Composite forming method for large curvature wall panels

By employing a composite forming method, first performing elastic pre-bending and aging treatment, and then shot peening forming, the problem of forming large curvature panels is solved, achieving high-precision forming results with large deformation, which is suitable for the manufacturing of aerospace vehicles.

CN123102837APending Publication Date: 2026-11-17AVIC BEIJING AERONAUTICAL MFG TECH RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611394986.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing creep aging forming and shot peening forming processes are difficult to simultaneously meet the forming accuracy and material performance requirements when forming aerospace aluminum alloy panels with large curvature and complex structures, which can easily lead to material cracking or insufficient forming accuracy.

Method used

A composite forming method is adopted, in which metal parts are first elastically pre-bent at room temperature, then aged, and then shot peening is performed. The large curvature wall panel is formed by combining the two processes.

Benefits of technology

It significantly enhances deformation capacity, avoids the risk of material cracking, improves forming accuracy and total deformation, and is suitable for the manufacture of high-end aerospace panels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102837A_ABST
    Figure CN123102837A_ABST
Patent Text Reader

Abstract

This invention provides a composite forming method for large-curvature wall panels, comprising: placing a solid solution metal part in a creep aging forming mold at room temperature for elastic pre-bending and bonding; placing the bonded part and the mold together in a heating device for aging and heat preservation treatment to allow the material to complete the transformation of its microstructure and properties; removing the constraint fixtures to obtain an artificially aged part with a basic curved shape and measuring its bending radius; elastically pre-bending the artificially aged part to the limit pre-bending radius; performing shot peening on the pre-bent part; and removing the fixtures to obtain the final formed large-curvature wall panel. This invention, through the combined process sequence of creep aging and shot peening, distributes the total deformation across the two processes, effectively overcoming the forming limits of a single process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal sheet plastic processing technology, and more specifically, to a composite forming method for large curvature wall panels. Background Technology

[0002] Large integral panels are key load-bearing components of modern aerospace vehicles, and their manufacturing technology directly affects the performance and lifespan of the equipment. Currently, the forming of such parts mainly relies on two technologies: creep aging forming and shot peening forming.

[0003] Creep aging forming combines the artificial aging of materials with part forming. It utilizes aging treatment to achieve the desired material properties, while simultaneously leveraging the creep deformation that occurs under elastic stress at a specific temperature (artificial aging temperature) to obtain a structural component with a defined shape. Its advantages include high shape accuracy, low residual stress, and good performance. However, its disadvantages include: for panels with large curvature and complex structures, the required forming stress is high, easily approaching the material's plastic forming limit, leading to cracking during forming; and the constraints of the mold make it difficult to flexibly adjust local surfaces.

[0004] Shot peening: This technology is a plastic forming method derived from surface shot peening strengthening. Its basic principle is to use a high-speed shot stream to impact the surface of a metal sheet, causing plastic deformation and elongation of the impacted surface and underlying metal material. This gradually leads to a bidirectional bending deformation of the sheet towards the peened surface, achieving the desired shape. Its advantages include no need for specialized molds, high flexibility, and particular suitability for manufacturing complex curvature panels. However, its disadvantages are equally prominent: it introduces significant gradient residual stress into the material surface, making it difficult to control forming precision. Summary of the Invention

[0005] (a) Technical problems to be solved Existing creep aging forming and shot peening forming processes are typically used independently, and both require forming under elastic pre-bending conditions. The amount of elastic pre-bending determines the achievable forming capability; therefore, the forming capability of both processes is limited by elastic deformation capacity. For aerospace aluminum alloy panels with large curvature and complex structures, a single process is insufficient to meet forming requirements, easily leading to material cracking or insufficient forming accuracy. The technical problem this invention aims to solve is to provide a novel, stable, and reliable composite forming method that can fully utilize the advantages of both creep aging forming and shot peening forming processes, effectively breaking through the forming limits of paneling.

[0006] (II) Technical Solution To achieve the above objectives, the technical solution adopted by the present invention is as follows: This invention provides a composite forming method for large curvature wall panels, comprising the following steps: S1. At room temperature, a solid solution metal part is placed in a creep aging forming mold. An external force is applied to cause the metal part to undergo elastic deformation and conform to the shape of the mold, thereby obtaining the ultimate bending radius R1 of the solid solution elastic pre-bending. It can be calculated from equation (1) based on the pure bending theory.

[0007] (1) In the formula: R is the bending radius of the neutral layer, mm; E is the elastic modulus of the part material, in MPa; y represents the distance from the neutral layer within the curved section, in mm; σ is the normal stress at a distance y from the neutral layer, in mm.

[0008] In engineering, the limit of elastic pre-bending is generally defined as the maximum stress in the bending section reaching 80% of the material's yield strength. Therefore, the limit bending radius of the solution-treated elastic pre-bending can be calculated from equation (1) as shown in equation (2).

[0009] (2) In the formula: E1 is the elastic modulus of the solid solution aluminum alloy, MPa; σ1 is the yield strength of the solid solution aluminum alloy, in MPa; h is the cross-sectional height, in mm.

[0010] It should be noted that in equation (2), "h / 2" represents the distance from the neutral layer to the point where the maximum stress is generated. For irregular cross sections, this distance can be easily calculated by the theory of mechanics of materials.

[0011] S2. Place the bonded metal parts and the mold together in a heating device for aging and heat preservation treatment, so that the material completes the transformation of structure and properties under the action of creep, stress relaxation and aging mechanism, and obtains artificially aged parts. S3. After the heat preservation is completed, remove the constraint fixture to transform the applied elastic deformation into permanent plastic deformation, obtain an artificially aged part with a basic bending shape, and measure its bending radius R2. The formula for calculating R2 is shown in equation (3): (3) In the formula: a is the distance measured by the arc height meter, in mm; f is the arc height value measured using an arc height meter, in mm.

[0012] S4. The artificially aged part is elastically pre-bent to reach the limit bending radius R3 of the artificially aged elastic pre-bending, thereby obtaining a basic shaped wall panel with a large curvature. For artificially aged parts with a certain curved shape, elastic pre-bending is performed. According to the bending theory of curved beams, when the ratio of the curvature radius to the section height of the curved beam is large enough (i.e. R2 / h>>10), the straight beam formula can be used approximately. At the same time, the limit bending radius R3 of the artificially aged elastic pre-bending with the initial bending state (bending radius R2) can be calculated by the linear superposition principle, as shown in equations (4)-(7).

[0013] (4) In the formula: M1 is the bending moment required to generate a pre-bending radius R2 in the artificially aged flat plate part, in MPa.mm. 3 ; E2 is the elastic modulus of artificially aged aluminum alloy, in MPa; I is the moment of inertia of the cross section about the neutral axis, in mm. 4 ; (5) In the formula: The limit radius of elastic pre-bending for artificially aged flat plate parts, in mm; M2 is used to produce artificially aged flat plate parts. The bending moment required for the pre-bending radius, in MPa.mm 3 ; Reference formula (2), It is obtained by calculation from equation (6).

[0014] (6) In the formula: σ2 is the yield strength of the artificially aged aluminum alloy, in MPa; (7) It should be noted that for wall panel structures with complex cross-sections, the elastic limit pre-bending radius of artificially aged parts with a certain curvature can also be obtained by establishing a pure bending simulation model.

[0015] S5. The pre-bent base forming panel is shot peened, and the tooling is removed to obtain the final large curvature panel part.

[0016] Preferably, in step S2, the temperature range of the aging and heat preservation treatment is the artificial aging temperature range of the material, and the heat preservation time is determined according to the alloy system and the aging process curve. After the aging treatment, the material state changes from the solid solution state to the artificial aging state.

[0017] Preferably, in step S5, the shot peening is performed using the maximum shot peening intensity parameter. After removing the pre-bending fixture, the wall panel springs back, resulting in the final bending radius R4. R4 can be calculated using an arc height meter.

[0018] Preferably, the shot peening intensity parameters include shot diameter, shot peening gas pressure, shot flow rate, and feed rate. Preferably, the material of the metal part is any one of the high-strength wrought aluminum alloys from the 2A series, 7A series, or aluminum-lithium alloy system.

[0019] Secondly, the present invention provides a large curvature wall panel, which is manufactured by the composite forming method described above.

[0020] Preferably, the large curvature wall panel has a total deformation amount obtained by successively superimposing creep aging forming and shot peening forming, and its forming limit bending radius R4 is greater than the deformation limit that can be achieved by single creep aging forming or single shot peening forming.

[0021] (III) Beneficial Effects The above-described technical solution of the present invention has at least the following advantages: 1. This invention creatively solves the problem of mutual constraints between performance and shape in traditional methods by first using creep aging to complete the performance curing and basic shaping of the material, and then using shot peening to achieve the precise final shape.

[0022] 2. First, creep aging establishes the excellent material properties and stable basic shape of the wall panel. Then, by utilizing the flexible processing capability of shot peening, further shape adjustment is achieved on the strengthened substrate, so that the total deformation is shared by two processes, effectively avoiding the risk of material cracking that may be caused by single creep aging.

[0023] 3. Significantly increased panel forming limits and comprehensive improvement in overall manufacturing quality were achieved. Through theoretical calculations and experimental verification, the final bending radius R4 of the composite forming strategy is significantly better than the limit achievable by a single process, and the deformation capability is significantly enhanced.

[0024] 4. The process has a clear sequence and well-defined stage objectives, making it particularly suitable for manufacturing high-end aerospace panel parts with stringent material performance requirements and complex shapes, and it has broad engineering application prospects. Attached Figure Description

[0025] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0026] Figure 1 This is a process flow diagram of the composite forming method provided in the embodiments of the present invention; Figure 2This is a schematic diagram of the creep aging forming stage provided in an embodiment of the present invention; Figure 3 This is a schematic diagram of the shot peening forming stage provided in an embodiment of the present invention; Figure 4 These are physical images comparing the deformation limits of different forming strategies provided in the embodiments of the present invention. Detailed Implementation

[0027] To make the technical problems to be solved, the technical solutions, and the beneficial effects of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the present invention and are not intended to limit the present invention.

[0028] The specific implementation of the present invention will be described in more detail below with reference to specific embodiments: Example 1 Taking a 2A97 aluminum-lithium alloy flat plate as an example (length × width × height = 260mm × 70mm × 2.5mm), the specific implementation process of the present invention is explained. The length direction of the flat plate is the rolling direction, and it is pre-bent along the rolling direction.

[0029] Step S1: At room temperature, place the solution-treated (T3 state) 2A97 aluminum-lithium alloy flat part in a creep aging forming mold, and mechanically load it to induce elastic deformation and conform it to the mold's outer surface. The 2A97-T3 aluminum-lithium alloy has E1=79000MPa and σ1=382MPa. From equation (2), R1=323mm is calculated. The flat part is pre-bent to the mold using mechanical loading, and the part and mold are placed in an oven.

[0030] Step S2: The aluminum-lithium alloy is subjected to a suitable two-stage aging process with aging parameters of 125℃ / 15h + 155℃ / 12h. After aging, the material reaches the T8 state from the T3 state. During this process, the material is subjected to creep, stress relaxation, and aging mechanisms, resulting in significant changes in its internal microstructure (including grain structure and strengthening phase distribution) and mechanical properties.

[0031] Step S3: After cooling and depressurization, the flat plate is removed. At this point, the bending radius R2 of the part is calculated to be 1262 mm using an arc height meter. Tensile testing yields the elastic modulus E2 and yield strength σ2 of the T8 state material to be 82000 MPa and 546 MPa, respectively.

[0032] Step S4: Calculate the ultimate elastic pre-bending radius R3 = 198 mm for the artificially aged part with initial bending state using equations (4) to (7). Specifically, first calculate... Then calculate (in Finally, by R3=198 mm is obtained. The artificially aged part is elastically pre-bent to R3=198 mm by a mechanical loading method.

[0033] Step S5: Prestress shot peening forming is performed using an MP15000 shot peening machine with the combined parameters of a shot diameter of 3.18 mm, a shot peening air pressure of 0.35 MPa, a shot flow rate of 10 kg / min, and a feed speed of 3000 mm / min. After unloading, the measured bending radius R4 of the part is 610 mm.

[0034] Comparative Example 1: Single shot peening forming of aged state A T8-state flat part is obtained by subjecting a 2A97-T3 Al-Li alloy flat part to two-stage aging at 125°C for 15 h plus 155°C for 12 h. The ultimate pre-bending radius for single shot peening forming in the artificially aged state is calculated to be 235 mm according to formula (6), and the bending radius after forming under the same shot peening parameters is 720 mm.

[0035] Comparative Example 2: Single creep aging forming Single creep aging forming in the solid solution state can only achieve a certain basic curvature (corresponding to R2=1262 mm in Example 1), and its deformation capacity is limited by the elastic pre-bending limit R1=323 mm, so the curvature cannot be further significantly increased.

[0036] Comparative Analysis of Deformation Limits For the convenience of comparison, the deformation limits of the three forming strategies are compared: the final bending radius of single creep aging forming in the solid solution state is R2=1262 mm; the final bending radius of single shot peening forming in the artificially aged state is 720 mm; while the final bending radius of the composite forming strategy in the solid solution state of the present invention is R4=610 mm. Obviously, the relationship of R4<720 mm<R2 indicates that the composite forming strategy can obtain a larger total deformation than any single process (that is, a smaller bending radius corresponds to a larger curvature), which effectively breaks through the forming limit of a single process.

[0037] The above analysis shows that, through the composite process route of creep aging forming plus shot peening forming, the present invention distributes the total deformation to two process stages: in the first stage, basic plastic deformation (R1→R2) is obtained through creep aging under relatively low stress conditions; in the second stage, the curvature (R3→R4) is further increased by elastic pre-bending and shot peening on the material that has been age-strengthened. After the deformations of the two stages are superimposed, the total forming limit significantly exceeds that of any single process, which effectively solves the forming problem of large-curvature panels.

[0038] Description of Process Parameters During the implementation of the present invention, the following process parameters need to be adjusted according to the specific alloy system: (1) Aging temperature and time: For 2A series aluminum alloys, single-stage or double-stage aging process is usually adopted; for 7A series aluminum alloys (such as 7075), the typical aging temperature is 120~135℃ and the holding time is 16~24h; for aluminum-lithium alloys (such as 2A97), double-stage aging process (such as 125℃ / 15h+155℃ / 12h) can be adopted. The specific parameters need to be determined according to the aging hardening curve of the alloy.

[0039] (2) Shot peening parameters: The shot material is usually cast iron shot or steel shot, with a shot diameter range of 2.0~4.0 mm; the shot peening gas pressure range of 0.2~0.5 MPa; the shot flow rate range of 5~15 kg / min; and the feed speed range of 1000~5000 mm / min. For the final forming stage, the maximum shot peening intensity parameter should be used to achieve the maximum deformation.

[0040] (3) Elastic pre-bending loading method: Mechanical loading (such as three-point bending, four-point bending) or vacuum loading method can be used. During the loading process, it is necessary to ensure that the parts fit evenly against the mold surface to avoid local stress concentration that could lead to cracking.

[0041] (4) Scope of application of materials: This invention is not only applicable to 2A97 aluminum-lithium alloy, but can also be extended to 2A series aluminum alloys such as 2A12 and 2A14, 7A series aluminum alloys such as 7075, 7050, and 7A04, as well as other high-strength wrought aluminum alloy materials. For different materials, only the aging process parameters and the corresponding material constants (E1, σ1, E2, σ2) need to be adjusted, while the process principle and flow remain unchanged.

[0042] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method of compound forming a large curvature panel, characterized by, Includes the following steps: S1. At room temperature, a solid solution metal part is placed in a creep aging forming mold. An external force is applied to cause the metal part to undergo elastic deformation and conform to the shape of the mold, thereby obtaining the ultimate bending radius R1 of the solid solution elastic pre-bending. S2. Place the bonded metal parts and the mold together in a heating device for aging and heat preservation treatment, so that the material completes the transformation of structure and properties under the action of creep, stress relaxation and aging mechanism, and obtains artificially aged parts. S3. After the heat preservation is completed, remove the constraint fixture to transform the applied elastic deformation into permanent plastic deformation, obtain an artificially aged part with a basic bending shape, and measure its bending radius R2. S4. The artificially aged part is elastically pre-bent to reach the limit bending radius R3 of the artificially aged elastic pre-bending, thereby obtaining a basic shaped wall panel with a large curvature. S5. The pre-bent base forming panel is shot peened, and the tooling is removed to obtain the final large curvature panel part.

2. The method of compound forming of large curvature panels of claim 1, wherein, The ultimate bending radius R1 of the solid solution elastic pre-bending is calculated according to the following formula based on pure bending theory: Where E1 is the elastic modulus of the solid solution metallic material, σ1 is the yield strength of the solid solution metallic material, and h is the cross-sectional height.

3. The method of compound forming of large curvature panels of claim 1, wherein, In step S2, the temperature range of the aging and heat preservation treatment is the artificial aging temperature range of the material, and the heat preservation time is determined according to the alloy system and the aging process curve. After the aging treatment, the material state changes from solid solution state to artificial aging state.

4. The method of compound forming of large curvature panels of claim 1, wherein, In step S3, the bending radius R2 is obtained by measuring the arc height using an arc height meter. The measurement and calculation formula is as follows: Where a is the distance measured by the arc height meter; f is the arc height value measured by the arc height meter.

5. The method of compound forming of large curvature panels of claim 1, wherein, In step S4, the artificially aged elastic pre-bending limit bending radius R3 is calculated based on the curved beam bending theory and the linear superposition principle. When the ratio of the bending radius R2 to the section height h satisfies R2 / h>>10, the straight beam formula is used for approximate calculation, and R3 is obtained by the following formula: Where M1 is the bending moment required to generate the bending radius R2, M2 is the bending moment required to generate the artificially aged elastic pre-bending limit bending radius R3, E2 is the elastic modulus of the artificially aged metallic material, and I is the moment of inertia of the cross section about the neutral axis.

6. The method of compound forming of large curvature panels of claim 1, wherein, In step S5, the shot peening is performed using the maximum shot peening intensity parameter. After removing the pre-bending fixture, the wall plate springs back, resulting in the final bending radius R4.

7. The method of compound forming of large curvature wall panels of claim 6, wherein, The parameters for shot peening intensity include shot diameter, shot peening gas pressure, shot flow rate, and feed rate.

8. The method of compound forming of large curvature panels of claim 1, wherein, The material of the metal parts is any one of the high-strength wrought aluminum alloys from the 2A series, 7A series, or aluminum-lithium alloy system.

9. A large-curvature wall panel, characterized by, Made by the composite molding method according to any one of claims 1 to 7.

10. The large curvature wall panel as described in claim 8, characterized in that, The large curvature wall panel has a total deformation amount obtained by successively superimposing creep aging forming and shot peening forming, and its forming limit bending radius R4 is greater than the deformation limit that can be achieved by single creep aging forming or single shot peening forming.