A foam control composition and its preparation method
By combining inert polyorganosiloxanes, vinyl butyl polysiloxanes, spatially structured hydrogen-containing polysiloxanes, silicone resins, and hydrophobic silica, the problem of insufficient defoaming performance of existing defoamers in strong alkaline or strong anionic systems is solved, achieving excellent defoaming and foam suppression effects and stability.
Patent Information
- Application Number
- CN202611499902.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-24
- Publication Date
- 2026-11-17
AI Technical Summary
Existing silicone defoamers have insufficient defoaming performance in strong alkaline or strong anionic systems, and gelation is difficult to control during preparation, resulting in poor foam suppression effect.
A foam control composition with excellent defoaming properties and storage stability is formed by combining inert polyorganosiloxane, vinyl butyl polysiloxane, spatially structured hydrogen-containing polysiloxane, silicone resin, hydrophobic silica and catalyst through reaction and mixing under specific process conditions.
It achieves excellent defoaming and foam suppression properties in strong alkaline or strong anionic systems, and can effectively control gelation during preparation, thus improving the stability of the foam control composition.
Smart Images

Figure SMS_3 
Figure QLYQS_1 
Figure QLYQS_2
Abstract
Description
Technical Field
[0001] This application belongs to the field of fine chemical formulation technology, and in particular relates to a foam control composition and its preparation method. Background Technology
[0002] Foam is a common phenomenon in daily life and industrial production. Its presence has both advantages and disadvantages. For example, people often use foam for firefighting, manufacturing polyurethane, and food production. However, in many industrial systems, foam poses a significant threat to production and daily life because it affects output, quality, the environment, and economic efficiency. Methods for eliminating foam are generally divided into mechanical and chemical methods. Mechanical methods use high-pressure impacts, increased temperatures, and negative pressure to eliminate harmful foam, but their overall effectiveness is limited. Chemical methods use chemical agents, such as defoamers, to eliminate foam. The basic principle is to change the surface tension of the foam film, but this does not involve reducing the concentration of foaming substances through a true chemical reaction. Currently, defoamers are generally chosen to eliminate, reduce, or control harmful foam; and defoamers are widely used in papermaking, coatings, chemicals, printing and dyeing, pharmaceuticals, water treatment, food processing, and oil extraction.
[0003] Among surfactant-rich systems, silicone-based defoamers have the widest application range compared to polyether, fatty alcohol, and mineral oil-based defoamers. They are favored by the market due to their advantages such as low dosage, strong defoaming ability, low volatility, non-toxicity, and lack of side effects. Silicone-based defoamers mainly consist of several basic components, including polysiloxanes, hydrophobic particles, silicone resins, and catalysts. US4639489 describes a foam-controlling composition obtained by high-temperature, long-term processing of polydimethylsiloxane and silica. This foam-controlling composition has a simple structure and poor foam-suppressing performance, but it is still used in some industries. US4338217A1 describes the preparation of organosilicon active materials by mixing alkoxy polysiloxanes with silica particles; US2008064806A1 investigates the difference between the viscosity and antifoaming effect of organosilicon compositions; CN201010213081.5 describes the preparation of silicone pastes by mixing polydimethylsiloxane, modified polydimethylsiloxane, silica, and silicone resin; EP0163398A1 studies the preparation of silicone pastes by mixing high- and low-viscosity polysiloxanes and silica. The preparation of these silicone pastes all revolve around the structure of polysiloxanes.
[0004] EP2794760A1 introduces both hydrophilic and hydrophobic silica, and uses equipment such as a colloid mill to reduce the viscosity of the composition to 50% of the viscosity measured before heating, so that the defoaming composition finally reaches a suitable viscosity to facilitate emulsification. However, the cross-linked structure formed by hydroxyl condensation is relatively weak, making it difficult to achieve good defoaming effect in anionic systems with strong foaming power. US5153258A introduces the introduction of a mildly cross-linked polysiloxane and silica mixture into the system to improve the defoaming and defoaming performance of the composition. US8053480B2 similarly describes a high-viscosity vinylsiloxane and a low-viscosity hydrogen-containing polysiloxane undergoing a cross-linking reaction in the presence of hydrophobic silica until partial gelation occurs. Then, by applying high shear until the composition reaches a suitable viscosity range, it exhibits relatively good defoaming performance in strongly alkaline systems, but the defoaming ability is still lacking, and the gelation generated during the preparation of this composition is difficult to control. US3455839A and CA2074060A1 both describe a cross-linked polysiloxane defoaming composition formed by reacting vinyl polysiloxane and hydrogen-containing polysiloxane under platinum conditions, which improves the later foam suppression ability. However, how to control the differences between batches has not yet been well resolved.
[0005] Therefore, silicone defoamers with excellent defoaming, foam-suppressing, and storage stability remain a research focus. Summary of the Invention
[0006] This application provides a foam control composition and its preparation method to solve the problems existing in related technologies. The technical solution is as follows: In a first aspect, embodiments of this application provide a foam control composition comprising the following raw materials: inert polyorganosiloxane, vinyl butyl polysiloxane, spatially structured hydrogen-containing polysiloxane, organosilicon resin, hydrophobic silica, addition catalyst, and alkaline catalyst. The spatially structured hydrogen-containing polysiloxane is prepared by reacting a linear hydrogen-containing polysiloxane of Formula II with the presence of platinum. (II); In formula (II), d and e are the degree of polymerization of the two repeating units. The linear hydrogen-containing polysiloxane has a viscosity of 2~20 mPa·s at 25°C and a hydrogen content of 0.3~1.0%.
[0007] In one embodiment, the method for preparing the spatially structured hydrogen-containing polysiloxane is as follows: The linear hydrogen-containing polysiloxane of Formula II was stirred and heated to 50-80°C, and then 1-10 ppm of chloroplatinic acid (based on platinum) was added. The reaction was carried out at 100-180°C for 0.1-1 h to prepare the hydrogen-containing polysiloxane with a spatial structure.
[0008] In one embodiment, chloroplatinic acid is used in the form of an alcoholic solution, an ether solution, or a ketone solution.
[0009] In one embodiment, the inert polysiloxane structure has the general formula shown in Formula I: R a SiO (4-a) / 2 (I); In formula (I), the value of a is 1.9 to 2.2; R is a monovalent substituted or unsubstituted hydrocarbon group with 1 to 30 carbon atoms, and the values may be the same or different.
[0010] Preferably, R is an alkyl group, wherein the alkyl group is methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, dodecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, dodecyl, tetradecyl, hexadecyl, octadecyl, or triadecyl.
[0011] Alternatively, R is an aryl group, wherein the aryl group is phenyl or α-methylphenethyl; In one embodiment, from the perspective of raw material availability and cost, at least 80% of the substituents R in the inert polysiloxane are methyl.
[0012] In one embodiment, the inert polysiloxane has a dynamic viscosity of 100~10,000 mPa•s at 25°C.
[0013] In one embodiment, the vinyl-butyl polysiloxane structure is of the general formula shown in Formula III: (III); In equation (III), R 1 and R 2 The molecule is an alkyl, aryl, or vinylbutyl group having 1-8 carbon atoms; and R 1 and R 2 It contains at least one vinyl butyl group.
[0014] Preferably, the alkyl group is methyl, ethyl, propyl, pentyl, hexyl, or octyl; the aryl group is phenyl or styryl; more preferably, R 1 and R 2 One is methyl and the other is vinylbutyl.
[0015] The subscripts b and c represent the degree of polymerization of the two repeating units. The dynamic viscosity of vinyl butyl polysiloxane at 25°C is 50~20000 mPa•s; including vinyl butyl polysiloxane with a mass ratio of 9:1~6:4 and a viscosity of 50~500 mPa•s, and vinyl butyl polysiloxane with a viscosity of 500~20000 mPa•s.
[0016] In one embodiment, the organosilicon resin is a methyl silicone resin comprising M-residue (CH3)3SiO 1 / 2 -, D-chain segment-SiO 2 / 2 -and Q-linker-SiO 4 / 2 -; The molar ratio of M-units, D-units, and Q-units is 1:(5~10):(1.2~2); The sum of hydroxyl and alkoxy content is less than or equal to 1%. The hydroxyl or alkoxy groups on the surface of the silicone resin may react with the spatially structured hydrogen-containing polysiloxanes, thereby affecting the addition reaction between the spatially structured hydrogen-containing polysiloxanes and vinyl-containing polysiloxanes, and thus affecting the structure of the target molecule. Therefore, the content of hydroxyl and alkoxy groups on the surface of the silicone resin is limited to ensure that the reaction between the spatially structured hydrogen-containing polysiloxanes and vinyl-containing polysiloxanes is absolutely dominant.
[0017] In one embodiment, the organosilicon resin is prepared by reacting hexamethyldisiloxane or trimethylchlorosilane, dimethyldimethoxysilane or dimethyldiethoxysilane, water glass or tetraethyl orthosilicate in the presence of hydrochloric acid, water, ethanol and toluene at a certain temperature.
[0018] In one embodiment, the addition catalyst is one or more of the following: platinum-alcohol complex, platinum-olefin complex, platinum-alkoxide complex, platinum-ether complex, platinum-ketone complex, 1% isopropanol chloroplatinate solution, rhodium-alcohol complex, and rhodium-alkoxide complex.
[0019] In one embodiment, the alkaline catalyst is one or a combination of two or more of sodium hydroxide, potassium hydroxide, cesium hydroxide, tetramethylammonium hydroxide, sodium methoxide, potassium methoxide, sodium carbonate, sodium bicarbonate, or monoethanolamine.
[0020] In one embodiment, the hydrophobic silica has a specific surface area of 50-500 m². 2 / g, hydrophobic silica with different specific surface areas can be used alone or in combination.
[0021] In one embodiment, hydrophobic silica is obtained by heating and stirring hydrophilic silica and a hydrophobic agent in a reaction vessel.
[0022] In one embodiment, the hydrophobic agent is selected from one or more of the following: low-viscosity trimethylsiloxy-terminated polydimethylsiloxane, low-viscosity hydroxyl-terminated polydimethylsiloxane, hexamethyldisilazane, hexamethyldisilazane, dimethyldiethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, trimethylchlorosilane, dimethyldichlorosilane, methyltrichlorosilane, tetrachlorosilane, stearic acid, stearyl alcohol, octamethylcyclotetrasiloxane, tetramethylcyclotetrasiloxane, and hexamethylcyclotrisiloxane.
[0023] In one embodiment, the composition includes 30-85% inert polyorganosiloxane, 10-60% vinyl-butyl polysiloxane, 0.1-5% spatially structured hydrogen-containing polysiloxane, 0.5-5% organosilicon resin, 1-6% hydrophobic silica, 1-15 ppm addition catalyst (calculated as pure metal), and 5-50 ppm alkaline catalyst.
[0024] Secondly, embodiments of this application provide a method for preparing a foam control composition, comprising the following steps: The first part consists of an inert polyorganosiloxane, a vinyl-butyl polysiloxane, a spatially structured hydrogen-containing polysiloxane, and an organosilicon resin. An addition catalyst is added at 60-80°C to carry out the first reaction until the viscosity is 10-20 times the initial viscosity. The first part of the alkaline catalyst is added to continue the second reaction, and the mixture is cooled to room temperature to obtain mixture A. The second part, consisting of inert polyorganosiloxane and hydrophobic silica, and the second part, consisting of alkaline catalyst, undergoes a third reaction to obtain mixture B. Mixture A is added to mixture B to carry out the fourth reaction. After being processed by a homogenizer and cooled to room temperature, the foam control composition is obtained.
[0025] In one embodiment, the mixing process involves heating to 60-120°C, stirring and dispersing at 500-5000 rpm, and grinding until the solid dispersion particle size is below 5 μm. The first reaction is carried out at 60~120℃ for 0.5~5 hours; the second reaction is carried out at 60~120℃ for 0.5~2 hours. The third reaction is carried out at 120~180℃ and 1000~3000rpm for 2~6 hours; the fourth reaction is carried out at 100~150℃ and 1000~3000rpm for 1~3 hours.
[0026] In one embodiment, the mass ratio of the first part of inert polyorganosiloxane to the second part of inert polyorganosiloxane is (1-3.5):1; the mass ratio of the first part of alkaline catalyst to the second part of alkaline catalyst is 1:(2-3).
[0027] Thirdly, embodiments of this application provide an antifoaming agent comprising the foam control composition described above.
[0028] In one embodiment, the foam control composition of this application may be provided directly for use, or it may be diluted with a solvent, or made into an emulsion, or made into a solid foam control product, depending on the actual requirements of the use.
[0029] In one embodiment, the defoamer also includes an emulsifier, water, or a thickener. The emulsifier is a nonionic surfactant, comprising one or more of the following: nonylphenol polyoxyethylene ether, octylphenol polyoxyethylene ether, lauric acid polyoxyethylene ether, oleic acid polyoxyethylene ether, lauryl alcohol polyoxyethylene ether, octyl alcohol polyoxyethylene ether, isooctyl alcohol polyoxyethylene ether, isodecyl alcohol polyoxyethylene ether, isotridecyl alcohol polyoxyethylene ether, hexadecyl alcohol polyoxyethylene ether, octadecyl alcohol polyoxyethylene ether, sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan tristearate, sorbitan trioleate, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan tristearate, polyoxyethylene sorbitan trioleate, and castor oil polyoxyethylene ether, preferably a mixture of multiple types.
[0030] The thickener is selected from polyacrylamide, polyvinyl alcohol, carbomer, xanthan gum, polyacrylate, and cellulose ethers. Xanthan gum and polyacrylate thickeners are preferred. The amount added is adjusted according to the required emulsion viscosity. The advantages or beneficial effects of the above technical solutions include at least the following: This application provides a foam control composition comprising an inert polyorganosiloxane, a vinyl butyl polysiloxane, a spatially structured hydrogen-containing polysiloxane, an organosilicon resin, hydrophobic silica, an addition catalyst, and an alkaline catalyst; the organosilicon foam control composition obtained by synthesizing under certain process conditions has excellent defoaming properties, foam suppression properties, and storage stability, and can be used in industries such as textile printing and dyeing, wastewater treatment, and industrial cleaning.
[0031] The above overview is for illustrative purposes only and is not intended to be limiting in any way. In addition to the illustrative aspects, embodiments, and features described above, further aspects, embodiments, and features of this application will become readily apparent from the following detailed description. Detailed Implementation
[0032] In the following description, only certain exemplary embodiments are briefly described. As those skilled in the art will recognize, the described embodiments can be modified in various ways without departing from the spirit or scope of this application. Therefore, the description is considered to be exemplary in nature and not restrictive.
[0033] Example 1 Preparation of spatially structured hydrogen-containing polysiloxane C1: Linear hydrogen-containing polysiloxane (viscosity of 2 mPa•s at 25℃, hydrogen content of 0.45%) was added to a container. Stirring was started and the temperature was raised to 50℃. Then, 3 ppm of chloroplatinic acid (calculated as platinum metal) was added. The temperature was kept at 120℃ for 0.5 h, and then cooled to room temperature to obtain the spatial structure hydrogen-containing polysiloxane C1.
[0034] Example 2 Preparation of spatially structured hydrogen-containing polysiloxane C2: Linear hydrogen-containing polysiloxane (viscosity of 20 mPa•s at 25℃, hydrogen content of 0.3%) was added to a container. Stirring was started and the temperature was raised to 80℃. Then, 1 ppm of chloroplatinic acid (calculated as platinum metal) was added. The temperature was kept at 180℃ for 0.1 h, and then cooled to room temperature to obtain the spatial structure hydrogen-containing polysiloxane C2.
[0035] Example 3 Preparation of spatially structured hydrogen-containing polysiloxane C3: Linear hydrogen-containing polysiloxane (viscosity of 8 mPa•s at 25℃, hydrogen content of 1.0%) was added to a container, stirring was started and the temperature was raised to 60℃, then 10 ppm of chloroplatinic acid (calculated as platinum metal) was added, and the temperature was kept at 100℃ for 1 h. After cooling to room temperature, the spatial structure hydrogen-containing polysiloxane C3 was obtained.
[0036] Example 4 Preparation of spatially structured hydrogen-containing polysiloxane C4: Linear hydrogen-containing polysiloxane (viscosity of 13 mPa•s at 25℃, hydrogen content of 0.75%) was added to a container. After stirring and heating to 70℃, 6 ppm of chloroplatinic acid (calculated as platinum) was added. The mixture was kept at 120℃ for 0.5 h and then cooled to room temperature to obtain the spatial structure hydrogen-containing polysiloxane C4.
[0037] Example 5 Preparation of spatially structured hydrogen-containing polysiloxane C5: Linear hydrogen-containing polysiloxane (viscosity of 15 mPa•s at 25℃, hydrogen content of 0.55%) was added to a container. Stirring was started and the temperature was raised to 58℃. Then, 8 ppm of chloroplatinic acid (calculated as platinum metal) was added. The mixture was kept at 150℃ for 0.6 h and then cooled to room temperature to obtain the spatial structure hydrogen-containing polysiloxane C5.
[0038] Example 6 Add 44 parts of trimethylsiloxy-terminated polydimethylsiloxane (viscosity 1000 mPa•s at 25°C) and 9 parts of vinylbutyl polysiloxane (R) to a container. 1 For vinylbutyl, R 2 Methyl, viscosity at 25°C is 350 mPa•s), 1 part containing vinyl butyl polysiloxane (R 1 For vinylbutyl, R2 The mixture consisted of methyl groups (with a viscosity of 9000 mPa•s at 25°C), 2 parts of a spatially structured hydrogen-containing polysiloxane C1, and 2 parts of organosilicon resin (M-D-Q linkage = 1:6:1.2, with a hydroxyl and alkoxy content of 0.8%). The mixture was heated to 60°C and rotated at 1000 rpm to ensure complete dispersion of solid particles in the polysiloxane. The final particle size was then reduced to below 5 μm using a grinding device. After adjusting the temperature to 65°C, 10 ppm of a platinum-alcohol solution catalyst (calculated as platinum) was added. The mixture was reacted at 100°C for 0.5 h, resulting in a viscosity 11 times the initial viscosity. 10 ppm of an alkaline catalyst was then added, and the mixture was kept at this temperature for another 1 h before cooling to room temperature to obtain mixture I. In another container, add 40 parts of trimethylsiloxy-terminated polydimethylsiloxane (viscosity at 25°C: 1000 mPa•s) and 1 part of hydrophobic silica (specific surface area: 55 m²). 2 / g of precipitated silica, treated with trimethylsiloxy-terminated polydimethylsiloxane (viscosity at 25℃ is 10mPa•s) and 20ppm of sodium hydroxide catalyst, were dispersed at 1500rpm for 2h at 120℃ to obtain mixture II; Mixture I was added to mixture II and dispersed at 3000 rpm at 150°C for 2 hours. After being processed by a homogenizer and cooled to room temperature, the silicone foam control composition S1 was obtained, with a viscosity of 36000 mPa•s at 25°C.
[0039] Example 7 Add 20 parts of trimethylsiloxy-terminated polydimethyl-methyloctylsiloxane (viscosity 10000 mPa•s at 25°C) and 36 parts of vinylbutyl polysiloxane (R) to a container. 1 R 2 All are vinyl butyl, with a viscosity of 60 mPa•s at 25°C; 24 parts contain vinyl butyl polysiloxane (R 1 R 2 All components are vinyl butyl with a viscosity of 20000 mPa•s at 25°C. 3.5 parts of spatially structured hydrogen-containing polysiloxane C4 and 0.5 parts of organosilicon resin (M-D-Q linkage = 1:10:2, hydroxyl and alkoxy content sum of 0.3%) were heated to 120°C and the rotation speed was controlled at 500 rpm to completely disperse the solid particles in the polysiloxane. The final particle size of the dispersed solid was reduced to less than 5 μm by grinding. After adjusting the temperature of the mixture to 60°C, 15 ppm of platinum-alcohol solution catalyst (calculated as platinum) was added. The mixture was reacted at 60°C for 5 h. The viscosity of the mixture was 20 times that of the initial viscosity. 15 ppm of alkaline catalyst was added and the mixture was kept at the same temperature for 2 h. The mixture was then cooled to room temperature to obtain mixture I. In another container, add 10 parts of trimethylsiloxy-terminated polydimethyl-methyloctylsiloxane (viscosity at 25°C: 10000 mPa•s) and 6 parts of hydrophobic silica (specific surface area: 500 m²). 2 / g of fumed silica (with dimethyldichlorosilane as the treatment agent) and 35ppm of potassium hydroxide catalyst were dispersed at 3000rpm for 6h at 180℃ to obtain mixture II; Mixture I was added to mixture II and dispersed at 100°C and 1000 rpm for 1 hour. After being processed by a homogenizer and cooled to room temperature, the silicone foam control composition S2 was obtained, with a viscosity of 58300 mPa•s at 25°C.
[0040] Example 8 Add 47 parts of trimethylsiloxy-terminated polydimethyl-methylcarbotrianesiloxane (viscosity at 25°C: 100 mPa•s) and 16 parts of vinylbutyl polysiloxane (R) to a container. 1 It is methyl, R 2 It is vinyl butyl with a viscosity of 500 mPa•s at 25°C, and 4 parts of vinyl butyl polysiloxane (R 1 For octylene, R 2 The mixture consisted of 5 parts vinyl butyl with a viscosity of 500 mPa•s at 25°C, 5 parts spatially structured hydrogen-containing polysiloxane C5, and 5 parts organosilicon resin (M-D-Q linkage = 1:5:1.8, with a hydroxyl and alkoxy content of 0.5%). The mixture was heated to 90°C and rotated at 5000 rpm to ensure complete dispersion of solid particles in the polysiloxane. The final particle size was reduced to below 5 μm using a grinding device. The temperature of the mixture was adjusted to 80°C, and 1.5 ppm platinum-ketone solution catalyst (calculated as platinum) was added. The mixture was reacted at 120°C for 2.5 h, resulting in a viscosity 15 times the initial viscosity. 1.5 ppm alkaline catalyst was then added, and the mixture was kept at this temperature for another 0.5 h before cooling to room temperature to obtain mixture I. In another container, add 20 parts of trimethylsiloxy-terminated polydimethyl-methylcarbamoylsiloxane (viscosity at 25°C: 100 mPa•s) and 3 parts of hydrophobic silica (specific surface area: 250 m²). 2 / g of precipitated silica (treated with hexamethyldisilazane) and 4ppm of catalyst cesium hydroxide were dispersed at 1000rpm for 4h at 140℃ to obtain mixture II; Mixture I was added to mixture II and dispersed at 125°C at 2000 rpm for 3 hours. After being processed by a homogenizer and cooled to room temperature, the silicone foam control composition S3 was obtained, with a viscosity of 27600 mPa•s at 25°C.
[0041] Example 9 Add 39 parts of trimethylsiloxy-terminated polydimethyl-methylphenethylsiloxane (viscosity 2000 mPa•s at 25°C) and 28 parts of vinylbutyl polysiloxane (R) to a container. 1 For vinylbutyl, R 2 Methyl, viscosity at 25°C is 100 mPa•s), 12 parts containing vinyl butyl polysiloxane (R 1 It is methyl, R 2 The mixture consisted of 2 parts vinyl butyl with a viscosity of 5800 mPa•s at 25°C, 2 parts spatially structured hydrogen-containing polysiloxane C2, and 3 parts organosilicon resin (M-D-Q = 1:8:1.25, with a hydroxyl and alkoxy content of 0.2%). The mixture was heated to 105°C and rotated at 3000 rpm to ensure complete dispersion of solid particles in the polysiloxane. The final particle size was reduced to below 5 μm using a grinding device. After adjusting the temperature of the mixture to 65°C, 10 ppm of platinum-ether solution catalyst (calculated as platinum) was added. The mixture was reacted at 90°C for 3 hours, resulting in a viscosity 13 times the initial viscosity. Then, 10 ppm of alkaline catalyst was added, and the mixture was kept at this temperature for 1.5 hours before cooling to room temperature to obtain mixture I. In another container, add 12 parts of trimethylsiloxy-terminated polydimethyl-methylphenylethylsiloxane (viscosity at 25°C: 2000 mPa•s) and 4 parts of hydrophobic silica (specific surface area: 380 m²). 2 / g of fumed silica, treated with hexamethyldisilazane) and 30ppm of monoethanolamine catalyst, were dispersed at 2500rpm for 3h at 160℃ to obtain mixture II; Mixture I was added to mixture II and dispersed at 135°C at 1000 rpm for 3 hours. After being processed by a homogenizer and cooled to room temperature, the silicone foam control composition S4 was obtained, with a viscosity of 42900 mPa•s at 25°C.
[0042] Example 10 Add 42.5 parts of trimethylsiloxy-terminated polydimethylsiloxane (viscosity 500 mPa•s at 25°C) and 27 parts of vinylbutyl polysiloxane (R) to a container. 1 For vinylbutyl, R 2 Methyl, viscosity at 25°C is 350 mPa•s), 3 parts containing vinyl butyl polysiloxane (R 1 For vinylbutyl, R 2The mixture consisted of 0.5 parts of a spatially structured hydrogen-containing polysiloxane C3 (M:D:Q = 1:5:1.6, with a hydroxyl and alkoxy content of 0.8%), methyl groups, and a viscosity of 9800 mPa•s at 25°C. The mixture was heated to 115°C and rotated at 4000 rpm to ensure complete dispersion of solid particles within the polysiloxane. The particles were then ground to a final particle size of less than 5 μm. The temperature of the mixture was adjusted to 68°C, and 8 ppm of platinum-ether solution catalyst (calculated as platinum) was added. The mixture was reacted at 108°C for 4 hours, resulting in a viscosity 15 times the initial viscosity. 8 ppm of sodium methoxide, an alkaline catalyst, was then added, and the mixture was kept at this temperature for another 1 hour before cooling to room temperature to obtain mixture I. In another container, add 20 parts of trimethylsiloxy-terminated polydimethylsiloxane (viscosity 500 mPa•s at 25°C) and 4 parts of hydrophobic silica (specific surface area 80 m²). 2 / g of precipitated silica (treated with hexamethyldisilazane) and 20ppm of sodium methoxide catalyst were dispersed at 3000rpm for 6h at 145℃ to obtain mixture II; Mixture I was added to mixture II and dispersed at 105°C at 2000 rpm for 1.5 h. After being processed by a homogenizer and cooled to room temperature, the silicone foam control composition S5 was obtained, with a viscosity of 28700 mPa•s at 25°C.
[0043] Comparative Example 1 The difference from Example 10 is that 30 parts of vinyl butyl polysiloxane (R) were used. 1 For vinylbutyl, R 2 (Methyl, viscosity at 25°C is 350 mPa•s) replaces 27 parts of vinyl-butyl polysiloxane (R) 1 For vinylbutyl, R 2 Methyl, viscosity at 25°C is 350 mPa•s), 3 parts containing vinyl butyl polysiloxane (R 1 For vinylbutyl, R 2 (Methyl group, viscosity at 25°C is 9800 mPa•s). The other components and methods were the same as in Example 10, and the silicone foam control composition S5-1 was prepared with a viscosity of 26800 mPa•s at 25°C.
[0044] Comparative Example 2 The difference from Example 10 is that 30 parts of vinyl butyl polysiloxane (R) were used. 1 For vinylbutyl, R 2 (Methyl, viscosity at 25°C is 9800 mPa•s) replaces 27 parts of vinyl butyl polysiloxane (R) 1For vinylbutyl, R 2 Methyl, viscosity at 25°C is 350 mPa•s), 3 parts containing vinyl butyl polysiloxane (R 1 For vinylbutyl, R 2 (Methyl group, viscosity at 25°C is 9800 mPa•s). The other components and methods were the same as in Example 10, and the silicone foam control composition S5-2 was prepared with a viscosity of 49800 mPa•s at 25°C.
[0045] Comparative Example 3 The difference from Example 10 is that 0.5 parts of linear hydrogen-containing polysiloxane (viscosity at 25°C 8 mPa•s, hydrogen content 1.0%) were used instead of 0.5 parts of spatially structured hydrogen-containing polysiloxane C3. The other components and methods were the same as in Example 10, and the silicone foam control composition S5-3 was prepared with a viscosity of 25900 mPa•s at 25°C.
[0046] Comparative Example 4 The difference from Example 10 is that 3 parts of silicone resin (M-chain segment:D-chain segment:Q-chain segment = 1:5:1.6, with a total hydroxyl and alkoxy content of 3%) are used instead of silicone resin with a total hydroxyl and alkoxy content of 0.8%. The other components and methods were the same as in Example 10, and the silicone foam control composition S5-4 was prepared with a viscosity of 67820 mPa•s at 25°C.
[0047] Comparative Example 5 Add 42.5 parts of trimethylsiloxy-terminated polydimethylsiloxane (viscosity 500 mPa•s at 25°C) and 27 parts of vinylbutyl polysiloxane (R) to a container. 1 For vinylbutyl, R 2 Methyl, viscosity at 25°C is 350 mPa•s), 3 parts containing vinyl butyl polysiloxane (R 1 For vinylbutyl, R 2 The composition consists of methyl groups (viscosity at 25°C is 9800 mPa•s), 0.5 parts of a spatially structured hydrogen-containing polysiloxane C3, 3 parts of organosilicon resin (M-D-Q linkage = 1:5:1.6, hydroxyl and alkoxy content summed to 0.8%), and 4 parts of hydrophobic silica (specific surface area 80 m² / s). 2 / g of precipitated silica (treated with hexamethyldisilazane) was heated to 115°C and the rotation speed was controlled at 4000 rpm to completely disperse the solid particles in the polyorganosiloxane. The final particle size of the dispersed solid particles was reduced to less than 5 μm by grinding equipment. After adjusting the temperature of the mixture to 68°C, 8 ppm of platinum-ether solution catalyst (calculated as platinum) was added. The mixture was reacted at 108°C for 4 h and then 28 ppm of sodium methoxide alkaline catalyst was added. The mixture was kept at the same temperature for 1 h and then cooled to room temperature to obtain the organosilicon foam control composition S5-5, which has a viscosity of 19260 mPa•s at 25°C.
[0048] Comparative Example 6 The difference from Example 10 is that 3 parts of silicone resin (M-chain segment: Q-chain segment = 1: 1.6, the sum of hydroxyl and alkoxy content is 0.8%) were used, and the other components and methods were the same as in Example 10 to prepare silicone foam control composition S5-6, which has a viscosity of 32320 mPa•s at 25°C.
[0049] Defoaming performance test: Preparation of test samples: Dilute the silicone foam control composition with cyclohexane as the dilution medium; Test medium: 2% sodium dodecyl sulfate, pH=12; Test method: Using the cyclic bubbling method; Test method: Add 500 mL of the above-mentioned foaming medium to the circulating bubbler, turn on the heater to 80°C, and then start circulation. When the foam reaches the highest mark of 300 mL, add 10 μL of the pre-diluted silicone foam control composition solution. Record the mark and time when the foam reaches its lowest point. The lower the mark, the more thorough the defoaming. Then continue bubbling and record the time when the foam reaches 300 mL again. The longer the time, the better the foam suppression effect; conversely, the shorter the time, the worse the effect.
[0050] The defoaming performance test results of the silicone foam control composition are shown in Table 1: Table 1 Comparison of defoaming performance of organosilicon foam control compositions
[0051] As can be seen from the data in Table 1, the silicone foam control compositions S1 to S5 of this application all have good defoaming speed and defoaming thoroughness. Comparing S5 and S5-1 to S5-6, the polymer molecular structure formed by vinyl butyl polysiloxane and hydrogen-containing polysiloxane has a significant impact on the performance of the defoaming composition; at the same time, the addition method of hydroxyl or alkoxy groups on the silicone resin and hydrophobic silica also has a significant impact on the molecular structure of the formed polymer.
[0052] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of this application. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of those different embodiments or examples.
[0053] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this application, "a plurality of" means two or more, unless otherwise explicitly specified.
[0054] The above description is merely a specific embodiment of this application, but the scope of protection of this application is not limited thereto. Any person skilled in the art can easily conceive of various variations or substitutions within the technical scope disclosed in this application, and these should all be included within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.
Claims
1. A foam control composition, characterized in that, The raw materials include: inert polyorganosiloxanes, vinyl-butyl polysiloxanes, spatially structured hydrogen-containing polysiloxanes, organosilicon resins, hydrophobic silica, addition catalysts, and basic catalysts. The spatially structured hydrogen-containing polysiloxane is prepared by reacting a linear hydrogen-containing polysiloxane of Formula II with the presence of platinum. (II); In formula (II), d and e are the degree of polymerization of the two repeating units. The linear hydrogen-containing polysiloxane has a viscosity of 2~20 mPa·s at 25°C and a hydrogen content of 0.3~1.0%.
2. The foam control composition according to claim 1, characterized in that, The preparation method of the spatially structured hydrogen-containing polysiloxane is as follows: The linear hydrogen-containing polysiloxane of Formula II was stirred and heated to 50-80°C, and then 1-10 ppm of chloroplatinic acid (based on platinum) was added. The reaction was carried out at 100-180°C for 0.1-1 h to prepare the hydrogen-containing polysiloxane with a spatial structure.
3. The foam control composition according to claim 1, characterized in that, The general structural formula of inert polysiloxane is shown in Formula I: R a SiO (4-a) / 2 (I); In formula (I), the value of a is 1.9 to 2.2; R is a monovalent substituted or unsubstituted hydrocarbon group with 1 to 30 carbon atoms, and the values may be the same or different. Preferably, R is an alkyl group, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, octyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, dodecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, dodecyl, tetradecyl, hexadecyl, octadecyl, or triadecyl. Alternatively, R can be aryl, phenyl, or α-methylphenethyl; The dynamic viscosity of inert polysiloxane at 25°C is 100~10,000 mPa•s.
4. The foam control composition according to claim 1, characterized in that, The general structural formula of vinyl-butyl polysiloxane is shown in Formula III: (III); In equation (III), R 1 and R 2 The molecule is an alkyl, aryl, or vinylbutyl group having 1-8 carbon atoms; and R 1 and R 2 It contains at least one vinyl butyl group; The subscripts b and c represent the degree of polymerization of the two repeating units. The dynamic viscosity of vinyl butyl polysiloxane at 25°C is 50~20000 mPa•s; including vinyl butyl polysiloxane with a mass ratio of 9:1~6:4 and a viscosity of 50~500 mPa•s, and vinyl butyl polysiloxane with a viscosity of 500~20000 mPa•s.
5. The foam control composition according to claim 1, characterized in that, The organosilicon resin is a methyl silicone resin, including the M repeating unit (CH3)3SiO 1 / 2 -, D-chain segment-SiO 2 / 2 -and Q-linker-SiO 4 / 2 -; The molar ratio of M-linkage, D-linkage, and Q-linkage is 1:(5~10):(1.2~2); The sum of the hydroxyl content and alkoxy content is less than or equal to 1%.
6. The foam control composition according to claim 1, characterized in that, The addition catalyst is one or more of the following: platinum-alcohol complex, platinum-olefin complex, platinum-alkoxide complex, platinum-ether complex, platinum-ketone complex, 1% isopropanol chloroplatinate solution, rhodium-alcohol complex, and rhodium-alkoxide complex. The alkaline catalyst is one or a combination of two or more of sodium hydroxide, potassium hydroxide, cesium hydroxide, tetramethylammonium hydroxide, sodium methoxide, potassium methoxide, sodium carbonate, sodium bicarbonate, or monoethanolamine.
7. The foam control composition according to claim 1, characterized in that, The percentage content of the raw materials is: The composition includes 30-85% inert polyorganosiloxane, 10-60% vinyl-butyl polysiloxane, 0.1-5% spatially structured hydrogen-containing polysiloxane, 0.5-5% organosilicon resin, 1-6% hydrophobic silica, 1-15 ppm addition catalyst (based on pure metals), and 5-50 ppm alkaline catalyst.
8. A method for preparing the foam control composition according to any one of claims 1-7, characterized in that, Includes the following steps: The first part consists of an inert polyorganosiloxane, a vinyl-butyl polysiloxane, a spatially structured hydrogen-containing polysiloxane, and an organosilicon resin. An addition catalyst is added at 60-80°C to carry out the first reaction until the viscosity is 10-20 times the initial viscosity. The first part of the alkaline catalyst is added to continue the second reaction, and the mixture is cooled to room temperature to obtain mixture A. The second part, consisting of inert polyorganosiloxane and hydrophobic silica, and the second part, consisting of alkaline catalyst, undergoes a third reaction to obtain mixture B. Mixture A is added to mixture B to carry out the fourth reaction. After being processed by a homogenizer and cooled to room temperature, the foam control composition is obtained.
9. The method for preparing the foam control composition according to claim 8, characterized in that, The mixing process involves heating to 60~120℃, stirring and dispersing at 500~5000rpm, and grinding until the solid dispersion particle size is below 5μm. The first reaction is carried out at 60~120℃ for 0.5~5 hours; the second reaction is carried out at 60~120℃ for 0.5~2 hours. The third reaction is carried out at 120~180℃ and 1000~3000rpm for 2~6 hours; the fourth reaction is carried out at 100~150℃ and 1000~3000rpm for 1~3 hours.
10. A defoamer, characterized in that, Includes the foam control composition according to any one of claims 1-9.
Citation Information
Patent Citations
Silicone foam control agent
CA2074060A1
Organosilicon composition and preparation method thereof
CN101885916B
Improved silicone foam control agent
EP0163398A1
Method For The Production Of Defoamer Formulations