium source is mixed with the reducing agent to form dispersion B; (4) Add dispersion B to dispersion A, and obtain the tobacco stalk-based BCDs / In2Se3 / WO by pre-reaction and microwave-assisted solvothermal reaction. 3-x Ternary composite photothermal catalytic materials.

4. The tobacco rod base BCDs / In2Se3 / WO according to claim 3 3-x The method for preparing ternary composite photothermal catalytic materials is characterized by... In step (1), the preparation method of the tobacco stem-based BCDs is as follows: it is obtained by carbonization, oxidation, filtration, dialysis and concentration drying of waste tobacco stems. Specifically, the waste tobacco stems are carbonized at 200~500 ℃ for 18~24 min under Ar atmosphere; the carbonization product is dispersed in 0.3 mol / L NH3·H2O solution at a ratio of 0.002~0.008 g / mL to obtain a mixture; H2O2 solution with a mass percentage concentration of 30% is added to the mixture at a volume ratio of NH3·H2O solution to H2O2 solution of (10~25):1; after stirring and reacting at room temperature, it is filtered through a 0.22 μm microporous membrane, dialyzed through a dialysis bag with a molecular weight cutoff of 1000 Da, and concentrated and dried to obtain tobacco stem-based BCDs.

5. The tobacco rod base BCDs / In2Se3 / WO according to claim 3 3-x The method for preparing ternary composite photothermal catalytic materials is characterized by... In step (2), the oxygen-rich vacancy WO 3-x The preparation method is as follows: Tungstate is dissolved in water at a ratio of 0.01~0.05 mol / L, citric acid and glucose are added sequentially, and the mixture is stirred until homogeneous to obtain a homogeneous solution. The molar ratio of tungstate, citric acid and glucose in the homogeneous solution is (1~4):(1~3):(2~6). Concentrated hydrochloric acid is added dropwise to the homogeneous solution at a ratio of 0.5~3 mL of 12 mol / L concentrated hydrochloric acid per 1 mmol of tungstate. After ultrasonic treatment, the homogeneous solution undergoes a first microwave reaction to prepare the WO3 precursor. Subsequently, the WO3 precursor is dissolved in an organic solvent to obtain a 0.01~0.025 mol / L precursor solution. An aqueous solution of 0.0045~0.009 g / mL is added dropwise to the precursor solution at a volume ratio of (4~10):

1. After ultrasonic treatment, the homogeneous solution undergoes a second microwave reaction to obtain oxygen-rich vacancy WO3. 3-x .

6. The tobacco stem base BCDs / In2Se3 / WO according to claim 5 3-x The method for preparing ternary composite photothermal catalytic materials is characterized by: In step (2), the conditions for the first microwave reaction are: temperature 100~160 ℃, power 200~800W, and time 1~3 h; the conditions for the second microwave reaction are: temperature 160~200 ℃, power 200~800 W, and time 1~3 h.

7. The tobacco rod base BCDs / In2Se3 / WO according to claim 3 3-x The method for preparing ternary composite photothermal catalytic materials is characterized by... In step (3), the solid-liquid ratio of the selenium source to the reducing agent is 0.009~0.047 g / mL.

8. The tobacco rod base BCDs / In2Se3 / WO according to claim 3 3-x The method for preparing ternary composite photothermal catalytic materials is characterized by... In step (4), the pre-reaction is a water bath heating reaction with a temperature of 60~120 ℃ and a time of 15~60 min; the microwave-assisted solvothermal reaction has a temperature of 160~240 ℃, a power of 200~800 W, and a time of 60~150 min.

9. The tobacco rod base BCDs / In2Se3 / WO according to any one of claims 1 to 8 3-x Application of ternary composite photothermal catalytic materials in the degradation of organic pollutants.