Camera lens shade light elimination method

By combining chemical and physical grinding methods, the light-absorbing effect of camera light shields is improved, solving the problem of unsatisfactory light absorption in internal holes, improving the optical performance and yield of the product, and making it suitable for optical applications in smart electronic products.

CN123104129APending Publication Date: 2026-11-17DONGGUAN HOUDE TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611236241.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing methods for extinguishing light in camera light shields have unsatisfactory light-extinguishing effects due to internal holes, resulting in a high defect rate. Furthermore, the materials are prone to deformation under different temperature conditions, affecting imaging performance.

Method used

A combination of chemical and physical polishing methods is used, which involves chemical matte treatment and UV adhesive protective coating followed by physical matte polishing to form a uniform matte black surface, ensuring that optical performance meets the standards.

Benefits of technology

It improves the optical characteristics and yield of camera light shields, reduces reflectivity, avoids stray light problems in actual lens shooting, and is suitable for demanding optical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123104129A_ABST
    Figure CN123104129A_ABST
Patent Text Reader

Abstract

The present application relates to camera lens hood processing technical field, specifically to a kind of camera lens hood extinction method, the extinction method includes the following steps: step one: camera lens hood product punch forming;Step two: chemical extinction treatment;Step three: cleaning and drying;Step four: UV glue protective layer coating;Step five: physical extinction polishing treatment;Step six: finished product self-checking and transfer order;The whole process of the present application is simple, reasonable in design, the present application is extinguished by chemical and physical grinding, to improve the optical properties of camera lens hood, help to improve the functional performance of final product, improve the yield of product, suitable for the optical application field requiring strict, reduce the reflectivity of lens hood, avoid the problem of lens real shot stray light.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of camera light shield processing technology, specifically a method for eliminating light from camera light shields. Background Technology

[0002] Light-shielding sheets are primarily used in camera devices of smart electronic products such as mobile phones and tablets. With the development of electronic products, the imaging devices mounted on them have also flourished. As technology advances, users have increasingly higher quality requirements for portable electronic devices. Currently, the mainstream materials for optical light-shielding sheets are PET and PI sheets. Their main advantages are ease of molding and a reduced reflectivity after carbon layer treatment. However, their disadvantages include high cross-sectional reflectivity after punching, significant glare, poor temperature resistance, and susceptibility to deformation after environmental testing. Therefore, they cannot support the long-term use and varying temperature conditions required for imaging devices in smart electronic products. On the other hand, hard, high-strength materials, such as metals, tend to have high reflectivity, which can lead to stray light in the lens during shooting, affecting image quality.

[0003] Currently, existing camera light-shielding sheets mainly use physical grinding to eliminate light. The main drawback of physical light elimination is that it is not ideal for eliminating light in the inner holes of the light-shielding sheet, resulting in a high defect rate. To address this, the inventor has improved the light-eliminating method for camera light-shielding sheets. Summary of the Invention

[0004] The purpose of this invention is to provide a method for eliminating light on a camera light shield. By using chemical and physical grinding to eliminate light, the optical properties of the camera light shield are improved, which helps to improve the functional performance of the final product and increase the product yield. This solves the problems mentioned in the above-mentioned technical background.

[0005] To achieve the above objectives, the present invention provides the following technical solution: a method for eliminating light from a camera light-blocking plate, comprising the following steps:

[0006] Step 1: Stamping and forming of camera light shield product. Select a camera light shield substrate, clean and pre-treat the surface of the camera light shield substrate, and use precision molds and punching equipment to punch and cut the camera light shield substrate to form a predetermined diameter shape, inner hole and cutting edge structure to obtain a qualified stamped camera light shield.

[0007] Step Two: Chemical Matting Treatment. Pour the matting solution into the soaking fixture, then place the stamped, qualified camera light shield into the fixture, ensuring it is completely submerged. The temperature of the matting solution is controlled between 30℃ and 60℃, and the soaking time is between 30 minutes and 150 minutes. Stir the stamped, qualified camera light shield every 10 minutes to ensure the PET material on the cutting edge of the stamped camera light shield is completely corroded and softened by the matting solution. The matting solution is prepared using a low-temperature stepwise mixing process. The specific preparation method follows the following weight ratio and process limitations: 10-30 parts by weight of alkaline corrosive agent, 1-10 parts by weight of functional matting filler, and 80-100 parts by weight of high-purity deionized water. The resistivity of the deionized water is not less than 18.25 MΩ·cm, and impurities in the water are removed to avoid affecting the matting process. The stability of the matting agent and the corrosion uniformity of the camera's light shield were investigated. The matting agent was prepared in a closed, alkali-resistant, corrosion-resistant, and stirred reaction vessel. First, the reaction vessel was cleaned and dried to avoid residual impurities and water stains contaminating the agent system. The temperature inside the reaction vessel was controlled below 70°C. Then, all the metered high-purity deionized water was injected into the reaction vessel, and a low-speed stirrer was turned on to maintain a uniform stirring state. The alkaline corrosive agent was then slowly added in batches. After the alkaline corrosive agent was completely dissolved and the temperature of the aqueous solution system was stable, the functional matting filler was added in batches. After all materials were added, the mixture was stirred at a constant temperature and speed for 3-5 minutes until the materials in the container were completely and uniformly dispersed. The system showed no visible particles, stratification, sedimentation, or agglomeration, forming a homogeneous and stable composite matting corrosion agent. After preparation, the solution was sealed and allowed to stand.

[0008] Step 3: Cleaning and drying. Take out the camera light shield after soaking and matting in Step 2, and use a multi-stage rinsing method with clean water to thoroughly remove any residual chemical components from the surface, inner holes, and crevices of the camera light shield. After draining the water from the cleaned camera light shield, put it into a constant temperature drying device for drying treatment to completely evaporate the moisture on the surface and in the crevices of the camera light shield, ensuring that the camera light shield is completely dry, without water stains or moisture. After drying, let it cool naturally to room temperature.

[0009] Step 4: UV adhesive protective layer coating. Apply UV protective adhesive evenly to the entire surface of the camera light shield after cooling and drying, ensuring that the adhesive layer is of uniform thickness, without any missed areas, adhesive accumulation, or bubbles, and completely covering the carbon black layer on the surface of the camera light shield. After coating, cure the adhesive using a UV curing device to quickly form a dense and stable protective film that adheres to the surface of the camera light shield product.

[0010] Step 5: Physical matte polishing treatment. The original glossy surface of the inner holes and blade edges of the camera lens hood from Step 4 is uniformly polished to make the glossy mirror surface uniformly matte black, achieving the matte finish requirements for product appearance and optical performance. At the same time, the UV adhesive protective coating on the surface of the camera lens hood is precisely removed by polishing. The force and precision are controlled during the polishing process to completely remove the UV adhesive without damaging the product substrate and internal carbon black layer, ensuring that the product surface texture is uniform and the optical performance meets the standards.

[0011] Step Six: Finished Product Self-Inspection and Transfer. Manual inspection confirms that the camera light shield products have no shiny surfaces, burrs, or scratches on the blades and inner holes, and are uniformly matte black overall. There is no UV glue residue, no carbon layer peeling, and no discoloration defects on the surface. Qualified camera light shield products are sorted and classified and transferred to the next processing stage. Defective products are individually marked, reworked, or scrapped.

[0012] Preferably, in step one, it is necessary to ensure that the blade structure is flat, burr-free, and deformation-free. The camera light shield substrate is a low-reflectivity camera light shield substrate. During the cleaning and pretreatment of the camera light shield substrate surface, an optical microscope with image analysis software is used to observe and measure the particle size on the camera light shield substrate surface. The camera light shield substrate surface is cleaned and degreased using an ultrasonic cleaning device.

[0013] Preferably, the particle density on the surface of the camera light shield substrate is ≤6g / cm³, and the size of a single particle on the surface of the camera light shield substrate is between 3 and 15 micrometers.

[0014] Preferably, the alkaline corrosive agent in step two is an aqueous solution of sodium hydroxide or potassium hydroxide. The alkaline corrosive agent can specifically corrode the surface polymer resin structure of the camera light shield, so that a uniform and dense microporous structure is formed on the flat surface of the camera light shield, breaking the mirror gloss of the substrate surface and achieving a basic chemical matting effect. At the same time, the controllable alkaline corrosion system can precisely control the corrosion depth of the camera light shield surface, avoiding excessive corrosion that could cause substrate damage and excessive thickness reduction.

[0015] Preferably, the functional matting filler in step two is selected from any one or more of fumed silica, silica sol, and ultrafine alumina powder; the functional matting filler can be uniformly filled into the microporous structure of the camera light shield surface formed by alkaline etching.

[0016] Preferably, the baking temperature of the constant temperature drying equipment in step three is 60℃-80℃, and the baking time is 20-40 minutes.

[0017] Preferably, in step four, the thickness of the UV protective adhesive coating is between 2 and 15 micrometers, the UV curing time is 3 to 15 seconds, and the temperature is between 40 and 50 degrees Celsius.

[0018] Preferably, the physical matte polishing process in step five specifically includes the following steps:

[0019] Step S1: Prepare the grinding material by adding 10-15 parts of modified epoxy resin, 5-8 parts of silicone rubber, 15-20 parts of nano-diamond powder, 6-10 parts of boron nitride powder, 10-15 parts of alumina powder, 2-5 parts of green silicon carbide powder, 3-6 parts of polyurethane elastic microspheres, 2-3 parts of zirconium oxide, 2-3 parts of graphene, 2-3 parts of molybdenum dioxide, 2-3 parts of self-healing microcapsules, 4-5 parts of carbon black or metal oxide, 2-3 parts of phosphate buffer solution, 0.5-1.5 parts of polyacrylic acid polymer, 1-3 parts of polyethylene wax, and 0.5-1.5 parts of antistatic agent to the grinding equipment in sequence and stirring evenly to obtain the grinding material.

[0020] Step S2: Select several camera light shields and place them in several grinding devices. The grinding devices are equipped with the grinding material from step S1. The grinding time of the several grinding machines is set between 20 min and 60 min, and the rotation speed is between 300 rpm and 1000 rpm.

[0021] Step S3: Test the camera light shields in several grinding devices in Step 2. If the camera light shield in a certain grinding device meets the test requirements, then select that grinding machine as the target grinding machine, and the parameters of that grinding machine are the target parameters.

[0022] Step S4: Place the semi-finished camera light shield into the target grinding machine and use the target parameters to remove the gloss from the semi-finished camera light shield to prepare the finished camera light shield.

[0023] Preferably, in step S3, if multiple semi-finished camera light shields processed by multiple grinding machines meet the detection requirements, the working parameters of the grinding machine with the shortest working time are selected as the target parameters.

[0024] Preferably, in step six, while manually checking and confirming the camera light shield, an infrared spectrometer is also used to randomly check the reflectivity parameters of the camera light shield product to confirm that it meets the process standards and that there are no abnormal parameters.

[0025] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0026] 1. This invention provides a method for eliminating light from a camera lens hood, which includes the following steps: Step 1: stamping and forming the camera lens hood product; Step 2: chemical matting treatment; Step 3: cleaning and drying; Step 4: applying a UV adhesive protective layer; Step 5: physical matting polishing treatment; Step 6: finished product self-inspection and transfer to the next process. The entire process is simple and reasonably designed. This invention improves the optical characteristics of the camera lens hood through chemical and physical polishing to eliminate light, thereby helping to improve the functional performance of the final product, increase the product yield, and is suitable for optical applications with strict requirements. It reduces the reflectivity of the lens hood and avoids the problem of stray light in actual lens shooting.

[0027] 2. By adding a chemical matting step, this invention can make the matting layer structure of the camera light shield more dense and uniform, the surface haze parameters controllable, and perfectly adapt to subsequent composite processing steps. It effectively solves the industry pain points of traditional chemical matting processes, such as easy damage to the substrate, unstable matting effect, and poor adhesion of subsequent composite bonding, forming a composite process technology feature that is different from existing single matting patents. Attached Figure Description

[0028] Figure 1 This is a process flow diagram of the present invention. Detailed Implementation

[0029] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0030] In the description of the embodiments of the present invention, it should be understood that the terms "length," "width," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," and "outer," etc., indicating orientation or positional relationships, are based on the orientation or positional relationships shown in the accompanying drawings and are only for the convenience of describing the embodiments of the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of the present invention. Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined with "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of the embodiments of the present invention, "a plurality of" means two or more, unless otherwise explicitly specified.

[0031] In the embodiments of the present invention, unless otherwise explicitly specified and limited, the terms "installation," "connection," "linking," "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components. Those skilled in the art can understand the specific meaning of the above terms in the embodiments of the present invention according to the specific circumstances.

[0032] Please see Figure 1 The present invention provides an embodiment of a method for eliminating light from a camera light-blocking plate, the method comprising the following steps:

[0033] Step 1: Stamping and forming of camera light shield product. Select a camera light shield substrate, clean and pre-treat the surface of the camera light shield substrate, and use precision molds and punching equipment to punch and cut the camera light shield substrate to form a predetermined diameter shape, inner hole and cutting edge structure to obtain a qualified stamped camera light shield.

[0034] Step Two: Chemical Matting Treatment. Pour the matting solution into the soaking fixture, then place the stamped, qualified camera light shield into the fixture, ensuring it is completely submerged. The temperature of the matting solution is controlled between 30℃ and 60℃, and the soaking time is between 30 minutes and 150 minutes. Stir the stamped, qualified camera light shield every 10 minutes to ensure the PET material on the cutting edge of the stamped camera light shield is completely corroded and softened by the matting solution. The matting solution is prepared using a low-temperature stepwise mixing process. The specific preparation method follows the following weight ratio and process limitations: 10-30 parts by weight of alkaline corrosive agent, 1-10 parts by weight of functional matting filler, and 80-100 parts by weight of high-purity deionized water. The resistivity of the deionized water is not less than 18.25 MΩ·cm. Removing impurities in the water affects the stability of the matting solution and the uniformity of corrosion of the camera light shield. The chemical solution is prepared in a closed, alkali-resistant, corrosion-resistant, stirred reaction vessel. First, the reaction vessel is cleaned and dried to avoid residual impurities and water stains contaminating the chemical solution system. The temperature inside the reaction vessel is controlled below 70°C to avoid the problems of polymerization, gelation, and agglomeration of strong alkali and silicon-based and aluminum-based fillers under high-temperature conditions, ensuring the stability of the chemical solution system components. Then, all the metered high-purity deionized water is injected into the reaction vessel, and a low-speed stirring device is turned on to maintain a uniform stirring state. Then, the alkaline corrosive agent is slowly added in batches. After the alkaline corrosive agent is completely dissolved and the temperature of the aqueous solution system is stable, the functional matting filler is added in batches. After all materials are added, the mixture is stirred at a constant temperature and uniform speed for 3-5 minutes until the materials in the vessel are completely dispersed and uniform, and there are no visible particles, stratification, sedimentation, or agglomeration in the system, forming a homogeneous and stable composite matting corrosion solution. After preparation, the solution is sealed and allowed to stand.

[0035] Step 3: Cleaning and drying. Take out the camera light shield after soaking and matting in Step 2, and use a multi-stage rinsing method with clean water to thoroughly remove any residual chemical components from the surface, inner holes, and crevices of the camera light shield. After draining the water from the cleaned camera light shield, put it into a constant temperature drying device for drying treatment to completely evaporate the moisture on the surface and in the crevices of the camera light shield, ensuring that the camera light shield is completely dry, without water stains or moisture. After drying, let it cool naturally to room temperature.

[0036] Step 4: UV adhesive protective layer coating. Apply UV protective adhesive evenly to the entire surface of the camera light shield after cooling and drying, ensuring that the adhesive layer is of uniform thickness, without any missed areas, adhesive accumulation, or bubbles, and completely covering the carbon black layer on the surface of the camera light shield. After coating, cure the adhesive using a UV curing device to quickly form a dense and stable protective film that adheres to the surface of the camera light shield product.

[0037] Step 5: Physical matte polishing treatment. The original glossy surface of the inner holes and blade edges of the camera lens hood from Step 4 is uniformly polished to make the glossy mirror surface uniformly matte black, achieving the matte finish requirements for product appearance and optical performance. At the same time, the UV adhesive protective coating on the surface of the camera lens hood is precisely removed by polishing. The force and precision are controlled during the polishing process to completely remove the UV adhesive without damaging the product substrate and internal carbon black layer, ensuring that the product surface texture is uniform and the optical performance meets the standards.

[0038] Step Six: Finished Product Self-Inspection and Transfer. Manual inspection confirms that the camera light shield products have no shiny surfaces, burrs, or scratches on the blades and inner holes, and are uniformly matte black overall. There is no UV glue residue, no carbon layer peeling, and no discoloration defects on the surface. Qualified camera light shield products are sorted and classified and transferred to the next processing stage. Defective products are individually marked, reworked, or scrapped.

[0039] Specifically, in step one, it is necessary to ensure that the blade structure is flat, burr-free, and deformation-free. The camera light shield substrate is a low-reflectivity camera light shield substrate. During the cleaning and pretreatment of the camera light shield substrate surface, an optical microscope with image analysis software is used to observe and measure the particle size on the camera light shield substrate surface. The camera light shield substrate surface is cleaned and degreased using ultrasonic cleaning equipment. The particle density of the camera light shield substrate surface is ≤6g / cm³, and the individual particle size value on the camera light shield substrate surface is between 3-15 micrometers.

[0040] Specifically, in step two, the alkaline corrosive agent is an aqueous solution of sodium hydroxide or potassium hydroxide. The alkaline corrosive agent can specifically corrode the surface polymer resin structure of the camera light shield, so that a uniform and dense micro-porous structure is formed on the flat surface of the camera light shield, breaking the mirror gloss of the substrate surface and achieving a basic chemical matting effect. At the same time, the controllable alkaline corrosion system can precisely control the corrosion depth of the camera light shield surface, avoiding excessive corrosion that could cause substrate damage and excessive thickness reduction.

[0041] Specifically, in step two, the functional matting filler is selected from any one or more of fumed silica, silica sol, and ultrafine alumina powder in combination. This functional matting filler can uniformly fill the microporous structure on the surface of the camera light shield formed by alkaline etching. On the one hand, it further refines the surface micro-roughness, improves the uniformity of matting of the camera light shield, and eliminates defects such as local bright spots and uneven gloss. On the other hand, it can buffer the continuous and in-depth corrosion of the camera light shield substrate by strong alkali, and play a role in corrosion control and substrate protection.

[0042] Specifically, in step three, the temperature of the constant temperature drying equipment is 60℃-80℃, and the baking time is 20-40 minutes.

[0043] Specifically, in step four, the thickness of the UV protective adhesive coating is between 2 and 15 micrometers, and the curing time of the UV curing equipment is between 3 and 15 seconds, with the temperature between 40 and 50 degrees Celsius.

[0044] Specifically, the physical matte polishing process in step five includes the following steps:

[0045] Step S1: Prepare the grinding material by adding 10-15 parts of modified epoxy resin, 5-8 parts of silicone rubber, 15-20 parts of nano-diamond powder, 6-10 parts of boron nitride powder, 10-15 parts of alumina powder, 2-5 parts of green silicon carbide powder, 3-6 parts of polyurethane elastic microspheres, 2-3 parts of zirconium oxide, 2-3 parts of graphene, 2-3 parts of molybdenum dioxide, 2-3 parts of self-healing microcapsules, 4-5 parts of carbon black or metal oxide, 2-3 parts of phosphate buffer solution, 0.5-1.5 parts of polyacrylic acid polymer, 1-3 parts of polyethylene wax, and 0.5-1.5 parts of antistatic agent to the grinding equipment in sequence and stirring evenly to obtain the grinding material.

[0046] Step S2: Select several camera light shields and place them in several grinding devices. The grinding devices are equipped with the grinding material from step S1. The grinding time of the several grinding machines is set between 20 min and 60 min, and the rotation speed is between 300 rpm and 1000 rpm.

[0047] Step S3: Inspect the camera light shields in several grinding equipment in Step 2. If the camera light shield in a certain grinding equipment meets the inspection requirements, then select that grinding machine as the target grinding machine, and the parameters of that grinding machine are the target parameters. If multiple semi-finished camera light shields processed by multiple grinding machines meet the inspection requirements, then select the working parameters of the grinding machine with the shortest working time as the target parameters.

[0048] Step S4: Place the semi-finished camera light shield into the target grinding machine and use the target parameters to remove the gloss from the semi-finished camera light shield to prepare the finished camera light shield.

[0049] Specifically, in step six, while manually checking and confirming the camera light shield, an infrared spectrometer is also used to randomly check the reflectivity parameters of the camera light shield product to confirm that it meets the process standards and that there are no abnormal parameters.

[0050] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No reference numerals in the claims should be construed as limiting the scope of the claims.

Claims

1. A method for light extinction of a camera lens shade, characterized in that: Includes the following steps: Step 1: Stamping and forming of camera light shield product. Select a camera light shield substrate, clean and pre-treat the surface of the camera light shield substrate, and use precision molds and punching equipment to punch and cut the camera light shield substrate to form a predetermined diameter shape, inner hole and cutting edge structure to obtain a qualified stamped camera light shield. Step Two: Chemical Matting Treatment. Pour the matting solution into the soaking fixture, then place the stamped, qualified camera light shield into the fixture, ensuring it is completely submerged. The temperature of the matting solution is controlled between 30℃ and 60℃, and the soaking time is between 30 minutes and 150 minutes. Stir the stamped, qualified camera light shield every 10 minutes to ensure the PET material on the cutting edge of the stamped camera light shield is completely corroded and softened by the matting solution. The matting solution is prepared using a low-temperature stepwise mixing process. The specific preparation method follows the following weight ratio and process limitations: 10-30 parts by weight of alkaline corrosive agent, 1-10 parts by weight of functional matting filler, and 80-100 parts by weight of high-purity deionized water. The resistivity of the deionized water is not less than 18.25 MΩ·cm, and impurities in the water are removed to avoid affecting the matting process. The stability of the matting agent and the corrosion uniformity of the camera's light shield were investigated. The matting agent was prepared in a closed, alkali-resistant, corrosion-resistant, and stirred reaction vessel. First, the reaction vessel was cleaned and dried to avoid residual impurities and water stains contaminating the agent system. The temperature inside the reaction vessel was controlled below 70°C. Then, all the metered high-purity deionized water was injected into the reaction vessel, and a low-speed stirrer was turned on to maintain a uniform stirring state. The alkaline corrosive agent was then slowly added in batches. After the alkaline corrosive agent was completely dissolved and the temperature of the aqueous solution system was stable, the functional matting filler was added in batches. After all materials were added, the mixture was stirred at a constant temperature and speed for 3-5 minutes until the materials in the container were completely and uniformly dispersed. The system showed no visible particles, stratification, sedimentation, or agglomeration, forming a homogeneous and stable composite matting corrosion agent. After preparation, the solution was sealed and allowed to stand. Step 3: Cleaning and drying. Take out the camera light shield after soaking and matting in Step 2, and use a multi-stage rinsing method with clean water to thoroughly remove any residual chemical components from the surface, inner holes, and crevices of the camera light shield. After draining the water from the cleaned camera light shield, put it into a constant temperature drying device for drying treatment to completely evaporate the moisture on the surface and in the crevices of the camera light shield, ensuring that the camera light shield is completely dry, without water stains or moisture. After drying, let it cool naturally to room temperature. Step 4: UV adhesive protective layer coating. Apply UV protective adhesive evenly to the entire surface of the camera light shield after cooling and drying, ensuring that the adhesive layer is of uniform thickness, without any missed areas, adhesive accumulation, or bubbles, and completely covering the carbon black layer on the surface of the camera light shield. After coating, cure the adhesive using a UV curing device to quickly form a dense and stable protective film that adheres to the surface of the camera light shield product. Step 5: Physical matte polishing treatment. The original glossy surface of the inner holes and blade edges of the camera lens hood from Step 4 is uniformly polished to make the glossy mirror surface uniformly matte black, achieving the matte finish requirements for product appearance and optical performance. At the same time, the UV adhesive protective coating on the surface of the camera lens hood is precisely removed by polishing. The force and precision are controlled during the polishing process to completely remove the UV adhesive without damaging the product substrate and internal carbon black layer, ensuring that the product surface texture is uniform and the optical performance meets the standards. Step Six: Finished Product Self-Inspection and Transfer. Manual inspection confirms that the camera light shield products have no shiny surfaces, burrs, or scratches on the blades and inner holes, and are uniformly matte black overall. There is no UV glue residue, no carbon layer peeling, and no discoloration defects on the surface. Qualified camera light shield products are sorted and classified and transferred to the next processing stage. Defective products are individually marked, reworked, or scrapped.

2. The method of claim 1, wherein: In step one, it is necessary to ensure that the blade structure is flat, burr-free, and deformation-free. The camera light shield substrate is a low-reflectivity camera light shield substrate. During the cleaning and pretreatment of the camera light shield substrate surface, an optical microscope with image analysis software is used to observe and measure the particle size on the camera light shield substrate surface. The camera light shield substrate surface is cleaned and degreased using an ultrasonic cleaning device.

3. The method of claim 2, wherein: The particle density on the surface of the camera light shield substrate is ≤6g / cm³, and the size of a single particle on the surface of the camera light shield substrate is between 3 and 15 micrometers.

4. The method of claim 1, wherein: In step two, the alkaline corrosive agent is an aqueous solution of sodium hydroxide or potassium hydroxide. The alkaline corrosive agent can specifically corrode the surface polymer resin structure of the camera light shield, so that a uniform and dense micro-porous structure is formed on the flat surface of the camera light shield, breaking the mirror gloss of the substrate surface and achieving a basic chemical matting effect. At the same time, the controllable alkaline corrosion system can precisely control the corrosion depth of the camera light shield surface, avoiding excessive corrosion that could cause substrate damage and excessive thickness reduction.

5. A method for eliminating light from a camera light-shielding plate according to claim 1, characterized in that: In step two, the functional matting filler is selected from any one or more of fumed silica, silica sol, and ultrafine alumina powder; the functional matting filler can be uniformly filled into the microporous structure of the camera light shield surface formed by alkaline etching.

6. The method for eliminating light from a camera light-shielding plate according to claim 1, characterized in that: In step three, the temperature of the constant temperature drying equipment is 60℃-80℃, and the baking time is 20-40 minutes.

7. A method for eliminating light from a camera light-shielding plate according to claim 1, characterized in that: In step four, the thickness of the UV protective adhesive coating is between 2 and 15 micrometers, and the curing time of the UV curing equipment is between 3 and 15 seconds, with the temperature between 40 and 50 degrees Celsius.

8. A method for eliminating light from a camera light-shielding plate according to claim 1, characterized in that: The physical matte polishing process in step five specifically includes the following steps: Step S1: Prepare the grinding material by adding 10-15 parts of modified epoxy resin, 5-8 parts of silicone rubber, 15-20 parts of nano-diamond powder, 6-10 parts of boron nitride powder, 10-15 parts of alumina powder, 2-5 parts of green silicon carbide powder, 3-6 parts of polyurethane elastic microspheres, 2-3 parts of zirconium oxide, 2-3 parts of graphene, 2-3 parts of molybdenum dioxide, 2-3 parts of self-healing microcapsules, 4-5 parts of carbon black or metal oxide, 2-3 parts of phosphate buffer solution, 0.5-1.5 parts of polyacrylic acid polymer, 1-3 parts of polyethylene wax, and 0.5-1.5 parts of antistatic agent to the grinding equipment in sequence and stirring evenly to obtain the grinding material. Step S2: Select several camera light shields and place them in several grinding devices. The grinding devices are equipped with the grinding material from step S1. The grinding time of the several grinding machines is set between 20 min and 60 min, and the rotation speed is between 300 rpm and 1000 rpm. Step S3: Test the camera light shields in several grinding devices in Step 2. If the camera light shield in a certain grinding device meets the test requirements, then select that grinding machine as the target grinding machine, and the parameters of that grinding machine are the target parameters. Step S4: Place the semi-finished camera light shield into the target grinding machine and use the target parameters to remove the gloss from the semi-finished camera light shield to prepare the finished camera light shield.

9. A method for eliminating light from a camera light-shielding plate according to claim 8, characterized in that: In step S3, if multiple semi-finished camera light shields processed by multiple grinding machines meet the detection requirements, the working parameters of the grinding machine with the shortest working time are selected as the target parameters.

10. A method for eliminating light from a camera light-blocking plate according to claim 1, characterized in that: In step six, while manually inspecting and confirming the camera light shield, an infrared spectrometer is also used to randomly check the reflectivity parameters of the camera light shield product to confirm that it meets the process standards and that there are no abnormal parameters.