Gradient filling casting method for thin-walled castings and its application
By employing reverse preheating and various temperature and pressure compensation methods, the problems of uneven temperature and insufficient filling pressure in investment casting of thin-walled complex structures have been solved, achieving efficient filling and high-quality casting of thin-walled castings, which is suitable for aero-engine blades and thin-walled parts of medical devices.
Patent Information
- Application Number
- CN202611174401.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-04
- Publication Date
- 2026-11-17
AI Technical Summary
Existing investment casting processes suffer from uneven temperature distribution and a lack of adaptive control over filling pressure when preparing thin-walled, complex-structure castings. This results in low filling rates in thin-walled areas, making them prone to defects such as under-casting, cold shuts, and shrinkage porosity. Consequently, they fail to meet the manufacturing requirements for thin-walled components in aero-engine blades and medical devices.
A gradient temperature field is formed by reverse preheating, combined with three-stage pressure control and various temperature and pressure compensation methods, including heat insulation coating, auxiliary heating elements and phase change heat storage materials, and mechanical vibration, to ensure temperature compensation and pressure adaptability of molten metal during long-process filling, so as to achieve balanced filling and sequential solidification.
It effectively eliminates undercasting and cold shut defects in thin-walled castings, broadens the process window, improves the density and mechanical properties of castings, and meets the quality requirements of high-end components.
Smart Images

Figure CN123102925A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of precision casting technology, specifically relating to a gradient filling casting method for thin-walled castings and its application. Background Technology
[0002] Investment casting is a crucial process for manufacturing complex and precision castings, widely used in aerospace, medical devices, and automotive industries. With the increasing trend towards lightweight and precision industrial equipment, the demand for thin-walled, complex-structure castings is growing, placing higher demands on the investment casting process.
[0003] The main characteristics of thin-walled complex structure castings are: local wall thickness less than 1.5mm, complex structure, long filling process, and drastic changes in cross-section of various parts of the casting. During the filling process, as the molten metal flows along the filling path, heat is continuously dissipated to the mold shell, resulting in the temperature of the molten metal at the end being significantly lower than that of the gating zone. This makes it very easy for premature solidification to occur at the thin-walled end, forming defects such as under-casting and cold shuts. At the same time, due to the large differences in wall thickness in different areas, the filling resistance in different areas varies significantly, and uniform filling pressure cannot simultaneously meet the filling requirements of the thin-walled high-resistance area and the feeding requirements of the thick-walled area. Summary of the Invention
[0004] This application addresses the shortcomings of existing investment casting processes in preparing thin-walled complex structural castings. Uneven temperature distribution along the filling path and lack of adaptive pressure control lead to low filling rates in thin-walled areas, resulting in defects such as under-casting, cold shuts, and shrinkage porosity, and ultimately, low yield rates. These issues prevent the process from meeting the manufacturing requirements of high-end components such as aero-engine blades and thin-walled parts for medical devices. The application proposes a gradient filling method for investment casting of thin-walled complex structural castings.
[0005] The objective of this application can be achieved through the following technical solutions.
[0006] In a first aspect of this application, a gradient filling casting method for thin-walled castings is provided, comprising the following steps: S1. The mold shell of the casting is preheated in reverse order along the filling path. The mold shell is divided into a gating zone, a transition zone and a cavity end zone along the filling path. The preset temperatures are T1, T2 and T3, respectively, where T3 > T2 > T1 and T3 - T1 ≥ 100℃. This application uses reverse preheating to create a gradient temperature field opposite to the filling direction, thereby compensating for the heat loss of molten metal during the long-process filling process, ensuring that the final molten metal still maintains good fluidity, and eliminating the hidden dangers of under-casting and cold shut from the source.
[0007] S2. The filling process includes an initial filling stage, a linear pressurization stage, and a pressure holding stage, with pressures P0, P1, and P2, respectively, where P0 is 0.05–0.10 MPa, P1 is 0.15–0.30 MPa, and P2 is 1.5–3.0 times that of P1; the linear pressurization stage begins when the filling rate reaches 30 vol.%, and the pressure holding stage is switched from the linear pressurization stage to the pressure holding stage when the filling rate reaches 85 vol.%. This application employs a three-stage pressure control system. The initial low pressure avoids splashing of molten metal, the pressure gradually increases during the linear pressure increase stage to accommodate the increased filling resistance, and the pressure holding stage maintains the unobstructed feeding channel with a higher pressure.
[0008] S3. During the filling process, the cavity includes a thin-walled high-resistance zone with a wall thickness < 1.5 mm, a medium-walled zone with a wall thickness of 1.5 mm ≤ 3 mm, and a thick-walled transition zone with a wall thickness > 3 mm. Temperature compensation amounts Q1, Q2, and Q3, and pressure increase amounts ΔP1, ΔP2, and ΔP3 are applied to these zones respectively. Specifically, Q1 is 35–50 J / g, Q2 is 25–35 J / g, Q3 is 12–20 J / g, ΔP1 is 0.1–0.15 MPa, ΔP2 is 0.07–0.1 MPa, and ΔP3 is 0.04–0.06 MPa. The local pressure increase refers to the additional pressure value added to each zone based on the P1 pressure. The purpose of step S3 is to ensure that the molten metal in each region has a continuous and stable flow capability, so as to achieve balanced filling and sequential solidification.
[0009] S4. After filling is completed, the holding pressure P2 is maintained for the time until the casting is completely solidified.
[0010] Preferably, the boost rate of the linear boost stage is 0.5–2.0 MPa / s; The vacuum degree before filling is 10-50 Pa.
[0011] In some embodiments, the pressure loading rate of the thin-walled high-resistivity region is 1.5 to 2.0 MPa / s, the pressure loading rate of the medium-walled region is 0.8 to 1.5 MPa / s, and the pressure loading rate of the thick-walled transition region is 0.5 to 0.8 MPa / s.
[0012] Furthermore, the pressure loading rate is positively correlated with the real-time temperature of the molten metal and negatively correlated with the dynamic viscosity of the molten metal.
[0013] Furthermore, a heat-insulating coating is sprayed onto the thin-walled high-resistivity region, and a cooling coating is sprayed onto the thick-walled transition region. The outer wall of the shell is provided with an auxiliary heating element with controllable power; Phase change thermal storage material is embedded in the end region of the cavity.
[0014] The heat insulation coating described in this application slows down heat dissipation in thin-walled areas, the auxiliary heating element actively replenishes heat, and the phase change heat storage material uses latent heat to stabilize the temperature.
[0015] In some embodiments, during the pressure holding stage, forced cooling is applied to the gating zone to allow the gating zone to solidify preferentially over the cavity end zone. The cooling medium is compressed air or water mist, and the cooling rate is 5–20 °C / s.
[0016] In some embodiments, the filling process includes mechanical vibration with a frequency of 20–80 Hz, an amplitude of 0.1–0.5 mm, and a vibration direction parallel to the main filling direction of the molten metal.
[0017] The mechanical vibration described in this application can reduce the apparent viscosity of molten metal, improve wettability, and assist in filling thin-walled areas. At the same time, vibration disturbance promotes grain refinement and improves the mechanical properties of castings.
[0018] Preferably, the system comprises a main gating system, branch gating systems, and an inner gating system, wherein the diameter ratio of the main gating system, branch gating systems, and inner gating system is 4:2:1, and the cross-sectional area of each gating system is 1.2 to 1.5 times the area of the front edge of the mold filling.
[0019] The graded gating system design described in this application ensures smooth flow of molten metal, gradually decelerates and reduces turbulence, while ensuring that the gating system has sufficient feeding capacity to avoid premature solidification in certain areas that cuts off the feeding path. The area of the filling front refers to the area of the cavity cross-section corresponding to the front end of the molten metal flow during the filling process. For sections with uniform wall thickness, this area is equal to the cross-sectional area of the cavity at that location. For sections with varying wall thickness, this area is taken as the maximum or average value of the cross-sectional area of the cavity within that section.
[0020] In a second aspect of this application, a gradient filling casting method for thin-walled castings is provided, wherein the molten metal includes high-temperature nickel-based alloys, copper alloys, TiAl-based alloys, or titanium alloys, and the pouring temperature is 30–80°C higher than the alloy liquidus temperature.
[0021] In a third aspect of this application, the application of a gradient filling casting method for thin-walled castings in the casting of thin-walled parts for aero-engine blades and medical devices is provided.
[0022] The beneficial effects of the gradient filling casting method for thin-walled castings in this application include: (1) Active gradient temperature field compensation to eliminate end casting defects; (2) Pressure-temperature coupled adaptive control broadens the process window and avoids defects such as flash and thermal cracking caused by relying solely on high-pressure filling; (3) The combination of reverse preheating and forced cooling of the gating zone during the pressure holding stage achieves sequential solidification from the end to the gating zone, effectively reducing shrinkage porosity and shrinkage defects, and improving the density of the casting; (4) Various temperature compensation methods such as heat insulation coating, auxiliary heating element, and phase change heat storage material can be used individually or in combination to meet the needs of castings with different wall thickness distribution and structural complexity. (5) Mechanical vibration can reduce the apparent viscosity of molten metal, improve the filling properties of thin-walled areas, refine grains, and enhance the mechanical properties of castings. Attached Figure Description
[0023] Figure 1 This is a general flowchart of the gradient filling casting method for thin-walled castings described in this application. Detailed Implementation
[0024] The following detailed description, with appropriate reference to the accompanying drawings, discloses embodiments of the gradient filling casting method for thin-walled castings according to this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0025] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of the particular range. The range defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range.
[0026] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0027] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0028] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used in this application is for the purpose of describing particular embodiments only and is not intended to limit this application; unless otherwise stated, the values of the parameters mentioned in this application can be measured using various measurement methods commonly used in the art (e.g., they can be tested according to the methods given in the embodiments of this application). Example 1
[0029] This embodiment provides a gradient filling casting method for thin-walled castings, used to prepare thin-walled blade castings of high-temperature nickel-based alloy (grade: K418) for aero-engines. The minimum wall thickness of the casting is 1.2 mm, and the maximum wall thickness is 4.5 mm.
[0030] S1. A silica sol-zircon powder mold shell is used. After shell preparation, dewaxing, and calcination, the shell is divided into a gating zone, a transition zone, and a cavity end zone along the filling path. A zoned induction heating device is used for reverse preheating. The preheating temperature T1 for the gating zone is set to 180℃, the preheating temperature T2 for the transition zone is set to 200℃, and the preheating temperature T3 for the cavity end zone is set to 300℃.
[0031] S2. A pneumatic investment casting machine is used, and the vacuum degree is evacuated to 30 Pa before filling the mold. The pouring temperature of the molten metal is controlled at 1510℃.
[0032] The filling process is divided into three stages: the initial filling stage pressure P0 is 0.08 MPa, which continues until the filling rate reaches 30%; the linear pressure increase stage pressure increase rate is 1.2 MPa / s, and the pressure increases linearly from P0 to P1 at 0.25 MPa. When the filling rate reaches 85%, the process switches to the pressure holding stage; the pressure holding stage pressure P2 is 0.6 MPa, and the pressure is held until the casting is completely solidified. The pressure holding time is 120 s.
[0033] S3. Based on the cavity wall thickness, divide the cavity into three regions: a thin-walled high-resistivity region (wall thickness 1.2 mm), a medium-walled region (wall thickness 2.0 mm), and a thick-walled transition region (wall thickness 4.5 mm). Apply temperature compensation amounts Q1=45 J / g, Q2=30 J / g, Q3=18 J / g, ΔP1=0.12 MPa, ΔP2=0.08 MPa, and ΔP3=0.05 MPa, respectively.
[0034] The temperature compensation method is as follows: a Y2O3-stabilized ZrO2 thermal insulation coating is sprayed on the thin-walled high-resistivity area, with a coating thickness of 0.3 mm; a graphite-based chilling coating is sprayed on the thick-walled transition area; and an Al-Si phase change thermal storage material is embedded in the cavity end area, with a phase change temperature of 560℃.
[0035] S4. Apply mechanical vibration during the filling process. The vibration frequency is 50 Hz, the amplitude is 0.3 mm, and the vibration direction is parallel to the main filling direction of the molten metal.
[0036] S5. After filling is completed, during the pressure holding stage, forced water mist cooling is applied to the gating area at a rate of 12℃ / s to allow the gating area to solidify preferentially, thus achieving sequential solidification from the end of the cavity to the gating area.
[0037] S6. It adopts a three-level structure of main runner, branch runner and ingate. The diameter ratio of the main runner, branch runner and ingate is 4:2:1. The cross-sectional area of each runner is 1.35 times the area of the front edge of the mold filling.
[0038] Upon inspection, the K418 thin-walled blade casting prepared in this embodiment showed no cold shuts or undercasting defects on the surface, and no shrinkage porosity or shrinkage cavities inside, as determined by X-ray flaw detection and fluorescence penetrant testing. The filling rate was 98.7%, and the casting density was 12% higher than that of the conventional uniform preheating process. Example 2
[0039] This embodiment provides a gradient filling casting method for thin-walled castings, used to prepare TiAl-based alloys (Ti-48Al-2Cr-2Nb). The minimum wall thickness of the casting is 0.8 mm, and the maximum wall thickness is 3.2 mm.
[0040] S1. The pouring temperature T0 is 1510℃. T1 is set to 180℃, T2 to 200℃, and T3 to 320℃.
[0041] S2, vacuum degree is 20 Pa. P0=0.06 MPa, P1=0.18 MPa, P2=0.45 MPa, pressurization rate is 0.8 MPa / s. The initial filling stage continues until the filling rate reaches 30%, and when the filling rate reaches 85%, it switches to the pressure holding stage, and the pressure holding time is 150s.
[0042] S3, Thin-walled high-resistivity region (wall thickness 0.8 mm): Q1=49 J / g, ΔP1=0.15 MPa; Medium-walled region (wall thickness 1.8 mm): Q2=35 J / g, ΔP2=0.10 MPa; Thick-walled transition region (wall thickness 3.2 mm): Q3=20 J / g, ΔP3=0.06 MPa.
[0043] An infrared auxiliary heating element with a power density of 0.8 W / cm² is installed on the outer wall of the shell in the thin-walled, high-resistivity region. 2 The cavity end region is embedded with Mg-Zn eutectic phase change thermal storage material, and its phase change temperature is 420℃.
[0044] S4. The mechanical vibration frequency is 80 Hz and the amplitude is 0.2 mm; the runner area is cooled by compressed air with a cooling rate of 8℃ / s; the runner diameter ratio is 4:2:1 and the cross-sectional area of each runner is 1.4 times the area of the front edge of the mold filling.
[0045] Testing showed that the TiAl alloy medical implant obtained in this embodiment had a filling rate of 98.2%, a smooth surface, and no internal shrinkage defects. Example 3
[0046] This embodiment provides a gradient filling casting method for thin-walled castings, used to prepare thin-walled complex shell castings of copper alloy (ZCuSn10P1). The minimum wall thickness of the casting is 1.0 mm, and the maximum wall thickness is 5.0 mm.
[0047] S1. The pouring temperature T0 is 1100℃. Set T1=150℃, T2=180℃, and T3=280℃.
[0048] S2, vacuum degree is 40 Pa. P0=0.10 MPa, P1=0.30 MPa, P2=0.90 MPa, pressurization rate is 2.0 MPa / s. The initial filling stage continues until the filling rate reaches 30%, and when the filling rate reaches 85%, it switches to the pressure holding stage, and the pressure holding time is 100s.
[0049] S3, Thin-walled high-resistivity region (wall thickness 1.0 mm): Q1=38 J / g, ΔP1=0.10 MPa; Medium-walled region (wall thickness 2.5 mm): Q2=25 J / g, ΔP2=0.07 MPa; Thick-walled transition region (wall thickness 5.0 mm): Q3=12 J / g, ΔP3=0.04 MPa.
[0050] The thin-walled high-resistivity zone is coated with an alumina thermal insulation coating; the thick-walled transition zone is coated with a copper-based quenching coating; and the end region of the cavity is embedded with a Sn-Bi eutectic phase change thermal storage material with a phase change temperature of 200℃.
[0051] S4. The mechanical vibration frequency is 20 Hz and the amplitude is 0.5 mm; the gating area is cooled by water mist with a cooling rate of 18℃ / s; the gating diameter ratio is 4:2:1 and the cross-sectional area of each gating stage is 1.2 times the area of the filling front edge.
[0052] Testing showed that the copper alloy shell casting produced in this embodiment had a filling rate of 98.5%, no cold shuts or shrinkage defects, and a density that was 10% higher than that produced by conventional processes.
[0053] Comparative Example 1 This comparative example provides a gradient filling casting method for thin-walled castings, which differs from Example 1 in that the mold shell is not preheated in a zonal reverse sequence, but is uniformly preheated to 200°C. The remaining process parameters (P0=0.08 MPa, P1=0.25 MPa, P2=0.6 MPa, pressure increase rate 1.2 MPa / s), alloy system, and casting structure are the same as in Example 1, and no zonal temperature compensation is applied.
[0054] The results showed that the casting had obvious undercasting and cold shut defects in the thin-walled area (wall thickness of 1.2 mm) at the end of the cavity, with a filling rate of only 82.3%. This indicates that the failure to establish a gradient temperature field by using reverse preheating resulted in an early drop in the temperature of the molten metal front end, which could not compensate for the heat loss in the long process, leading to the failure of filling at the thin-walled end.
[0055] Comparative Example 2 This comparative example provides a gradient filling casting method for thin-walled castings. The difference from Example 2 is that it does not perform zoned temperature compensation (i.e., Q1=Q2=Q3=0) or apply pressure-temperature coupling control; instead, it uses a single filling pressure P=0.18MPa constant pressure filling. All other conditions are the same as in Example 2.
[0056] The results showed that the filling rate in the thin-walled high-resistivity region (wall thickness 0.8 mm) was only 79.5%, resulting in large-area cold shuts; while the thick-walled transition region (wall thickness 3.2 mm) exhibited shrinkage porosity and thermal cracking. The overall filling rate was 85.1%, which failed to meet the quality requirements for medical implants. This indicates that without zoned temperature compensation and adaptive pressure control, the filling behavior in different wall thickness regions is mismatched, with under-casting in the thin-walled region and defects in the thick-walled region coexisting.
[0057] The embodiments of this application cover any points not exhaustively covered by the technical scope claimed in this application, as well as new technical solutions formed by equivalent substitutions of one or more technical features in the technical solutions of the embodiments, all of which are within the scope of protection claimed in this application. At the same time, in all the listed or unlisted embodiments of the solution in this application, each parameter in the same embodiment merely represents an instance (i.e., a feasible solution) of its technical solution, and there is no strict coordination or limitation relationship between the parameters. The parameters can be substituted for each other without violating axioms and the claims of this application, unless otherwise stated.
[0058] The technical means disclosed in this application are not limited to those described above, but also include technical solutions composed of any combination of the above technical features. The above descriptions are specific embodiments of this application. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of this application, and these improvements and modifications are also considered within the scope of protection of this application.
[0059] The specific embodiments described herein are merely illustrative examples of the spirit of this application. Those skilled in the art to which this application pertains may make various modifications or additions to the described specific embodiments or use similar methods to substitute them, without departing from the spirit of this application or exceeding the scope defined by the appended claims.
Claims
1. A gradient filling casting method for thin-walled castings, characterized in that, Includes the following steps: S1. The mold shell of the casting is preheated in reverse order along the filling path. The mold shell is divided into a gating zone, a transition zone and a cavity end zone along the filling path. The preset temperatures are T1, T2 and T3, respectively, where T3 > T2 > T1 and T3 - T1 ≥ 100℃. S2. The filling process includes an initial filling stage, a linear pressurization stage, and a pressure holding stage, with pressures of P0, P1, and P2, respectively, where P0 is 0.05–0.10 MPa, P1 is 0.15–0.30 MPa, and P2 is 1.5–3.0 times that of P1; the linear pressurization stage occurs when the filling rate reaches 30 vol.%, and the pressure holding stage is switched when the filling rate reaches 85 vol.%. S3. During the filling process, the cavity includes a thin-walled high-resistance region with a wall thickness < 1.5 mm, a medium-walled region with a wall thickness of 1.5 mm ≤ 3 mm, and a thick-walled transition region with a wall thickness > 3 mm. Temperature compensation amounts Q1, Q2, and Q3, and pressure increase amounts ΔP1, ΔP2, and ΔP3 are applied to these regions respectively. Among them, Q1 is 35–50 J / g, Q2 is 25–35 J / g, Q3 is 12–20 J / g, ΔP1 is 0.1–0.15 MPa, ΔP2 is 0.07–0.1 MPa, and ΔP3 is 0.04–0.06 MPa. The local pressure increase amount refers to the additional pressure value added to each region based on the pressure P1. S4. After filling, maintain pressure at pressure P2 until the casting is completely solidified.
2. The method according to claim 1, characterized in that, The pressure increase rate during the linear pressure increase stage is 0.5–2.0 MPa / s; the vacuum degree before filling is 10–50 Pa.
3. The method according to claim 2, characterized in that, The pressure loading rate of the thin-walled high-resistivity region is 1.5–2.0 MPa / s, the pressure loading rate of the medium-walled region is 0.8–1.5 MPa / s, and the pressure loading rate of the thick-walled transition region is 0.5–0.8 MPa / s.
4. The method according to claim 2, characterized in that, The pressurization rate is positively correlated with the real-time temperature of the molten metal and negatively correlated with the dynamic viscosity of the molten metal.
5. The method according to claim 1, characterized in that, The temperature compensation method includes one or more of the following: A heat-insulating coating is sprayed onto the thin-walled high-resistivity region, and a cooling coating is sprayed onto the thick-walled transition region. The outer wall of the shell is provided with an auxiliary heating element with controllable power; Phase change thermal storage material is embedded in the end region of the cavity.
6. The method according to claim 1, characterized in that, During the pressure holding stage, forced cooling is applied to the gating area to cause the gating area to solidify preferentially over the cavity end area. The cooling medium is compressed air or water mist, and the cooling rate is 5 to 20°C / s.
7. The method according to claim 1, characterized in that, The filling process includes mechanical vibration, with a frequency of 20–80 Hz, an amplitude of 0.1–0.5 mm, and the vibration direction parallel to the main filling direction of the molten metal.
8. The method according to claim 1, characterized in that, It includes a main gating system, branch gating systems, and an ingate system. The diameter ratio of the main gating system, branch gating systems, and ingate system is 4:2:1, and the cross-sectional area of each gating system is 1.2 to 1.5 times the area of the front edge of the mold filling.
9. The method according to any one of claims 1 to 8, characterized in that, The molten metal includes high-temperature nickel-based alloys, copper alloys, TiAl-based alloys, or titanium alloys, and the casting temperature is 30–80°C higher than the alloy liquidus temperature.
10. The application of the method described in any one of claims 1 to 9 in the casting of thin-walled parts for aero-engine blades and medical devices.