A method for replacing and repairing the edge plate of a sewage settling tank
By using expansion ring supports and increasing the thickness of the edge plates in the sewage settling tank, the problems of multiple support measures and low construction efficiency in edge plate replacement were solved, achieving efficient and safe edge plate replacement and reducing costs.
Patent Information
- Application Number
- CN202510593030.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-10
AI Technical Summary
The existing method for replacing the edge plates of sewage settling tanks requires a large number of support devices, which results in low construction efficiency and high cost, and the reduction in tank elevation poses a safety hazard.
The tank wall plates are supported by expansion rings, and the thickness of the edge plates is increased to compensate for cutting damage. Welding quality is ensured by water jet cutting, laser welding repair, and other technologies, combined with X-ray and penetrant testing.
It improved construction efficiency, reduced construction costs, ensured the safety and welding quality of the storage tank, and avoided the risk of the storage tank elevation being lowered.
Smart Images

Figure CN123060366A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of oil and gas field surface engineering, specifically a method for replacing and repairing the edge plate of a wastewater settling tank. Background Technology
[0002] Oil and gas field storage tanks are crucial containers for storing crude oil, oily wastewater, and other media. Due to condensation from oil storage and transfer processes, if not drained promptly, a water layer accumulates at the bottom, forming a layer of highly mineralized oily wastewater that causes electrochemical corrosion. Furthermore, this oily wastewater contains Cl- and SRB (sulfate-reducing bacteria), dissolved with harmful substances such as SO2, H2S, CO2, and O2, making the media at the bottom of the tank extremely corrosive. In addition, the fillet welds between the tank edge plates and the lowest ring plate are prone to stress corrosion cracking due to high welding stress, large deformation restraint, and welding difficulty, coupled with the lack of reliable testing methods. The resulting welds often contain numerous defects exceeding standards. The deformation of the tank body caused by changes in the load of the stored medium also indirectly promotes the corrosion of the edge plates. Therefore, corrosion of the tank edge plates is a key area of corrosion within the tank. When pitting, erosion, or perforation occurs on the edge plates, there are two main conventional replacement and repair methods: The first method involves cutting off 50mm of the connecting tank wall plates along with the edge plates during removal, causing the entire tank to drop uniformly by 50mm before reassembling and welding. This method is suitable for vertical storage tanks without complex internal structures, where the drop in tank elevation has minimal impact on internal accessories. However, in wastewater settling tanks, internal components such as heating coils, oil collection tanks, inlet and outlet pipelines, and upper and lower octagonal pipes of the settling tank have supports connected to the central cylinder on one side and the tank wall on the other. If the tank elevation drops while the central cylinder elevation remains unchanged, these supports will bear significant stress as the tank wall descends, potentially leading to deformation and tearing, thus posing a safety hazard.
[0003] The second method involves removing and replacing the connected bottom ring tank wall plate along with the edge plate, which does not change the tank elevation. However, this method requires the simultaneous removal of the inlet and outlet pipelines connected to the bottom ring tank wall plate. To prevent the tank from tilting and becoming unstable, extensive support is needed during the replacement process, resulting in low construction efficiency and high construction costs. Furthermore, the bottom ring tank wall plate of the storage tank is relatively thick, and corrosion is not significant, so complete replacement is not necessary. Summary of the Invention
[0004] To overcome the shortcomings of existing methods for replacing edge plates in settling tanks, such as requiring numerous support devices, low construction efficiency, and high costs, this invention provides a method for replacing and repairing edge plates in wastewater settling tanks. This efficient method for replacing and repairing edge plates in wastewater settling tanks solves the technical problems of requiring numerous additional support measures and lowering the tank elevation during edge plate removal and replacement, thereby improving construction efficiency and reducing construction costs.
[0005] The technical solution of this invention is: a method for replacing and repairing the edge plate of a sewage settling tank, comprising the following steps: S1. Fix an expansion ring on the inner wall of the bottom ring tank wall plate, wherein the vertical position of the expansion ring is 200mm-300mm above the fillet weld. S2. Determine the cutting position on the tank wall plate and cut it. The cutting position is located 2mm-5mm below the weld foot of the corner weld on the outer side of the storage tank. S3. Replace or repair the edge plate; S4. Weld the new edge plate. First, weld the butt weld between the two edge plates, and then weld the fillet weld between the edge plate and the tank wall plate. S5. Remove the expansion ring.
[0006] Furthermore, the expansion ring is a channel steel, which is bent into a circle that matches the inner wall of the tank wall and then welded to the tank wall.
[0007] Furthermore, in step S1, the expansion ring is composed of several discontinuous channel steel segments, the outer arc of each channel steel segment mates with the inner wall of the tank wall plate, and the bottom of each channel steel segment is connected to the old edge plate through a support pipe.
[0008] Furthermore, in step S2, the tank wall panel is cut using a water jet method.
[0009] Furthermore, step S3 includes: ① When the edge plate is located in the valve chamber of the tank room, add a new edge plate to the old edge plate, or repair the local defects by laser welding; ② Remove the old edge plates outside the valve chamber of the tank room, and replace two of the three old edge plates with new edge plates.
[0010] Furthermore, in step S3, the thickness of the new edge plate is greater than the thickness of the old edge plate, and the thickness of the new edge plate is the sum of the thickness of the old edge plate and the height of the weld leg cut by the fillet weld.
[0011] Furthermore, in step S4, when welding the butt joint between the two edge plates, iron wedges are installed at the bottom of the tank wall plate for support, and the iron wedges are removed before welding the fillet weld between the edge plate and the tank wall plate.
[0012] Furthermore, in step S4, before welding the fillet weld between the edge plate and the tank wall plate, the remaining weld allowance at the bottom of the bottom ring tank wall plate is ground down.
[0013] Furthermore, in step S4, after the butt weld between the two edge plates is welded, the outer 300mm of the weld is subjected to radiographic testing, and the remaining welds are subjected to a tightness test using a vacuum chamber method. After the test is passed, the fillet weld between the edge plate and the tank wall plate is then welded.
[0014] Furthermore, in step S4, when welding the edge plate to the tank wall plate, after the root weld is completed, a penetrant test is performed within a range of 200mm in each of the three directions; after all welding is completed, a penetrant test or magnetic particle test is performed.
[0015] The present invention has the following beneficial effects: By adopting the above-mentioned solution, the present invention solves the technical problems of requiring a large number of support measures and lowering the tank elevation during the removal and replacement of edge plates by appropriately increasing the thickness of the edge plates to compensate for cutting damage. This improves construction efficiency and reduces construction costs. Simultaneously, the use of expansion rings to support the tank wall plates during construction avoids damage to the settling tank and ensures the safety of the edge plate replacement process. The invention has shown good application results in renovation projects, demonstrating significant economic and social benefits. Attached Figure Description
[0016] Figure 1 This is a flowchart of the present invention; Figure 2 This is a schematic diagram comparing the edge plate before and after replacement according to the present invention.
[0017] In the diagram, 1-bottom ring tank wall plate, 2-old edge plate, 3-old fillet weld, 4-new fillet weld, 5-cutting line, 6-new edge plate. Detailed Implementation
[0018] The present invention will now be described in detail with reference to the accompanying drawings and embodiments. The technical solutions in the embodiments of the present invention will be clearly and completely described. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0019] In the description of this invention, it is necessary to understand that the orientations or positional relationships indicated by terms such as "upper," "lower," "left," "right," "inner," "outer," "top," and "bottom" are based on the orientations or positional relationships shown in the accompanying drawings. They are intended only to facilitate the description of this invention and to simplify the description, and are not intended to indicate or imply that the components referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.
[0020] Depend on Figure 1 As shown, a method for replacing and repairing the edge plate of a sewage settling tank includes construction preparation. First, the construction equipment, personnel, and materials are inspected and prepared. The control valves corresponding to the tank are closed. The process flow is checked to confirm that the tank is completely cut off and sealed from other processes in the station. The tank is cleaned and hot-washed. An explosion-proof axial flow fan is used to ventilate the manhole and the ventilation hole on the top of the tank for more than 2 hours. The key parts of the tank are inspected to ensure the safety and continuity of the construction.
[0021] Then proceed with the following steps: S1. Fix an expansion ring on the inner wall of the bottom ring tank wall plate. The expansion ring can reinforce the tank wall plate during cutting and welding to prevent deformation of the tank wall plate.
[0022] The expansion ring is made of channel steel and should be fabricated before construction. The fixing position of the expansion ring depends on the site conditions inside the tank. Since most wastewater settling tanks have a sludge discharge pipe inside, the expansion ring cannot be placed near the fillet weld. Typically, the expansion ring is fixed 200mm-300mm above the fillet weld, while welding or support measures are taken to ensure that the tank wall does not sink during the cutting process.
[0023] The expansion ring can have two structures: one is an integral type, where the channel steel is bent into a ring that fits the inner wall of the tank wall and then welded to it; the expansion ring is removed entirely after the work is completed. The other is a split type, where the expansion ring consists of several discontinuous segments of channel steel, each segment's outer arc fitting the inner wall of the tank wall. During fixing, the bottom of each segment is welded to the old edge plate via a support pipe; in this case, some expansion rings can be removed after the local edge plate replacement is completed, and then the next construction area can be moved on. The entire expansion ring can be removed after all edge plates have been replaced. However, when installing expansion rings locally, care should be taken to ensure that the support pipes for the expansion rings are installed on the removed old edge plates to facilitate subsequent construction.
[0024] S2. Determine the cutting position on the tank wall plate and cut. Set the cutting position 2mm-5mm below the weld foot of the outer corner weld of the storage tank. When cutting the tank wall plate, use the water jet method. Remove the filler metal of the original weld of the tank wall directly with carbon arc gouging to ensure a smooth cut and minimize damage to the bottom ring tank wall plate.
[0025] S3. Replace or repair the edge plate. Depending on the location of the edge plate, the following two methods may be used for replacement or repair: ① Edge Plate of the Valve Chamber in Tank Interchange. Since some settling tanks are equipped with valve chambers on their exterior, the edge plate of the outer tank is partially submerged under the concrete of the valve chamber. Replacing the edge plate would require removing wall joints and excavating the ground, resulting in low efficiency and complex operations. Therefore, this method first uses magnetic flux leakage testing to inspect the corrosion of the edge plate in the valve chamber area. For edge plates with minor corrosion such as pits and grooves, laser welding is used for repair, followed by grinding to smooth the surface. For edge plates with large corrosion areas and significant defects, a reinforcement method is used, i.e., adding a new edge plate of the same area to the old edge plate before welding.
[0026] ②Except for the valve chamber in the tank room, remove the old edge plates and replace them with two new edge plates for every three old edge plates.
[0027] The edge plate thickness of a typical settling tank is 6-20mm. The fillet weld height between the edge plate and the bottom ring tank wall plate is the minimum of the thicknesses of the edge plate and the bottom ring tank wall plate, and not more than 13mm. Because the bottom ring tank wall plate may be damaged during the cutting process, a gap may appear between the new edge plate and the original tank wall plate after installation, making welding impossible.
[0028] When replacing the edge plate, the present invention appropriately increases the thickness of the new edge plate, setting the thickness of the new edge plate to the sum of the thickness of the old edge plate and the height of the weld leg cut by the fillet weld, thereby compensating for the height of the bottom ring tank wall plate cut. This not only compensates for the amount of damage caused by cutting, keeping the height of the storage tank unchanged, but also ensures that the weldability of the steel plate remains unchanged.
[0029] like Figure 2 As shown, before replacement, the bottom ring tank wall plate 1 is cut. The cutting line 5 is 2-5mm below the upper edge of the weld leg of the old fillet weld 3. The height of the new edge plate 6 after replacement is greater than the height of the old edge plate 2 to compensate for the damage caused during cutting. After replacement, the bottom ring tank wall plate 1 and the new edge plate 6 are welded together to create a new fillet weld 4.
[0030] S4. Weld the new edge plate. The specific process for welding the new edge plate is as follows: S41. Since a section of the edge plate weld is located below the bottom ring tank wall plate, which is difficult to weld, iron wedges are first installed at the bottom of the tank wall plate for support.
[0031] S42. Weld the butt weld between the two edge plates. After the butt weld is welded, the outer 300mm of the weld is subjected to radiographic testing, and the remaining welds are subjected to a tightness test using the vacuum chamber method.
[0032] S43. After the butt weld between the edge plates passes inspection, remove all the supporting iron wedges and grind the remaining weld allowance at the bottom of the bottom ring tank wall plate to ensure that the tank wall plate and the edge plate are fully assembled.
[0033] S44. Fillet weld between the weld edge plate and the bottom ring tank wall plate. Due to the cutting of the bottom ring tank wall plate, gaps may occur in some areas during assembly. In this case, welding can be used to fill the gaps, ensuring that the number of weld layers and the reinforcement height of the fillet weld meet the standard specifications. During the welding process, after the root weld is completed, penetrant testing is performed within a 200mm range in three directions; after all welding is completed, penetrant testing or magnetic particle testing is performed.
[0034] S5. After all welding is completed, remove the expansion ring. After all welds pass non-destructive testing, perform anti-corrosion treatment.
[0035] This invention adopts the principle of appropriately increasing the thickness of the edge plate to compensate for cutting damage, which solves the technical problems of needing to add a lot of support measures and reducing the tank elevation during the removal and replacement of the edge plate. It improves construction efficiency, reduces construction costs, and has good application results in renovation projects, with significant economic and social benefits.
[0036] The various embodiments of the present invention have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments. The terminology used herein is chosen to best explain the principles, practical application, or technical improvements to the embodiments in the market, or to enable others skilled in the art to understand the embodiments disclosed herein.
Claims
1. A method for replacing and repairing the edge plate of a sewage settling tank, characterized in that... Includes the following steps: S1. Fix an expansion ring on the inner wall of the bottom ring tank wall plate, wherein the vertical position of the expansion ring is 200mm-300mm above the fillet weld. S2. Determine the cutting position on the tank wall plate and cut it. The cutting position is located 2mm-5mm below the weld foot of the corner weld on the outer side of the storage tank. S3. Replace or repair the edge plate; S4. Weld the new edge plate. First, weld the butt weld between the two edge plates, and then weld the fillet weld between the edge plate and the tank wall plate. S5. Remove the expansion ring.
2. The method for efficient replacement and repair of the edge plate of a sewage settling tank according to claim 1, characterized in that: In step S1, the expansion ring is a channel steel, which is bent into a circle that matches the inner wall of the tank wall and then welded to the tank wall.
3. The method for efficient replacement and repair of the edge plate of a sewage settling tank according to claim 1, characterized in that: In step S1, the expansion ring is composed of several discontinuous channel steel segments. The outer arc of each channel steel segment matches the inner wall of the tank wall plate, and the bottom of each channel steel segment is connected to the old edge plate through a support pipe.
4. The method for efficient replacement and repair of the edge plate of a sewage settling tank according to claim 1, characterized in that: In step S2, the tank wall panel is cut using a water jet method.
5. The method for efficient replacement and repair of the edge plate of a sewage settling tank according to claim 1, characterized in that: Step S3 includes: ① When the edge plate is located in the valve chamber of the tank room, add a new edge plate to the old edge plate, or repair the local defects by laser welding; ② Remove the old edge plates outside the valve chamber of the tank room, and replace two of the three old edge plates with new edge plates.
6. The method for efficient replacement and repair of the edge plate of a sewage settling tank according to claim 1, characterized in that: In step S3, the thickness of the new edge plate is greater than the thickness of the old edge plate, and the thickness of the new edge plate is the sum of the thickness of the old edge plate and the height of the weld leg cut by the fillet weld.
7. The method for efficient replacement and repair of the edge plate of a wastewater settling tank according to claim 1, characterized in that: In step S4, when welding the butt joint between the two edge plates, iron wedges are installed at the bottom of the tank wall plate for support, and the iron wedges are removed before welding the fillet weld between the edge plate and the tank wall plate.
8. The method for efficient replacement and repair of the edge plate of a sewage settling tank according to claim 7, characterized in that: In step S4, before welding the fillet weld between the edge plate and the tank wall plate, the remaining weld allowance at the bottom of the bottom ring tank wall plate is ground down.
9. The method for efficient replacement and repair of the edge plate of a sewage settling tank according to claim 7, characterized in that: In step S4, after the butt weld between the two edge plates is welded, the outer 300mm of the weld is subjected to radiographic testing, and the remaining welds are subjected to a tightness test using a vacuum chamber method. After the test is passed, the fillet weld between the edge plate and the tank wall plate is then welded.
10. The method for efficient replacement and repair of the edge plate of a sewage settling tank according to claim 9, characterized in that: In step S4, when welding the edge plate to the tank wall plate, after the root weld is completed, a penetrant test is performed within a range of 200mm in each of the three directions; after all welding is completed, a penetrant test or magnetic particle test is performed.