A method for producing high-performance polycyclopentene rubber

High-performance polycyclopentene rubber was prepared by modifying the WCl6/toluene solution catalyst and the triisobutylaluminum/toluene solution catalyst modified with n-hexanol. This method overcomes the shortcomings of existing polycyclopentene rubber in terms of low-temperature performance and thermal fluidity, and achieves an overall performance improvement.

CN123062679APending Publication Date: 2026-11-10NINGBO BEIYI NEW MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202611337875.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing polycyclopentene rubber has shortcomings in terms of low heat generation, low fuel consumption, wet grip, fracture strength and abrasion resistance, and has poor thermal fluidity in high-temperature environments, making it difficult to process.

Method used

A catalyst was prepared by mixing a modified WCl6/toluene solution with a hexanol-modified triisobutylaluminum/toluene solution. High-performance polycyclopentene rubber was prepared by ring-opening metathesis polymerization using cyclopentene, 2-norbornene, 2,5-norbornadiene and vinyltriethoxysilane as monomers.

Benefits of technology

It improves the overall performance of polycyclopentene rubber, including low temperature resistance, low heat generation, low fuel consumption, wet grip, fracture strength, abrasion resistance and thermal fluidity, and solves the shortcomings of existing technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_4
    Figure SMS_4
  • Figure SMS_5
    Figure SMS_5
  • Figure SMS_6
    Figure SMS_6
Patent Text Reader

Abstract

This invention discloses a method for producing high-performance polycyclopentene rubber, belonging to the field of polycyclopentene rubber production technology. The method includes the following steps: mixing and aging WCl6 with trichlorophenol in an inert atmosphere and toluene solvent to obtain a modified WCl6 / toluene solution; reacting triisobutylaluminum with n-hexanol in toluene under a nitrogen atmosphere to obtain a n-hexanol-modified triisobutylaluminum / toluene solution; mixing the modified WCl6 / toluene solution with the n-hexanol-modified triisobutylaluminum / toluene solution to obtain a catalyst solution; and conducting a ring-opening metathesis polymerization reaction of cyclopentene, 2-norbornene, 2,5-norbornadiene, and vinyltriethoxysilane in the presence of the catalyst solution under an inert atmosphere and n-hexane solvent to obtain a cyclopentene ring-opening polymer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polycyclopentene rubber production technology, and specifically to a method for producing high-performance polycyclopentene rubber. Background Technology

[0002] Polycyclopentene rubber (CPR) is produced by ring-opening metathesis polymerization (ROMP) of cyclopentene. It is a promising synthetic rubber variety and can be used as a substitute for butadiene rubber in tire production. Pure CPR is a novel elastomer with a linear structure. Due to its linear structure, it has a low glass transition temperature of around -110°C, exhibiting excellent flexibility even at low temperatures. Therefore, pure CPR has better low-temperature resistance than other rubbers.

[0003] By adding end-modifiers as chain transfer agents during polymerization, the ends of the main chain can be modified, improving the affinity of the resulting CPR (carbon precipitate rubber) with the tire filler silica and carbon black. Tires made with modified CPR exhibit low heat generation, low fuel consumption, and excellent wet grip. For example, in patent CN 201480010349.1, the poor wet grip of pure cyclopentene rubber is solved by grafting methoxysilyl groups onto the ends of the ring-opening copolymer copolymerized from cyclopentene and aromatic cyclic olefins. In patent CN201580030431.5, a cyclopentene ring-opening polymer with halogen atoms at the polymer chain ends is manufactured, and the halogen atoms react with the amino groups of a compound containing alkoxysilyl groups and amino groups in the molecule. The modified polymer exhibits excellent low heat generation.

[0004] Although tires made using the modified CPR described above show significant improvements in low heat generation, low fuel consumption, and wet grip, they still have shortcomings in terms of fracture strength and abrasion resistance. For example, in patent CN201680050642.X, a CPR with improved wet grip, low heat generation, and improved fracture strength and abrasion resistance is obtained by copolymerizing norbornene compound with cyclopentene. However, due to the excessive amount of norbornene used, not only will the production cost be greatly increased, but the basic characteristics of CPR will also be lost.

[0005] On the other hand, CPR, due to the lack of branches on its main chain, is considered to exhibit mutual adhesion at high temperatures, resulting in poor thermal flowability and processing difficulties. Therefore, research on improving the thermal flowability of CPR has been ongoing. Patent CN201880012937.7 discloses a cyclopentene ring-opening copolymer with a branched structure, comprising at least four cyclopentene ring-opening polymer chains linked by branched structural units. At least a portion of these cyclopentene ring-opening polymer chains undergoes end modification, thus solving the problem of mutual adhesion and poor thermal flowability of cyclopentene rubber at high temperatures.

[0006] For CPRs to be used in tire production and possess excellent overall performance, they must exhibit superior low-temperature resistance, low heat generation, low fuel consumption, good wet grip, good tensile strength, abrasion resistance, and thermal fluidity. While the above-mentioned technical solutions improve specific properties of CPRs by introducing modifiers, monomers, and improving polymerization processes, they cannot produce CPRs with excellent overall performance. Summary of the Invention

[0007] To address the shortcomings of existing technologies, this invention proposes a method for producing high-performance polycyclopentene rubber.

[0008] The objective of this invention can be achieved through the following technical solutions:

[0009] A method for producing high-performance polycyclopentene rubber includes the following steps:

[0010] A modified WCl6 / toluene solution was prepared by mixing and aging WCl6 with trichlorophenol in an inert atmosphere and toluene solvent.

[0011] Triisobutylaluminum was reacted with n-hexanol in toluene under a nitrogen atmosphere to prepare a n-hexanol-modified triisobutylaluminum / toluene solution.

[0012] The modified WCl6 / toluene solution was mixed with the n-hexanol-modified triisobutylaluminum / toluene solution to prepare a catalyst solution;

[0013] In an inert atmosphere and in a hexane solvent, cyclopentene, 2-norbornene, 2,5-norbornadiene, and vinyltriethoxysilane are subjected to a ring-opening metathesis polymerization reaction in the presence of the catalyst solution to obtain a cyclopentene ring-opening polymer.

[0014] Optionally, when preparing the modified WCl6 / toluene solution, WCl6 is mixed with trichlorophenol and stirred and aged for 20 to 90 minutes under stirring conditions of -30 to 10°C to obtain a 1.0% by weight modified WCl6 / toluene solution.

[0015] Optionally, the amount of trichlorophenol used is 0.5 to 2.0 moles relative to 1.0 mole of WCl6.

[0016] Optionally, before mixing the modified WCl6 / toluene solution with the hexanol-modified triisobutylaluminum / toluene solution, the water content in the reaction system is controlled to be less than or equal to 10 ppm, and the 1,2-pentadiene content in the cyclopentene is less than 10 ppm.

[0017] Optionally, when preparing the hexanol-modified triisobutylaluminum / toluene solution, toluene and triisobutylaluminum are added to a glass container under a nitrogen atmosphere, the glass container is cooled to -45°C, hexanol is added dropwise under stirring, and the mixture is stirred to room temperature after the addition.

[0018] Optionally, the molar ratio of triisobutylaluminum to n-hexanol is 1.0, and the content of the n-hexanol-modified triisobutylaluminum / toluene solution is 2.5% by weight.

[0019] Optionally, the catalyst solution is prepared by mixing the modified WCl6 / toluene solution with the n-hexanol-modified triisobutylaluminum / toluene solution and stirring for 15 min, wherein the Al / W molar ratio in the catalyst solution is 1 to 6.

[0020] Optionally, when carrying out the ring-opening metathesis polymerization reaction, the reaction temperature is -20 to 70°C, the reaction pressure is 0.05 to 0.5 MPa, the polymerization reaction time is 1 to 6 h, the concentration of the polymerization monomer is 10 to 50%, and the amount of catalyst calculated as WCl6 is 0.05 to 1.0% relative to the molar amount of cyclopentene.

[0021] Optionally, the amount of 2-norbornene is 0.03 to 1.8% relative to the molar amount of cyclopentene, the amount of 2,5-norbornadiene is 0.04 to 0.8%, and the amount of vinyltriethoxysilane is 0.01 to 0.5%.

[0022] Optionally, after the ring-opening metathesis polymerization reaction is completed, ethanol is added to terminate the polymerization. The reaction solution is injected into ethanol containing 2,6-di-tert-butyl-p-cresol, the precipitated polymer is recovered, washed with ethanol, and then vacuum dried at 40°C to obtain the cyclopentene ring-opening polymer. The cyclopentene ring-opening polymer has a weight-average molecular weight of 300,000 to 850,000, a molecular weight distribution index of 1.1 to 3, a trans structure content of more than 80% by weight, and a glass transition temperature of -100 to -90°C. Detailed Implementation

[0023] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0024] In some embodiments of the present invention, a method for producing high-performance polycyclopentene rubber is disclosed, comprising the following steps:

[0025] 1. Modification of WCl6: Under an inert atmosphere and in toluene solvent, WCl6 was mixed with trichlorophenol (2,4,6-trichlorophenol, 95-95-4, 99% purity, manufactured by Sigma-Aldrich) activator at -30 to 10°C with stirring, and the mixture was stirred and aged for 20 to 90 minutes to obtain a 1.0% WCl6 / toluene solution. The amount of trichlorophenol activator used was 0.5 to 2.0 mol relative to 1.0 mol of the main catalyst component.

[0026] 2. Alkylaluminum Modification: Under a nitrogen atmosphere, toluene and triisobutylaluminum are added to a glass container with a stir bar. The container is cooled to -45°C, and while stirring vigorously, one-third the molar amount of n-hexanol (one-third the molar amount of triisobutylaluminum) is slowly added dropwise. Then, while stirring, the mixture is allowed to cool to room temperature to obtain a diisobutylaluminum / toluene solution. The prepared diisobutylaluminum / toluene solution is typically stored at room temperature, but the storage period usually does not exceed 24 hours.

[0027] 3. Preparation of the main catalyst: Under nitrogen environment, add the 1% WCl6 / toluene solution obtained in step 1 and the 2.5% diisobutylhexylaluminum / toluene solution obtained in step 2 to a glass container equipped with a stirrer, and stir for 15 minutes to obtain the catalyst solution. The Al / W molar ratio is 1~6. The preparation temperature is room temperature.

[0028] 4. Polymerization: Under an inert atmosphere and in n-hexane solvent, and in a nitrogen environment, cyclopentene, 2-norbornene, 2,5-norbornadiene, vinyltriethoxysilane, and the catalyst solution prepared in step 3 are added to a pressure-resistant glass reaction vessel equipped with a stirrer. The polymerization reaction is carried out at a reaction temperature of -20 to 70°C and a reaction pressure of 0.05 to 0.5 MPa for 1 to 6 hours. The concentration of monomers in the polymerization reaction is 10 to 50%, wherein the amount of 2-norbornene is 0.03 to 1.8% relative to the molar amount of cyclopentene; the amount of 2,5-norbornadiene is 0.04 to 0.8%; and the amount of vinyltriethoxysilane is 0.01 to 0.5%. The catalyst, calculated as WCl6, is used at a molar amount of 0.05 to 1.0% relative to the molar amount of cyclopentene.

[0029] In the modification of WCl6 described in step 1 above, the molar ratio of WCl6 to trichlorophenol activator is preferably 0.9~1.5.

[0030] In step 2 above, the alkylaluminum modification is preferably performed with a triisobutylaluminum to n-hexanol molar ratio of 0.333, and the prepared diisobutyl-n-hexylaluminum / toluene solution has a content of 2.5%.

[0031] In the preparation of the main catalyst described in step 3 above, the amount of organoaluminum used is preferably 2.0-5.0 moles relative to 1.0 mole of WCl6.

[0032] The polymerization described in step 4 above is preferably carried out at a reaction temperature of -10 to 60°C, a reaction pressure of 0.05 to 0.5 MPa, and a polymerization time of 2.0 to 4.0 hours. The concentration of the monomers in the reaction mixture is preferably 15 to 30%, wherein the amount of 2-norbornene is preferably 0.05 to 1.5% relative to the molar amount of cyclopentene; the amount of 2,5-norbornadiene is preferably 0.1 to 0.6%; and the amount of vinyltriethoxysilane is preferably 0.08 to 0.3%. The catalyst, calculated as WCl6, is preferably used at an amount of 0.06 to 0.3% relative to the molar amount of cyclopentene.

[0033] As the main catalyst component in polymerization, WCl6 can be precisely controlled through the complex formed by the complexation reaction between WCl6 and trichlorophenol. This not only improves polymerization activity but also increases the molecular weight of the resulting CPR, enhances trans-selectivity, and reduces gel content. The amount of trichlorophenol activator relative to 1.0 mole of WCl6 is 0.5–2.0 moles; using too little or too much will affect the catalyst activity.

[0034] Modifying triisobutylaluminum (TIBA) with n-hexanol is not intended to alter the aluminum core itself, but rather to utilize controlled alkoxylation to transform some of the Al–C bonds into Al–O–R, thereby converting the originally water-sensitive and overly reactive triisobutylaluminum into a mild and controllable alkylaluminum-alcohol complex.

[0035] Before WCl6 reacts with diisobutylhexylaluminum, the water content must be controlled to ≤10 ppm. WCl6 hydrolyzes immediately upon contact with water to form... , even Precipitation prevents the formation of W–C active species, resulting in the loss of active sites for reaction with alkylaluminum, reducing catalytic activity to zero, and simultaneously releasing HCl that corrodes equipment. Industrially, solvents and olefin monomers are required to be dehydrated to ≤10 ppm, the total amount of dienes in olefins is required to be ≤10 ppm (mol), and the 1,2-pentadiene content in cyclopentene monomers is required to be below 10 ppm. However, dienes can reduce catalyst activity because they form complexes with W.

[0036] In CPR, the proportion of cyclopentene repeating units relative to all repeating units is preferably set to 95 mol% or more. However, as long as the characteristics of CPR can be maintained, repeating units from other monomers that can copolymerize with cyclopentene may also be included. The proportion of repeating units from other monomers relative to all repeating units is preferably 5 mol% or less. As other monomers that can copolymerize with cyclopentene, the introduction of 2-norbornene can improve the fracture strength and abrasion resistance of CPR. The introduction of vinyltriethoxysilane terminal modifier can improve the low heat generation, low fuel consumption, and wet grip of CPR. The addition of 2,5-norbornadiene further improves the fracture strength and abrasion resistance of CPR while solving the problems of high adhesion, poor thermal fluidity, and difficulty in processing CPR at high temperatures.

[0037] When using tungsten-based catalysts, the time to steady state in the cyclopentene polymerization reaction is related to the amount and activity of the catalyst, but the conversion rate of cyclopentene is determined only by the reaction temperature. There is an equilibrium relationship between polymer chain growth and monomer concentration. The activation enthalpy and activation entropy of the reaction are: ΔH = -5.6 kcal / mol. -1 ΔS = -18.5 cal mol -1 K -1 The molecular weight of the polymer is significantly dependent on the applied reaction temperature. Lower polymer molecular weights are observed at higher temperatures. The ring strain energy of cyclopentene is between that of cyclohexene and cyclooctene, at 6.8 kcal / mol. This energy value makes k... 1 and k -1 The equilibrium concentrations of cyclopentene tend to be equal, and ΔS is negative and relatively large, indicating that the equilibrium concentration of cyclopentene exhibits a strong temperature dependence. When cyclopentene is copolymerized with norbornene and other monomers, the concentration of cyclopentene monomer decreases slightly, but this does not lead to a significant change in equilibrium.

[0038] CPR has a weight-average molecular weight of 300,000 to 850,000 and a molecular weight distribution index of 1.1 to 3. If the molecular weight is too low, the rubber properties are poor; if the molecular weight is too high, manufacturing and handling become difficult. CPR contains more than 95% linear structure, more than 80% trans structure by weight, a glass transition temperature of -100 to -90°C, a Mooney viscosity of 40-140, and a gel content of less than 0.02% by weight.

[0039] Compared with existing processes, the present invention uses cyclopentene, 2-norbornene, and 2,5-dinorbornediene as monomers in the polymerization reaction, vinyltriethoxysilane as the end modifier, and modified tungsten-containing catalyst and diisobutylhexylaluminum co-catalyst to produce CPR via ROMP reaction using solution polymerization. The CPR exhibits improved comprehensive performance in terms of low temperature resistance, low heat generation, low fuel consumption, wet grip, fracture strength, abrasion resistance, and thermal fluidity.

[0040]

Preparation Example

[0041] Preparation of aluminum diisobutylhexanoate / toluene solution (2.5%):

[0042] Under nitrogen conditions, 61 parts of toluene and 7.8 parts of a 25.4 wt% triisobutylaluminum / n-hexane solution were mixed.

[0043] Add the contents to a glass container with a stir bar and cool the container to -45°C. Stir vigorously and slowly add 0.32 parts of n-hexanol dropwise. Then, while stirring, allow the mixture to cool to room temperature.

[0044] Modification of WCl6:

[0045] Under nitrogen conditions, 98.5 parts toluene, 1 part WCl6, and 1.5 parts trichlorophenol solvent were added to a glass container with a stir bar. The container was cooled to -30 to 10°C and stirred and aged for 20 to 90 minutes to obtain a 1.0% modified WCl6 / toluene solution.

[0046] Catalyst preparation:

[0047] Under nitrogen conditions, 87 parts of a 1.0 wt% WCl6 / toluene solution and 43 parts of a 2.5 wt% diisobutyl-n-hexylaluminum mono / toluene solution prepared in Reference Example 1 were added to a glass container with a stirrer and stirred for 15 minutes to obtain a catalyst solution.

[0048] [Examples 1-7]

[0049] Under nitrogen conditions, metered amounts of monomers cyclopentene, 2-norbornene, 2,5-norbornadiene, and vinyltriethoxysilane, along with a catalyst solution prepared in the preparation example, are added to a pressure-resistant glass reaction vessel equipped with a stirrer. The monomer concentration is 10–50%, wherein the amount of 2-norbornene is 0.03–1.8% relative to the molar amount of cyclopentene; the amount of 2,5-norbornadiene is 0.04–0.8%; and the amount of vinyltriethoxysilane is 0.01–0.5%. The catalyst, calculated as WCl6, is 0.05–1.0% relative to the molar amount of cyclopentene. The reaction temperature is -20–70°C, the reaction pressure is 0.05–0.5 MPa, and the polymerization reaction time is 1–6 hours. After the polymerization reaction was completed, excess ethanol was added to the pressure-resistant glass reaction vessel to terminate the polymerization. The solution in the pressure-resistant glass reaction vessel was then injected into a large excess of ethanol containing 2,6-di-tert-butyl-p-cresol (BHT). The precipitated polymer was then recovered, washed with ethanol, and dried under vacuum at 40°C for 3 days to obtain the cyclopentene ring-opening polymer. The number-average molecular weight and molecular weight distribution index of the sample were determined using a Shimadzu LC-10AVP gel permeation chromatography (GPC) system at 25°C, with tetrahydrofuran as the mobile phase and a flow rate of 1.0 ml / min. The contents of the direct and trans structures were determined using a Bruker AVANCE400 superconducting nuclear magnetic resonance spectrometer (¹H-NMR) at 25°C, with deuterated chloroform (CDCl₃) as the solvent, and calibrated using TMS. The glass transition temperature was determined using a TA MDSC2910 differential scanning calorimeter (DSC). The modulation cycle was 60 seconds, the modulation amplitude was ±1.5℃, the heating rate was 10℃ / min, nitrogen protection was used, and the flow rate was 50mL / min. Mooney viscosity was tested according to the method specified in national standard GB / T1232.1-2000. The gel content was tested by placing the polymer in a stainless steel mesh, immersing it in toluene for a certain time, and measuring the percentage of the portion insoluble in toluene. The polymerization conversion rate was calculated from the weight of the obtained polymer using the formula (W1-W2) / W1×100%, where W1 is the mass of the polymerized monomer and W2 is the mass of the obtained polymer. Catalyst preparation conditions and polymerization conditions are shown in Table 1, and the test results of the prepared CPR samples are shown in Table 2.

[0050] [Comparative Examples 1-3]

[0051] Under nitrogen conditions, measured amounts of monomers cyclopentene, 2-norbornene, 2,5-norbornadiene, and vinyltriethoxysilane, along with a catalyst solution prepared in the preparation example, were added to a pressure-resistant glass reaction vessel equipped with a stirrer for polymerization. The reaction conditions and results are shown in Tables 1 and 2.

[0052] Table 1

[0053]

[0054] Table 2

[0055]

[0056]

Test Examples 1-7

[0057] The performance of the rubbers obtained in Examples 1-7 and the comparative examples was evaluated. First, they were blended with isoprene rubber and vulcanized to prepare vulcanized rubber. Following the method specified in GB / T 6038-2006 "Rubber Test Compounds - Batching, Mixing and Vulcanization Equipment and Operating Procedures", 100 parts by weight of one of the rubbers obtained in Examples 1-7 and Comparative Examples 1-3 were mixed with 100 parts by weight of isoprene rubber, 3 parts by weight of zinc oxide, 4 parts by weight of stearic acid, 1 part by weight of antioxidant 4020, 1 part by weight of antioxidant RD, 48 parts by weight of carbon black N330, 1.8 parts by weight of accelerator NS, 1.5 parts by weight of sulfur, and 8 parts by weight of aromatic oil to obtain compound rubbers. Then, they were vulcanized according to the method specified in GB / T528-2009 "Determination of Tensile Stress-Strain Properties of Vulcanized Rubber or Thermoplastic Rubber" to obtain vulcanized rubber. The tensile strength, elongation at break, permanent stress at break, and stress at a given elongation of the samples were tested according to GB / T 528-2009 "Determination of Tensile Stress-Strain Properties of Vulcanized Rubber or Thermoplastic Rubber". The tear strength of the samples was tested according to GB / T 529-2008 "Determination of Tear Strength of Vulcanized Rubber or Thermoplastic Rubber (Pants-shaped, Right-angled and Crescent-shaped Specimens)". The resilience of the samples was tested according to GB / T1681-2009 "Determination of Resilience of Vulcanized Rubber". The wet slip resistance of the samples was determined by pressing and crosslinking the rubber composition at 160℃ for 20 minutes to prepare test pieces. The tanδ at 0℃ was measured using the specified ARES at a dynamic strain of 0.5% and 10Hz on the obtained test pieces. The low-heating properties of the samples were assessed by compressing and crosslinking the rubber composition at 160°C for 20 minutes to prepare test pieces. The tanδ of these test pieces at 60°C was measured using the specified ARES at a dynamic strain of 2.0% and a frequency of 10 Hz. The thermal fluidity of the samples was evaluated by measuring the storage modulus G' at 108°C at a frequency of 0.1 Hz using a viscoelasticity measuring device.

[0058] The above measurement results were calculated with the measured value of the sample of Comparative Example 1 as 100. The measurement results of each sample are shown in Table 3.

[0059]

[0060] As shown in Tables 1 and 2, cyclopentene ring-opening polymers were obtained in Examples 1–7 under the following conditions: monomer concentration 10–50%, catalyst dosage (based on WCl6) 0.05–1.00%, 2-norbornene dosage 0.03–1.80%, 2,5-norbornadiene dosage 0.04–0.80%, Al / W molar ratio 1.0–6.0, WCl6 / trichlorophenol molar ratio 0.5–2.0, reaction temperature -20–70°C, reaction time 1.0–6.0 h, and reaction pressure 0.05–0.50 MPa. The obtained cyclopentene ring-opening polymers had a weight-average molecular weight of 302,000–683,000, a molecular weight distribution index of 1.50–2.8, a trans content of 82.2–85.6%, a glass transition temperature of -92.6–90.3°C, and a monomer conversion rate of 83.5–85.4%. The above results indicate that, under the conditions of modified tungsten catalyst, modified alkylaluminum co-catalyst, and combination of cyclopentene, 2-norbornene, 2,5-norbornadiene, and vinyltriethoxysilane as defined in this invention, polycyclopentene rubber with higher molecular weight, narrower molecular weight distribution, higher trans structure content, and lower glass transition temperature can be prepared.

[0061] Furthermore, as shown in Table 3, when using Comparative Example 1 as the benchmark, the relative indices of thermal fluidity in Examples 1-7 are 148-250, low heat generation relative index is 80-85, wet skid resistance relative index is 116-150, tear strength relative index is 180-231, rolling resistance relative index is 80-85, and abrasion volume relative index is 72-80. Compared with Comparative Example 1 without the addition of 2-norbornene and 2,5-norborndiene, Examples 1-7 show a comprehensive improvement trend in thermal fluidity, low heat generation, wet skid resistance, tear strength, rolling resistance, and abrasion resistance. This indicates that the present invention uses cyclopentene, 2-norbornene, 2,5-norborndiene, and vinyltriethoxysilane in a modified tungsten-based catalytic system for ring-opening metathesis polymerization, which enables the resulting polycyclopentene rubber to maintain a low glass transition temperature while possessing good processing and tire rubber-related properties.

[0062] Comparative Example 2, based on Example 7, did not include 2,5-norbornadiene, and Comparative Example 3, based on Example 7, also did not include 2-norbornadiene. According to Table 3, although Comparative Examples 2 and 3 showed changes in some individual indicators, neither simultaneously achieved the balanced results of Example 7 in multiple indicators such as low heat generation, anti-slip properties, rolling resistance, and wear volume. These results indicate that, under the same catalyst dosage, Al / W molar ratio, WCl6 / trichlorophenol molar ratio, reaction temperature, reaction time, and reaction pressure, simultaneously introducing 2-norbornadiene and 2,5-norbornadiene, combined with vinyltriethoxysilane, is more beneficial for obtaining polycyclopentene rubber with balanced overall performance.

[0063] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0064] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the claimed invention.

Claims

1. A method for producing high-performance polycyclopentene rubber, characterized in that, The process includes the following steps: mixing and aging WCl6 with trichlorophenol in an inert atmosphere and toluene solvent to obtain a modified WCl6 / toluene solution; Triisobutylaluminum was reacted with n-hexanol in toluene under a nitrogen atmosphere to prepare a n-hexanol-modified triisobutylaluminum / toluene solution. The modified WCl6 / toluene solution was mixed with the n-hexanol-modified triisobutylaluminum / toluene solution to prepare a catalyst solution; In an inert atmosphere and in a hexane solvent, cyclopentene, 2-norbornene, 2,5-norbornadiene, and vinyltriethoxysilane are subjected to a ring-opening metathesis polymerization reaction in the presence of the catalyst solution to obtain a cyclopentene ring-opening polymer.

2. The method for producing high-performance polycyclopentene rubber according to claim 1, characterized in that, In preparing the modified WCl6 / toluene solution, WCl6 and trichlorophenol are mixed and stirred and aged for 20 to 90 minutes under stirring conditions of -30 to 10°C to obtain a 1.0% by weight modified WCl6 / toluene solution.

3. The method for producing high-performance polycyclopentene rubber according to claim 1 or 2, characterized in that, The amount of trichlorophenol used is 0.5 to 2.0 moles relative to 1.0 mole of WCl6.

4. The method for producing high-performance polycyclopentene rubber according to claim 1, characterized in that, Before mixing the modified WCl6 / toluene solution with the hexanol-modified triisobutylaluminum / toluene solution, the water content in the reaction system is controlled to be less than or equal to 10 ppm, and the 1,2-pentadiene content in the cyclopentene is less than 10 ppm.

5. The method for producing high-performance polycyclopentene rubber according to claim 1, characterized in that, In preparing the hexanol-modified triisobutylaluminum / toluene solution, toluene and triisobutylaluminum are added to a glass container under a nitrogen atmosphere, the glass container is cooled to -45°C, hexanol is added dropwise under stirring, and the mixture is stirred to room temperature after the addition.

6. The method for producing high-performance polycyclopentene rubber according to claim 1 or 5, characterized in that, The molar ratio of triisobutylaluminum to n-hexanol is 1.0, and the content of the n-hexanol-modified triisobutylaluminum / toluene solution is 2.5% by weight.

7. The method for producing high-performance polycyclopentene rubber according to claim 1, characterized in that, The catalyst solution is prepared by mixing the modified WCl6 / toluene solution with the n-hexanol-modified triisobutylaluminum / toluene solution and stirring for 15 min. The Al / W molar ratio in the catalyst solution is 1-6.

8. The method for producing high-performance polycyclopentene rubber according to claim 1, characterized in that, When carrying out the ring-opening metathesis polymerization reaction, the reaction temperature is -20 to 70°C, the reaction pressure is 0.05 to 0.5 MPa, the polymerization reaction time is 1 to 6 h, the concentration of the monomer in the polymerization reaction is 10 to 50%, and the amount of catalyst calculated as WCl6 is 0.05 to 1.0% relative to the molar amount of cyclopentene.

9. The method for producing high-performance polycyclopentene rubber according to claim 1 or 8, characterized in that, The amount of 2-norbornene is 0.03 to 1.8% relative to the molar amount of cyclopentene, the amount of 2,5-norbornadiene is 0.04 to 0.8%, and the amount of vinyltriethoxysilane is 0.01 to 0.5%.

10. The method for producing high-performance polycyclopentene rubber according to claim 1, characterized in that, After the ring-opening metathesis polymerization reaction is completed, ethanol is added to terminate the polymerization. The reaction solution is then injected into ethanol containing 2,6-di-tert-butyl-p-cresol, and the precipitated polymer is recovered. After washing with ethanol, the polymer is dried under vacuum at 40°C to obtain the cyclopentene ring-opening polymer. The cyclopentene ring-opening polymer has a weight-average molecular weight of 300,000 to 850,000, a molecular weight distribution index of 1.1 to 3, a trans structure content of more than 80% by weight, and a glass transition temperature of -100 to -90°C.

Citation Information

Patent Citations

  • Cyclopentene ring-opening copolymer, method for producing same, and rubber composition

    CN105073823A

  • Cyclopentene ring-opening polymer and method for producing same, polymer composition, and polymer crosslinked product

    CN106459383A

  • Cyclopentene ring-opened copolymer

    CN107922594A

  • Cyclopentene ring-opening copolymer and method for producing same

    CN110312749A