A surface-modified steel fiber reinforced aluminosilicate refractory castable and its preparation method

By forming a continuous inorganic SiO2 modified layer and chemical bonding on the surface of steel fibers, the problems of insufficient steel fiber reinforcement and high-temperature oxidation are solved, thereby improving the mechanical properties and thermal shock stability of aluminosilicate refractory castables, which are suitable for iron and steel smelting and non-ferrous metallurgy.

CN123062282APending Publication Date: 2026-11-10ANHUI UNIVERSITY OF TECHNOLOGY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611533745.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In the existing technology, the reinforcing effect of steel fibers in aluminosilicate refractory castables is insufficient, and the problems of interfacial bonding strength and high-temperature oxidation have not been effectively solved, resulting in the deterioration of mechanical properties and thermal shock stability.

Method used

A continuous inorganic SiO2 modified layer was formed on the surface of steel fibers by LiOH activation and TEOS sol-gel method. Combined with components such as α-Al2O3 micro powder and dense corundum fine powder, the interfacial bonding strength was improved by mechanical interlocking and chemical bonding, and high-temperature oxidation was inhibited.

Benefits of technology

It significantly improves the mechanical strength, post-cracking load-bearing capacity, and thermal shock stability of aluminosilicate refractory castables, making them suitable for key thermal equipment under high-temperature oxidizing conditions in steel smelting and non-ferrous metallurgy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123062282A_ABST
    Figure CN123062282A_ABST
Patent Text Reader

Abstract

This invention discloses a surface-modified steel fiber reinforced aluminosilicate refractory castable and its preparation method, belonging to the field of refractory materials. The raw materials of the castable include: fused mullite, andalusite, silicon carbide, dense corundum fine powder, α-Al₂O₃ micro powder, silica powder, calcium aluminate cement, dispersant, and surface-modified heat-resistant steel fibers. The surface-modified heat-resistant steel fibers consist of a heat-resistant stainless steel fiber matrix and a continuously coated SiO₂ layer tightly bonded to its surface. The SiO₂ modified layer is mainly composed of an amorphous Si-O-Si network with Si-OH on the surface. The surface roughness Sa of the surface-modified heat-resistant steel fibers is 3.2~4.2 μm, and the water contact angle is 55°~66°. The preparation method involves dry mixing the raw materials, adding water, stirring, casting, curing, and drying to obtain the castable. The castable of the present invention aims to improve the non-failure of steel fiber reinforcement during high-temperature service, thereby enhancing the mechanical strength, post-cracking load-bearing capacity, fracture toughness and thermal shock stability of aluminosilicate refractory castables.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of refractory materials technology, and more specifically, relates to a surface-modified steel fiber reinforced aluminosilicate refractory castable and its preparation method. Background Technology

[0002] Aluminosilicate refractory castables possess good high-temperature stability, construction adaptability, and thermal shock resistance, and are widely used in steel smelting, non-ferrous metallurgy, high-temperature furnaces, and key thermal equipment. To improve the flexural strength, fracture toughness, and thermal shock resistance of refractory castables, heat-resistant steel fibers are typically added as reinforcing and toughening phases. Steel fibers are widely used as reinforcing and toughening phases in aluminosilicate refractory castables due to their excellent crack bridging, deflection, and pull-out energy dissipation properties, aiming to improve the material's flexural strength, fracture toughness, and thermal shock resistance. However, in actual high-temperature service, the reinforcing effect of steel fibers presents two main problems: Firstly, untreated steel fibers have smooth surfaces, low activity and wettability, and rely solely on mechanical embedding and interfacial friction to transfer loads with the castable matrix. The interfacial bonding strength and load transfer efficiency are insufficient, making it difficult to fully realize their toughening potential. Secondly, under high-temperature oxidizing atmosphere, oxygen migrates to the fiber surface along the interfacial defects between the steel fiber and the castable matrix, causing steel fiber oxidation and interfacial diffusion of alloying elements (such as Fe and Cr). The accumulation of oxidation products leads to interfacial volume expansion and induces porosity, microcracks and local debonding, which seriously weakens the interfacial bonding state and causes the mechanical properties, crack propagation resistance and thermal shock stability of the castable to deteriorate.

[0003] Therefore, how to simultaneously improve the load transfer capacity of the steel fiber-matrix interface and suppress the high-temperature oxidation of steel fibers and the diffusion of interfacial elements is a core technical problem that urgently needs to be solved in this field.

[0004] Currently, researchers have attempted to introduce SiO2 modified layers onto the surface of steel fibers. For example, Chinese patent application CN119019178A discloses a surface-modified steel fiber toughened bauxite castable and its preparation method. This method combines silane coupling agent pretreatment with silica sol vacuum impregnation to load a SiO2 modified layer onto the steel fiber surface. While this method improves fiber surface wettability and interfacial interactions to some extent, the modified layer relies on the organosilane coupling layer and physical loading. During the high-temperature service of the refractory castable, the organic components are prone to thermal decomposition, leading to impaired continuity of the modified layer and insufficient high-temperature interfacial stability. Furthermore, this method fails to synergistically regulate the original surface state of the steel fiber, the degree of SiO2 loading, and the adhesion stability of the modified layer during dry mixing. An excessively thick or uneven modified layer may actually become a new source of interfacial defects.

[0005] Korean patent KR20230113078A discloses a method for depositing nano-SiO2 particles on the surface of steel fibers. It uses a system of tetraethyl orthosilicate, hexadecyltrimethylammonium bromide, and ammonia to prepare a SiO2 particle layer through a hydrolysis-condensation reaction, and then applies it to cement-based composite materials. However, while this steel fiber can improve interfacial bonding performance in cement-based systems at room temperature or medium-low temperatures, aluminosilicate refractory castables require stringent processes and service life, including dry mixing, water addition and stirring, curing, high-temperature sintering, and repeated thermal cycling. Furthermore, the SiO2 particle layer prepared by this technology struggles to meet the specific requirements of high-temperature refractory systems in terms of loading, particle distribution, and continuity.

[0006] In addition, various steel fiber modification methods have been developed in the field of concrete and cement-based materials, such as polydopamine self-polymerization, impregnation with polyallylamine hydrochloride and sodium silicate, and surface mineralization to introduce CaCO3 particles. These methods mainly focus on improving the surface roughness and hydrophilicity of the fibers to enhance the bonding with cement hydration products at room temperature. However, the modified layers are mostly organic polymers or carbonates, which are prone to thermal decomposition, oxidation failure, or decomposition and gasification in high-temperature oxygen-containing environments. If directly applied to refractory castables, they will introduce defects such as pores and cracks at the fiber-matrix interface, thus deteriorating the material properties.

[0007] Therefore, there is an urgent need for a surface-modified steel fiber reinforced aluminosilicate refractory castable and its preparation method to achieve synergistic effects of low-temperature interface reinforcement and high-temperature oxidation protection, ultimately significantly improving the mechanical strength, post-cracking load-bearing capacity, fracture toughness and thermal shock stability of aluminosilicate refractory castable. Summary of the Invention

[0008] 1. The problem to be solved One of the objectives of this invention is to provide a surface-modified steel fiber reinforced aluminosilicate refractory castable, which aims to improve the non-failure of steel fiber reinforcement during high-temperature service and significantly enhance the mechanical strength, post-cracking load-bearing capacity, fracture toughness, and thermal shock stability of aluminosilicate refractory castable.

[0009] Another objective of this invention is to provide a method for preparing surface-modified steel fiber reinforced aluminosilicate refractory castable, thereby achieving controllable preparation of a continuous SiO2 modified layer on the surface of the steel fiber and synergistic interface enhancement with the aluminosilicate matrix.

[0010] 2. Technical Solution To solve the above problems, the technical solution adopted by the present invention is as follows: The first aspect of the present invention provides a surface-modified steel fiber-reinforced aluminosilicate refractory castable, the castable comprising fused mullite, andalusite, silicon carbide (a functional component for improving thermal shock resistance and corrosion resistance), dense corundum fine powder, α-Al2O3 micro powder, silica micro powder, calcium aluminate cement (binder), dispersant (an admixture for improving the dispersibility and workability of the castable), and surface-modified heat-resistant steel fibers (reinforcing and toughening phase), wherein the surface-modified heat-resistant steel fibers are a heat-resistant stainless steel fiber matrix and a SiO2 modified layer tightly bonded to its surface and continuously coated thereon, the SiO2 modified layer being mainly composed of an amorphous Si-O-Si network with Si-OH on the surface, the surface roughness Sa of the surface-modified heat-resistant steel fibers being 3.2~4.2 μm, and the water contact angle of the surface-modified heat-resistant steel fibers being 55°~66°.

[0011] Using the above technical solution, on the one hand, the surface roughness Sa of the surface-modified heat-resistant steel fiber reaches 3.2~4.2 μm, while the water contact angle is significantly reduced by 55°~66°. A suitable micro-rough morphology is constructed on the surface of the surface-modified heat-resistant steel fiber, enhancing the physical and mechanical anchoring effect, while introducing active hydrophilic groups, significantly improving surface wettability. Under the synergistic effect of mechanical interlocking and wetting, the SiO2 modified layer and the heat-resistant stainless steel fiber matrix form a strong interfacial bond, effectively alleviating the porosity defects in the interfacial transition zone during subsequent casting molding, and significantly improving the interfacial bonding strength.

[0012] On the other hand, the continuously coated SiO2 modified layer works closely with the various components in the aluminosilicate refractory castable at different temperature ranges to improve the mechanical strength, post-cracking load-bearing capacity, fracture toughness, and thermal shock stability of the castable. During the low-temperature curing stage, the continuous SiO2 modified layer on the surface-modified heat-resistant steel fiber is rich in silanol groups (Si-OH), which rapidly react with the calcium aluminate cement hydration and release Ca after water addition and stirring. 2+ Al 3+ Plasma reaction forms Si-containing CASH-like hydration products, constructing a dense hydration transition layer. The CASH gel grows in situ on the surface of the steel fiber, filling the inherent pores of the interfacial transition zone around the traditional steel fiber, transforming the fiber-matrix interface from loose and porous to dense and continuous, significantly improving early interfacial bonding strength. Simultaneously, it works with fine powders such as α-Al₂O₃ micropowder and silicon micropowder to construct a dense interfacial transition zone, significantly enhancing early bonding strength.

[0013] Fine powder components such as α-Al₂O₃ micro powder, dense corundum fine powder, and silica micro powder form a fine powder transition layer with a gradual change in composition between the SiO₂ modified layer on the steel fiber surface and the castable matrix after high-temperature heat treatment. During the medium-to-high temperature heat treatment stage, on the one hand, the fine powder transition layer undergoes a mullite formation reaction, forming an aluminosilicate glass phase and secondary mullite phase from the fiber surface to the mullite / andalusite aggregate, achieving a ceramicized connection between the fiber and the matrix and creating a gradient thermal expansion, effectively alleviating thermal stress. On the other hand, the Si-O enriched coverage area on the steel fiber surface acts as a barrier to the diffusion of oxygen and alloying elements, inhibiting the migration of oxygen into the steel fiber and the outward diffusion of alloying elements such as chromium, slowing down steel fiber oxidation and interface deterioration, and reducing the tendency to form defects such as interface porosity, microcracks, and local debonding.

[0014] In addition, as a functional component, silicon carbide, through edge oxidation, generates SiO2, which synergistically enhances the interfacial oxygen barrier capacity with the SiO2 modified layer on the fiber surface. Meanwhile, fused mullite and andalusite aggregates form an integral ceramic network with the fiber through a fine powder transition layer, further suppressing the high-temperature oxidation of steel fibers and the diffusion of alloying elements.

[0015] As one possible implementation, the proportion of the exposed area of ​​the steel fiber surface not covered by the SiO2 modified layer to the total surface area of ​​the steel fiber is no more than 40%; preferably no more than 5%, and more preferably 4%, 3%, or 2.7%.

[0016] As one possible implementation, SEM / EDS surface scanning shows that the apparent Si element coverage on the steel fiber surface is ≥60%, the average thickness of the SiO2 modified layer is 150~180 nm, and the length of the continuous uncoated segment within any 1 mm steel fiber does not exceed 80 μm. The apparent Si element coverage on the surface is obtained as follows: A surface-modified heat-resistant steel fiber sample is taken and subjected to SEM... EDS surface scanning was performed, using the mean of the unmodified steel fiber background Si signal plus three times the standard deviation as the threshold. The percentage of the effective area of ​​the Si signal relative to the effective area of ​​the steel fiber surface in each field of view was statistically analyzed. At least five fibers were randomly selected, each fiber had at least three segments, and each segment had at least three fields of view, and the average value was taken. The apparent Si coverage of the modified steel fiber of this invention is not less than 60%, indicating that the SiO2 modified layer is basically continuously coated on the surface of the steel fiber.

[0017] As one possible implementation, the castable includes the following raw materials in parts by weight: 40-55 parts of fused mullite, 15-25 parts of andalusite, 1-5 parts of silicon carbide, 6-12 parts of dense corundum fine powder, 5-10 parts of α-Al2O3 micro powder, 2-6 parts of silica powder, 3-7 parts of calcium aluminate cement, 1-4 parts of surface-modified heat-resistant steel fiber, and 0.05-0.20 parts of dispersant.

[0018] As one possible implementation, the electrofused mullite comprises 20-28 parts of 5-3 mm electrofused mullite, 10-16 parts of 3-1 mm electrofused mullite, 4-8 parts of 1-0 mm electrofused mullite, and 4-8 parts of 325 mesh electrofused mullite; The andalusite comprises 5-10 parts of 3-1 mm andalusite and 10-18 parts of 1-0 mm andalusite; The silicon carbide particle size is 1~0 mm; The particle size of the dense corundum powder is no greater than 0.075 mm; The median particle size d of the α-Al2O3 micro powder 50 The preferred size is 3 μm.

[0019] As one possible implementation, the preparation method of the surface-modified heat-resistant steel fiber is as follows: heat-resistant steel fiber is placed in an alkaline solution for cleaning and surface activation treatment, then washed with water until neutral and dried; then tetraethyl orthosilicate, hexadecyltrimethylammonium bromide and concentrated ammonia are dispersed in an anhydrous ethanol solution, and then the surface-activated heat-resistant steel fiber is added; wherein concentrated ammonia is used as a catalyst and the source of water required for hydrolysis and condensation reaction, and no additional water source is added, so that tetraethyl orthosilicate hydrolyzes, condenses and deposits on the surface of the steel fiber to form a continuous coating of SiO2 modified layer.

[0020] In the above technical solution, deionized water is not added separately during the hydrolysis-condensation reaction; the water required for the hydrolysis-condensation reaction is introduced by concentrated ammonia. Concentrated ammonia not only acts as an alkaline catalyst to promote the hydrolysis and condensation of tetraethyl orthosilicate, but its own water content also serves as the water source required for the hydrolysis reaction. By controlling the water content in the system, the hydrolysis and homogeneous nucleation rates of tetraethyl orthosilicate can be avoided from being too rapid, reducing the formation and aggregation of free SiO2 particles. This is beneficial for heterogeneous nucleation and deposition of SiO2 on the steel fiber surface, thereby forming a more uniform SiO2 modified layer. Deionized water is only used for cleaning the steel fibers after alkaline pretreatment and for washing after the modification reaction is completed; therefore, the amount added is not fixed, but rather determined by cleaning the steel fibers to neutrality or removing residual reactants.

[0021] As one possible implementation, the alkaline solution is preferably a lithium hydroxide solution with a concentration of 0.1~1.0 mol / L.

[0022] Using the above technical solution, lithium hydroxide solution can remove oil, loose oxides, and other attached impurities from the surface of steel fibers, and perform alkaline activation on the steel fiber surface, exposing or forming more metal oxide / hydroxide and hydroxyl active sites. Surface hydroxyl groups can provide favorable sites for subsequent heterogeneous nucleation and deposition of SiO2; the Si-OH groups formed by the hydrolysis of tetraethyl orthosilicate can further condense with the M-OH sites on the steel fiber surface, which is beneficial for forming MO-Si type interface connections, where M includes one or more of Fe and Cr, thereby improving the bonding stability between the SiO2 modified layer and the steel fiber matrix. Simultaneously, using LiOH as an alkaline pretreatment agent can avoid introducing additional Na into the system. + Impurities help reduce the likelihood of foreign alkali metal ions adversely affecting the high-temperature performance of refractory materials.

[0023] As one possible implementation, the cleaning and surface activation treatment is carried out at a temperature of room temperature to 60°C for a treatment time of 10 to 60 minutes to remove oil, loose oxides and other attached impurities from the surface of the steel fiber and improve its surface activity. After the treatment, the fiber is repeatedly washed with deionized water until the washing solution is neutral, and then dried for later use.

[0024] As one possible implementation, the amount of tetraethyl orthosilicate added is 0.1% to 0.52% of the mass of the heat-resistant steel fiber.

[0025] When the above technical solution is adopted, the theoretical SiO2 modification concentration (based on the theoretical mass of SiO2 generated by the complete hydrolysis and condensation of tetraethyl silicate and calculated according to the mass of heat-resistant steel fiber) is controlled at 0.05~0.15 wt.%, which can enable submicron-sized SiO2 particles to form a relatively uniform coverage area on the surface of steel fiber. This avoids the difficulty in forming an effective interface regulation effect due to the low loading degree, and also avoids the cracking and peeling of the modified layer during dry mixing, heating or thermal cycling due to the high loading degree or particle agglomeration.

[0026] As one possible implementation, the amount of tetraethyl orthosilicate added is 4-12 wt.% of the mass of the anhydrous ethanol. The mass ratio of the tetraethyl orthosilicate to the hexadecyltrimethylammonium bromide is 8:1.

[0027] As one possible approach, after adding concentrated ammonia, hydrolysis condensation and surface deposition reactions are carried out at 40-50°C, with the hydrolysis condensation reaction time being at least 12 hours.

[0028] As one possible solution, 40 mL of concentrated ammonia is added to every 1000 mL of anhydrous ethanol.

[0029] As one possible approach, after the hydrolysis-condensation reaction is completed, the steel fibers are aged at room temperature for 18-30 hours, then filtered, washed with deionized water, and dried at 70-90°C to obtain heat-resistant steel fibers with a SiO2 modified layer on the surface.

[0030] As one possible implementation, in the castable, the dispersant is at least one of sodium hexametaphosphate, sodium tripolyphosphate, and polyethylene glycol-type condensate dispersant.

[0031] The second aspect of the present invention provides a method for preparing the above-mentioned surface-modified steel fiber reinforced aluminosilicate refractory castable, comprising the following steps: fused mullite, andalusite, silicon carbide, dense corundum fine powder, α-Al2O3 micro powder, silica micro powder, calcium aluminate cement, dispersant and surface-modified heat-resistant steel fiber are mixed evenly to obtain a dry mixture; water accounting for 3-6 wt.% of the total mass of the dry mixture is added to the dry mixture, and the mixture is stirred, cast into shape, cured and dried to obtain the surface-modified steel fiber reinforced aluminosilicate refractory castable.

[0032] As one possible implementation, water is added to the dry mix, wet-mixed for 90-180 s, then poured into a mold and vibrated for 30-60 s. After curing at room temperature for 18-30 h, the mixture is demolded and then dried at 100-120 ℃ for 18-30 h to obtain a surface-modified steel fiber reinforced aluminosilicate refractory castable.

[0033] 3. Beneficial effects Compared with the prior art, the beneficial effects of the present invention are as follows: (1) The present invention forms a continuous inorganic SiO2 layer through LiOH activation and TEOS sol-gel method, which avoids the problems of high temperature decomposition of organic components and peeling of modified layer. It realizes interface strengthening and anti-oxidation protection throughout the entire cycle from low temperature curing to high temperature service, and comprehensively improves the mechanical properties, thermal shock resistance and service life of aluminosilicate refractory castables. It is especially suitable for key thermal equipment under high temperature oxidation conditions such as iron and steel smelting and non-ferrous metallurgy.

[0034] (2) This invention employs a sol-gel method to form a SiO2 modified layer in situ on the surface of heat-resistant steel fibers. After LiOH pretreatment, oil stains, loose oxides, and attached impurities on the surface of the heat-resistant steel fibers are removed, increasing the reactivity of the steel fiber surface. This facilitates the nucleation and stable adhesion of SiO2 particles on the surface, forming or exposing hydroxyl active sites on the steel fiber surface. The silanol groups generated by the hydrolysis of tetraethyl silicate can further undergo condensation reactions with the active sites on the steel fiber surface, allowing the SiO2 modified layer to be bonded to the steel fiber surface through the synergistic effect of chemical bonding and physical adhesion. Compared with traditional silica sol impregnation or simple physical coating methods, the modified layer obtained by this invention has a more uniform and continuous coverage, and a more stable interface bonding, which can improve the problems of weak coating adhesion, easy cracking, or peeling.

[0035] (3) The SiO2 modified layer formed by the present invention is an inorganic oxide layer with good high-temperature stability. It can slow down the transport of oxygen to the steel fiber / matrix interface, reduce the degree of high-temperature oxidation of steel fiber and interface deterioration, and avoid the decomposition, oxidation or gas release of organic coating or carbonate modified layer at high temperature, thereby improving the thermal shock stability and high-temperature service stability of castable.

[0036] (4) In the castable of the present invention, fused mullite of different particle sizes constitutes the refractory skeleton of the castable, providing high-temperature structural stability for the material; andalusite undergoes mullitization during high-temperature process and produces a moderate volume effect, which helps to compensate for matrix sintering shrinkage, alleviate thermal stress concentration and improve thermal shock stability; dense corundum fine powder, α-Al2O3 micro powder, 325 mesh fused mullite powder and silica micro powder can fill the aggregate gaps, optimize particle packing and promote the sintering densification of the matrix during heat treatment; silicon carbide helps to improve the thermal shock resistance and erosion resistance of the castable; calcium aluminate cement provides bonding strength for castable molding and low-temperature curing.

[0037] (5) The surface-modified steel fibers prepared by the present invention have high roughness and wettability, which can enhance the mechanical embedding and interfacial bonding between the steel fibers and the aluminosilicate refractory castable matrix, improve the energy dissipation of crack bridging, deflection and pull-out, thereby improving the mechanical strength and post-cracking load-bearing capacity of the castable.

[0038] (6) The castable of the present invention does not take the formation of a specific mullite reaction layer above 1400 °C as an essential technical feature. Instead, it improves the structural stability and oxidation resistance of the interface region around the steel fiber under high temperature conditions of 1100~1350 °C through the synergistic effect between the SiO2 modified layer and the aluminosilicate refractory matrix. Attached Figure Description

[0039] Figure 1 The Fourier transform infrared spectra are of the unmodified steel fibers in Comparative Example 1 and the surface-modified heat-resistant steel fibers in Example 2.

[0040] Figure 2 This is a comparison of the surface roughness and wettability of the unmodified steel fiber in Comparative Example 1 and the surface-modified heat-resistant steel fiber in Examples 1-3.

[0041] Figure 3 This is a comparison of the load-displacement curves and flexural toughness of the unmodified steel fiber in Example 1 and the surface-modified heat-resistant steel fiber reinforced castables in Examples 1-3.

[0042] Figure 4 This study examines the interface morphology and elemental distribution of unmodified steel fibers in Comparative Example 1 and surface-modified heat-resistant steel fiber reinforced castables in Examples 1-3 after high-temperature treatment.

[0043] Figure 5 The interface morphology of the unmodified steel fiber in Comparative Example 1 and the surface-modified heat-resistant steel fiber reinforced castables in Examples 1-3 after thermal shock is shown. Detailed Implementation

[0044] The present invention will be further described below with reference to specific embodiments, but the scope of protection of the present invention is not limited to the following embodiments. All equivalent substitutions, conventional adjustments, or improvements made based on the technical solutions of the present invention should be included within the scope of protection of the present invention. Raw materials, equipment, and testing methods not specifically described in the specific embodiments can all be conventional raw materials, equipment, and testing methods in the art.

[0045] This invention discloses a surface-modified steel fiber reinforced aluminosilicate refractory castable, comprising fused mullite, andalusite, silicon carbide, dense corundum fine powder, α-Al2O3 micro powder, silica micro powder, calcium aluminate cement, dispersant, and surface-modified heat-resistant steel fibers. The surface-modified heat-resistant steel fibers consist of a heat-resistant stainless steel fiber matrix and a continuously coated SiO2 modified layer on its surface. The SiO2 modified layer is primarily composed of an amorphous Si-O-Si network with Si-OH atoms on its surface. The surface roughness Sa of the surface-modified heat-resistant steel fibers is 3.2~4.2 μm, and the water contact angle of the surface-modified heat-resistant steel fibers is 55°~66°.

[0046] Specifically, the surface-modified steel fiber reinforced aluminosilicate refractory castable of the present invention comprises the following raw materials in parts by weight: (a) Aggregates It includes 20-28 parts of 5-3 mm fused mullite, 10-16 parts of 3-1 mm fused mullite, 4-8 parts of 1-0 mm fused mullite, 5-10 parts of 3-1 mm andalusite, and 10-18 parts of 1-0 mm andalusite.

[0047] (ii) Matrix powder Includes 4-8 parts of 325-mesh fused mullite, 6-12 parts of dense corundum powder with a particle size not exceeding 0.075 mm, and a median particle size d. 50 5-10 parts of α-Al2O3 micro powder with a diameter of 3 μm and 2-6 parts of silica micro powder.

[0048] (iii) Binder 3-7 parts of calcium aluminate cement.

[0049] (iv) Functional components 1 to 5 parts of silicon carbide with a particle size of 1 to 0 mm.

[0050] (v) Enhance the toughening phase 1-4 parts of surface-modified heat-resistant steel fiber. The preparation method is as follows: At room temperature to 60°C, 446# heat-resistant stainless steel fibers are placed in an alkaline solution for cleaning and surface activation treatment for 10-60 min. They are then washed with water until neutral and dried. Tetraethyl orthosilicate, hexadecyltrimethylammonium bromide, and concentrated ammonia are then dispersed in an anhydrous ethanol solution, and the surface-activated heat-resistant steel fibers are added. Concentrated ammonia serves as a catalyst and a source of water for the hydrolysis-condensation reaction; no additional water is added. At 40-50°C, tetraethyl orthosilicate hydrolyzes, condenses, and deposits on the steel fiber surface to form a continuously coated SiO2 modified layer. The hydrolysis-condensation reaction takes at least 12 h. After the hydrolysis-condensation reaction is complete, the fibers are aged at room temperature for 18-30 h. The steel fibers are then filtered, washed with deionized water, and dried at 70-90°C to obtain heat-resistant steel fibers with a tightly bonded SiO2 modified layer on the surface.

[0051] The alkaline solution used is a lithium hydroxide solution with a concentration of 0.1~1.0 mol / L.

[0052] The amount of tetraethyl orthosilicate added is 0.17% to 0.52% of the mass of the heat-resistant steel fiber.

[0053] The amount of tetraethyl orthosilicate added is 4 to 12 wt. of the mass of anhydrous ethanol.

[0054] The mass ratio of tetraethyl orthosilicate to hexadecyltrimethylammonium bromide is 8:1.

[0055] Add 40 mL of concentrated ammonia to every 1000 mL of anhydrous ethanol.

[0056] (vi) Admixtures 0.05~0.20 parts of dispersant. The dispersant is at least one of sodium hexametaphosphate, sodium tripolyphosphate, and polyethylene glycol-type condensate dispersant. In the specific embodiment, BASF Castament FS 20 dispersant is used, which is a polyethylene glycol-type condensate dispersant.

[0057] The present invention discloses a method for preparing a surface-modified steel fiber reinforced aluminosilicate refractory castable, comprising the following steps: fused mullite, andalusite, silicon carbide, dense corundum fine powder, α-Al2O3 micro powder, silica micro powder, calcium aluminate cement, dispersant, and surface-modified heat-resistant steel fibers are mixed uniformly to obtain a dry mixture; 3-6 wt.% water is added to the dry mixture, and the mixture is wet-mixed for 90-180 seconds; then, the mixture is poured into a mold and vibrated for 30-60 seconds; after curing at room temperature for 18-30 hours, the mixture is demolded; and then dried at 100-120°C for 18-30 hours to obtain the surface-modified steel fiber reinforced aluminosilicate refractory castable.

[0058] The following examples and comparative examples illustrate this.

[0059] Example 1 The surface-modified steel fiber reinforced aluminosilicate refractory castable of this embodiment comprises the following raw materials by weight: 24 parts of 5-3 mm fused mullite, 13 parts of 3-1 mm fused mullite, 6 parts of 1-0 mm fused mullite, 6 parts of 325 mesh fused mullite powder, 7 parts of 3-1 mm andalusite, 14 parts of 1-0 mm andalusite, 9 parts of dense corundum fine powder with a particle size not greater than 0.075 mm, and d 50 The composition consists of 7 parts of 3μm α-Al2O3 micro powder, 4 parts of silica micro powder, 5 parts of calcium aluminate cement, 2.5 parts of 1~0 mm silicon carbide, 2.5 parts of surface-modified heat-resistant steel fiber, and 0.1 parts of dispersant.

[0060] The preparation method of surface-modified heat-resistant steel fiber in this embodiment is as follows: At room temperature, 446# heat-resistant stainless steel fiber is placed in a 1.0 mol / L lithium hydroxide solution for cleaning and surface activation treatment for 30 min, then washed with water until neutral and dried; then tetraethyl orthosilicate, hexadecyltrimethylammonium bromide and concentrated ammonia are ultrasonically dispersed in anhydrous ethanol solution for 20 min, and then the surface-activated 446# heat-resistant stainless steel fiber is added; wherein concentrated ammonia is used as a catalyst and the source of water required for hydrolysis and condensation reaction, and no additional water source is added. At 45°C, tetraethyl orthosilicate is hydrolyzed and condensed on the surface of the steel fiber to form a continuously coated SiO2 modified layer. The hydrolysis and condensation reaction time is 12 h. After the hydrolysis and condensation reaction is completed, it is aged at room temperature for 18 h, the steel fiber is filtered, washed with deionized water, and then dried at 80°C to obtain heat-resistant steel fiber with a SiO2 modified layer on the surface.

[0061] The amount of tetraethyl orthosilicate added is 0.17% of the mass of heat-resistant steel fiber, that is, the theoretical SiO2 modification concentration is 0.05 wt.% (the theoretical SiO2 modification concentration is based on the theoretical mass of SiO2 generated by the complete hydrolysis and condensation of tetraethyl orthosilicate, and is calculated according to the mass of heat-resistant steel fiber).

[0062] The amount of tetraethyl orthosilicate added was 8 wt.% of the mass of anhydrous ethanol. The mass ratio of tetraethyl orthosilicate to hexadecyltrimethylammonium bromide is 8:1; Add 40 mL of concentrated ammonia to every 1000 mL of anhydrous ethanol.

[0063] Fourier transform infrared spectroscopy tests revealed that the surface-modified heat-resistant steel fiber prepared in this embodiment consists of a heat-resistant stainless steel fiber matrix and a SiO2 modified layer that is tightly bonded to its surface and continuously coated. The SiO2 modified layer is mainly composed of an amorphous Si-O-Si network and contains Si-OH on its surface.

[0064] According to SEM / EDS testing, the exposed area of ​​the surface-modified heat-resistant steel fiber prepared in this embodiment, which is not covered by the SiO2 modification layer, accounts for 3% of the total surface area of ​​the steel fiber. SEM / EDS surface scanning showed that the apparent Si element coverage on the steel fiber surface was ≥90%, the average thickness of the SiO2 modification layer was 150 nm, and the length of any continuous uncoated segment within a 1 mm steel fiber did not exceed 50 μm.

[0065] The preparation method of the surface-modified steel fiber-reinforced aluminosilicate refractory castable in this embodiment is as follows: the raw materials, dispersant and surface-modified heat-resistant steel fibers of the above castable are added to a mixing device and dry-mixed for 120 s; 4 wt.% of the total dry material mass of water is added and wet-mixed for another 120 s; then the uniformly mixed castable is poured into a mold and vibrated to form the casting. After curing at room temperature for 24 h, the casting is demolded and then dried at 110 ℃ for 24 h to obtain the surface-modified steel fiber-reinforced aluminosilicate refractory castable of this embodiment.

[0066] Example 2 The surface-modified steel fiber reinforced aluminosilicate refractory castable and its preparation method in this embodiment are basically the same as those in Example 1. The difference is that in the surface-modified steel fiber preparation method, the amount of tetraethyl orthosilicate added is 0.35% of the mass of the heat-resistant steel fiber, that is, the theoretical SiO2 modification concentration is 0.10 wt.%.

[0067] Fourier transform infrared spectroscopy tests revealed that the surface-modified heat-resistant steel fiber prepared in this embodiment consists of a heat-resistant stainless steel fiber matrix and a continuously coated SiO2 modified layer formed on its surface. The SiO2 modified layer is mainly composed of an amorphous Si-O-Si network and contains Si-OH on its surface.

[0068] According to SEM / EDS testing, the exposed area of ​​the surface-modified heat-resistant steel fiber prepared in this embodiment, which is not covered by the SiO2 modification layer, accounts for 2.7% of the total surface area of ​​the steel fiber. SEM / EDS surface scanning showed that the apparent Si element coverage on the steel fiber surface was ≥90%, the average thickness of the SiO2 modification layer was 150 nm, and the length of any continuous uncoated segment within a 1 mm steel fiber did not exceed 50 μm.

[0069] Example 3 The surface-modified steel fiber reinforced aluminosilicate refractory castable and its preparation method in this embodiment are basically the same as those in Example 1. The difference is that in the surface-modified steel fiber preparation method, the amount of tetraethyl orthosilicate added is 0.52% of the mass of the heat-resistant steel fiber, that is, the theoretical SiO2 modification concentration is 0.15 wt.%.

[0070] Fourier transform infrared spectroscopy tests revealed that the surface-modified heat-resistant steel fiber prepared in this embodiment consists of a heat-resistant stainless steel fiber matrix and a continuously coated SiO2 modified layer formed on its surface. The SiO2 modified layer is mainly composed of an amorphous Si-O-Si network and contains Si-OH on its surface.

[0071] According to SEM / EDS testing, the exposed area of ​​the surface-modified heat-resistant steel fiber prepared in this embodiment, which is not covered by the SiO2 modification layer, accounts for 33.8% of the total surface area of ​​the steel fiber. SEM / EDS surface scanning showed that the apparent Si element coverage on the steel fiber surface was ≥60%, the average thickness of the SiO2 modification layer was 180 nm, and the length of any continuous uncoated segment within a 1 mm steel fiber did not exceed 80 μm.

[0072] Example 4 The surface-modified steel fiber reinforced aluminosilicate refractory castable and its preparation method in this embodiment are basically the same as those in Example 2, except that the mass fractions of the raw materials are different, specifically: The raw materials, by weight, include: 20 parts of 5-3 mm fused mullite, 10 parts of 3-1 mm fused mullite, 4 parts of 1-0 mm fused mullite, 4 parts of 325 mesh fused mullite powder, 8 parts of 3-1 mm andalusite, 10 parts of 1-0 mm andalusite, 12 parts of dense corundum fine powder with a particle size not exceeding 0.075 mm, and d 50 The composition consists of 10 parts of 3 μm α-Al2O3 micro powder, 6 parts of silica micro powder, 7 parts of calcium aluminate cement, 5.5 parts of 1~0 mm silicon carbide, 3.5 parts of surface-modified heat-resistant steel fiber, and 0.05 parts of dispersant.

[0073] Example 5 The surface-modified steel fiber reinforced aluminosilicate refractory castable and its preparation method in this embodiment are basically the same as those in Example 2, except that the mass fractions of the raw materials are different, specifically: The raw materials, by mass, include: 23 parts of 5-3 mm fused mullite, 14 parts of 3-1 mm fused mullite, 7 parts of 1-0 mm fused mullite, 8 parts of 325 mesh fused mullite powder, 10 parts of 3-1 mm andalusite, 15 parts of 1-0 mm andalusite, 10 parts of dense corundum fine powder with a particle size not exceeding 0.075 mm, and d 50 The composition consists of 5 parts of 3 μm α-Al2O3 micro powder, 2 parts of silica micro powder, 3 parts of calcium aluminate cement, 1.5 parts of 1~0 mm silicon carbide, 1.5 parts of surface-modified heat-resistant steel fiber, and 0.2 parts of dispersant.

[0074] Example 6 The aluminosilicate refractory castable in this embodiment is basically the same as that in Example 2, except that in the preparation method of the surface-modified heat-resistant steel fiber, the amount of tetraethyl orthosilicate added is 0.1040% of the mass of the heat-resistant steel fiber, that is, the theoretical SiO2 modification concentration is 0.03 wt.% (the theoretical SiO2 modification concentration is based on the theoretical mass of SiO2 generated by the complete hydrolysis and condensation of tetraethyl orthosilicate, and is calculated according to the mass of the heat-resistant steel fiber).

[0075] Fourier transform infrared spectroscopy tests revealed that the surface-modified heat-resistant steel fiber prepared in this comparative example consists of a heat-resistant stainless steel fiber matrix and a continuously coated SiO2 modified layer formed on its surface. The SiO2 modified layer is mainly composed of an amorphous Si-O-Si network and contains Si-OH on its surface.

[0076] According to SEM / EDS testing, the surface-modified heat-resistant steel fibers prepared in this comparative example have an exposed area of ​​4% of the total surface area of ​​the steel fibers that is not covered by the SiO2 modification layer. SEM / EDS surface scanning shows that the apparent Si element coverage on the steel fiber surface is ≥90%, the average thickness of the SiO2 modification layer is 140 nm, and the length of any continuous uncoated segment within a 1 mm steel fiber does not exceed 60 μm.

[0077] Example 7 The aluminosilicate refractory castable in this comparative example is basically the same as that in Example 2, except that in the preparation method of the surface-modified heat-resistant steel fiber, the 446# heat-resistant stainless steel fiber is cleaned and surface-activated with 1.0 mol / L NaOH.

[0078] Comparative Example 1 The aluminosilicate refractory castable in this comparative example is basically the same as that in Example 2, except that it uses untreated 446# heat-resistant stainless steel fibers.

[0079] Comparative Example 2 The aluminosilicate refractory castable in this comparative example is basically the same as that in Example 2, except that the treatment method of the 446# heat-resistant stainless steel fiber is different. The specific treatment method is as follows: the 446# heat-resistant stainless steel fiber is placed in a 1 mol / L LiOH solution and treated at 30°C for 30 min; after treatment, it is washed with deionized water until the washing solution is neutral and dried at 60°C to obtain LiOH pretreated heat-resistant steel fiber.

[0080] Comparative Example 3 The aluminosilicate refractory castable in this comparative example is basically the same as that in Example 2, except that the treatment method for the 446# heat-resistant stainless steel fibers is different. The specific treatment method is as follows: A modified system was prepared using anhydrous ethanol as solvent, tetraethyl orthosilicate as SiO2 precursor, hexadecyltrimethylammonium bromide as surfactant, and ammonia as catalyst. The mass ratio of tetraethyl orthosilicate to hexadecyltrimethylammonium bromide was 8:1.

[0081] Untreated 446# heat-resistant stainless steel fibers were added to the modified system and ultrasonically dispersed for 30 min. Hydrolysis, condensation, and surface deposition reactions were then carried out at 45 °C, followed by aging for 24 h. After the reaction was completed, the steel fibers were filtered, washed, and dried at 80 °C. The amount of tetraethyl orthosilicate added was 0.35% of the mass of the heat-resistant steel fibers, resulting in surface-modified heat-resistant steel fibers with a theoretical SiO2 modification concentration of 0.10 wt.%.

[0082] Fourier transform infrared spectroscopy tests revealed that the surface-modified heat-resistant steel fiber prepared in this comparative example consists of a heat-resistant stainless steel fiber matrix and a continuously coated SiO2 modified layer formed on its surface. The SiO2 modified layer is mainly composed of an amorphous Si-O-Si network and contains Si-OH on its surface.

[0083] According to SEM / EDS testing, the surface-modified heat-resistant steel fibers prepared in this comparative example have an exposed area of ​​58% of the total surface area of ​​the steel fibers that is not covered by the SiO2 modification layer. SEM / EDS surface scanning shows that the apparent Si element coverage on the steel fiber surface is ≥40%, the average thickness of the SiO2 modification layer is 130 nm, and the length of any continuous uncoated segment within a 1 mm steel fiber does not exceed 50 μm.

[0084] Comparative Example 4 The aluminosilicate refractory castable in this comparative example is basically the same as that in Example 2, except that in the preparation method of the surface-modified heat-resistant steel fiber, the amount of tetraethyl orthosilicate added is 0.6936% of the mass of the heat-resistant steel fiber, that is, the theoretical SiO2 modification concentration is 0.2 wt.% (the theoretical SiO2 modification concentration is based on the theoretical mass of SiO2 generated by the complete hydrolysis and condensation of tetraethyl orthosilicate, and is calculated according to the mass of the heat-resistant steel fiber).

[0085] Fourier transform infrared spectroscopy tests revealed that the surface-modified heat-resistant steel fiber prepared in this comparative example consists of a heat-resistant stainless steel fiber matrix and a continuously coated SiO2 modified layer formed on its surface. The SiO2 modified layer is mainly composed of an amorphous Si-O-Si network and contains Si-OH on its surface.

[0086] According to SEM / EDS testing, the surface-modified heat-resistant steel fibers prepared in this comparative example have an exposed area of ​​50% of the steel fiber surface that is not covered by the SiO2 modification layer. SEM / EDS surface scanning shows that the apparent Si element coverage on the steel fiber surface is ≥50%, the average thickness of the SiO2 modification layer is 190 nm, and the length of any continuous uncoated segment within a 1 mm steel fiber does not exceed 85 μm.

[0087] To further illustrate the effects of different surface treatments and SiO2 modification conditions on the surface condition of steel fibers, the fiber-matrix interface structure, and the mechanical and thermal shock properties of castables, this study combines... Figures 1-5 The above-mentioned embodiments and comparative examples are analyzed.

[0088] like Figure 1 As shown, compared with unmodified heat-resistant steel fibers, SiO2 surface-modified steel fibers exhibit improved heat resistance at approximately 1064~1092 cm⁻¹. -1 A significantly enhanced absorption band was observed nearby, which is related to the vibration of the Si-O-Si structure, indicating that the modified component containing silicon-oxygen structure has been loaded onto the steel fiber surface after TEOS hydrolysis and condensation. Combined with subsequent SEM / EDS characterization results, this further illustrates the formation of the SiO2 modified component on the steel fiber surface.

[0089] like Figure 2 As shown, compared with the unmodified heat-resistant steel fibers in Comparative Example 1, the surface morphology of the surface-modified heat-resistant steel fibers obtained in Examples 1-3 changed significantly, with increased surface undulation and improved surface roughness. Specifically, the arithmetic mean height Sa of the steel fibers in Comparative Example 1 was 0.61 μm, while in Examples 1-3 it increased to 3.51 μm, 4.14 μm, and 3.24 μm, respectively. This indicates that SiO2 surface modification can form a rough modified region on the steel fiber surface, thereby increasing the effective contact area and mechanical embedding effect between the steel fiber and the castable matrix.

[0090] Meanwhile, the wettability of the steel fibers was improved after surface modification. The initial water contact angle of the steel fibers in Comparative Example 1 was 69.95°, while those in Examples 1-3 were 65.40°, 55.45°, and 55.85°, respectively. As the wetting time increased to 30 s, the contact angle of Comparative Example 1 decreased to 53.2°, while that of Examples 1-3 decreased to approximately 48.0°, 37.4°, and 46.1°, respectively. Example 2 exhibited a lower water contact angle and higher surface roughness, indicating that the SiO2 modified layer obtained under these process conditions can effectively improve the surface wetting behavior of the steel fibers. This surface condition facilitates the spreading of the castable slurry on the steel fiber surface and the effective contact of the fiber-matrix interface, providing favorable conditions for improving interfacial bonding performance.

[0091] like Figure 3 As shown, under drying conditions of 110 ℃ and heat treatment conditions of 1100 ℃ and 1350 ℃, the load-displacement responses of different steel fiber reinforced castables showed significant differences. Compared with Comparative Example 1, the samples of Examples 1-3 maintained a relatively significant post-peak load-bearing capacity after reaching the peak load, and the load gradually decreased with increasing displacement. This indicates that the surface-modified steel fibers can continue to play a role in crack bridging and pull-out energy dissipation after the matrix cracks, thereby delaying crack propagation.

[0092] Under drying conditions at 110 ℃, the load-displacement curves of Examples 1-3 showed a significantly longer peak segment compared to Comparative Example 1, with Example 2 exhibiting a higher peak load and greater post-peak deformation capacity. After heat treatment at 1100 ℃, the peak load of each specimen further increased, and the surface-modified steel fiber reinforced specimen still maintained good post-cracking load-bearing capacity. After heat treatment at 1350 ℃, due to further sintering and densification of the castable matrix, the specimens as a whole exhibited a higher peak load and smaller failure displacement, with fracture behavior tending to be concentrated, but the surface-modified steel fiber reinforced specimen still showed good load-bearing capacity.

[0093] The bending toughness results show that, under various heat treatment conditions, Examples 1-3 are generally superior to Comparative Example 1, with Example 2 showing the most significant improvement. This indicates that appropriate SiO2 surface modification can improve the interfacial bonding between steel fibers and the matrix, allowing the energy-consuming processes such as bridging, interfacial debonding, and pull-out of steel fibers during crack propagation to be more fully utilized, thereby improving the post-cracking load-bearing capacity and bending toughness of the castable.

[0094] like Figure 4 As shown, after high-temperature heat treatment, a relatively obvious interfacial reaction zone was formed between the unmodified steel fibers and the castable matrix in Comparative Example 1. Oxidation of the steel fiber surface and migration of interfacial elements were more pronounced, and interfacial defects were observed in some areas. In contrast, the interfacial structure between the surface-modified steel fibers and the matrix in Examples 1-3 was more complete, the fiber outline was better maintained, and obvious defects at the interface were reduced, indicating that SiO2 surface modification can slow down the oxidation of steel fibers and interfacial deterioration under high-temperature conditions.

[0095] The interface elemental line scan results show that in Comparative Example 1, the oxygen element has a wide distribution range from the matrix side into the steel fiber interior, while elements such as Fe and Cr in the steel fiber exhibit a significant diffusion trend towards the matrix side. After SiO2 surface modification, a Si and O enriched region is formed at the fiber-matrix interface, and the concentration changes between Fe, Cr, and other steel fiber constituent elements and matrix elements are more pronounced. This indicates that the SiO2 modified layer on the steel fiber surface can, to a certain extent, form an element diffusion barrier region, reducing the migration of oxygen into the steel fiber interior and the diffusion of steel fiber alloying elements towards the matrix side.

[0096] In Example 2, the fiber-matrix interface was relatively intact, and the continuity of the interface transition region was good, indicating that an appropriate amount of SiO2 can form a relatively stable modified region on the steel fiber surface and play a role in interface regulation and anti-oxidation under high temperature conditions. When the degree of modification is further increased, uneven deposition or agglomeration of local SiO2 particles may affect the uniformity of the interface structure. Therefore, a higher amount of SiO2 precursor added does not necessarily lead to a more significant interface improvement effect.

[0097] like Figure 5 As shown, after thermal shock treatment, the degree of damage to the fiber-matrix interface of different steel fiber reinforced castables varies significantly. In Comparative Example 1, obvious cracks and localized interface debonding were observed around the unmodified steel fibers. Some cracks propagated along the steel fiber-matrix interface, indicating that the thermal stress generated by repeated temperature changes tends to concentrate in the interface region and induce interface damage.

[0098] Compared with Comparative Example 1, the overall interface integrity around the surface-modified steel fibers in Examples 1-3 was improved, the number and propagation of interface cracks were reduced, and the steel fibers maintained a good contact state with the matrix. Among them, the fiber-matrix interface in Example 2 was relatively intact, with relatively few obvious interface cracks and debonding areas, indicating that the formed SiO2 modified layer can improve the interfacial bonding between the steel fibers and the aluminosilicate refractory matrix and reduce the tendency of interface damage during thermal cycling.

[0099] The above results indicate that SiO2 surface modification can enhance the fiber-matrix interface bonding by improving the surface roughness and wettability of steel fibers, and can also slow down the oxidation of steel fibers and the diffusion of interfacial elements under high temperature conditions. This reduces interface defects caused by oxidation and the initiation and propagation of cracks under thermal stress, which is beneficial to improving the thermal shock stability of steel fiber reinforced aluminosilicate refractory castables.

[0100] comprehensive Figures 1-5 As can be seen, the surface modification of heat-resistant steel fibers using a combination of surface activation and in-situ SiO2 deposition improves the surface roughness and wettability of the steel fibers, and further enhances the interfacial bonding between the steel fibers and the aluminosilicate refractory castable. At low temperatures, the modified steel fibers improve the effective contact and crack bridging ability of the fiber-matrix interface; at high temperatures, the SiO2-modified region on the steel fiber surface slows down steel fiber oxidation and interfacial element diffusion, maintaining good fiber-matrix interface integrity; and during thermal shock, it reduces the tendency for interfacial cracks and local debonding. Therefore, the surface modification method described in this invention can synergistically improve the comprehensive performance of steel fiber-reinforced aluminosilicate refractory castables from multiple aspects, including surface wetting, interfacial bonding, high-temperature oxidation resistance, and thermal shock stability.

[0101] The surface properties of the steel fibers and the resulting castables in the above embodiments and comparative examples, and the test results of mechanical strength, post-cracking bearing capacity, fracture toughness and thermal shock stability measured by the three-point bending method using a room temperature flexural testing machine are shown in Table 1.

[0102]

[0103] As shown in Table 1, after treating the heat-resistant steel fibers with the surface modification method described in this invention, the surface condition of the steel fibers and the comprehensive performance of the reinforced aluminosilicate refractory castable are significantly improved. Compared with Comparative Example 1, which uses untreated steel fibers, the surface roughness Sa of the modified steel fibers in Examples 1-3 is significantly increased, and the overall contact angle is reduced, indicating that SiO2 modification can improve the surface roughness of steel fibers and improve their wettability. In Example 2, the Sa thickness reached 4.14 μm, and the contact angle decreased to 55.45°. Its flexural strength after heat treatment at 1100 ℃ and 1350 ℃ reached 13.8 MPa and 16.4 MPa, respectively, both higher than the 10.9 MPa and 14.4 MPa of Comparative Example 1. At the same time, the flexural toughness increased from 2.5 J to 4.5 J, the residual strength retention rate after thermal shock increased from 10.7% to 14.8%, the tensile stress increased from 8.5 MPa to 10.1 MPa, and the fracture energy increased from 657.9 J / m² to 1136.8 J / m². This indicates that SiO2 surface modification can effectively improve the interfacial bonding and load transfer capacity between steel fibers and the matrix, and improve the crack propagation resistance and thermal shock stability of the castable.

[0104] Further comparison of Examples 1-3 reveals that a higher theoretical SiO2 modification concentration is not necessarily more beneficial. When the theoretical modification concentration increases from 0.05 wt.% to 0.10 wt.%, the surface roughness and wettability of the steel fibers, as well as the flexural strength, bending toughness, and fracture energy of the castable, are all further improved. However, when the modification concentration continues to increase to 0.15 wt.%, the aforementioned mechanical properties actually decrease, with the fracture energy decreasing from 1136.8 J / m. 2 Decreased to 846.3 J / m 2 This indicates that an appropriate amount of SiO2 is beneficial for forming a more uniform and stable surface modification layer, while excessive SiO2 may lead to particle agglomeration or local non-uniformity of the modification layer, resulting in a decrease in the interface enhancement effect. Therefore, in this set of examples, 0.10 wt.% exhibits better overall performance.

[0105] Furthermore, Comparative Example 3, without LiOH surface activation treatment and using the same SiO2 modification process, exhibited flexural strength at 1100 ℃, flexural strength at 1350 ℃, flexural toughness, and fracture energy of 12.1 MPa, 15.2 MPa, 3.1 J, and 934.5 J / m, respectively. 2All of these values ​​were lower than those of Example 2, which were 13.8 MPa, 16.4 MPa, 4.5 J, and 1136.8 J / m³. 2 This indicates that there is a synergistic effect between the steel fiber surface activation treatment and the subsequent in-situ SiO2 deposition, and that the pretreatment is beneficial to improving the effective deposition of SiO2 on the steel fiber surface and the interface strengthening effect.

[0106] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Any simple modifications, equivalent substitutions, and improvements made by those skilled in the art to the above embodiments without departing from the scope of the technical solution of the present invention, based on the technical essence of the present invention, shall still fall within the protection scope of the technical solution of the present invention.

Claims

1. A surface-modified steel fiber reinforced aluminosilicate refractory castable, characterized in that: The raw materials of the castable include: fused mullite, andalusite, silicon carbide, dense corundum fine powder, α-Al2O3 micro powder, silica micro powder, calcium aluminate cement, dispersant, and surface-modified heat-resistant steel fiber. The surface-modified heat-resistant steel fiber is a heat-resistant stainless steel fiber matrix and a SiO2 modified layer that is tightly bonded to its surface and continuously coated. The SiO2 modified layer is mainly composed of an amorphous Si-O-Si network with Si-OH on the surface. The surface roughness Sa of the surface-modified heat-resistant steel fiber is 3.2~4.2 μm, and the water contact angle of the surface-modified heat-resistant steel fiber is 55°~66°.

2. The surface-modified steel fiber reinforced aluminosilicate refractory castable according to claim 1, characterized in that: In the surface-modified heat-resistant steel fiber, the proportion of the exposed area of ​​the surface not covered by the SiO2 modification layer to the total surface area of ​​the steel fiber is no more than 40%; preferably no more than 5%.

3. The surface-modified steel fiber reinforced aluminosilicate refractory castable according to claim 2, characterized in that: In the surface-modified heat-resistant steel fiber, the apparent coverage of Si element on the surface is ≥60%, the average thickness of the SiO2 modified layer is 150~180 nm, and the length of the continuous uncoated section within any 1 mm steel fiber length does not exceed 80 μm.

4. The surface-modified steel fiber reinforced aluminosilicate refractory castable according to claim 3, characterized in that: The preparation method of the surface-modified heat-resistant steel fiber is as follows: heat-resistant steel fiber is placed in an alkaline solution for cleaning and surface activation treatment, then washed with water until neutral and dried; then tetraethyl orthosilicate, hexadecyltrimethylammonium bromide and concentrated ammonia are dispersed in anhydrous ethanol solution, and then the surface-activated heat-resistant steel fiber is added, so that tetraethyl orthosilicate hydrolyzes, condenses and deposits on the surface of the steel fiber to form a continuous SiO2 modified layer.

5. The surface-modified steel fiber reinforced aluminosilicate refractory castable according to claim 4, characterized in that: The alkaline solution is a lithium hydroxide solution with a concentration of 0.1~1.0 mol / L.

6. The surface-modified steel fiber reinforced aluminosilicate refractory castable according to claim 4, characterized in that: The amount of tetraethyl orthosilicate added is 0.1% to 0.52% of the mass of the heat-resistant steel fiber; the amount of tetraethyl orthosilicate added is 4 to 12 wt.% of the mass of the anhydrous ethanol; the mass ratio of tetraethyl orthosilicate to hexadecyltrimethylammonium bromide is 8:

1.

7. The surface-modified steel fiber reinforced aluminosilicate refractory castable according to claim 4, characterized in that: The cleaning and surface activation treatments are performed at temperatures ranging from room temperature to 60°C for 10 to 60 minutes. The hydrolysis-condensation reaction temperature is 40~50℃, and the hydrolysis-condensation reaction time is at least 12 h; After the hydrolysis-condensation reaction is completed, the steel fibers are aged at room temperature for 18-30 h, then filtered, washed with deionized water, and dried at 70-90℃ to obtain heat-resistant steel fibers with a SiO2 modified layer on the surface.

8. A surface-modified steel fiber reinforced aluminosilicate refractory castable according to any one of claims 1 to 7, characterized in that: The castable refractory comprises the following raw materials in parts by weight: 40-55 parts of fused mullite, 15-25 parts of andalusite, 1-5 parts of silicon carbide, 6-12 parts of dense corundum fine powder, 5-10 parts of α-Al2O3 micro powder, 2-6 parts of silica powder, 3-7 parts of calcium aluminate cement, 1-4 parts of surface-modified heat-resistant steel fiber, and 0.05-0.20 parts of dispersant.

9. A surface-modified steel fiber reinforced aluminosilicate refractory castable according to claim 8, characterized in that: The electrofused mullite comprises 20-28 parts of 5-3 mm electrofused mullite, 10-16 parts of 3-1 mm electrofused mullite, 4-8 parts of 1-0 mm electrofused mullite, and 4-8 parts of 325 mesh electrofused mullite; The andalusite comprises 5-10 parts of 3-1 mm andalusite and 10-18 parts of 1-0 mm andalusite; The silicon carbide particle size is 1~0 mm; The particle size of the dense corundum powder is no greater than 0.075 mm; The median particle size d of the α-Al2O3 micro powder 50 The preferred size is 3 μm.

10. A method for preparing the surface-modified steel fiber reinforced aluminosilicate refractory castable according to any one of claims 1 to 9, characterized in that: The steps are as follows: fused mullite, andalusite, silicon carbide, dense corundum fine powder, α-Al2O3 micro powder, silica micro powder, calcium aluminate cement, dispersant, and surface-modified heat-resistant steel fiber are mixed evenly to obtain a dry mixture; water accounting for 3~6 wt.% of the total mass of the dry mixture is added to the dry mixture, stirred, cast into molds, cured, and dried to obtain a surface-modified steel fiber-reinforced aluminosilicate refractory castable.

Citation Information

Patent Citations

  • Surface modified steel fiber toughened bauxite castable and preparation method thereof