A textile fiber auxiliary agent with high emulsification stability and its preparation method

By initiating free radical polymerization at the oil-water interface to generate a high-molecular surfactant and chemically bonding it, combined with polyether-modified silicone oil and isomeric alcohol polyoxyethylene ether, the problem of emulsion stability of textile fiber auxiliaries is solved, achieving high stability and consistent finishing effect.

CN123064016APending Publication Date: 2026-11-10HANGZHOU HUIHE NEW MATERIAL TECHNOLOGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611409229.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Traditional textile fiber auxiliaries suffer from problems such as poor emulsion stability, easy stratification, and short storage period during the emulsification process, which affect the consistency of finishing effect and the reliability of industrial application.

Method used

Amphiphilic reactive emulsifying monomers are used to initiate free radical polymerization at the oil-water interface, generating high molecular surfactants that are chemically bonded to the interface. Combined with polyether-modified silicone oil and isomeric alcohol polyoxyethylene ether, chemical anchoring barriers and steric hindrance are formed, enhancing the mechanical strength and hard water resistance of the interfacial film.

Benefits of technology

It improves the stability of the emulsion, ensures the reproducibility and washability of the soft and smooth finishing effect, reduces stratification and flocculation, and enhances storage stability and consistency of finishing effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123064016A_ABST
    Figure CN123064016A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of textile fiber auxiliaries technology and discloses a textile fiber auxiliary with high emulsification stability and its preparation method, comprising: 15-25% amino silicone oil; 5-12% amphiphilic reactive emulsifying monomer; 3-8% isomeric alcohol polyoxyethylene ether; 1-4% fatty alcohol polyoxyethylene ether; 2-6% polyether-modified silicone oil; 0.05-0.3% oil-soluble initiator; 2.5-4% glacial acetic acid; and the balance being propylene glycol. The amphiphilic reactive emulsifying monomer initiates free radical polymerization at the oil-water interface, converting it in situ into a high molecular weight surfactant, which is then chemically bonded to the oil-water interface film. This enhances the mechanical strength and density of the interface film. Even after high temperature, high shear pumping, or months of standing, the emulsifier molecules will not desorb from the interface. After the emulsifier is fixed at the interface through polymerization, the average particle size and distribution of the emulsion are frozen at the ideal state at the end of shearing, thus ensuring extremely high reproducibility of the soft and smooth finishing effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of textile fiber auxiliaries technology, specifically a textile fiber auxiliary agent with high emulsification stability and its preparation method. Background Technology

[0002] In textile fiber processing, textile fiber auxiliaries are often applied in emulsion form to finish fibers such as softening, smoothing, and antistatic properties. However, traditional fiber finishing auxiliaries generally suffer from problems such as poor emulsion stability, easy stratification, and short storage period during emulsification, which directly affect the consistency of finishing effects and the reliability of industrial applications.

[0003] Currently, to improve emulsion stability, the common practice in the field is to use a variety of low-molecular-weight emulsifiers in combination to form a mixed emulsifier system to match the hydrophilic-lipophilic balance (HLB) value of the oil phase components. Patent CN115948918A discloses a textile softener and its preparation method, using a mixture of dehydrated sorbitan fatty acid ester and fatty alcohol polyoxyethylene ether as the emulsification system. However, these low-molecular-weight emulsifiers mainly locate at the oil-water interface through physical adsorption, resulting in weak binding forces between them and the oil phase droplets. During high-temperature storage, high-shear processing, or long-term storage, emulsifier molecules are prone to desorption from the interface, leading to droplet aggregation, merging, and stratification. Ultimately, this reduces the emulsification stability of the textile fiber auxiliaries, resulting in batch-to-batch variations in finishing effects. Summary of the Invention

[0004] To address the problems mentioned in the background section, this invention provides a textile fiber auxiliary agent with high emulsification stability and its preparation method.

[0005] To achieve the above objectives, the present invention provides the following technical solution: a textile fiber auxiliary agent with high emulsification stability, comprising: 15-25% amino silicone oil; 5-12% amphiphilic reactive emulsifying monomer; 3-8% isomeric alcohol polyoxyethylene ether; 1-4% fatty alcohol polyoxyethylene ether; 2-6% polyether-modified silicone oil; 0.05-0.3% oil-soluble initiator; 2.5-4% glacial acetic acid; and the balance being propylene glycol.

[0006] Preferably, the amino silicone oil is an amino-terminated modified polydimethylsiloxane with an ammonia value of 0.3-0.9 mmol / g.

[0007] Preferably, the amphiphilic reactive emulsifying monomer is an amphiphilic reactive emulsifying monomer that simultaneously contains hydrophilic polyethylene glycol segments and hydrophobic long-chain alkyl groups, and whose end groups have carbon-carbon double bonds that can participate in free radical polymerization.

[0008] Preferably, the isomeric alcohol polyoxyethylene ether is isomeric deca-ol polyoxyethylene ether or isomeric trideca-ol polyoxyethylene ether, with an HLB value of 10-14.

[0009] Preferably, the fatty alcohol polyoxyethylene ether is one or a mixture of two or more of AEO-3, AEO-5 or AEO-9.

[0010] Preferably, the polyether-modified silicone oil is polyethylene glycol-grafted modified polydimethylsiloxane, wherein the degree of polymerization n of the polyethylene glycol segment is selected from 13-40, and the degree of polymerization m of the organosiloxane segment is selected from 20-70.

[0011] Preferably, the oil-soluble initiator is one of azobisisobutyronitrile (AIBN) and benzoyl peroxide.

[0012] The above-mentioned method for preparing a high emulsification stability textile fiber auxiliary agent includes the following steps: Step 1: Weigh out the following ingredients by weight percentage: amino silicone oil, amphiphilic reactive emulsifying monomer, isomeric alcohol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, polyether modified silicone oil, oil-soluble initiator, glacial acetic acid, and propylene glycol. Step 2: Add propylene glycol to the reactor, control the reactor temperature to 40-50℃, add amphiphilic reactive emulsifying monomers, isomeric alcohol polyoxyethylene ethers and fatty alcohol polyoxyethylene ethers, stir for 15-25 minutes until fully dissolved, forming a homogeneous organic phase emulsifier solution. Step 3: Slowly add amino silicone oil and polyether modified silicone oil to the reaction vessel and perform high-speed shear emulsification at a speed of 1500-3000 r / min for 20-40 minutes to form a uniform milky white primary emulsion. Step 4: Add an oil-soluble initiator to the emulsion, heat to 60-75℃, and stir under nitrogen protection for 1-3 hours to initiate the free radical polymerization reaction of the amphiphilic reactive emulsion monomer at the oil-water interface, generating an interfacial crosslinking network in situ. Step 5: After the reaction is complete, cool the temperature to 40-50℃, add glacial acetic acid to adjust the pH of the system to 4-7, and continue stirring for 10-15 minutes. Step 6: Cool to room temperature, filter, discharge, package and store.

[0013] Preferably, in step four, the temperature is raised to 65-70°C, and the stirring time is maintained for 1.5-2.5 hours.

[0014] Preferably, the nitrogen flow rate for nitrogen protection in step four is 0.5-2.0 L / min.

[0015] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. By using amphiphilic reactive emulsifying monomers (containing terminal methacrylate groups) to initiate free radical polymerization at the oil-water interface, the emulsifiers are converted in situ into high molecular weight surfactants and locked onto the oil-water interface film by chemical bonding, which enhances the mechanical strength and density of the interface film. Even after high temperature, high shear pumping or standing for several months, the emulsifier molecules will not desorb from the interface. 2. After the emulsifier is fixed at the interface through polymerization reaction, the average particle size and distribution of the emulsion are frozen at the ideal state at the end of shearing, and do not coarsen over time. When each batch of products is applied to fibers, the spreading and film-forming behavior of amino silicone oil droplets on the fiber surface remains consistent, thus ensuring extremely high reproducibility of the soft and smooth finishing effect. 3. On the one hand, the polymerized reactive monomers constitute the first chemical anchoring barrier; on the other hand, the polyether-modified silicone oil in the formulation contains long-chain polyethylene glycol side chains, which intersect inside and outside the interfacial film, providing strong steric repulsion forces and effectively preventing droplets from approaching. Simultaneously, the unique branched structure of isomeric alcohol polyoxyethylene ether endows the system with excellent hard water resistance and a low gelation temperature. Combined with glacial acetic acid, the pH is precisely controlled at 5.0–6.5, causing the amino silicone oil to be moderately protonated and positively charged, providing electrostatic repulsion. This allows the product to maintain a highly stable dispersion even when diluted with hard water or mixed with anionic or nonionic additives, and it is less prone to oil drift, flocculation, or roller sticking. Attached Figure Description

[0016] Figure 1 This is a flowchart illustrating the overall preparation process of the present invention. Figure 2 The detailed process for preparing the organic phase and emulsion system of this invention is as follows; Figure 3 This is a detailed process of the in-situ polymerization stabilization reaction at the interface according to the present invention; Figure 4 This is a detailed process for pH adjustment, purification, and finished product packaging of the present invention. Detailed Implementation

[0017] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0018] like Figures 1 to 4As shown, this invention provides a textile fiber auxiliary agent with high emulsification stability and its preparation method, comprising: 15%–25% amino silicone oil; 5%–12% amphiphilic reactive emulsifying monomer; 3%–8% isomeric alcohol polyoxyethylene ether; 1%–4% fatty alcohol polyoxyethylene ether; 2%–6% polyether-modified silicone oil; 0.05%–0.3% oil-soluble initiator; 2.5%–4% glacial acetic acid; and the balance being propylene glycol.

[0019] Detailed description of each component: (a) Amino silicone oil: Terminally amino-modified polydimethylsiloxane is selected, with an ammonia value of 0.3–0.9 mmol / g, a number-average molecular weight of 5000–30000, and a viscosity of 100–500 cSt (25℃). Terminally amino-modified silicone oil has lower steric hindrance than side-amino-modified silicone oil, resulting in a more continuous and uniform soft film on the fiber surface. The preferred ammonia value is 0.5–0.7 mmol / g, within which the optimal balance between softness and emulsion stability is achieved.

[0020] (II) Amphiphilic reactive emulsifying monomer: The general structural formula is CH2=C(CH3)-COO-(CH2CH2O)n-CO-(CH2)m-CH3, where n=10~45 and m=11~21. Preferably, n=20~30 and m=15~18. This monomer can be prepared by the following synthetic route (taking n=25, m=17 as an example): Polyethylene glycol monomethyl ether (molecular weight about 1100) is esterified with stearic acid in the presence of a catalyst (p-toluenesulfonic acid) to obtain polyethylene glycol monomethyl ether stearate (amphiphilic intermediate), which is then reacted with methacrylic anhydride in the presence of a polymerization inhibitor to introduce terminal methacrylate groups. After purification, the target product is obtained. This synthetic method is well known to those skilled in the art and will not be described in detail here.

[0021] (iii) Isomeric alcohol polyoxyethylene ether: Isomeric decayl alcohol polyoxyethylene ether (e.g., commercially available Isalchem ​​10 series) or isomeric tridecayl alcohol polyoxyethylene ether (e.g., commercially available Isalchem ​​13 series) are selected, with an HLB value of 10-14, preferably 11-13. Its branched structure endows it with excellent hard water resistance and low gel temperature.

[0022] (iv) Fatty alcohol polyoxyethylene ether: AEO-3 (HLB8), AEO-5 (HLB10), or AEO-9 (HLB13) can be selected, and can be used alone or in combination. It is preferred that AEO-5 and AEO-9 be mixed at a weight ratio of 1:1 to 2:1 so that the HLB value of the composite emulsifier is about 11 to 12, which matches the required emulsification HLB value of amino silicone oil.

[0023] (v) Polyether-modified silicone oil: This is a polyethylene glycol-grafted modified polydimethylsiloxane, with a polyethylene glycol segment degree of polymerization n = 13–40 and an organosiloxane segment degree of polymerization m = 20–70. Preferably, n = 20–30 and m = 35–55. This polyether-modified silicone oil can be prepared by hydrosilylation reaction of hydrogen-containing silicone oil with allyl polyethylene glycol under a platinum catalyst, which is a conventional technique in this field.

[0024] (vi) Oil-soluble initiator: One of azobisisobutyronitrile (AIBN) and benzoyl peroxide is selected. AIBN is preferred because it has a moderate decomposition temperature (gradual decomposition begins at 40℃, typical decomposition temperature is 64℃, 10-hour half-life temperature is 65℃, and 66~72℃ is the commonly used experimental temperature), is easily soluble in organic solvents, and residues are easily removed by washing with water. The amount used is 0.5% to 3.0% of the mass of the amphiphilic reactive emulsifying monomer.

[0025] (vii) Glacial acetic acid: industrial grade, 99% purity.

[0026] (viii) Propylene glycol.

[0027] Detailed description of each step in the preparation method: Step 1: Accurately weigh each component raw material according to the above-mentioned mass percentages. The weighing accuracy should be controlled within 0.1%.

[0028] Step 2: Add propylene glycol to a reactor equipped with a stirrer, thermometer, nitrogen inlet pipe, and reflux condenser. Start stirring and maintain the reactor temperature at 40–50°C (preferably 452°C) using jacketed circulating water. Add the amphiphilic reactive emulsifying monomer, isomeric alcohol polyoxyethylene ether, and fatty alcohol polyoxyethylene ether, and stir at 150–300 r / min for 15–25 minutes until all emulsifiers are completely dissolved, forming a transparent or semi-transparent organic phase solution. Observe the dissolution state during stirring to avoid undissolved particles remaining.

[0029] Step 3: Slowly add amino silicone oil and polyether-modified silicone oil (which can be pre-mixed evenly) to the reactor, controlling the addition rate to be completed within 5-10 minutes. After addition is complete, increase the stirring speed to 1500-3000 r / min (preferably 2000-2500 r / min) for high-speed shear emulsification, with a shearing time of 20-40 minutes (preferably 25-35 minutes). During shearing, the system gradually changes from transparent to milky white, and the viscosity increases slightly. After shearing, take a small amount of emulsion and observe it under an optical microscope. The droplets should be uniformly spherical, and the average particle size should be 200-800 nm (preferably 300-600 nm) measured using a laser particle size analyzer. If the particle size is too large, the shearing time can be appropriately extended or the stirring speed increased; if the particle size is too small (<200 nm), it should be noted that the system may be over-emulsified, leading to an abnormal increase in viscosity.

[0030] Step 4: Dissolve the oil-soluble initiator in a small amount of propylene glycol (approximately 5-10 mL, a small portion of the total volume) to prepare an initiator solution with a mass fraction of 1%-5%. After the primary emulsion temperature stabilizes, slowly add the solution dropwise to the reactor. Purge with high-purity nitrogen (99.99% purity) at a flow rate of 0.5-2.0 L / min for 15-30 minutes to displace air from the reactor. Then, heat the reactor to 60-75°C (preferably 65-70°C) using a jacket heating system. Maintain this temperature under nitrogen protection and stir for 1-3 hours (preferably 1.5-2.5 hours). During this process, the viscosity of the system will increase slightly, but good fluidity should be maintained. If the viscosity increases sharply or gelation occurs, it indicates that the initiator dosage is too high or the temperature is too high, and adjustments should be made accordingly. After the polymerization reaction is complete, take samples to determine the degree of interfacial polymerization to confirm that the reaction has proceeded sufficiently.

[0031] Step 5: After the polymerization reaction is complete, turn off the heating and circulate cooling water through the jacket to lower the temperature inside the reactor to 40–50°C. Slowly add glacial acetic acid while stirring (200–300 r / min), monitoring the pH value of the system with a precision pH meter until the pH stabilizes within the range of 4–7 (preferably 5.0–6.5). The acid addition rate should not be too fast to avoid localized over-acidity, which could lead to excessive protonation and flocculation of the amino silicone oil. After the acid addition is complete, continue stirring for 10–15 minutes to ensure pH uniformity.

[0032] Step Six: Continue to circulate cooling water to cool the emulsion to room temperature (25°C). Filter using a 200-400 mesh stainless steel filter (or bag filter) to remove any small amounts of polymer particles or mechanical impurities. The filtered additive product should be a uniform milky white liquid, free of visible particles or flocculent matter. Seal the qualified product in plastic drums or iron drums lined with plastic bags and store in a cool, dry place.

[0033] Example 1 The high emulsification stability textile fiber auxiliary agent of this embodiment has the following components and their mass percentage content as follows: Amino silicone oil (terminated amino, amine value 0.6 mmol / g, number average molecular weight 15000) 20%; amphiphilic reactive emulsifying monomer (n=25, m=17) 8%; isomeric tridecyl alcohol polyoxyethylene ether (HLB=12) 5%; fatty alcohol polyoxyethylene ether (AEO-5:AEO-9=1:1) 3%; polyether modified silicone oil (n=25, m=45) 4%; azobisisobutyronitrile 0.12%; glacial acetic acid 3%; propylene glycol 56.88%.

[0034] Preparation method: Step 1: Accurately weigh each raw material according to the above mass percentages. Specifically, amino silicone oil 20.0 kg, amphiphilic reactive emulsifying monomer 8.0 kg, isomeric tridecyl alcohol polyoxyethylene ether 5.0 kg, AEO-5 1.5 kg, AEO-9 1.5 kg, polyether-modified silicone oil 4.0 kg, azobisisobutyronitrile 0.12 kg, glacial acetic acid 3.0 kg, and propylene glycol 56.88 kg (total mass 100.0 kg).

[0035] Step 2: Add propylene glycol to a 200 L stainless steel reactor, start stirring (200 r / min), and control the jacket circulating water to stabilize the reactor temperature at 45℃. Add the amphiphilic reactive emulsifying monomer, isomeric tridecyl alcohol polyoxyethylene ether, and AEO-5 / AEO-9 mixture, and stir at 200 r / min for 20 minutes until fully dissolved to obtain a transparent organic phase solution.

[0036] Step 3: Mix the amino silicone oil and polyether-modified silicone oil thoroughly in a beaker beforehand, then slowly add them to the reactor (addition time approximately 8 minutes). After addition, increase the stirring speed to 2500 r / min and perform high-speed shear emulsification for 30 minutes. After shearing, the emulsion is uniformly milky white, and the average particle size observed under a microscope is approximately 450 nm.

[0037] Step 4: Dissolve azobisisobutyronitrile (AIBN) in 5 mL of propylene glycol to prepare an initiator solution, and add it to the reactor. Purge the air with nitrogen (99.99% purity, flow rate 1.0 L / min) for 15 minutes, then raise the temperature to 68°C and maintain the temperature under nitrogen protection with stirring for 2 hours. After the reaction is complete, infrared spectroscopy analysis shows that the characteristic peaks of the carbon-carbon double bonds have essentially disappeared, indicating that the polymerization reaction is complete.

[0038] Step 5: Turn off the heating, cool the water to 45°C, add glacial acetic acid, stir at 250 r / min, monitor the pH with a pH meter until it reaches 5.5, and continue stirring for 12 minutes.

[0039] Step 6: Continue cooling to room temperature (25℃), filter with a 200-mesh stainless steel filter, discharge, and seal in a plastic bucket.

[0040] Upon testing, the textile fiber auxiliary agent obtained in this embodiment is a milky white uniform liquid with a pH of 5.5, a solid content of 26.5%, an average particle size of 480 nm (laser particle size analyzer), and a potential of +38.5 mV.

[0041] Example 2 The high emulsification stability textile fiber auxiliary agent of this embodiment has the following components and their mass percentage content as follows: Amino silicone oil (terminated amino, amine value 0.5 mmol / g, number average molecular weight 20000) 18%; amphiphilic reactive emulsifying monomer (n=30, m=15) 10%; isomeric deca-ol polyoxyethylene ether (HLB=13) 4%; fatty alcohol polyoxyethylene ether (AEO-5) 2%; polyether-modified silicone oil (n=30, m=50) 5%; potassium persulfate 0.15%; glacial acetic acid 3.5%; propylene glycol 57.35%.

[0042] The preparation method is the same as in Example 1, except that: in step two, the temperature inside the reactor is controlled at 48°C and the stirring time is 18 minutes; in step three, the shear emulsification speed is 2800 r / min and the emulsification time is 25 minutes; in step four, the initiator is potassium persulfate, the temperature is raised to 70°C, and the mixture is kept warm and stirred for 1.5 hours; and in step five, the pH is adjusted to 5.0.

[0043] Upon testing, the textile fiber auxiliary agent obtained in this embodiment is a milky white uniform liquid with a pH of 5.0, a solid content of 24.8%, an average particle size of 520 nm, and a potential of +35.2 mV.

[0044] Example 3 The high emulsification stability textile fiber auxiliary agent of this embodiment has the following components and their mass percentage content as follows: Amino silicone oil (terminated amino, amine value 0.7 mmol / g, number average molecular weight 10000) 22%; amphiphilic reactive emulsifying monomer (n=20, m=18) 6%; isomeric tridecyl alcohol polyoxyethylene ether (HLB=11) 6%; fatty alcohol polyoxyethylene ether (AEO-9) 3%; polyether modified silicone oil (n=20, m=35) 3%; AIBA 0.08%; glacial acetic acid 2.8%; propylene glycol 57.12%.

[0045] The preparation method is the same as in Example 1, except that: in step two, the temperature inside the reactor is controlled at 42°C and the stirring time is 25 minutes; in step three, the shear emulsification speed is 2200 r / min and the emulsification time is 35 minutes; in step four, the initiator is AIBA, the temperature is raised to 65°C, and the temperature is maintained and stirred for 2.5 hours; in step five, the pH is adjusted to 6.0.

[0046] Upon testing, the textile fiber auxiliary agent obtained in this embodiment is a milky white uniform liquid with a pH of 6.0, a solid content of 25.2%, an average particle size of 440 nm, and a potential of +41.0 mV.

[0047] Comparative Example 1 (Traditional low-molecular-weight emulsion system, interface-free polymerization) To compare the effect of the in-situ polymerization stabilization mechanism of this invention, this comparative example provides a textile fiber auxiliary agent with essentially the same composition as Example 1, except that: instead of adding amphiphilic reactive emulsifying monomers and oil-soluble initiators, their amounts are replaced proportionally with isotridecyl alcohol polyoxyethylene ether and fatty alcohol polyoxyethylene ether, i.e., isotridecyl alcohol polyoxyethylene ether is 11% (original 5% + 6% replacement), AEO-5 is 3.5% (original 1.5% + 2% replacement), and AEO-9 is 3.5% (original 1.5% + 2% replacement). The total emulsifier amount is the same as in Example 1. The preparation method follows the traditional emulsification process: all emulsifiers are added to the organic phase at 45°C, dissolved, and then amino silicone oil and polyether-modified silicone oil are added. High-speed shear emulsification is performed at 2500 r / min for 30 minutes. After cooling, the pH is adjusted to 5.5 with glacial acetic acid, and the product is discharged. No heating polymerization step is performed.

[0048] Comparative Example 2 (Polymer Thickener Stabilization Scheme) To compare the differences between the interfacial polymerization of this invention and conventional polymer thickening methods, this comparative example provides a textile fiber auxiliary agent with essentially the same components as Example 1. The difference lies in that: instead of adding amphiphilic reactive emulsifying monomers and initiators, their dosage (8%) is replaced with a polymeric thickener, sodium polyacrylate (molecular weight approximately 5 million), at a dosage of 0.5% (to maintain a viscosity level comparable to Example 1). Simultaneously, the dosage of isomeric tridecyl alcohol polyoxyethylene ether is increased to 11% (same as Comparative Example 1), and the total AEO series content is increased to 5% (same as Comparative Example 1). Preparation method: After fully dissolving the thickener in an organic phase at 45°C, an emulsifier is added, followed by the same procedure as Comparative Example 1.

[0049] Application performance testing and results I. Emulsion Stability Test The auxiliary agent samples from Examples 1-3 and Comparative Examples 1-2 were subjected to the following stability tests: (1) Long-term storage stability at room temperature: The sample was sealed in a transparent glass bottle and stored at a constant temperature and humidity of 25°C. The appearance was observed every 30 days, and the time when layering, oil separation or precipitation occurred was recorded.

[0050] (2) High temperature accelerates storage stability: The sample is sealed in a transparent glass bottle and stored in a constant temperature oven at 50℃. The sample is observed every 7 days and the time when instability occurs is recorded.

[0051] (3) Centrifugation stability: Take 10 mL of sample into a centrifuge tube and centrifuge at 3000 r / min for 30 minutes and at 5000 r / min for 60 minutes (enhanced conditions) to observe whether layering, precipitation or oil separation occurs.

[0052] (4) High shear stability: The sample was placed in a high-speed disperser and sheared at 10,000 r / min for 10 minutes. Samples were taken before and after treatment and the droplet morphology was observed under an optical microscope. The average particle size was measured using a laser particle size analyzer, and the particle size change rate was calculated as (|particle size after treatment - particle size before treatment| / particle size before treatment 100%).

[0053] The results are shown in Table 1: Test Project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Stability period at 25°C (in months) >12 >12 >12 Approximately 4 Approximately 6 Stability period at 50°C (in months) >6 >6 >6 Approximately 1 Approximately 2 Centrifuge at 3000 rpm for 30 min No layering No layering No layering Slight stratification Slight stratification Centrifuge at 5000 rpm for 60 min No layering No layering No layering Clearly layered Layering Particle size change rate after high shear (%) <8 <10 <7 >120 >80 Table 1 Comparison of emulsification stability between each example and the comparative example As shown in Table 1, Examples 1-3 significantly outperformed Comparative Examples 1 and 2 in all stability tests. Particularly in the 5000 r / min 60 min intensive centrifugation test, the sample from the examples remained completely homogeneous and did not stratify, while the control sample showed obvious stratification or precipitation, fully verifying the superior effect of the in-situ polymerization stabilization mechanism of the present invention. In the high shear test, the particle size change rate of the sample from the examples was less than 10%, indicating that the interfacial cross-linking network has a strong protective effect on the droplets and can effectively resist external shear stress; while the particle size of the control sample increased by more than 80%, and some droplets underwent irreversible agglomeration, indicating that its interfacial film strength was insufficient. Furthermore, although the addition of a thickener made Comparative Example 2 slightly more stable at room temperature than Comparative Example 1, it was still far inferior to the examples under high shear and intensive centrifugation conditions, proving that simple thickening cannot replace the essential stabilizing effect of interfacial chemical anchoring.

[0054] II. Fiber softening effect test The textile fiber auxiliaries of Examples 1-3 and Comparative Example 1 were applied to pure cotton knitted fabric (specification: 32 count, white) by padding. The process conditions were: auxiliary dosage 40 g / L, one dip and one pad (pick-up rate 75%), pre-drying at 80℃ for 3 minutes, and baking at 150℃ for 2 minutes. Untreated raw fabric was used as a blank control. The softness (referring to ASTM D1388 standard, using the drape test method, sample size 25cm x 2.5cm, the shorter the drape length, the softer the fabric), whiteness (referring to AATCC 110 standard, expressed as CIE whiteness index WI), and softness retention rate after 5 household washes (washing conditions: 40℃ water temperature, standard laundry detergent, tumble drying) of the finished fabrics were tested. The results are shown in Table 2. Test sample Drape (mm) White (WI) Softness retention rate after 5 washes (%) Blank control 68 82.5 - Example 1 42 81.8 92.5 Example 2 44 81.5 91.8 Example 3 41 82.0 93.2 Comparative Example 1 43 81.6 90.5 Table 2 Comparison of fiber finishing effects of various auxiliaries As shown in Table 2, the fiber finishing agents of the present invention are at the same level as Comparative Example 1 (traditional emulsion system) in terms of softening effect. The drape is in the range of 41–44 mm, significantly better than the 68 mm of the blank control, indicating that the interfacial polymer network has no negative impact on the softening activity of amino silicone oil. Regarding whiteness, all samples showed a slight decrease in whiteness after treatment (approximately 1 unit), which is within the normal range. It is noteworthy that the softness retention rate after washing in the embodiments (91.8%–93.2%) is slightly better than that in Comparative Example 1 (90.5%). This may be due to the coating and protection effect of the interfacial polymer network on the amino silicone oil droplets, reducing the mechanical loss of the finishing agent during washing and thus improving the wash resistance of the softening effect.

[0055] III. Consistency Test of Post-Storage Cleaning Effect To investigate the stability of the finishing effect after storage, samples from Example 1 and Comparative Example 1 were stored at 50°C for 3 months, and then pure cotton fabrics were finished using the same padding process. The drape was tested and compared with the finishing effect of fresh samples. Simultaneously, five professional graders conducted a blind evaluation of the hand feel of the finished fabrics (using a 5-point scale, with 5 being the best soft hand feel). The results are shown in Table 3: Test sample Drape after storage (mm) Difference in drape compared to fresh sample Feel rating (after storage) Example 1 (Fresh) 42 - Level 4.5 Example 1 (50℃ for 3 months) 43 +1 Level 4.5 Comparative Example 1 (Fresh) 43 - Level 4.5 Comparative Example 1 (50℃ in March) 52 +9 Level 3.5 Table 3 Comparison of the consistency of finishing effects after high-temperature storage The results showed that after 3 months of high-temperature storage, the finishing effect of the textile fiber auxiliary agent of the present invention remained basically unchanged (drape increased by only 1 mm, and the hand feel rating did not decrease), while the finishing effect of Comparative Example 1 decreased significantly (drape increased by 9 mm, hand feel became stiffer, and the rating dropped to 3.5). This fully demonstrates that the in-situ interfacial polymerization mechanism of the present invention not only improves the storage stability of the auxiliary agent itself, but also ensures a high degree of consistency of the finishing effect during storage.

[0056] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "include," "contain," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus.

[0057] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A textile fiber auxiliary agent with high emulsification stability, characterized in that, include: Amino silicone oil 15-25%; amphiphilic reactive emulsifying monomer 5-12%; 3-8% isomeric alcohol polyoxyethylene ether; 1-4% fatty alcohol polyoxyethylene ether; 2-6% polyether-modified silicone oil; 0.05-0.3% oil-soluble initiator; 2.5-4% glacial acetic acid; balance propylene glycol.

2. The high emulsification stability textile fiber auxiliary agent according to claim 1, characterized in that: The amino silicone oil is an amino-terminated modified polydimethylsiloxane with an ammonia value of 0.3-0.9 mmol / g.

3. The high emulsification stability textile fiber auxiliary agent according to claim 2, characterized in that: The amphiphilic reactive emulsifying monomer is an amphiphilic reactive emulsifying monomer that simultaneously contains hydrophilic polyethylene glycol segments and hydrophobic long-chain alkyl groups, and whose end groups have carbon-carbon double bonds that can participate in free radical polymerization.

4. The high emulsification stability textile fiber auxiliary agent according to claim 3, characterized in that: The isomeric alcohol polyoxyethylene ether is isomeric deca-ol polyoxyethylene ether or isomeric trideca-ol polyoxyethylene ether, with an HLB value of 10-14.

5. The high emulsification stability textile fiber auxiliary agent according to claim 4, characterized in that: The fatty alcohol polyoxyethylene ether is one or a mixture of two or more of AEO-3, AEO-5 or AEO-9.

6. The high emulsification stability textile fiber auxiliary agent according to claim 5, characterized in that: The polyether-modified silicone oil is polyethylene glycol-grafted modified polydimethylsiloxane, wherein the degree of polymerization n of the polyethylene glycol segment is selected from 13-40, and the degree of polymerization m of the organosiloxane segment is selected from 20-70.

7. The high emulsification stability textile fiber auxiliary agent according to claim 6, characterized in that: The oil-soluble initiator is one of azobisisobutyronitrile (AIBN) and benzoyl peroxide.

8. A method for preparing a high emulsification stability textile fiber auxiliary agent according to any one of claims 1-7, characterized in that, Includes the following steps: Step 1: Weigh out the following ingredients by weight percentage: amino silicone oil, amphiphilic reactive emulsifying monomer, isomeric alcohol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, polyether modified silicone oil, oil-soluble initiator, glacial acetic acid, and propylene glycol. Step 2: Add propylene glycol to the reactor, control the reactor temperature to 40-50℃, add amphiphilic reactive emulsifying monomers, isomeric alcohol polyoxyethylene ethers and fatty alcohol polyoxyethylene ethers, stir for 15-25 minutes until fully dissolved, forming a homogeneous organic phase emulsifier solution. Step 3: Slowly add amino silicone oil and polyether modified silicone oil to the reaction vessel and perform high-speed shear emulsification at a speed of 1500-3000 r / min for 20-40 minutes to form a uniform milky white primary emulsion. Step 4: Add an oil-soluble initiator to the emulsion, heat to 60-75℃, and stir under nitrogen protection for 1-3 hours to initiate the free radical polymerization reaction of the amphiphilic reactive emulsion monomer at the oil-water interface, generating an interfacial crosslinking network in situ. Step 5: After the reaction is complete, cool the temperature to 40-50℃, add glacial acetic acid to adjust the pH of the system to 4-7, and continue stirring for 10-15 minutes. Step 6: Cool to room temperature, filter, discharge, package and store.

9. The method for preparing the high emulsification stability textile fiber auxiliary agent according to claim 8, characterized in that: In step four, the temperature is raised to 65-70℃, and the stirring time is 1.5-2.5 hours.

10. The method for preparing the high emulsification stability textile fiber auxiliary agent according to claim 9, characterized in that: The nitrogen flow rate for nitrogen protection in step four is 0.5-2.0 L / min.

Citation Information

Patent Citations

  • Heat-storage warm-keeping nano slurry for improving warm-keeping performance of goose down fabric

    CN115948918A