A long acting shrinkage inhibiting permanent mold aluminum alloy feeding process

By using retractable vibration feeding pins and pulse injection feeding devices in the die-casting aluminum alloy process, combined with real-time monitoring and activation treatment, the problem of insufficient feeding in the hot spot area of ​​the casting is solved, achieving efficient densification and improved mechanical properties of the casting, which is suitable for the production of high-end precision aluminum alloy castings.

CN123060076APending Publication Date: 2026-11-10SHUNBO ALUMINUM ALLOY HUBEI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611402188.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-10
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing die-cast aluminum alloy feeding processes cannot accurately adapt to the dynamic solidification process in the hot spot region of the casting, resulting in insufficient filling of the feeding melt, failure to completely eliminate shrinkage defects, affecting the internal density and mechanical properties of the casting, and making it difficult to meet the production needs of high-end precision aluminum alloy castings.

Method used

By employing a retractable vibration feeding pin and a pulsed injection feeding device, the solid fraction in the hot spot region is monitored in real time, and the feeding, vibration, and pressurization parameters are adjusted in stages. Combined with reducing gas or plasma activation treatment, the solidification characteristics of the aluminum alloy melt are precisely matched, and the solidification shrinkage in the hot spot region is dynamically compensated.

Benefits of technology

It achieves efficient feeding in the hot spot area of ​​castings, completely solves the problem of poor fusion of feeding melt, improves the internal density and mechanical properties of castings, extends service life, and is suitable for the large-scale production of high-precision and high-reliability aluminum alloy die castings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123060076A_ABST
    Figure CN123060076A_ABST
Patent Text Reader

Abstract

The application discloses a long-acting anti-shrinkage die-casting aluminum alloy feeding process, and relates to the technical field of aluminum alloy die-casting forming. At least one retractable vibration feeding pin is arranged in the die-casting die corresponding to the hot spot region of a casting. The retractable vibration feeding pin is internally provided with an internal feeding runner, and one end of the internal feeding runner is communicated with a pulsating injection feeding device. The die-casting die cavity is filled with aluminum alloy melt, and the injection feeding is completed. The real-time solid phase fraction of the hot spot region is obtained. The application realizes adaptive feeding processing in the whole solidification process by monitoring the solid phase fraction of the hot spot region of the casting in real time, and precisely controlling the feeding, vibration and pressurizing parameters in stages. Through reduction gas or plasma activation treatment, the oxide film at the semi-solid feeding interface is effectively removed, the problem of poor fusion of the feeding melt is completely solved, and the material uniformity of the feeding region is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of aluminum alloy die casting technology, and in particular to a long-term shrinkage compensation process for die-cast aluminum alloys that effectively suppresses shrinkage cavities. Background Technology

[0002] Aluminum alloy die casting is a core process for manufacturing lightweight parts, widely used in automobiles, precision machinery, aerospace components, and many other fields. During the die casting process, as the molten aluminum alloy fills and solidifies, it shrinks due to the decrease in temperature. The hot spots of the casting solidify slowly and shrink significantly, and the surrounding molten metal cannot replenish the shrinkage in time, making it very easy to form shrinkage cavities and porosity defects.

[0003] Existing die-casting feeding processes mostly employ conventional pressure-holding feeding and simple melt injection feeding methods, resulting in a limited range of processes. Conventional feeding structures cannot accurately adapt to the dynamic solidification process in hot spots. A dense oxide film forms on the surface of the casting during the semi-solid forming stage, hindering the fusion of the feeding melt and the base melt, leading to insufficient filling by the feeding melt. Furthermore, traditional feeding processes cannot dynamically adjust feeding parameters based on the solidification changes of the casting, resulting in poor matching between feeding pressure, melt injection rhythm, and solidification shrinkage rate.

[0004] Most existing technologies can only achieve shallow feeding and cannot eliminate deep shrinkage defects in the hot spot area. After casting, the internal density is insufficient, and problems such as leakage and mechanical property degradation are prone to occur during long-term use. This greatly reduces the service life and finished product qualification rate of die-cast aluminum alloy castings, making it difficult to meet the high-quality forming production requirements of high-precision aluminum alloy castings. Summary of the Invention

[0005] To address the aforementioned technical problems, this invention provides a long-lasting shrinkage cavity suppression process for die-cast aluminum alloys. The technical solution is as follows: A long-term shrinkage cavity suppression process for die-cast aluminum alloys includes the following steps: Step 1: Set at least one retractable vibration feeding pin in the die casting mold corresponding to the hot spot area of ​​the casting. The retractable vibration feeding pin is provided with an internal feeding channel. One end of the internal feeding channel is connected to the pulse injection feeding device. Step 2: Fill the cavity of the die-casting mold with molten aluminum alloy and complete the injection molding process; Step 3: Obtain the real-time solid fraction in the hot spot region; Step 4: When the real-time solid fraction reaches the first solid fraction threshold, the retractable vibration compensation pin is retracted along the axis of the retractable vibration compensation pin, forming an annular compensation gap between the retractable vibration compensation pin and the hot spot area. Step 5: After forming the annular feeding gap, a reducing gas or plasma is introduced into the annular feeding gap through the internal feeding channel to activate the semi-solid surface in the annular feeding gap in order to remove the surface oxide film. Step 6: After activation treatment, start the pulse injection feeding device, and inject aluminum alloy melt of the same material as the casting into the annular feeding gap through the internal feeding channel, and apply axial vibration to the retractable vibration feeding pin. Step 7: When the real-time solid fraction reaches the intermediate solid fraction threshold, increase the frequency of axial vibration and the injection pressure of pulsating injection, so that the intermediate solid fraction threshold is greater than the first solid fraction threshold. Step 8: When the real-time solid fraction reaches the second solid fraction threshold, stop the pulsating injection and maintain the pressure of the retractable vibration feeding pin on the annular feeding gap until solidification is complete. The first solid phase fraction threshold, the intermediate solid phase fraction threshold, and the second solid phase fraction threshold increase sequentially.

[0006] Optionally, in step 1, the internal feeding channel includes a central hole arranged along the axis of the retractable vibrating feeding pin and a plurality of lateral outflow holes extending from the central hole to the outer wall of the retractable vibrating feeding pin; a heating element is provided in the internal feeding channel to ensure that the temperature of the internal feeding channel is not lower than the liquidus temperature of the aluminum alloy; the internal feeding channel is connected to a gas source switching device for switching between reducing gas or plasma and molten aluminum alloy.

[0007] Optionally, the reducing gas is a mixture of argon and hydrogen, wherein the hydrogen component is 2% to 10%; the reducing gas is introduced at a pressure of 0.1 MPa to 0.5 MPa, for a time of 0.5 s to 5 s, and at a flow rate of 50 mL / min to 200 mL / min; and the plasma is argon plasma.

[0008] Optionally, the first solid fraction threshold is 0.15 to 0.35; the retraction distance of the retractable vibration compensation pin is 0.3 to 3.0 mm, and the retraction speed is 0.05 to 1.0 mm / s; the time interval from the completion of the activation treatment to the start of pulse injection does not exceed 1 second.

[0009] Optionally, the axial vibration includes a first vibration stage and a second vibration stage; the first vibration stage starts when the real-time solid fraction reaches the first solid fraction threshold and ends when the real-time solid fraction reaches the intermediate solid fraction threshold, with a vibration frequency of 20Hz to 80Hz and an amplitude of 0.1mm to 0.5mm. The second vibration stage begins when the real-time solid fraction reaches the intermediate solid fraction threshold and ends when the real-time solid fraction reaches the second solid fraction threshold. The vibration frequency is 100Hz to 300Hz, and the amplitude is 0.02mm to 0.15mm. The intermediate solid fraction threshold is 0.55 to 0.75. The injection pressure of the pulsating injection is 2MPa to 8MPa in the first vibration stage and 10MPa to 30MPa in the second vibration stage.

[0010] Optionally, the average flow rate of the pulsating injection is equal to the solidification and shrinkage volume of the hot spot region per unit time; the waveform of the pulsating injection flow rate is a sine wave or a square wave, and the pulsation frequency is 1 / n of the axial vibration frequency of the corresponding vibration stage, where n is an integer from 1 to 10; the peak flow rate of the pulsating injection is 2 to 5 times the average flow rate.

[0011] Optionally, obtaining the real-time solid fraction at the center of the hot spot region includes: placing thermocouples near the center of the hot spot region to obtain the real-time temperature; establishing a mapping relationship between temperature and solid fraction using numerical simulation; and obtaining the real-time solid fraction based on the real-time temperature and the mapping relationship.

[0012] Optionally, when the casting has multiple hot spots, a retractable vibration feeding pin is set in each hot spot area; according to the order in which the real-time solid fraction of each hot spot area reaches the first solid fraction threshold, the corresponding retractable vibration feeding pin is activated in sequence to perform retraction, activation treatment, pulsating injection and axial vibration.

[0013] Optionally, the pulse injection feeding device includes a thermostatic quantitative injection cylinder and a servo valve. The thermostatic quantitative injection cylinder stores aluminum alloy melt of the same material as the casting, and the temperature of the aluminum alloy melt is 50-100°C higher than the liquidus of the aluminum alloy. The servo valve controls the melt outflow according to a preset pulse waveform.

[0014] Optionally, the second solid fraction threshold is 0.85 to 0.95; the holding pressure is 30 MPa to 50 MPa; during the holding pressure stage, the retractable vibration compensation pin can maintain a slight vibration with an amplitude of 0.01 mm to 0.05 mm and a frequency of 100 Hz to 200 Hz.

[0015] In summary, the present invention has at least one of the following beneficial technical effects: This invention provides a long-lasting feeding process for die-cast aluminum alloys that effectively suppresses shrinkage cavities. By real-time monitoring of the solid fraction in the hot spot region of the casting, feeding, vibration, and pressurization parameters are precisely controlled in stages to achieve adaptive feeding processing throughout the solidification process. Through activation treatment with reducing gas or plasma, the oxide film at the semi-solid feeding interface is effectively removed, completely solving the problem of poor melt fusion and ensuring material uniformity in the feeding area.

[0016] By adjusting the vibration frequency, amplitude, and pulsating injection pressure and flow rate in a gradient manner, the shrinkage characteristics of the aluminum alloy melt at different solidification stages are precisely matched, dynamically compensating for the solidification shrinkage volume in the hot spot region and significantly improving the feeding effect in the hot spot region of the casting. The process of holding pressure at the end combined with micro-amplitude vibration can completely seal the micro-pores generated at the end of solidification, effectively inhibiting the formation of shrinkage cavities and porosity defects in the casting.

[0017] It can be adapted to synchronous differentiated feeding of multi-heat-section castings, effectively improving the internal density and overall mechanical properties of die-cast aluminum alloy castings, increasing the finished product qualification rate and service stability, extending the service life of castings, and meeting the needs of large-scale production of high-precision and high-reliability aluminum alloy die-castings. Attached Figure Description

[0018] Figure 1 This is a schematic diagram of the process for a long-term suppression of shrinkage cavities in die-cast aluminum alloy feeding according to the present invention. Figure 2 This is a schematic diagram of the mapping relationship between the center temperature of the hot spot region and the solid fraction during the solidification process of a specific embodiment of the present invention. Detailed Implementation

[0019] The present invention will be further described in detail below with reference to the accompanying drawings.

[0020] This invention discloses a long-term shrinkage cavity suppression process for die-cast aluminum alloys.

[0021] Reference Figure 1 and Figure 2 Example 1: A long-term shrinkage cavity suppression process for die-cast aluminum alloys includes the following steps: Step 1: Set at least one retractable vibration feeding pin in the die casting mold corresponding to the hot spot area of ​​the casting. The retractable vibration feeding pin is provided with an internal feeding channel. One end of the internal feeding channel is connected to the pulse injection feeding device. Step 2: Fill the cavity of the die-casting mold with molten aluminum alloy and complete the injection molding process; Step 3: Obtain the real-time solid fraction in the hot spot region; Step 4: When the real-time solid fraction reaches the first solid fraction threshold, the retractable vibration compensation pin is retracted along the axis of the retractable vibration compensation pin, forming an annular compensation gap between the retractable vibration compensation pin and the hot spot area. Step 5: After forming the annular feeding gap, a reducing gas or plasma is introduced into the annular feeding gap through the internal feeding channel to activate the semi-solid surface in the annular feeding gap in order to remove the surface oxide film. Step 6: After activation treatment, start the pulse injection feeding device, and inject aluminum alloy melt of the same material as the casting into the annular feeding gap through the internal feeding channel, and apply axial vibration to the retractable vibration feeding pin. Step 7: When the real-time solid fraction reaches the intermediate solid fraction threshold, increase the frequency of axial vibration and the injection pressure of pulsating injection, so that the intermediate solid fraction threshold is greater than the first solid fraction threshold. Step 8: When the real-time solid fraction reaches the second solid fraction threshold, stop the pulsating injection and maintain the pressure of the retractable vibration feeding pin on the annular feeding gap until solidification is complete. The first solid phase fraction threshold, the intermediate solid phase fraction threshold, and the second solid phase fraction threshold increase sequentially.

[0022] By adopting the above technical solution, in step 1, at least one retractable vibration-assisted feeding pin is provided in the die-casting mold corresponding to the hot spot area of ​​the casting. This retractable vibration-assisted feeding pin has an internal feeding channel, one end of which is connected to a pulsed injection feeding device. The internal feeding channel runs through the pin body, serving both as a transport channel for reducing gas or plasma and as a feeding channel for the molten aluminum alloy, thus achieving two purposes in one hole. This avoids the structural complexity and reduced strength caused by opening multiple independent channels on the pin body.

[0023] Step 2: Fill the cavity of the die-casting mold with molten aluminum alloy and complete the injection filling. After filling, keep the injection punch stationary to maintain the initial static pressure in the cavity, providing a basic pressure environment for subsequent feeding.

[0024] Step 3: Obtain the real-time solid fraction in the hot spot region. The center of the hot spot region is where shrinkage cavities and porosity are most concentrated. The real-time solid fraction directly reflects the solidification process and feeding window status at this location. Only by accurately determining the solid fraction can the feeding action be initiated at the most appropriate time. Initiating it too early will result in an inability to establish an effective feeding pressure differential due to excessive liquid phase, while initiating it too late will result in the dendrite network being closed, and the feeding channel being irreversibly blocked.

[0025] Step 4: When the real-time solid fraction reaches the first solid fraction threshold, the retractable vibratory feeding pin is retracted along its axis, forming an annular feeding gap between the retractable vibratory feeding pin and the hot spot area. The first solid fraction threshold corresponds to the initial stage of solidification, at which point the center of the hot spot is still predominantly liquid, but the metal near the surface of the feeding pin has formed a semi-solid shell. The retraction action creates a controllable annular space between the pin and the semi-solid shell. This space serves as both the reaction zone for subsequent activation treatment and the containment space for the injected aluminum alloy melt. The retraction process requires precise control of distance and speed. Excessive retraction distance will damage the integrity of the semi-solid shell, while excessive retraction speed will generate negative pressure that draws in air.

[0026] Step 5: After forming the annular feeding gap, a reducing gas or plasma is introduced into the annular feeding gap through the internal feeding channel to activate the semi-solid surface within the gap and remove the surface oxide film. During die casting, aluminum alloy melt easily forms a dense alumina film on its surface. This oxide film severely hinders the metallurgical bonding between the subsequently injected feeding melt and the semi-solid matrix. Without activation, even if the feeding melt is injected into the gap, it can only exist as a mechanical filler and cannot form complete grain continuity with the matrix. A weak bonding interface remains in the feeding area after solidification, equivalent to embedding a metallurgical defect at the shrinkage cavity location. The reducing gas or plasma undergoes a chemical reaction on the semi-solid surface at high temperatures, reducing or decomposing the alumina and exposing fresh metal to the semi-solid surface. This ensures that the subsequently injected feeding melt can undergo sufficient atomic diffusion and grain epitaxial growth with the matrix.

[0027] Step 6: After activation, start the pulse injection feeding device. Pulsate aluminum alloy melt, identical to the casting material, is injected into the annular feeding gap through the internal feeding channel. Axial vibration is applied to the retractable vibratory feeding pin. After entering the annular feeding gap, the feeding melt, driven by both injection pressure and capillary action, penetrates into the liquid phase region and dendrite gaps within the hot spot area. The introduction of axial vibration causes the pin to apply periodic shear stress to the melt within the gap, reducing the apparent viscosity of the semi-solid slurry and making it easier for the feeding melt to flow into the narrow interdendritic channels. The essential difference between pulse injection and continuous injection is that pulse injection can generate peak pressures higher than the average pressure in a short time. These peak pressures can effectively overcome the surface tension and viscous resistance at the entrance of the interdendritic channels, while the average flow rate still matches the solidification shrinkage rate, avoiding over-injection that could cause localized bulging or coarsening of the microstructure.

[0028] Step 7: When the real-time solid fraction reaches the intermediate solid fraction threshold, increase the frequency of axial vibration and the injection pressure of pulsating injection. The intermediate solid fraction threshold is greater than the first solid fraction threshold, corresponding to the mid-to-late stage of solidification. At this time, a significant solid dendritic network has formed in the center of the hot spot region, and the liquid phase is separated in the dendritic interstices, rendering conventional feeding methods ineffective. The purpose of increasing the vibration frequency is to utilize the thixotropic thinning effect induced by high-frequency shear to cause local depolymerization and rearrangement of the dendritic network, temporarily opening the seepage channels. At the same time, increasing the injection pressure is to push the feeding melt into the depth with sufficient driving force within the time window when the seepage channels are open. The frequency is increased while the amplitude is decreased because the semi-solid slurry with a high solid fraction is more sensitive to small-amplitude high-frequency vibrations, and excessively large amplitudes may damage the already formed semi-solid skeleton.

[0029] Step 8: When the real-time solid fraction reaches the second solid fraction threshold, stop the pulsating injection and maintain the pressure applied to the annular feeding gap by the retractable vibrating feeding pin until solidification is complete. The second solid fraction threshold corresponds to the end of solidification. At this point, most of the center of the hot spot region has solidified, and the remaining liquid phase is distributed in isolated islands. Continuing to inject melt will not effectively penetrate and may even lead to local overpressure and microsegregation. The purpose of maintaining the pressure after stopping injection is to maintain the hydrostatic pressure in the annular feeding gap and prevent the injected feeding melt from flowing back due to the negative pressure generated by solidification shrinkage. The pressure holding stage continues until complete solidification to ensure that the feeding melt and the matrix solidify synchronously, forming a dense final structure.

[0030] The first solid fraction threshold, the intermediate solid fraction threshold, and the second solid fraction threshold increase sequentially, forming a complete feeding time series that covers the entire feeding window from the initial stage of solidification to the final stage of solidification.

[0031] In Example 2, step 1, the internal feeding channel includes a central hole along the axis of the retractable vibrating feeding pin and multiple lateral outflow holes extending from the central hole to the outer wall of the retractable vibrating feeding pin; a heating element is provided in the internal feeding channel to ensure that the temperature of the internal feeding channel is not lower than the liquidus temperature of the aluminum alloy; the internal feeding channel is connected to a gas source switching device for switching between reducing gas or plasma and molten aluminum alloy.

[0032] By adopting the above technical solution, the central hole serves as the main delivery channel, with its axis coinciding with the pin's axis. This minimizes the flow path within the pin and reduces pressure loss, while ensuring the pin's dynamic balance during retraction and vibration is unaffected by flow channel eccentricity. Lateral outlet holes are evenly distributed along the pin's circumference, ranging from 4 to 12 in number, with diameters from 0.5 to 2.0 mm. The outlets of these lateral outlet holes are located on the outer wall of the pin, near the front end, allowing reducing gas and feeding melt to directly enter the annular feeding gap. The outlet direction forms a 0°–45° angle with the pin's radial direction to guide the fluid deeper into the hot spot region.

[0033] The internal feeding channel is equipped with a heating element, which is a resistance wire or induction coil, embedded in the wall of the central hole or wound around the outside of the pin near the channel. The heating element ensures that the temperature of the internal feeding channel is always above the liquidus temperature of the aluminum alloy, preventing the molten aluminum alloy from solidifying and blocking the channel. Although the molten aluminum alloy spends only a short time in the channel, if the channel temperature falls below the liquidus, the boundary layer of the melt on the channel wall will solidify rapidly, forming a gradually thickening solidified shell, eventually reducing the effective cross-sectional area of ​​the channel or even causing complete blockage. The continuous operation of the heating element ensures that the channel wall temperature remains above the liquidus, keeping the melt completely liquid within the channel.

[0034] The internal feeding channel is connected to a gas source switching device, which switches between reducing gas or plasma and molten aluminum alloy. The gas source switching device includes a three-way valve or two parallel shut-off valves, one end connected to the inlet of the internal feeding channel, and the other end connected to the gas source and the pulse injection feeding device, respectively. During the activation treatment stage, the gas source switching device connects the internal feeding channel to the gas source while simultaneously cutting off the connection to the pulse injection feeding device; during the pulse injection stage, the gas source switching device connects the internal feeding channel to the pulse injection feeding device while simultaneously cutting off the connection to the gas source. The switching action is automatically triggered by the control system based on the real-time solid phase fraction, with a switching time not exceeding 0.1 seconds, to ensure a tight time connection between the activation treatment and pulse injection, preventing the semi-solid surface from being exposed for too long in the gap and re-oxidizing.

[0035] The gas source switching device is also equipped with an exhaust bypass, which is used to discharge residual gas or melt in the flow channel during the switching process to prevent the two media from mixing in the flow channel and causing defects.

[0036] In Example 3, the reducing gas was a mixture of argon and hydrogen, with hydrogen comprising 2% to 10% of the total gas volume; the reducing gas was introduced at a pressure of 0.1 MPa to 0.5 MPa for 0.5 s to 5 s for 5 s and at a flow rate of 50 mL / min to 200 mL / min; and the plasma was argon plasma.

[0037] By employing the above technical solution, the reducing gas is a mixture of argon and hydrogen, with hydrogen comprising 2%–10%. Argon serves as both a carrier gas and a diluent, and its chemical inertness ensures it does not react with the molten aluminum alloy or mold materials at high temperatures. Hydrogen, as the active component, possesses extremely strong reducing properties at high temperatures and can reduce the alumina on the aluminum alloy surface. Alumina has an extremely low formation free energy and is very difficult to reduce under standard conditions. However, under high temperatures and a hydrogen atmosphere, hydrogen molecules undergo chemical adsorption on the alumina surface, disrupting the continuity of the oxide film by generating water vapor and low-valence aluminum oxides. When the hydrogen component is below 2%, the reduction reaction rate is too low, and the oxide film cannot be effectively removed within the limited activation treatment time. When the hydrogen component is above 10%, excess hydrogen may be absorbed by the semi-solid matrix, forming porosity defects after solidification. Controlling the hydrogen component between 2% and 10% achieves a balance between activation effectiveness and the risk of residual gas.

[0038] The reducing gas is introduced at a pressure of 0.1 MPa to 0.5 MPa. If the pressure is too low, the gas cannot effectively penetrate the semi-solid surface boundary layer within the annular feeding gap, and the activation treatment only remains on the macroscopic surface, resulting in insufficient effectiveness. If the pressure is too high, the gas may be forced into the interior of the semi-solid slurry, forming cavitation in the dendrite interstices. Subsequent pulsed injection of melt cannot completely expel the gas, ultimately forming diffuse pores within the feeding region. Within the pressure range of 0.1 MPa to 0.5 MPa, the gas flows through the annular feeding gap in a stable laminar or slightly turbulent state, ensuring sufficient contact and reaction with the semi-solid surface without penetrating too deeply into the dendrite interstices.

[0039] The reduction gas introduction time is 0.5s to 5s. If the introduction time is too short, the oxide film reduction reaction will be incomplete. If the introduction time is too long, the semi-solid surface will be continuously exposed at high temperatures. Although the oxide film is removed, alloying elements in the matrix, such as magnesium and zinc, may selectively evaporate, leading to changes in surface composition and affecting the bonding between the feeding melt and the matrix. Within the time range of 0.5s to 5s, the oxide film can be effectively removed while keeping surface composition changes within an acceptable range.

[0040] The gas flow rate is 50 mL / min to 200 mL / min. The gas flow rate, the introduction time, and the gap volume together determine the residence time and turnover rate of the gas in the gap. If the flow rate is too low, the turnover rate of the gas in the gap is low, and the byproducts generated by the activation reaction cannot be discharged in time. If the flow rate is too high, the gas velocity is too high, which may have a cooling effect on the semi-solid surface.

[0041] The plasma is argon plasma. Under discharge conditions, argon plasma generates high-energy argon ions and electrons. These high-energy particles bombard the semi-solid surface, removing the oxide film through a combination of physical sputtering and chemical activation. Argon plasma does not contain hydrogen, making it suitable for aluminum alloy grades sensitive to hydrogen embrittlement.

[0042] In Example 4, the first solid fraction threshold is 0.15 to 0.35; the retraction distance of the retractable vibration compensation pin is 0.3 to 3.0 mm, and the retraction speed is 0.05 to 1.0 mm / s; the time interval between the completion of the activation treatment and the start of the pulse injection does not exceed 1 second.

[0043] By adopting the above technical solution, the first solid fraction threshold is 0.15–0.35. The physical significance of this range is that the center of the hot spot region is in a semi-solid slurry state within this solid fraction range; the solid particles have not yet formed a continuous network, and there are still a large number of interconnected liquid phase channels. When the feeding action is initiated at this time, the feeding melt can flow into the depth of the hot spot along the interconnected liquid phase channels, with minimal feeding resistance. If the first solid fraction threshold is below 0.15, the liquid phase ratio at the center of the hot spot is too high, making it difficult to establish fluid pressure within the annular feeding gap formed by the pullback. The injected feeding melt will be diluted by a large amount of liquid phase, resulting in an insignificant feeding effect. If the first solid fraction threshold is above 0.35, the solid particles have begun to form a continuous network, partially blocking the feeding channels, and significantly reducing the effective penetration depth of the feeding melt. Setting the first solid fraction threshold between 0.15 and 0.35 ensures that feeding is initiated while the feeding channels are still unobstructed, and that the liquid phase ratio has been reduced to a level sufficient to establish an effective feeding pressure differential.

[0044] The retraction distance of the retractable vibration-assisted feeding pin is 0.3–3.0 mm. This retraction distance determines the volume of the annular feeding gap. If the retraction distance is less than 0.3 mm, the gap volume is too small, preventing the reducing gas from flowing sufficiently within the gap, resulting in poor activation treatment and insufficient space for the feeding melt. If the retraction distance is greater than 3.0 mm, the gap volume is too large, leading to an excessively long flow path for the feeding melt within the gap, significant pressure attenuation, and obvious feeding marks after the semi-solid matrix solidifies, increasing subsequent processing workload. Within the retraction distance range of 0.3–3.0 mm, the gap volume matches the solidification shrinkage of the hot spot region, allowing both activation treatment and pulsed injection to be effectively performed under appropriate pressure.

[0045] The retraction speed is 0.05–1.0 mm / s. If the retraction speed is too slow, the feeding window is compressed, reducing the available time for activation treatment and pulse injection. If the retraction speed is too fast, the pin exerts a sudden tensile force on the semi-solid matrix, which may lead to matrix cracking or irregular gap shape. Within the retraction speed range of 0.05–1.0 mm / s, the pin smoothly detaches from the semi-solid surface, and the gap formation process is controllable.

[0046] The time interval between the completion of the activation treatment and the start of pulse injection should not exceed 1 second. The physical significance of this time interval is that after the activation treatment removes the oxide film, the semi-solid surface is exposed to a high-temperature environment. If the interval is too long, the surface will rapidly re-oxidize. Although the die-casting mold cavity may have been evacuated before filling or filled with a protective atmosphere during the filling process, the reaction rate between the semi-solid surface and trace amounts of oxygen is still very high at high temperatures. By controlling the time interval to within 1 second, the thickness of the re-oxidized film becomes negligible, and the feeding melt can achieve good metallurgical bonding with the activated surface.

[0047] Example 5: Axial vibration includes a first vibration stage and a second vibration stage; the first vibration stage begins when the real-time solid fraction reaches the first solid fraction threshold and ends when the real-time solid fraction reaches the intermediate solid fraction threshold, with a vibration frequency of 20Hz to 80Hz and an amplitude of 0.1mm to 0.5mm. The second vibration stage begins when the real-time solid fraction reaches the intermediate solid fraction threshold and ends when the real-time solid fraction reaches the second solid fraction threshold. The vibration frequency is 100Hz to 300Hz, and the amplitude is 0.02mm to 0.15mm. The intermediate solid fraction threshold is 0.55 to 0.75. The injection pressure of the pulsating injection is 2MPa to 8MPa in the first vibration stage and 10MPa to 30MPa in the second vibration stage.

[0048] By adopting the above technical solution, the first vibration stage begins when the real-time solid fraction reaches the first solid fraction threshold and ends when the real-time solid fraction reaches the intermediate solid fraction threshold. The vibration frequency of the first vibration stage is 20Hz to 80Hz, and the amplitude is 0.1mm to 0.5mm. In the first vibration stage, the solid fraction at the center of the hot spot region is at a low level, the liquid phase ratio in the semi-solid slurry is high, and the dendritic network has not yet formed. The purpose of applying low-frequency large-amplitude vibration at this time is to promote the macroscopic flow and uniform distribution of the feeding melt in the annular feeding gap, while removing any residual air bubbles in the gap through mechanical vibration. Low-frequency large-amplitude vibration produces a strong macroscopic stirring effect on the semi-solid slurry, which helps to mix the feeding melt with the matrix liquid phase. However, if the frequency is too low or the amplitude is too large, it will cause the mold vibration transmission and the surface quality of the casting to decrease; if the frequency is too high or the amplitude is too small, it will be difficult to produce a sufficient stirring effect.

[0049] The second vibration stage begins when the real-time solid fraction reaches the intermediate solid fraction threshold and ends when the real-time solid fraction reaches the second solid fraction threshold. The vibration frequency in the second stage is 100Hz–300Hz, and the amplitude is 0.02mm–0.15mm. During the second vibration stage, the solid fraction at the center of the hot spot region has entered a medium-to-high level, and the dendritic network forms and gradually densifies. The purpose of applying high-frequency micro-amplitude vibration at this time is to reduce the apparent viscosity between the dendritic networks using the shear thinning effect. High-frequency vibration generates periodic shear strain in the semi-solid slurry, causing shear flow of the liquid phase between the dendrite arms, local depolymerization of the dendritic network, and temporary opening of the seepage channels. Micro-amplitude vibration ensures that it does not cause destructive deformation to the already formed semi-solid framework, and high frequency ensures that a sufficient number of shear cycles are completed within the finite solidification time. The frequency range of 100Hz–300Hz corresponds to the thixotropic response time scale of the semi-solid aluminum alloy slurry; within this frequency range, the depolymerization and rearrangement rate of the dendritic network can keep up with the vibration frequency. If the frequency is higher than 300Hz, the vibrational energy decays too quickly in the slurry, resulting in insufficient effective depth of action. If the frequency is lower than 100Hz, the dendritic network has enough time to reconnect between two shear cycles, leading to a discontinuous thixotropic thinning effect.

[0050] The intermediate solids fraction threshold is 0.55–0.75. This range corresponds to the stage in the semi-solid slurry where the dendritic network has formed but is not yet fully closed. Switching vibration parameters at this stage allows for adjustments to the feeding strategy in response to the physical changes during solidification. When the intermediate solids fraction threshold is below 0.55, the dendritic network is not yet fully formed, making it unnecessary to increase frequency and pressure. When the intermediate solids fraction threshold is above 0.75, the dendritic network is already highly developed, and even increasing frequency and pressure will have extremely limited penetration ability of the feeding melt.

[0051] The injection pressure for pulsating injection is 2 MPa–8 MPa in the first vibration stage and 10 MPa–30 MPa in the second vibration stage. The injection pressure is lower in the first vibration stage because the feeding channels are unobstructed, and the low pressure is sufficient to drive the feeding melt to penetrate. Excessive pressure, especially in stages with a high liquid phase ratio, may lead to over-penetration of the feeding melt, causing localized mold bulging or microstructure coarsening. The injection pressure is significantly increased in the second vibration stage because the interdendritic channels are narrow, and capillary and viscous resistances increase sharply, requiring a higher driving force to push the feeding melt deeper. The pressure range of 10 MPa–30 MPa has been calculated and experimentally verified to effectively overcome seepage resistance in the presence of dendritic networks without exceeding the strength limit of the die-casting mold.

[0052] Example 6: The average flow rate of the pulsating injection is equal to the solidification and shrinkage volume of the hot spot region per unit time; the waveform of the pulsating injection flow rate is a sine wave or a square wave, and the pulsating frequency is 1 / n of the axial vibration frequency of the corresponding vibration stage, where n is an integer from 1 to 10; the peak flow rate of the pulsating injection is 2 to 5 times the average flow rate.

[0053] By employing the above technical solution, the average flow rate of the pulsed injection is equal to the solidification shrinkage volume of the hot spot region per unit time. The solidification shrinkage volume is obtained through solidification simulation calculations or experimental calibration; its physical meaning is the volume reduction in the hot spot region per unit time due to the liquid-to-solid phase transition. If the average flow rate is less than the solidification shrinkage volume, the feeding melt cannot completely fill the shrinkage space, and shrinkage cavities will still exist. If the average flow rate is greater than the solidification shrinkage volume, excessive feeding melt will create excessively high local pressure in the hot spot region, potentially leading to mold bulging or hot cracking in the later stages of solidification. Precise matching of the average flow rate and the solidification shrinkage volume ensures that the feeding process is carried out on the basis of volume equilibrium.

[0054] The flow waveform of the pulsed injection is either a sine wave or a square wave. A sine wave has a smooth flow rate change, causing minimal impact on the semi-solid slurry, making it suitable for the first vibration stage. A square wave has a rapid flow rate change between peaks and troughs, generating stronger pressure pulses, making it suitable for the second vibration stage. The high instantaneous flow rate change rate of the square wave generates a water hammer effect at the dendrite channel inlet, helping to overcome the surface tension barrier.

[0055] The pulsation frequency is one-nth of the axial vibration frequency of the corresponding vibration stage, where n is an integer from 1 to 10. This integer ratio between the pulsation frequency and the vibration frequency ensures that each pulsation cycle contains an integer number of vibration cycles, maintaining a stable phase relationship between vibration and injection in time. When n equals 1, the pulsation frequency is the same as the vibration frequency, and each vibration cycle corresponds to one flow fluctuation, with injection and vibration completely synchronized. When n equals 10, every 10 vibration cycles correspond to one flow fluctuation; vibration provides high-frequency shear thinning, while injection provides low-frequency feeding driving force. In engineering practice, the choice of the n value depends on the size of the hot spot region and the solidification rate; a larger hot spot region and a lower solidification rate are suitable for a larger n value.

[0056] The peak flow rate of pulsed injection is 2 to 5 times the average flow rate. The peak flow rate determines the amount of feed melt that can enter the interdendritic channels within a brief high-pressure window. If the peak flow rate is too low, the difference in effect between pulsed and continuous injection is not significant. If the peak flow rate is too high, it may generate local high-speed jets within the gaps, scouring the surface of the semi-solid matrix and destroying the already formed dendritic structure. Within the peak-to-average ratio range of 2 to 5 times, the pulsation effect is significant without producing destructive impact.

[0057] Example 7, obtaining the real-time solid fraction at the center of the hot spot region includes: placing thermocouples near the center of the hot spot region to obtain the real-time temperature; establishing a mapping relationship between temperature and solid fraction using numerical simulation; and obtaining the real-time solid fraction based on the real-time temperature and the mapping relationship.

[0058] By adopting the above technical solution, thermocouples are arranged near the center of the hot spot region. The thermocouples are inserted through pre-drilled mounting holes on the mold, with their measuring ends positioned at a predetermined location in the center of the hot spot region. The response time of the thermocouples should be less than 0.1 seconds to ensure real-time performance. High-temperature resistant sealing material is used to fill the space between the mold mounting holes and the thermocouples to prevent molten aluminum alloy from seeping in.

[0059] Numerical simulation is used to establish a mapping relationship between temperature and solid fraction. During the die-casting process development phase, numerical simulations of the solidification process are performed on the casting to obtain the temperature and solid fraction change curves at the center of the hot spot region throughout the solidification process. The temperature and solid fraction at the same moment are then correlated to establish a mapping relationship. This mapping relationship can be represented using a lookup table, polynomial fitting, or piecewise linear interpolation.

[0060] The real-time solid fraction is obtained based on the real-time temperature and mapping relationship. During the die-casting process, the control system reads the thermocouple temperature values ​​at a sampling frequency of no less than 10Hz and calculates the solid fraction in real time through the mapping relationship. When the calculated solid fraction reaches a preset threshold, the corresponding feeding action is triggered.

[0061] The advantage of this method is that thermocouple temperature measurement technology is mature and reliable, the numerical simulation mapping relationship can be repeatedly calibrated during the process development stage, and in actual production, only real-time temperature data is needed to obtain the solid phase fraction, without the need for complex online solidification calculations.

[0062] Example 8: When the casting has multiple hot spots, a retractable vibration feeding pin is set in each hot spot area; according to the order in which the real-time solid fraction of each hot spot area reaches the first solid fraction threshold, the corresponding retractable vibration feeding pin is activated in sequence to perform retraction, activation treatment, pulsating injection and axial vibration.

[0063] By adopting the above technical solution, when the casting has multiple hot spots, a retractable vibratory feeding pin is installed in each hot spot area. Each feeding pin is independently equipped with an internal feeding channel, an axial vibrator, and a retraction drive mechanism. The pulsating injection feeding devices of each feeding pin can share a centralized feeding system, but the flow rate and pressure of each feeding pin are independently controlled.

[0064] Based on the order in which the real-time solids fraction of each hot spot region reaches the first solids fraction threshold, the corresponding retractable vibration-assisted feeding pins are sequentially activated for retraction, activation treatment, pulsating injection, and axial vibration. The solidification process varies among hot spot regions; the thicker the wall and the worse the heat dissipation, the slower the solids fraction rises, and the later it reaches the first solids fraction threshold. Feeding actions are activated sequentially according to time sequence to ensure that each hot spot region receives feeding within its own feeding window, avoiding premature or delayed feeding caused by simultaneous activation.

[0065] When multiple feeding pins are simultaneously in the activation treatment or pulsating injection stage, the centralized feeding system distributes the melt according to the average flow rate required by each feeding pin, and the servo valve controls the pulsating waveform of each branch to ensure that each hot spot area simultaneously obtains a feeding flow rate that matches its solidification shrinkage rate.

[0066] The control system independently monitors and determines the solid fraction of each hot spot region, and the triggering conditions do not interfere with each other. When one hot spot region has entered the pressure holding stage, another hot spot region may have just started the retraction action, and each feeding pin operates independently according to its own feeding sequence.

[0067] Example 9: The pulsed injection feeding device includes a thermostatic quantitative injection cylinder and a servo valve. The thermostatic quantitative injection cylinder stores aluminum alloy melt of the same material as the casting. The temperature of the aluminum alloy melt is 50-100°C higher than the liquidus of the aluminum alloy. The servo valve controls the melt outflow according to a preset pulsed waveform.

[0068] By adopting the above technical solution, the isothermal quantitative injection cylinder stores molten aluminum alloy of the same material as the casting. The outer wall of the cylinder is equipped with a heating jacket, and an internal temperature sensor is installed. Closed-loop control maintains the temperature of the molten material within the cylinder consistently within the range of 50–100°C above the liquidus line of the aluminum alloy. Maintaining a temperature 50°C above the liquidus line ensures that the molten material retains sufficient superheat and fluidity as it flows through the internal feeding channel into the annular feeding gap. Maintaining a temperature not exceeding 100°C above the liquidus line prevents excessive oxidation and gas absorption of the molten material, while also reducing corrosion of the cylinder material.

[0069] The piston of the thermostatic quantitative injection cylinder is driven by a servo motor or hydraulic servo system, with a piston displacement accuracy of no less than 0.01 mm, enabling the injection cylinder to accurately output the amount of melt that matches the solidification shrinkage volume. The volume of the injection cylinder is determined based on the maximum solidification shrinkage volume in the hot spot region, with a margin of more than 20%.

[0070] The servo valve controls the melt flow according to a preset pulsating waveform. The servo valve is installed on the connecting pipe between the thermostatic metering injection cylinder and the internal compensation channel. Its valve core position is adjusted in real time by the control system based on the preset pulsating waveform. The servo valve's response frequency is no less than 500Hz to ensure accurate reproduction of pulsating flow waveforms up to 300Hz. The valve body and valve core are made of high-temperature resistant alloy, and a heating channel is provided within the valve body to prevent the melt from solidifying inside the valve cavity.

[0071] The connecting pipeline between the pulse injection feeding device and the internal feeding channel is insulated throughout, and the inner wall of the pipeline is equipped with heating elements to maintain the temperature at 50°C above the liquidus line, ensuring that the melt does not solidify during the transportation process.

[0072] In Example 10, the second solid fraction threshold is 0.85 to 0.95; the holding pressure is 30 MPa to 50 MPa; during the holding pressure stage, the retractable vibration compensation pin can maintain a slight vibration with an amplitude of 0.01 mm to 0.05 mm and a frequency of 100 Hz to 200 Hz.

[0073] By adopting the above technical solution, the second solid fraction threshold is 0.85–0.95. When the solid fraction reaches 0.85, the dendritic network at the center of the hot spot region is already highly dense, and the remaining liquid phase exists in the dendritic interstices as isolated islands and thin films. The seepage resistance for feeding through external injection of melt is already extremely high, and the actual feeding effect of continued injection is negligible. When the solid fraction reaches above 0.95, the remaining liquid phase is extremely small, and the solidification process is basically complete. Setting the second solid fraction threshold between 0.85 and 0.95 ensures that the pulsed injection continues before it truly loses its feeding ability, making full use of the last effective stage of the feeding window, while stopping all external actions after complete solidification.

[0074] The holding pressure is 30MPa to 50MPa. After stopping the pulsating injection during the holding phase, sufficient static pressure needs to be maintained between the feeding pin and the feeding melt within the annular feeding gap. A holding pressure of 30MPa to 50MPa can counteract the negative pressure generated in the gap due to volume shrinkage at the end of solidification, preventing backflow of the feeding melt and ensuring that the feeding melt maintains close contact with the semi-solid matrix throughout the solidification process. When the pressure is below 30MPa, the tensile stress generated by the contraction of the dendrite network at the end of solidification may cause a small separation gap between the feeding melt and the matrix. When the pressure is above 50MPa, the mold and feeding pin need to withstand a higher stress level, placing higher demands on the strength and service life of the mold material.

[0075] During the holding pressure stage, the vibrating feeding pin can be retracted to maintain a slight vibration, with an amplitude of 0.01mm to 0.05mm and a frequency of 100Hz to 200Hz. The slight vibration during the holding pressure stage is fundamentally different in function from the vibration in the second vibration stage. The high-frequency vibration in the second stage primarily aims to open the interdendritic flow channels and promote the penetration of the feeding melt. The slight vibration during the holding pressure stage primarily aims to prevent the feeding melt from forming a static solidified shell within the gap, maintaining the fluidity and pressure transmission capacity of the melt within the gap. The amplitude of the slight vibration is much smaller than that in the second vibration stage because the semi-solid matrix is ​​nearly completely solidified at this point, and an excessively large amplitude could cause cracking at the solidification front. The frequency is maintained in a relatively high range of 100Hz to 200Hz to ensure sufficient shear force is generated to maintain the fluidity of the melt within the gap even with a limited vibration amplitude. The holding pressure stage continues until the center of the hot spot region is completely solidified, then vibration and holding pressure are stopped, and preparations are made to open the mold and remove the casting.

[0076] The implementation principle of the present invention is illustrated below through specific embodiments: A certain type of automotive engine mount bracket, made of ADC12 aluminum alloy, has casting dimensions of approximately 200mm × 150mm × 80mm and a main body wall thickness of 4mm. The bracket has two mounting bosses, each 30mm in diameter and 18mm in height. The connection point between the boss and the main body is a typical thick, hot spot area with a hot spot modulus of approximately 0.45cm. During die casting, this hot spot area is far from the ingate, and the feeding channel is cut off by the thin-walled main body in the early stages of solidification. Traditional processes struggle to effectively feed this hot spot, resulting in shrinkage cavities and porosity defects concentrated in the center of the boss.

[0077] The process implementation steps of this invention are as follows: Step 1: Thermal analysis and mold design; Numerical simulations of the solidification process of the suspension bracket were performed to obtain the solid fraction variation curves of the hot spot center of the two mounting bosses over time. The simulation results show that the solid fraction of the hot spot center reaches 0.20 in about 2.5s after filling, 0.65 in about 5.8s, and 0.90 in about 8.2s.

[0078] Two retractable vibration-assisted feeding pins are installed at the center of each mounting boss hot spot in the die-casting mold. Each feeding pin has a diameter of 8mm and an internal feeding channel consisting of a central hole along the axis and eight lateral outlet holes, each 0.8mm in diameter. The outlet direction forms a 15° angle with the radial direction of the pin, pointing towards the depth of the hot spot. A resistance wire heating element is installed within the internal feeding channel, and the channel temperature is controlled at 620℃, approximately 40℃ higher than the liquidus temperature of ADC12. The internal feeding channel is connected to an argon-hydrogen mixed gas source and a pulsed injection feeding device via a gas source switching device. The pulsed injection feeding device includes a thermostatic metering injection cylinder and a servo valve. The injection cylinder stores molten ADC12 aluminum alloy, and the melt temperature is controlled at 680℃.

[0079] Step 2: Die casting filling; The die-casting mold cavity is pre-evacuated to below 5 kPa to create a vacuum die-casting environment. A cold chamber die-casting machine is used to complete the filling process with an injection pressure of 75 MPa and an injection speed of 3.5 m / s. After filling, the injection punch is kept stationary.

[0080] Step 3: Real-time solid fraction acquisition; A type K thermocouple is pre-embedded in the mold at the center of each hot spot corresponding to a boss. The thermocouple response time is 0.05s. The control system reads the thermocouple temperature values ​​at a sampling frequency of 20Hz and calculates the solid fraction at the center of the hot spot in real time using a pre-established mapping relationship between temperature and solid fraction. The mapping relationship is calibrated jointly by solidification simulation results and differential scanning calorimetry.

[0081] Figure 2 This is a curve showing the mapping relationship between the center temperature of the hot spot region and the solid fraction during the solidification process of ADC12 aluminum alloy. The horizontal axis represents temperature in °C, and the vertical axis represents the solid fraction, ranging from 0 to 1. The curve is S-shaped, with the solid fraction approaching 0 above the liquidus line at 580 °C, approaching 1 below the solidus line at 520 °C, and smoothly increasing with decreasing temperature in the intermediate temperature range. This mapping relationship was calibrated using a combination of solidification numerical simulation and differential scanning calorimetry, and is used to calculate the real-time solid fraction at the center of the hot spot based on the real-time temperature of the thermocouple during the die-casting process.

[0082] Step 4: Retraction and activation treatment; When the real-time solid fraction at the center of the hot spot on the boss reaches 0.20, the control system triggers the corresponding retractable vibration-assisted feeding pin to retract. The retraction distance is 1.5 mm, and the retraction speed is 0.3 mm / s. After the retraction is completed, an annular feeding gap is formed between the feeding pin and the hot spot area.

[0083] The gas source switching device immediately switches to the gas source channel, introducing a mixture of argon and hydrogen into the annular feeding gap through the internal feeding channel. The hydrogen component is 5%, the injection pressure is 0.3 MPa, the gas flow rate is 120 mL / min, and the injection time is 2 s. The mixed gas activates the semi-solid surface within the gap, removing the alumina film. After activation, the gas source switching device switches to the pulsed injection channel within 0.08 s, with a time interval of 0.5 s, less than 1 s.

[0084] Step 5: First stage of shrinkage repair; Start the pulsating injection compensation device and axial vibrator. The first vibration stage has a frequency of 40Hz and an amplitude of 0.3mm. The pulsating injection uses a sinusoidal waveform, with an average injection pressure of 5MPa and an average flow rate equal to the solidification shrinkage volume per unit time in the hot spot region of the boss, calculated through solidification simulation to be 0.35cm³ / s. The pulsating frequency is 1 / 4 of the vibration frequency, i.e., 10Hz, and the peak flow rate is 3 times the average flow rate, i.e., 1.05cm³ / s.

[0085] Step 6: Second stage of shrinkage repair; When the real-time solid fraction at the center of the hot spot reaches 0.65, the control system automatically switches to the second vibration stage. The vibration frequency increases to 180Hz, and the amplitude decreases to 0.06mm. The pulsating injection pressure increases to 25MPa, the pulsating frequency is adjusted to 45Hz, and the peak flow rate is four times the average flow rate. The second vibration stage continues until the solid fraction reaches 0.90.

[0086] Step 7: Pressure holding and solidification completed; When the solid fraction at the center of the hot spot reaches 0.90, stop the pulsed injection. Maintain a holding pressure of 40 MPa on the annular feeding gap using the feeding pin, while simultaneously maintaining micro-vibration at a frequency of 150 Hz and an amplitude of 0.03 mm. Continue the holding pressure phase until the center of the hot spot is completely solidified, lasting approximately 1.5 seconds.

[0087] Step 8: Reset and Post-processing; After solidification, the retraction drive mechanism completely retracts the feeding pin, allowing the mold to be opened and the casting removed. Residual metal in the feeding channel is removed, the condition of the feeding pin tip is inspected, and a new lubricant layer is applied.

[0088] Comparative Examples of Traditional Processes: Traditional processes employ vacuum die casting combined with localized extrusion pins. The die casting mold cavity is pre-vacuumed to below 5 kPa, with an injection pressure of 75 MPa and an injection speed of 3.5 m / s. Solid extrusion pins, 8 mm in diameter, are placed at the hot spots of two mounting bosses. After filling, the extrusion pins are activated 3 seconds later, with an extrusion stroke of 2 mm and an extrusion pressure of 60 MPa. The extrusion pins are held until solidification is complete. Traditional processes do not include internal feeding channels, activation treatment, pulsating injection, or axial vibration.

[0089] Twenty suspension brackets were produced using both processes, and the two mounting boss areas of each casting were inspected.

[0090] Shrinkage and porosity were detected using X-ray computed tomography. The shrinkage level of the central area of ​​the boss was rated according to the ASTM E505 standard. The average and maximum shrinkage levels of 40 bosses in 20 castings were statistically analyzed.

[0091] Density testing was performed using Archimedes' displacement method. A 10mm×10mm×10mm sample was cut from the center of the boss, the actual density was measured, and compared with the theoretical density of ADC12 aluminum alloy (2.70g / cm³) to calculate the density percentage.

[0092] For mechanical property testing, tensile specimens are cut axially from the boss area. The specimen diameter is 6 mm and the gauge length is 30 mm. The room temperature tensile test is carried out according to GB / T228.1 standard to determine the tensile strength and elongation.

[0093] Metallographic analysis involved grinding and polishing the central part of the boss, etching it with a 0.5% hydrofluoric acid aqueous solution, observing the morphology of the shrinkage cavities and the microstructure under an optical microscope, and measuring the spacing between the secondary dendrite arms.

[0094] The test results are compared in Table 1: Table 1 The shrinkage cavity defect rate refers to the percentage of bosses with shrinkage cavities exceeding grade 2 detected in the central area of ​​the boss, out of the total number of bosses detected.

[0095] The comparative results show that the feeding effect of the process of this invention in the hot spot area of ​​the mounting boss of the suspension bracket is significantly better than that of the traditional vacuum die casting process combined with local extrusion pins. The average shrinkage cavity grade of the boss is reduced from 3.5 to 0.5, the maximum shrinkage cavity grade is reduced from 5 to 1, the density of the boss center is increased from 96.2% to 99.6%, and the shrinkage cavity defect rate is reduced from 85% to 5%. The average tensile strength is increased by 39 MPa, the average elongation is increased by 1.7 percentage points, and the secondary dendrite arm spacing is refined from 18 μm to 14 μm. In the traditional process, the solid extrusion pin can only compact a limited area around the pin body and cannot replenish the aluminum alloy melt to the depth of the hot spot. Moreover, the extrusion pin action time is fixed and cannot adapt to the real-time changes in the solidification process. This invention uses a retractable vibrating feeding pin to form an annular feeding gap, removes the oxide film through activation treatment with reducing gas, and then pulses in a molten aluminum alloy of the same composition. As the solid fraction increases, the vibration frequency and injection pressure are increased, allowing the feeding melt to continuously penetrate into the interdendritic channels until the solid fraction reaches 0.90. This achieves long-term feeding of thick, hot-nodule regions and significantly inhibits the formation of shrinkage cavities and porosity.

[0096] The above are all preferred embodiments of the present invention and are not intended to limit the scope of protection of the present invention. Therefore, all equivalent changes made in accordance with the structure, shape and principle of the present invention should be covered within the scope of protection of the present invention.

Claims

1. A long-term shrinkage cavity suppression process for die-cast aluminum alloys, characterized in that, Includes the following steps: Step 1: Set at least one retractable vibration feeding pin in the die casting mold corresponding to the hot spot area of ​​the casting. The retractable vibration feeding pin is provided with an internal feeding channel. One end of the internal feeding channel is connected to the pulse injection feeding device. Step 2: Fill the cavity of the die-casting mold with molten aluminum alloy and complete the injection molding process; Step 3: Obtain the real-time solid fraction in the hot spot region; Step 4: When the real-time solid fraction reaches the first solid fraction threshold, the retractable vibration compensation pin is retracted along the axis of the retractable vibration compensation pin, forming an annular compensation gap between the retractable vibration compensation pin and the hot spot area. Step 5: After forming the annular feeding gap, a reducing gas or plasma is introduced into the annular feeding gap through the internal feeding channel to activate the semi-solid surface in the annular feeding gap in order to remove the surface oxide film. Step 6: After activation treatment, start the pulse injection feeding device, and inject aluminum alloy melt of the same material as the casting into the annular feeding gap through the internal feeding channel, and apply axial vibration to the retractable vibration feeding pin. Step 7: When the real-time solid fraction reaches the intermediate solid fraction threshold, increase the frequency of axial vibration and the injection pressure of pulsating injection, so that the intermediate solid fraction threshold is greater than the first solid fraction threshold. Step 8: When the real-time solid fraction reaches the second solid fraction threshold, stop the pulsating injection and maintain the pressure of the retractable vibration feeding pin on the annular feeding gap until solidification is complete. The first solid phase fraction threshold, the intermediate solid phase fraction threshold, and the second solid phase fraction threshold increase sequentially.

2. The die-cast aluminum alloy feeding process for long-term suppression of shrinkage cavities according to claim 1, characterized in that, In step 1, the internal feeding channel includes a central hole along the axis of the retractable vibrating feeding pin and multiple lateral outflow holes extending from the central hole to the outer wall of the retractable vibrating feeding pin; a heating element is provided in the internal feeding channel to ensure that the temperature of the internal feeding channel is not lower than the liquidus temperature of the aluminum alloy; the internal feeding channel is connected to a gas source switching device for switching between reducing gas or plasma and molten aluminum alloy.

3. The die-cast aluminum alloy feeding process for long-term suppression of shrinkage cavities according to claim 2, characterized in that, The reducing gas is a mixture of argon and hydrogen, with hydrogen comprising 2% to 10% of the total gas content; the reducing gas is introduced at a pressure of 0.1 MPa to 0.5 MPa, for a duration of 0.5 s to 5 s, and at a flow rate of 50 mL / min to 200 mL / min; the plasma is argon plasma.

4. The die-cast aluminum alloy feeding process for long-term suppression of shrinkage cavities according to claim 3, characterized in that, The first solid fraction threshold is 0.15 to 0.35; the retraction distance of the retractable vibration compensation pin is 0.3 to 3.0 mm, and the retraction speed is 0.05 to 1.0 mm / s; the time interval between the completion of the activation treatment and the start of the pulse injection does not exceed 1 second.

5. The die-cast aluminum alloy feeding process for long-term suppression of shrinkage cavities according to claim 4, characterized in that, Axial vibration includes a first vibration stage and a second vibration stage; the first vibration stage begins when the real-time solid fraction reaches the first solid fraction threshold and ends when the real-time solid fraction reaches the intermediate solid fraction threshold, with a vibration frequency of 20Hz to 80Hz and an amplitude of 0.1mm to 0.5mm. The second vibration stage begins when the real-time solid fraction reaches the intermediate solid fraction threshold and ends when the real-time solid fraction reaches the second solid fraction threshold. The vibration frequency is 100Hz to 300Hz, and the amplitude is 0.02mm to 0.15mm. The intermediate solid fraction threshold is 0.55 to 0.

75. The injection pressure of the pulsating injection is 2MPa to 8MPa in the first vibration stage and 10MPa to 30MPa in the second vibration stage.

6. The die-cast aluminum alloy feeding process for long-term suppression of shrinkage cavities according to claim 5, characterized in that, The average flow rate of the pulsating injection is equal to the solidification and shrinkage volume of the hot spot region per unit time; the waveform of the pulsating injection flow rate is a sine wave or a square wave, and the pulsation frequency is 1 / n of the axial vibration frequency of the corresponding vibration stage, where n is an integer from 1 to 10; the peak flow rate of the pulsating injection is 2 to 5 times the average flow rate.

7. The die-cast aluminum alloy feeding process for long-term suppression of shrinkage cavities according to claim 6, characterized in that, Obtaining the real-time solid fraction at the center of the hot spot region involves: placing thermocouples near the center of the hot spot region to obtain the real-time temperature; establishing a mapping relationship between temperature and solid fraction using numerical simulation; and obtaining the real-time solid fraction based on the real-time temperature and the mapping relationship.

8. The die-cast aluminum alloy feeding process for long-term suppression of shrinkage cavities according to claim 7, characterized in that, When the casting has multiple hot spots, a retractable vibration feeding pin is set in each hot spot area; according to the order in which the real-time solid fraction of each hot spot area reaches the first solid fraction threshold, the corresponding retractable vibration feeding pin is activated in sequence to perform retraction, activation treatment, pulsating injection and axial vibration.

9. The die-cast aluminum alloy feeding process for long-term suppression of shrinkage cavities according to claim 8, characterized in that, The pulse injection feeding device includes a thermostatic quantitative injection cylinder and a servo valve. The thermostatic quantitative injection cylinder stores aluminum alloy melt of the same material as the casting. The temperature of the aluminum alloy melt is 50-100°C higher than the liquidus of the aluminum alloy. The servo valve controls the melt outflow according to a preset pulse waveform.

10. The die-cast aluminum alloy feeding process for long-term suppression of shrinkage cavities according to claim 9, characterized in that, The second solid fraction threshold is 0.85 to 0.95; the holding pressure is 30 MPa to 50 MPa; during the holding pressure stage, the retractable vibration compensation pin can maintain a slight vibration with an amplitude of 0.01 mm to 0.05 mm and a frequency of 100 Hz to 200 Hz.