Carbon composite active material materials and their manufacturing methods, electrodes and their manufacturing methods, and secondary batteries
By coating the surface of the electrode active material in lithium-ion secondary batteries with graphene material and optimizing its structure and content, the problem of low electronic conductivity was solved and the battery capacity was improved.
Patent Information
- Application Number
- CN202480090320.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-03-29
- Filing Date
- 2024-12-16
- Publication Date
- 2026-11-10
AI Technical Summary
In existing lithium-ion secondary batteries, the contact method between the positive electrode active material and the conductive additive results in low electron conductivity. Increasing the amount of conductive additive will reduce the ratio of active material and affect battery capacity.
A surface layer is formed by coating the surface of the electrode active material with graphene material. The coating rate and the content of graphene material are controlled, and the structural defects of the graphene material are optimized. Carbon composite active material is prepared through spraying and firing processes.
It improves the battery's electronic conductivity, reduces the proportion of conductive additives, and increases the amount of active material, thereby increasing the battery's capacity.
Smart Images

Figure CN123076934A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to carbon composite active material materials and their manufacturing methods, electrodes and their manufacturing methods, and secondary batteries. Background Technology
[0002] With the miniaturization and lightweighting of electronic materials and the advancements in HEVs or EVs, there is a demand for miniaturization or increased capacity of secondary batteries, which serve as their power source. In the secondary battery sector, various technologies have been developed for lithium-ion secondary batteries, which offer advantages such as high voltage and high energy density.
[0003] Patent Document 1 discloses the following technology: a composite material is used as the positive electrode active material in a lithium-ion secondary battery, in which a large number of carbon material particles (such as acetylene black) are attached to the surface of a phosphate compound as a conductive additive, and the specific surface area per unit mass of the positive electrode active material is set to a size of more than a specified value. Phosphate compounds have advantages such as high safety, but on the other hand, they have the problem of low electronic conductivity. However, it has been reported that in the aforementioned composite material, the contact area between the positive electrode active material and the conductive additive is increased, and the electronic conductivity is improved.
[0004] However, acetylene black consists of large particles with an average particle size of tens to hundreds of nm, resulting in point contacts with high contact resistance when they come into contact with the active material. In the active material layer where the active material and conductive additive are interconnected through point contacts, it is difficult to form a network for electron conduction, leading to low electronic conductivity. To improve electronic conductivity, the amount of conductive additive needs to be increased to increase the number of contact points. However, increasing the amount of conductive additive reduces the ratio of active material in the electrode, resulting in a decrease in the discharge capacity of the secondary battery using this electrode.
[0005] Patent Document 2 discloses a technique for using graphene as a conductive additive in the positive electrode active material layer. In the positive electrode active material layer where graphene is used as a conductive additive, graphene particles are interconnected through surface contacts to form an electronic conduction network. The active material layer with conductive paths connected by surface contacts has high electronic conductivity.
[0006] Existing technical documents
[0007] Patent documents
[0008] Patent document 1: Japanese Patent Application Publication No. 2002-110162.
[0009] Patent Document 2: Japanese Patent Application Publication No. 2020-21745. Summary of the Invention
[0010] The problem that the invention aims to solve
[0011] In recent years, there has been a demand for further increases in battery capacity in secondary batteries, but neither of the technologies in patent documents 1 and 2 has yet achieved sufficient battery capacity.
[0012] This disclosure was made in view of the above-mentioned circumstances, and its purpose is to provide carbon composite active material materials and related technologies that can improve battery capacity.
[0013] Methods for solving problems
[0014] To achieve the aforementioned objectives, this disclosure provides the following means.
[0015] <Carbon Composite Active Material Materials>
[0016] [1] A carbon composite active material, wherein, It contains electrode active materials and graphene materials. The carbon composite active material has a repose angle of 20° to 45°.
[0017] [2] Based on the carbon composite active material in [1], wherein, The aforementioned graphene material forms a surface layer that coats at least a portion of the surface of the aforementioned electrode active material. The aforementioned surface layer has a coverage rate of over 10%.
[0018] [3] Based on the carbon composite active material of [1] or [2], wherein, The aforementioned graphene material contains anionic functional groups and countercations of these anionic functional groups at its ends. Furthermore, the peak intensity ratio (Id) of the D and G bands in the Raman spectra obtained by Raman spectroscopy is... D / I G () is below 0.50.
[0019] [4] Carbon composite active material according to any one of [1] to [3], wherein, The content ratio of the aforementioned graphene material to the aforementioned electrode active material, by mass ratio, is 0.1 to 2.4.
[0020] [5] A carbon composite active material based on any one of [1] to [4], wherein, The ratio (DG / DA) of the surface dimension DG of the aforementioned graphene material to the particle size DA of the aforementioned electrode active material is 0.002 to 3.000.
[0021] [6] A carbon composite active material based on any one of [2] to [5], wherein, The aforementioned surface layer comprises the aforementioned graphene material and binder.
[0022] [7] A carbon composite active material based on any one of [1] to [6], wherein, The aforementioned electrode active material is a positive electrode active material.
[0023] [8] Based on the carbon composite active material material in [7], wherein, The aforementioned positive electrode active material is a lithium-containing composite oxide.
[0024] Secondary batteries
[0025] [9] A secondary battery, wherein the aforementioned secondary battery has an electrode formed from a slurry comprising a carbon composite active material comprising any one of [1] to [8].
[0026] <Manufacturing Method of Carbon Composite Active Material>
[0027]
[10] A method for manufacturing a carbon composite active material, wherein the carbon composite active material is formed by coating the surface of an electrode active material with graphene material, wherein in the manufacturing method... The device includes a spraying process, in which the aforementioned electrode active material flows within a rotating fluidized bed granulation apparatus, and a solution containing the aforementioned graphene material is sprayed into the rotating fluidized bed granulation apparatus. The aforementioned carbon composite active material has a repose angle of 20° to 45°.
[0028]
[11] According to the method for manufacturing carbon composite active material of
[10] , wherein, The aforementioned spraying shall be carried out under the following conditions: Solution concentration (mass%): 1–10; Spray velocity (g / s): 2~4; Spraying time (minutes): 5-180.
[0029]
[12] According to the method for manufacturing carbon composite active material of
[11] , wherein, It includes a firing process, in which the granules obtained in the aforementioned spraying process are fired under the following conditions. Firing environment: Nitrogen; Firing temperature (°C): 200~350°C; Firing time (hours): 24-48 hours.
[0030]
[13] A method for manufacturing carbon composite active material according to any one of
[10] to
[12] , wherein, The aforementioned carbon composite active material has a surface layer on which the aforementioned graphene material coats at least a portion of the surface of the aforementioned electrode active material, and the coating rate of the aforementioned surface layer is 10% or more.
[0031]
[14] A method for manufacturing carbon composite active material according to any one of
[10] to
[13] , wherein, The aforementioned graphene material contains anionic functional groups and countercations of these anionic functional groups at its ends. Furthermore, the peak intensity ratio (Id) of the D and G bands in the Raman spectra obtained by Raman spectroscopy is... D / I G () is below 0.50.
[0032] Invention Effects
[0033] According to this disclosure, the battery capacity of a secondary battery can be increased. Attached Figure Description
[0034] Figure 1 This image is an image of the electrode active material observed at 4000x magnification using a JEM-ARM200F NEOARM atomic resolution analytical electron microscope (TEM) manufactured by Nippon Electron, and processed using the image analysis software TEM Control System (TEMCON).
[0035] Figure 2 The image is a result of processing the image analysis software Digital Micrograph on an image of the carbon composite active material of one embodiment of the present disclosure observed at 4000x magnification using a JEM-ARM200FNEOARM atomic resolution analytical electron microscope manufactured by Nippon Electronics.
[0036] Figure 3 This is a graph showing the results of the powder resistance measurement.
[0037] Figure 4 This is a simplified diagram illustrating a rotating fluidized bed granulation apparatus. Detailed Implementation
[0038] The present disclosure will now be described in detail with reference to one embodiment.
[0039] In this specification, "XX~YY" refers to "above XX and below YY". Furthermore, in this specification, the lower and upper limits of numerical ranges (e.g., ranges of content) can be independently combined. Additionally, the upper or lower limit of the numerical ranges described in this specification can be replaced with the values shown in the examples.
[0040] [Carbon composite active material materials]
[0041] The carbon composite active material disclosed herein comprises an electrode active material and a graphene material, and has a repose angle of 20° to 45°. The repose angle can be 20° to 40° or 20° to 30°.
[0042] Here, "angle of repose" refers to the angle formed between the inclined surface of a carbon composite active material pile and the horizontal plane when the material is dropped from a certain height and spontaneously forms a stable, non-collapsed pile. The smoother the surface of the carbon composite active material and the stronger its flowability, the smaller the angle of repose. The angle of repose can also be measured using known equipment for determining the properties of powders. For example, it can be measured using a powder analyzer manufactured by Hosokawa Micron Group, Japan.
[0043] The aforementioned graphene material can form a surface layer that coats at least a portion of the surface of the aforementioned electrode active material.
[0044] The coverage rate of the aforementioned surface layer can be 10% or more, 15% or more, or 20% or more.
[0045] Here, "coverage rate" refers to the degree of coverage relative to the particle area of the electrode active material.
[0046] For the coating rate, for example, using a field emission scanning electron microscope (FE-SEM) (Hitachi Advanced Technology SU8600), the observation mode is set to reflective electron image TD (accelerating voltage: 1.5kV during observation, observation magnification: 3500x). Using image processing software ImageJ (National Institutes of Health), threshold processing is used to clarify the difference between the electrode active material (white) and the coated graphene (black), and the coating area is measured, thereby calculating the coating rate relative to the overall area.
[0047] Electrode active materials that do not have the aforementioned surface layer based on the aforementioned graphene material, such as Figure 1 As shown, the surface has unevenness. On the other hand, in the carbon composite active material formed by forming the aforementioned surface layer based on the aforementioned graphene material on the surface of the aforementioned electrode active material, such as... Figure 2 As shown, it has a highly smooth surface.
[0048] like Figure 3 As shown, the carbon composite active material formed by forming a surface layer based on the aforementioned graphene material on the surface of the aforementioned electrode active material has a lower powder resistivity compared to the electrode active material without the aforementioned surface layer based on the aforementioned graphene material. The powder resistivity can be less than 7 Ω·cm, less than 5 Ω·cm, or less than 2 Ω·cm.
[0049] Here, "powder resistance" refers to a parameter used to represent the conductivity of a material itself. Powder resistance is the volume resistivity of the powder, which differs from the resistivity of an electrode. Powder resistance can be measured, for example, using the Nittoseiko Analytech Co., Ltd. powder resistance measurement system MCP-PD51 and low-resistance probe MCP-PD511 for powders, via a four-probe method with constant current application. Specifically, for example, a powder sample can be uniformly mixed and filled into a dedicated measurement unit. A maximum pressure of 20 kN is applied to the powder sample in stages using a built-in load cell. A suitable probe (ring probe or four-probe probe) is selected according to JISK 7194:1994, and a current is applied through the probe to calculate the volume resistivity of the powder.
[0050] In electrodes using carbon composite active material materials formed by forming a surface layer based on the aforementioned graphene material on the surface of the aforementioned electrode active material, electronic conductivity is improved, the ratio of conductive additives in the electrode composition can be reduced, the amount of active material can be increased, and the battery capacity can be improved.
[0051] The mechanism for the aforementioned improved electronic conductivity is speculated to be that, since the graphene material, as a conductive additive, exists in a manner that coats the surface of the aforementioned electrode active material, the conductive additive is efficiently utilized when electrons move within the electrode.
[0052] In carbon composite active material materials, the content of the aforementioned graphene material can be 0.1–2.4% by mass, 0.6–2.4% by mass, or 1.0–2.4% by mass.
[0053] When the graphene content is 0.1% by mass or higher, the highly conductive graphene material uniformly coats the surface of the active material, reducing the proportion of existing conductive additives in the electrode composition. As a result, the amount of conductive additives used can be reduced, while the amount of active material can be increased. This, in turn, improves the overall battery capacity. By limiting the graphene content to 2.4% by mass or lower, material costs are optimized. In other words, by setting the graphene content within the aforementioned range, maximum electrode performance can be achieved with the minimum required amount of graphene.
[0054] The carbon content of graphene materials can be calculated by the difference between the carbon content (mass%) in the carbon composite active material and the carbon content (mass%) in the electrode active material.
[0055] Regarding carbon content, for example, a solid sample can be heated at high temperature in a high-frequency induction furnace, causing the carbon components in the sample to react and vaporize into carbon dioxide. The carbon dioxide is then introduced into an infrared detector, and the absorbance of the carbon dioxide molecules is detected by the infrared detector. The carbon dioxide concentration is calculated based on the absorbance, and the carbon content is calculated from the carbon dioxide concentration data.
[0056] In the carbon composite active material, the content ratio of the aforementioned graphene material to the aforementioned electrode active material, by mass ratio, can be 0.01 to 0.3, 0.01 to 0.17, or 0.01 to 0.06.
[0057] When the carbon composite active material contains a binder, the content of the aforementioned binder in the carbon composite active material can be 0.01 to 0.7% by mass, 0.01 to 0.25% by mass, or 0.01 to 0.06% by mass.
[0058] If the binder content is 0.01% by mass or higher, graphene material exfoliation can be avoided, thus preventing a decrease in conductivity or stability caused by graphene exfoliation. If the binder content is 0.7% by mass or lower, the reduction in the reactive surface area of the electrode active material can be avoided, thus preventing a decrease in the diffusion efficiency of lithium ions or electrolyte caused by the reduction in the reactive surface area of the electrode active material. In other words, by setting the binder content within the above range, electrode performance can be improved without degrading battery characteristics.
[0059] When the carbon composite active material contains a binder, the content ratio of the aforementioned graphene material to the aforementioned binder, by mass ratio, can be 3 to 40, 15 to 40, or 25 to 40.
[0060] If the content ratio is within the above range, the high electronic conductivity of graphene can be effectively utilized, and the structure of the electrode can be stabilized through interaction with the binder, improving the movement path of electrons and lithium ions, thereby reducing the internal resistance.
[0061] In the obtained carbon composite active material, the ratio of the surface dimension DG of the aforementioned graphene material to the particle size DA of the aforementioned electrode active material (DG / DA) can be 0.002 to 3.000, 0.003 to 0.400, or 0.020 to 0.100.
[0062] If the DG / DA ratio is below 3.000, it is easy to coat the surface of the particles of the electrode active material with graphene material. If the DG / DA ratio is above 0.002, the internal resistance (electron / lithium-ion mobility resistance) of the secondary battery using the electrode formed by the carbon composite active material is reduced and the electronic conductivity is increased.
[0063] The face dimension DG of the aforementioned graphene material refers to the face dimension, i.e., the long side of the graphene material in a plate-like shape. Specifically, it can be measured using the method described in the examples.
[0064] The particle size DA of the aforementioned electrode active material refers to the average of the longest and shortest diameters of the electrode active material particles. Specifically, it can be determined using the method described in the examples.
[0065] <Graphene Materials>
[0066] The graphene material contained in the surface layer of the carbon composite active material can also be a graphene material formed by introducing modifying groups into graphene, which serves as the parent material. Specifically, the aforementioned graphene material can also contain anionic functional groups and countercations of these anionic functional groups at its ends, and its Raman spectra are located in the 1300–1400 cm⁻¹ range. -1 The peak intensity of the D band within the range of I D With a height of 1550-1650cm -1 The peak intensity of the G-band within the range of I G Peak intensity ratio (I) D / I G () is a graphene material with a thickness of less than 0.50.
[0067] From the perspective of improving ionic conductivity, graphene materials can also possess a certain degree of structural defects. If graphene materials contain structural defects, ions can move through these defects, thus improving ionic conductivity. On the other hand, if graphene materials have too many structural defects, they become low conductive.
[0068] Structural defects in graphene materials can be determined using Raman spectroscopy. The D band represents peaks originating from defects in the graphene material, while the G band represents peaks originating from the graphite structure. The I band does not normally appear in fully crystalline graphite. D The peak, but with the loss of symmetry in the graphite structure, I D As peak intensity increases, if the graphene material has more structural defects, the peak intensity ratio (I0) will increase. D / I G It also gets bigger.
[0069] By using a counter cation containing an anionic functional group at the end and that anionic functional group, and the aforementioned peak intensity ratio (I) D / I G Using graphene materials with a density below 0.50 as conductive additives can balance ionic conductivity and electrical conductivity.
[0070] Peak intensity ratio (I) D / I G The lower limit is not specified, but from the perspective of current manufacturing technology, it can be above 0.10.
[0071] Peak intensity ratio (I) D / I G The value can be 0.10 to 0.50, 0.11 to 0.40, or 0.12 to 0.30.
[0072] It should be noted that the aforementioned peak intensity ratios are all measured using a solid-state laser as the excitation laser at an excitation wavelength of 514.79 nm. In Raman spectroscopy, graphene powder at 1570 cm⁻¹... -1 Nearby and 1345cm -1 There are peaks nearby.
[0073] (graphene)
[0074] In this disclosure, graphene refers to graphene with a thickness of a single atom. 2 A sheet-like material consisting of stacked sheets of bonded carbon atoms (monolayer graphene). The number of stacked layers can be less than 100, less than 50, or less than 20.
[0075] The average particle size of graphene is not particularly limited; from a dispersibility point of view, it can be 0.5–15 μm, 1.0–10 μm, or 1.5–5 μm. In this disclosure, the average particle size of graphene refers to the particle size that, relative to the particle size distribution, constitutes 50% of the total particle size (D50). The average particle size of graphene can be measured using a laser diffraction type particle size analyzer (e.g., MT3300EXII, manufactured by Microtrac BEL Co., Ltd., Japan).
[0076] Graphene with the aforementioned average particle size can be obtained by pulverizing carbon materials with a particle size of 1–700 μm using a known pulverizing device. The aforementioned carbon material can be 3–500 μm, 5–300 μm, or 10–200 μm. Known pulverizing devices include, for example, dry pulverizing devices such as ball mills, planetary mills, stirred mills, bead mills, jet mills, hammer mills, and high-speed mixers, as well as ball mills, planetary mills, stirred mills, and bead mills that utilize media. From the viewpoint of improving productivity, a high stirring speed and a short stirring time are preferred.
[0077] There is no particular limit to the carbon atom content in graphene; it can be 95% or more by mass, 99% or more by mass, or 100% by mass.
[0078] The content of impurities in graphene is not particularly limited; it can be less than 5% by mass, less than 1% by mass, or even 0% by mass.
[0079] From a dispersive perspective, the thickness of graphene can be 0.3–60.0 nm, 0.3–30.0 nm, or 0.6–12.0 nm.
[0080] The "thickness" mentioned here refers to the thickness of a single layer in the case of a single layer, and to the overall thickness of the layers in the case of multiple layers.
[0081] The thickness of graphene can be measured, for example, using an atomic force microscope.
[0082] (Modifying group)
[0083] In graphene materials, the modifying groups introduced into the graphene that serves as the parent material consist of anionic functional groups and countercations of those anionic functional groups.
[0084] It is inferred that in the aforementioned modified groups, anionic functional groups are bonded to the ends of graphene particles, counteracting the attraction of cations to the surrounding negatively charged graphene.
[0085] As will be discussed later, during the manufacture of graphene materials, the graphite is pulverized, and free radicals are generated at the fracture surface during this process. It is believed that through the free radicals generated at the graphite fracture surface and the weak acid reaction forming a weak acid, the counter anion of the water-soluble salt bonds with the graphene. This bonding can be any of the following: covalent, ionic, or coordination bonds. Alternatively, it can involve the physical adsorption of the water-soluble salt component onto the carbon material.
[0086] The mechanical energy generated during crushing promotes the reaction and bonding of free radicals generated on the fracture surface of graphite with weak acid salts (e.g., lithium acetate).
[0087] If a solvent is added to a graphene material in which modified groups have been incorporated, the aforementioned countercations dissociate in the solvent, and electrostatic repulsion acts on the graphene bonded to anionic functional groups. Therefore, this graphene material exhibits good dispersibility in the solvent and is difficult to re-aggregate.
[0088] By bonding anionic modifiers to graphene, it exhibits a high degree of negative charge in the dispersion. If the negative charge increases, the dispersibility properties described later become higher. General-purpose graphene (e.g., commercially available graphene nanosheets (XGsciense, trade name: R10)) and only pulverized graphite have small negative charges, and van der Waals forces dominate, thus resulting in lower dispersibility properties through aggregation.
[0089] From the perspective of the anionic functional group's ability to counteract the dissociation of cations, the anionic functional group constituting the modifying group can be at least one selected from the group consisting of carboxyl, carbonate, sulfonic acid, and phosphate groups, or it can be a carboxyl or carbonate group.
[0090] From the perspective of ionization trend, the counter cation constituting the modifying group can be selected from at least one of the group consisting of potassium ion, sodium ion, lithium ion, barium ion, calcium ion, magnesium ion, rubidium ion and ammonium ion, or it can be potassium ion, lithium ion and sodium ion.
[0091] When the modifying group consists of an anionic functional group and a countercation of that anionic functional group, the concentration of the countercation in the graphene material can be 50–15000 ppm by mass, 50–13000 ppm by mass, 50–10000 ppm by mass, 50–5000 ppm by mass, or 100–5000 ppm by mass. If the concentration of the countercation is above 50 ppm by mass, the dispersibility of the graphene material in the solvent can be further improved. If it is below 15000 ppm by mass, the electrostatic repulsion acting on the graphene material in the solvent becomes stronger, thus the graphene material can be further maintained in a dispersed state in the solvent.
[0092] The concentration of countercations contained in graphene materials can be determined by ICP-OES (Inductively Coupled Plasma Optical Emission Spectrometry) and ICP-MS (Inductively Coupled Plasma Mass Spectrometry). Specifically, it can be determined by the methods described in the examples.
[0093] (pH)
[0094] The pH (25°C) of the dispersion obtained by dispersing graphene material (concentration: 0.3% by mass) in a mixed solvent containing deionized water and 2-propanol in a volume ratio of 6:4 can be 5.1 to 8.1, 5.5 to 8.0, or 6.0 to 7.9.
[0095] For graphene materials with modifying groups consisting of anionic functional groups and countercations of those anionic functional groups, when the pH is within the aforementioned range, the countercations readily dissociate in the solvent, and the anionic functional groups readily become charged. Consequently, electrostatic repulsion acts on the graphene bonded to the anionic functional groups, thus further improving the dispersibility of the graphene material in the solvent and making it difficult for it to re-aggregate.
[0096] The pH can be set within the above range by appropriately adjusting the properties of graphene, the type of water-soluble salt, the ratio of graphene to water-soluble salt, and the mixing and pulverizing conditions.
[0097] (particle size)
[0098] In the cumulative particle size distribution on a volume basis determined by laser diffraction scattering, the cumulative 50% particle size (D50) of graphene material from the small particle side can be 0.5 to 15.0 μm.
[0099] If the particle size (D50) is above 0.5 μm, the crystallinity of the graphene material is easily maintained, and the dispersibility is improved. If the particle size (D50) is below 15.0 μm, the crystallinity of the graphene material is maintained, and the dispersibility is improved. The particle size (D50) can be 1.0–10.0 μm or 1.5–5.0 μm.
[0100] (Dispersed Indicators)
[0101] For graphene materials, the dispersion index calculated by the following <Equation 1> can be 20-70%.
[0102] <Formula 1>
[0103] Dispersion index (X) [%] = [(Absorbance) / (Absorbance coefficient × Unit thickness) / (Initial concentration)] × 100
[0104] (In Equation 1, the absorbance coefficient is 3200 (L / g·m), the unit thickness is 0.0001 (m), and the initial concentration is the solid component concentration when the graphene material is dispersed in a mixed solvent of water and 2-propanol (IPA) with a volume ratio of water:IPA=6:4, which is set to 3 (g / L).)
[0105] If the aforementioned dispersion index is above 20%, the graphene material exhibits good dispersibility. If the dispersion index is below 70%, maintaining the interparticle distance within the graphene material can reduce cohesion. The aforementioned dispersion index can be 25–65%, or 30–60%.
[0106] The aforementioned dispersion parameters can be set within the above range by appropriately adjusting the average particle size of the carbon material used as the parent material, the concentration of water-soluble salts, the pH of the solvent, and the conductivity of the solvent.
[0107] In graphene materials, the larger the absolute value of the Zeta potential, the greater the electrostatic repulsion between graphene materials, and the more stable the dispersion. From the perspective of further improving the dispersion of graphene materials, the absolute value of the Zeta potential can be 30–60 mV, 30–55 mV, or 30–50 mV.
[0108] (Methods for manufacturing graphene materials)
[0109] The aforementioned graphene material contains anionic functional groups and countercations of these anionic functional groups at its ends, and its Raman spectra are located in the 1300–1400 cm⁻¹ range. -1 The peak intensity of the D band within the range of I D and at 1550-1650cm -1 The peak intensity of the G-band within the range of I G Peak intensity ratio (I) D / I G In the case of graphene materials with a density of 0.50 or less, a method for manufacturing such materials can be, for example, adding a water-soluble salt to graphite and dry mixing it, and then washing the resulting mixture with water.
[0110] Anions released from water-soluble salts bond with graphene and enter the graphene, thereby promoting the exfoliation and fragmentation of the graphene. It should be noted that, in this disclosure, "fragmentation" is not limited to breaking or disintegrating the graphene into smaller pieces than the graphene used as a raw material, but also includes the purpose of simply breaking up the aggregates of graphene.
[0111] The graphene described above can be used.
[0112] There are no restrictions on the type of water-soluble salt, as long as it is soluble in water. Specific examples of water-soluble salts include tripotassium citrate, potassium tartrate, potassium acetate, potassium glutamate, potassium carbonate, and tripotassium phosphate. Furthermore, examples can be made by replacing the potassium in these water-soluble salts with salts of sodium, lithium, barium, calcium, magnesium, rubidium, and ammonium. One type of water-soluble salt can be used, or a combination of two or more can be used.
[0113] The amount of water-soluble salt relative to 100 parts by mass of carbon material can be 1–500 parts by mass, 10–400 parts by mass, or 100–300 parts by mass. When the amount of water-soluble salt is more than 1 part by mass, the dispersibility in the solvent is improved through the formation of graphene material. When the amount of water-soluble salt is less than 500 parts by mass, excessive reaction and adsorption of water-soluble salt can be reduced.
[0114] There are no particular limitations on the environmental conditions for mixing and pulverizing water-soluble salts and graphene. It can be carried out under similar environmental conditions as the aforementioned pulverization, i.e., at room temperature (25°C) in air, or in a nitrogen environment or an inert gas environment such as argon. In addition, it can also be carried out under high or low temperature conditions, or under pressure or depressurization conditions, as needed.
[0115] Regarding the pulverizing apparatus and its examples, as mentioned above, known apparatus can be used without limitation. Examples include dry pulverizing apparatus such as ball mills, bead mills, jet mills, hammer mills, and high-speed mixers. The processing conditions can be appropriately adjusted according to the type and particle size of the carbonaceous material.
[0116] After mixing the water-soluble salt and graphene, the resulting mixture is washed with water. This removes any remaining water-soluble salt.
[0117] The amount of water added during washing is only sufficient to obtain a suspension; there is no particular limitation. Heating can also be performed as needed. For example, add water at a ratio of 10 to 10,000 times the combined mass of the water-soluble salt and carbon material, and mix and stir. The number of washes can be, for example, 2 to 10 times, or 2 to 8 times. The washing conditions can be appropriately set according to the type of graphene and water-soluble salt used.
[0118] After washing, a filter can be used for filtration and separation. The appropriate pore size for the filter is selected based on the intended use of the obtained graphene material. The resulting graphene material can be dried and extracted as a powder, dispersed in a liquid, or used as a paste. Drying can be performed by any method. For example, the graphene material can be dried using spray drying.
[0119] <Adhesive>
[0120] The surface layer of the carbon composite active material disclosed herein may include a binder. The binder serves to connect and fix the electrode active material and the graphene material, and may include at least one selected from the group consisting of fluorinated resins, olefin resins, vinyl resins, polyamides, polyimides, polyethers, polysaccharides, and rubbers.
[0121] For example, it can also be fluoropolymers such as polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polytetrafluoroethylene (PTFE), and ethylene-tetrafluoroethylene copolymer (ETFE); olefin resins such as polyethylene (PE) and polypropylene (PP); vinyl resins such as polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyacrylic acid (PAA), and lithium polyacrylate (LiPAA); polyamide (PA); polyimide (PI); polyethers such as polyethylene oxide (PEO); polysaccharides such as cellulose, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, and regenerated cellulose; and rubbers such as fluororubber, styrene-butadiene rubber (SBR), ethylene-propylene-diolefin rubber (EPDM), and sulfonated EPDM.
[0122] <Electrode Active Materials>
[0123] In the carbon composite active material disclosed herein, the electrode active material can be either a positive electrode active material or a negative electrode active material.
[0124] (Positive electrode active material)
[0125] The positive electrode active material can be a lithium-containing composite oxide.
[0126] The positive electrode active material can also be a lithium-containing composite oxide with at least one crystal structure selected from the group consisting of olivine type, layered rock salt type and spinel type.
[0127] Lithium-containing composite oxides with olivine-type structures can be composite oxides represented by the general formula LiMPO4 (where M is one or more of Fe(II), Mn(II), Co(II), and Ni(II)). Representative examples of the general formula LiMPO4 include LiFePO4, LiNiPO4, LiCoPO4, LiMnPO4, and LiFe... a Ni b PO4, LiFe a Co b PO4, LiFe a Mn b PO4, LiNi a Co b PO4, LiNi a Mn b PO4 (a+b is less than 1, 0<a<1, 0<b<1), LiFe c Ni d Co e PO4, LiFe c Ni d Mn e PO4, LiNi c Cod Mn e PO4 (c+d+e is less than 1, 0<c<1, 0<d<1, 0<e<1), LiFe f Ni g Co h Mn i PO4 (f+g+h+i is less than 1, 0<f<1, 0<g<1, 0<h<1, 0<i<1), etc.
[0128] Lithium-containing composite oxides with a layered rock salt-type crystal structure can be lithium cobalt oxide (LiCoO2), LiNiO2, LiMnO2, Li2MnO3, LiNi 0.8 Co 0.2 O2 and other NiCo-based compounds (general formula is LiNi) x Co 1-x O2 (0 < x < 1)), LiNi 0.5 Mn 0.5 O2 and other NiMn-based compounds (general formula is LiNi) x Mn 1-x O2 (0 < x < 1)), LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2 and other NiMnCo systems (also known as NMC. The general formula is LiNi). x Mn y Co 1-x-y O2 (x > 0, y > 0, x + y < 1)). It can also be Li (Ni). 0.8 Co 0.15 Al 0.05 O2, Li2MnO3-LiMO2 (M=Co, Ni, Mn), etc.
[0129] Lithium-containing composite oxides with a spinel-type crystal structure can be LiMn2O4, Li 1+x Mn 2-x O4, Li(MnAl)2O4, LiMn 1.5 Ni 0.5 O4.
[0130] In addition, the positive electrode active material can also be made of the general formula Li (2-j) MSiO4 (where M is one or more of Fe(II), Mn(II), Co(II), and Ni(II), 0 ≤ j ≤ 2) represents a composite oxide. As a general formula Li (2-j) A representative example of MSiO4 is Li. (2-j) FeSiO4, Li (2-j) NiSiO4, Li (2-j) CoSiO4, Li (2-j)MnSiO4, Li (2-j) Fe k Ni l SiO4, Li (2-j) Fe k Co l SiO4, Li (2-j) Fe k Mn l SiO4, Li (2-j) Ni k Co l SiO4, Li (2-j) Ni k Mn l SiO4 (k+l is less than 1, 0 < k < 1, 0 < l < 1), Li (2-j) Fe m Ni n Co q SiO4, Li (2-j) Fe m Ni n Mn q SiO4, Li (2-j) Ni m Co n Mn q SiO4 (m+n+q is less than 1, 0<m<1, 0<n<1, 0<q<1), Li (2-j) Fe r Ni s Co t Mn u SiO4 (r+s+t+u is less than 1, 0<r<1, 0<s<1, 0<t<1, 0<u<1), etc.
[0131] (Negative electrode active material)
[0132] The negative electrode active material can be carbon materials such as natural graphite, artificial graphite, mesophase carbon microspheres, mesophase carbon fiber (MCF), coke, glassy carbon, and sintered organic compounds; silicon-containing materials SiO2 x (0≤x<2), Sn, aluminum and other metals that can combine with lithium, alloys of these, composite materials of these metals and carbon materials, lithium titanate (Li4Ti5O) 12 Oxides such as SnO2 and metallic lithium. One of these can be used, or a combination of two or more.
[0133] The negative electrode active material can also be selected from materials including graphite and SiO2. x (0≤x<2) and at least one of the group consisting of lithium titanate.
[0134] There are no particular limitations on the shape of the active substance; examples include spherical, non-spherical, scaly, and plate-like shapes. Additionally, the active substance can also be a hollow particle with a void in the center.
[0135] When the active material is a particle, its average particle size can be greater than 1 nm and less than 100 μm, greater than 100 nm and less than 50 μm, or greater than 1000 nm and less than 25 μm.
[0136] It should be noted that the average particle size in this disclosure refers to the particle size D50, which, relative to the particle size distribution, represents 50% of the total particle size and can be measured by a laser diffraction particle size analyzer.
[0137] <Combination of Electrode Active Materials and Graphene Materials>
[0138] The composite of electrode active material and graphene material can be carried out by a spraying process, in which the electrode active material is flowed within a rotating fluidized bed granulator, and a solution containing the aforementioned graphene material is sprayed into the rotating fluidized bed granulator. The carbon composite active material produced by this method comprises the electrode active material and graphene material and has an angle of repose of 20° to 40°.
[0139] The aforementioned rotating fluidized bed granulation device can be as follows: Figure 4 The rotary fluidized bed granulation apparatus shown is an example of such an apparatus. Examples of rotary fluidized bed granulation apparatus include the Multiplex manufactured by Powrex Corporation of Japan and the Flow Coater manufactured by Freund Corporation of Japan.
[0140] The aforementioned solution can be sprayed onto active material particles flowing within a rotating fluidized bed granulation apparatus. During this process, by supplying dry air, inactive gas, or atmospheric conditions at a specific temperature, the solution uniformly adheres to the particle surface and dries. Through this simultaneous spraying / drying process, graphene is efficiently coated onto the surface of the active material particles, improving structural stability in subsequent sintering processes.
[0141] The spray speed of the aforementioned solution can be appropriately set according to the environment of the device (device size, set temperature, etc.) or the amount of active material particles. For example, in the initial stage, in order to prevent the active material particles from agglomerating due to the adhesion of the solution, a low spray speed can be started, and then the speed can be adjusted in stages while checking the uniformity of the particle surface.
[0142] It is also possible to increase the spray speed and the supply of gas used in drying. The time when the gas supply is increased can be simultaneous with the time when the spray speed is increased, or it can be at a different time.
[0143] The spraying temperature can be any temperature that allows volatile components such as solvents and hydrates to evaporate from the aforementioned solution. For example, it can be above 120°C, above 140°C, or above 160°C. Alternatively, to ensure complete removal of volatile components without damaging the active material particles or graphene, the temperature can be below 220°C, below 200°C, or below 180°C.
[0144] There are no particular restrictions on the environment for spraying, but an environment that maintains the chemical stability of the active material particles and the aforementioned solution is recommended. Specifically, this can be an environment where the active material particles and the aforementioned solution are essentially inactive, or a dry air environment or an atmospheric environment, etc.
[0145] The spraying time can be set appropriately by taking into account the size of the device being used and the amount of coating liquid supplied.
[0146] In one embodiment, when the rotary fluidized bed granulation apparatus is a Multiplex manufactured by Powrex Corporation of Japan, the aforementioned spraying can be performed under the following conditions.
[0147] Solution concentration (mass%): 1–10; Spray velocity (g / s): 2~4; Spraying time (minutes): 5-180.
[0148] The process may include a firing step, in which the granules obtained in the aforementioned spraying step are fired to produce a carbon composite active material. The granules obtained in the aforementioned spraying step can be further processed into a carbon composite active material through a subsequent firing step. In this firing step, graphene is firmly bonded to the surface of the active material particles, improving conductivity and structural stability.
[0149] As a firing device, a muffle furnace or a hot plate can be used, but it is not limited to these.
[0150] There are no particular limitations on the firing conditions; they can be appropriately set considering factors such as the firing equipment and the type of graphene material.
[0151] In one embodiment, when the firing apparatus is an explosion-proof dryer, the aforementioned spraying can also be performed under the following conditions: Firing environment: Nitrogen; Firing temperature (°C): 200~350°C; Firing time (hours): 24-48 hours.
[0152] [electrode]
[0153] The electrode disclosed herein can be formed using a slurry containing a carbon composite active material having the aforementioned angle of repose. The electrode's structure and manufacturing method are not particularly limited; any method already known may be used.
[0154] As a carbon composite active material, besides carbon composite active materials with the aforementioned angle of repose, a carbon composite active material can also be obtained by mechanically attaching graphene material to the surface of the electrode active material. Mechanical attachment refers to repeatedly applying shear or compressive forces to a mixture of materials, causing the materials to adhere to each other. This is achieved through a so-called mechanical composite method. The specific method of mechanical composite is not particularly limited; any known composite method can be used. It can be dry composite or wet composite. For example, a binder can be added to an water / IPA solution composed of isopropanol and water to disperse the material, then graphene material can be added, ultrasonically dispersed, centrifuged to prepare a graphene dispersion, and the active material can be mixed in the graphene dispersion, filtered, and dried to obtain the carbon composite active material.
[0155] For example, the positive electrode for a lithium secondary battery according to one embodiment can be manufactured by preparing a slurry by mixing a carbon composite active material having the aforementioned angle of repose, a conductive additive, a binder, and a solvent in a suitable ratio, uniformly coating the slurry onto the positive electrode current collector, drying it, and then pressing it.
[0156] As conductive additives, carbon materials such as Ketjen black, metallic materials such as Al, and conductive oxides can be used. These materials supplement the conductivity of the electrode by combining with carbon composite active materials, thereby maximizing the efficiency of electron conduction from the current collector to the active material. As binders, polyvinylidene fluoride, acrylic resins, polytetrafluoroethylene resins, or rubber-based resins can be used to effectively combine the carbon composite active material and conductive additives, ensuring the long-term stability of the electrode structure.
[0157] As a solvent, N-methylpyrrolidone, water, ethanol, or mixtures thereof can be used. As the positive current collector, a thin metal film mainly containing aluminum can be used. The thickness of the positive current collector is not particularly limited, and can be set to, for example, 5 to 50 μm.
[0158] There are no particular limitations on the method of applying the paste to the current collector, and examples include doctor blade coating, dip coating, reverse roller coating, forward roller coating, gravure printing, extrusion, and brush coating. There are no particular limitations on the amount of paste applied; it can be appropriately set according to the desired thickness of the electrode composite layer.
[0159] There are no particular limitations on the method for drying the slurry on the current collector. Examples include drying based on warm air, hot air, or low-humidity air; vacuum drying; and drying based on (far)infrared radiation, electron beam irradiation, etc. Drying conditions can be appropriately set; for example, the drying temperature can be 50–250°C or 80–200°C. There are no particular limitations on the drying time, which is usually within the range of 10–60 minutes. The electrode can be stabilized by pressing it after drying. Pressing methods include die pressing and roller pressing, but are not limited to these.
[0160] In one embodiment, when the pressing device is a pneumatic-hydraulic heating roller, the aforementioned pressing can be performed under the following conditions.
[0161] Compression pressure: 50~300MPa.
[0162] Compression speed: 0.5~2m / min.
[0163] Pressing temperature: room temperature to 150℃.
[0164] Pressing gap: 30μm~200μm.
[0165] [Rechargeable Battery]
[0166] The secondary battery of this disclosure has the aforementioned electrodes. In other words, in the secondary battery of this disclosure, at least one of the positive or negative electrodes is an electrode of this disclosure. The secondary battery of this disclosure has a high discharge capacity. When one of the positive or negative electrodes is an electrode of this disclosure and the other is not, the electrode of the other electrode is not particularly limited, and any electrode can be used.
[0167] Examples of secondary batteries disclosed herein include lithium-ion secondary batteries, but they can also be applied to next-generation batteries such as sodium-ion batteries, lithium-sulfur batteries, and solid-state batteries.
[0168] In addition to the electrodes described above, the secondary battery of this disclosure may also have an electrolyte layer. For example, the secondary battery of this disclosure is stacked with a positive electrode and a negative electrode facing each other, separated by an electrolyte layer.
[0169] The electrolyte layer can be composed of an electrolyte solution or a solid electrolyte. If the electrolyte layer is an electrolyte solution, it can also be a non-aqueous electrolyte solution formed by dissolving electrolyte salts in a non-aqueous solvent.
[0170] Examples of non-aqueous solvents include ethylene carbonate, fluoroethylene carbonate, chloroethylene carbonate, propylene carbonate, butene carbonate, vinylene carbonate, cyclopentanone, cyclohexylbenzene, sulfolane, propane sulpholactone, 3-methylsulfolane, 2,4-dimethylsulfolane, 3-methyl-1,3-oxazolidine-2-one, γ-butyrolactone, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, methyl butyl carbonate, ethyl propyl carbonate, ethyl butyl carbonate, dipropyl carbonate, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, methyl acetate, ethyl acetate, trimethyl phosphate, and triethyl phosphate. One or more of these can be used in combination.
[0171] Examples of electrolyte salts include lithium salts. There are no particular limitations on lithium salts, as long as they are soluble in non-aqueous solvents and exhibit high ionic conductivity; they can be appropriately selected according to the purpose. Examples include lithium hexafluorophosphate (LiPF6) and lithium tetrafluoroborate (LiBF4).
[0172] The concentration of the electrolyte salt is not particularly limited and can be appropriately selected according to the purpose. From the viewpoint of lithium ion mobility and viscosity, in non-aqueous solvents, it can be 0.5 to 3.0 mol / L or 0.8 to 1.5 mol / L.
[0173] (spacer)
[0174] To prevent short circuits between the positive and negative terminals, a spacer is placed between them.
[0175] Materials used as spacers include, for example, kraft paper, vinylon blended paper, synthetic pulp blended paper, etc.; polyolefin nonwovens such as cellophane, polyethylene grafted film, polypropylene meltblown nonwoven fabric, polyamide nonwoven fabric, glass fiber nonwoven fabric, microporous membrane, etc.
[0176] The size of the spacer is not particularly limited as long as it can be used in an electrochemical device. To ensure uniform ion movement between the positive and negative electrodes, the thickness of the spacer can be appropriately adjusted. For example, by designing the thickness of the spacer to be around 20–40 μm, both low internal resistance and high energy density can be achieved.
[0177] The spacer can be a single-layer structure or a stacked structure.
[0178] It should be noted that when using solid electrolytes, the spacer can be omitted.
[0179] Example
[0180] The present disclosure will now be described in detail with reference to specific examples, but the present disclosure is not limited to these examples.
[0181] <The Making of Positive Electrode>
[0182] The positive electrode active material, conductive additive, and binder were mixed in a ratio of 97:2:1 (unit: wt%) using a rotary mixer (manufactured by Thinky Corporation, product name "Awatori Rentaro") at a speed of 2000 rpm for 2 minutes.
[0183] Then, solvent is added, and using a high-speed mixer (FILMIX), under the conditions of "slurry input of 200g, circumferential speed of 20m / s, and running time of 30 minutes," the amount of solvent is adjusted while mixing until a uniform paste is formed. The solvent content is 87% by mass relative to the total mass of binder and solvent.
[0184] The resulting slurry (hereinafter also referred to as positive electrode paste) is then coated onto the surface of the current collector made of aluminum foil. The coating method uses a doctor blade to form an electrode layer of uniform thickness (82 μm).
[0185] Then, the current collector with the electrode layer formed is dried at 85°C for 24 hours to allow the solvent to evaporate completely.
[0186] Then, by using a pneumatic-hydraulic heating roller, the density of the electrode was increased by applying a pressure of 150 MPa, resulting in a high-performance electrode that can be used as a positive electrode material for secondary batteries.
[0187] (Example 1: Preparation of a comparative positive electrode using acetylene black as a conductive additive)
[0188] The following substances were used as positive electrode active material, binder, conductive additive and solvent to prepare a comparative positive electrode-1 by the method described above in <Preparation of Positive Electrode>.
[0189] Positive electrode active material: lithium nickelate, manufactured by JFE Mineral & Alloy Company, Ltd., with an average particle size D50 of 10 μm.
[0190] Conductive additive: Acetylene black (hereinafter referred to as AB), manufactured by Denka Co., Ltd., with a specific surface area of 68 m². 2 / g, average particle size 35nm.
[0191] Adhesive: Polyvinylidene fluoride (hereinafter PVDF), manufactured by Kureha Corporation.
[0192] Solvent: N-methyl-2-pyrrolidone (hereinafter NMP).
[0193] (Example 2: Fabrication of a comparative cathode using acetylene black and carbon nanotubes as conductive additives)
[0194] As a conductive additive, AB and carbon nanotubes (hereinafter referred to as CNT) were used in a 1:1 ratio, and the ratio of positive electrode paste (positive electrode active material: conductive additive (AB): conductive additive (CNT): PVDF) was set to 97:1:1:1 (unit: wt%). Otherwise, a comparative positive electrode-2 was prepared by the same method as in Example 1.
[0195] The following substances were used as CNTs.
[0196] Conductive additive: CNT, manufactured by Resonac Corporation, SSA: 15m 2 / g, outer diameter: 150nm, length: 4μm.
[0197] (Example 3: Fabrication of a comparative cathode using graphene as a conductive additive - 3)
[0198] Graphene was used as a conductive additive, and the ratio of the positive electrode paste (positive electrode active material: conductive additive (graphene): PVDF) was set to 97:2:1 (unit: wt%). Otherwise, a comparative positive electrode-3 was prepared by the same method as in Example 1.
[0199] The following substances were used as graphene.
[0200] Conductive additive: Graphene, manufactured by Graphene Supermarket, with a specific surface area of 600 m². 2 / g, flake size is 10μm, thickness is less than 1nm, O / C is 0.02.
[0201] (Example 4: Fabrication of a comparative cathode using graphene material with modified groups -4)
[0202] <Fabrication of "Graphene Materials with Modified Groups">
[0203] At room temperature (25°C) and in a nitrogen environment, 4g of natural graphite (ACB-50, manufactured by Nippon Graphite Industries, Ltd., average particle size 350μm) and 8g of potassium L-glutamate were pulverized in a planetary ball mill (Fritsch, model: P-6, ball diameter 10mm, speed 540rpm) for 40 minutes. The pulverized material was then washed with deionized water, filtered, and dried at 60°C to obtain "graphene material with modified groups".
[0204] 0.3 g of the obtained graphene material was added to 100 mL of a mixed solvent of deionized water and 2-propanol (IPA) (volume ratio: 60 / 40). The mixture was ultrasonically treated for 3 minutes using an ultrasonic homogenizer (UH-600S, SMT Corporation, 26 mm Φ) to obtain a dispersion. The dispersion was sprayed onto a mica plate to prepare a test sample. The sample was observed using an atomic force microscope (AFM5300E, Hitachi High Technology Corporation, model: AFM5300E) to determine the thickness of the graphene material. The results confirmed a thickness of 0.99 nm, indicating that the graphene layer count was less than 3 layers, and that natural graphite was exfoliated between its layers to form graphene. The obtained graphene material was then ashed in a platinum crucible, subjected to alkaline dissolution, and dissolved in hydrochloric acid solution. The sample was diluted with ultrapure water, and the cations were quantitatively analyzed using an ICP-ELISA system (Analytik-jena, Germany, model: PQ9000 Elite). The results confirmed the presence of potassium at 2200 ppm as a countercation.
[0205] <Comparison of the production of positive electrode-4>
[0206] As a conductive additive, a "graphene material with modified groups" was used, and the ratio of the positive electrode paste (positive electrode active material: conductive additive (graphene material with modified groups): PVDF) was set to 97:2:1 (unit: wt%). Otherwise, a comparative positive electrode-4 was prepared by the same method as in Example 1.
[0207] (Example 5: Fabrication of a comparative positive electrode -5 without the use of conductive additives)
[0208] Without using conductive additives, the ratio of positive electrode paste (positive electrode active material: PVDF) was set to 99:1 (unit: wt%). Otherwise, a comparative positive electrode -5 was prepared using the same method as in Example 1.
[0209] (Example 6: Comparative cathode fabrication using carbon composite active material-1)
[0210] <Preparation of Carbon Composite Active Material-1>
[0211] Add 0.02g of binder (carboxymethyl cellulose (CMC)) to 100g of a water / IPA solution consisting of isopropanol (hereinafter IPA) and water (water:IPA=60:40 (unit: wt%)), and stir with a magnetic stirrer at 60°C for 6 hours to fully dissolve it.
[0212] Then, add 0.65g of conductive additive (graphene powder, manufactured by Graphene Supermarket, with a specific surface area of 250m²). 2 The graphene dispersion was prepared by dispersing the graphene with a particle size of 0.5 μm and an average particle size of 0.5 μm using an ultrasonic dispersion device at a frequency of 80 kHz and a dispersion time of 3 minutes × 3 times, followed by centrifugation (2000 rpm, 10 minutes).
[0213] Then, 150g of positive electrode active material (lithium nickelate, manufactured by JFE Mineral & Alloy Company, Ltd., with an average particle size D50 of 10μm) was mixed into the graphene dispersion, filtered, and dried (80°C, 10 hours) to obtain carbon composite active material material-1. The graphene content in carbon composite active material material-1 was 0.26% by mass, and the binder content was 0.01% by mass.
[0214] <Comparison of the production of positive electrode-6>
[0215] As the positive electrode active material and conductive additive, composite active material-1 was used, and the ratio of positive electrode paste (positive electrode active material: conductive additive (graphene): PVDF) was set to 97:2:1 (unit: wt%). Otherwise, comparative positive electrode-6 was prepared by the same method as in preparation example 1.
[0216] (Example 7: Comparative cathode fabrication using carbon composite active material-2)
[0217] <Preparation of Carbon Composite Active Material-2>
[0218] A coating solution was prepared by dissolving 1g of conductive additive (acetylene black, manufactured by Denka Co., Ltd.) in 100g of water / IPA solution (water:IPA=60:40 (unit: wt%)).
[0219] Next, using a rotary flow granulation coating apparatus (Powrex, MP-01, Japan), the aforementioned coating solution was sprayed onto 1 kg of positive electrode active material (lithium nickel oxide, manufactured by JFE Mineral & Alloy Company, Ltd., average particle size D50: 10 μm), causing the solution to adhere to the surface of the positive electrode active material particles. The coating apparatus was operated under the following conditions: nitrogen was used as the suction gas, the suction temperature was 140°C, and the suction airflow was 0.4 m³ / s. 3The rotor speed was 400 rpm, and the spraying speed was 3.0 g / min. After spraying, the coated powder was collected and calcined at 200°C for 5 hours in the atmosphere, and then pulverized again with an agate mortar (with a target particle size distribution D50 of 10 μm) to obtain a composite active material material-2 composed of acetylene black and positive electrode active material.
[0220] <Comparison of the production of positive electrode-7>
[0221] As the positive electrode active material and conductive additive, composite active material material-2 was used, and the ratio of positive electrode paste (positive electrode active material: conductive additive (AB): PVDF) was set to 97:2:1 (unit: wt%). Otherwise, a comparative positive electrode-7 was prepared by the same method as in Example 1.
[0222] (Example 8: Fabrication of cathode-1 using carbon composite active material-3)
[0223] <Preparation of Carbon Composite Active Material-3>
[0224] As a conductive additive, the aforementioned "graphene material with modified groups" was used instead of the aforementioned graphene powder. Otherwise, composite active material-3 was obtained by the same method as in the preparation of carbon composite active material-1.
[0225] <The Production of Positive Electrode-1>
[0226] As the positive electrode active material and conductive additive, composite active material material-3 was used, and the ratio of positive electrode paste (positive electrode active material: conductive additive (graphene material with modified group): PVDF) was set to 97:2:1 (unit: wt%). Otherwise, positive electrode-1 was prepared by the same method as in preparation example 1.
[0227] (Example 9: Fabrication of cathode-2 using carbon composite active material-4)
[0228] <Preparation of Carbon Composite Active Material-4>
[0229] As a conductive additive, the aforementioned graphene powder (manufactured by Graphene Supermarket) was used instead of the aforementioned acetylene black. Otherwise, composite active material-4 was obtained by the same method as in the preparation of carbon composite active material-2.
[0230] <The Production of Positive Electrode-2>
[0231] As the positive electrode active material and conductive additive, composite active material-4 was used, and the ratio of positive electrode paste (positive electrode active material: conductive additive (graphene): PVDF) was set to 97:2:1 (unit: wt%). Otherwise, positive electrode-2 was prepared by the same method as in preparation example 1.
[0232] (Example 10: Fabrication of cathode-3 using carbon composite active material-5)
[0233] <Preparation of Carbon Composite Active Material-5>
[0234] As a conductive additive, the aforementioned “graphene material with modified groups” was used instead of the aforementioned acetylene black. Otherwise, composite active material-5 was obtained by the same method as in the preparation of carbon composite active material-2.
[0235] <The Production of Positive Electrode-3>
[0236] As the positive electrode active material and conductive additive, composite active material material-5 was used, and the ratio of positive electrode paste (positive electrode active material: conductive additive (graphene material with modified group): PVDF) was set to 97:2:1 (unit: wt%). Otherwise, positive electrode-3 was prepared by the same method as in preparation example 1.
[0237] (Example 11: Fabrication of cathode-4 using carbon composite active material-6)
[0238] <Preparation of Carbon Composite Active Material-6>
[0239] As a conductive additive, the aforementioned “graphene material with modified groups” was used instead of the aforementioned acetylene black. Otherwise, composite active material-6 was obtained by the same method as in the preparation of carbon composite active material-2.
[0240] <The Production of Positive Electrode-4>
[0241] As the positive electrode active material and conductive additive, composite active material-6 was used, and the ratio of positive electrode paste (positive electrode active material: conductive additive (graphene material with modified group): conductive additive (AB): conductive additive (CNT): PVDF) was set to 95:2:1:1:1 (unit: wt%). Otherwise, positive electrode-4 was prepared by the same method as in preparation example 1.
[0242] <Cape of Repose>
[0243] The angle of repose was measured for carbon composite active materials -1 to 6 and the aforementioned positive electrode active material. The angle of repose was measured using a powder flow meter (manufactured by Furukawa Machinery & Metal Co., Ltd., according to JIS R9301-2-2:1999) via the injection method. 20 g of each of the carbon composite active material -1 to 6 and the aforementioned positive electrode active material were weighed and injected from the bottom of a funnel (tilted at a 60° angle). A discharge orifice with a diameter of 4 mm allows the sulfide-based inorganic solid electrolyte material to be supplied in a circular manner along the circumference of the funnel wall, causing it to accumulate into a cone shape. The angle (angle of repose) α between the generatrix of the cone and the base is measured.
[0244] α = arctan[2h / (Dd)]
[0245] h: Height of the cone (distance between the base plate and the tip of the funnel nozzle) (mm).
[0246] D: The average diameter (mm) in the four directions.
[0247] d: Diameter (mm) of the funnel nozzle.
[0248] Here, the distance from the discharge hole of the funnel to the circular plate is 25mm.
[0249] <Powder Resistance>
[0250] The powder resistivity of carbon composite active materials -1 to 6 and the aforementioned positive electrode active materials was measured. The powder resistivity was measured using the Nittoseiko Analytech Co., Ltd. powder resistivity measuring system MCP-PD51 and the powder low-resistivity probe MCP-PD511. According to JISK 7194:1994, the volume resistivity (powder resistance) of the powder was calculated using the four-probe method with constant current application.
[0251] The measurement results are shown in Table 1.
[0252] <Electron conductivity>
[0253] The electronic conductivity (25°C) was measured for positive electrodes -1 to 4 (Examples 1 to 4) and comparative positive electrodes -1 to 7 (Comparative Examples 1 to 7). The electronic conductivity was measured using an electrode resistance measurement system (RM2611, manufactured by Nippon Denki Co., Ltd.). The volume resistivity of the current collector foil used in the measurement was 2.5 × 10⁻⁶. ?8 Ω?m. The measurement results are shown in Table 1.
[0254] [Table 1]
[0255] The use of the carbon composite active material disclosed herein (Examples 1-4) confirmed an improvement in electronic conductivity. By using a carbon composite active material with excellent electronic conductivity, the ratio of conductive additives can be increased while reducing the ratio of active material compared to the prior art. The increase in the ratio of active material is related to an increase in battery capacity.
[0256] Industrial applicability
[0257] The carbon composite active material disclosed herein is suitable for use as an electrode in secondary batteries where further increases in battery capacity are required. In particular, the carbon composite active material disclosed herein is suitable for use in next-generation mobile devices such as EVs and drones where the weight of the battery accounts for a large proportion and lightweighting and long battery life are required.
Claims
1. A carbon composite active material, wherein, It contains electrode active materials and graphene materials. The carbon composite active material has a repose angle of 20° to 45°.
2. The carbon composite active material according to claim 1, wherein, The graphene material forms a surface layer that coats at least a portion of the surface of the electrode active material. The surface layer has a coverage rate of 10% or more.
3. The carbon composite active material according to claim 1 or 2, wherein, The graphene material contains anionic functional groups and countercations of these anionic functional groups at its ends, and the peak intensities of the D and G bands in the Raman spectra obtained by Raman spectroscopy are I... D / I G It is below 0.
50.
4. The carbon composite active material according to claim 1 or 2, wherein, The content ratio of the graphene material to the electrode active material is 0.1 to 2.4 by mass.
5. The carbon composite active material according to claim 1 or 2, wherein, The ratio of the planar dimension DG of the graphene material to the particle size DA of the electrode active material, DG / DA, is 0.002 to 3.
000.
6. The carbon composite active material according to claim 2, wherein, The surface layer comprises the graphene material and a binder.
7. The carbon composite active material according to claim 1 or 2, wherein, The electrode active material is a positive electrode active material.
8. The carbon composite active material according to claim 7, wherein, The positive electrode active material is a lithium-containing composite oxide.
9. A secondary battery, wherein, The secondary battery has electrodes formed from a slurry containing a carbon composite active material as described in claim 1 or 2.
10. A method for manufacturing a carbon composite active material, wherein the carbon composite active material is formed by coating the surface of an electrode active material with graphene material, wherein in the manufacturing method, The device includes a spraying process, in which the electrode active material flows within a rotating fluidized bed granulation apparatus, and a solution containing the graphene material is sprayed into the rotating fluidized bed granulation apparatus. The carbon composite active material has a repose angle of 20° to 45°.
11. The method for manufacturing carbon composite active material according to claim 10, wherein, The spraying is carried out under the following conditions. Solution concentration: 1–10% by mass% Spray speed: 2-4 g / s; Spraying time: 5 to 180 minutes.
12. The method for manufacturing carbon composite active material according to claim 11, wherein, It includes a firing process in which the granules obtained in the spraying process are fired under the following conditions. Firing environment: Nitrogen; Firing temperature: 200~350℃; Firing time: 24-48 hours.
13. The method for manufacturing carbon composite active material according to claim 10, wherein, The carbon composite active material has a surface layer in which the graphene material coats at least a portion of the surface of the electrode active material, and the coating rate of the surface layer is 10% or more.
14. The method for manufacturing carbon composite active material according to claim 10, wherein, The graphene material contains anionic functional groups and countercations of these anionic functional groups at its ends, and the peak intensities of the D and G bands in the Raman spectra obtained by Raman spectroscopy are I... D / I G It is below 0.50.
Citation Information
Patent Citations
Positive electrode active material and nonaqueous electrolytic battery
JP2002110162A
Manufacturing method of positive electrode
JP2020021745A