A dual-mode thermal and humidity management nanofiber membrane, its preparation method and application
By integrating radiative cooling and photothermal conversion layers through a double-layer nanofiber membrane, the problem of thermal comfort regulation of textiles under complex climates is solved, achieving dynamic thermal comfort regulation and waterproof and breathable performance in different environments, making it suitable for outdoor clothing and building materials.
Patent Information
- Application Number
- CN202611288236.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-24
- Publication Date
- 2026-11-17
AI Technical Summary
Existing textiles have significant shortcomings in integrating thermal and moisture management. Single-function cooling or photothermal textiles cannot meet the thermal comfort regulation requirements in different environments, and their waterproof and breathable properties are insufficient, leading to problems of being too cold or too hot in complex climates.
The nanofiber membrane with a double-layer structure integrates a radiation cooling layer and a photothermal conversion layer. It is prepared by electrospinning technology. The material is passively cooled in high-temperature environments and solar heated in low-temperature environments. It also has the functions of liquid water barrier and water vapor discharge, realizing dynamic thermal comfort regulation.
Without the need for power or active control, it meets the thermal comfort regulation needs of day-night cycles, seasonal changes, and cross-climate regions, while also possessing high waterproof and breathable properties, thus improving the overall applicability of the material for outdoor wear.
Smart Images

Figure SMS_3 
Figure SMS_4 
Figure SMS_5
Abstract
Description
Technical Field
[0001] This invention belongs to the field of functional fiber materials technology, specifically relating to a dual-mode heat and humidity management nanofiber membrane, its preparation method, and its application. Background Technology
[0002] With the increasing severity of global climate anomalies, extreme heat waves, cold waves, and drastic diurnal temperature variations are becoming more frequent, highlighting the growing pressure on human thermal comfort regulation and building energy consumption. Traditional active thermal management systems, such as air conditioning and HVAC equipment, are not only energy-intensive and complex, but also difficult to operate continuously outdoors, in mobile settings, and in environments without power. Personal thermal management textiles, by directly regulating the heat flux at the human-clothing-environment interface, offer significant advantages such as localized regulation, rapid response, and zero energy consumption, making them a key solution to this problem.
[0003] Currently, passive thermal management mainly falls into two technical routes. The first is passive radiative cooling, which achieves high reflectivity in the solar spectrum and high emissivity in the atmospheric window band, releasing heat into outer space without energy loss. The second is photothermal conversion heating, utilizing high solar absorptivity and heat retention effects to convert solar energy into heat energy, meeting the warmth requirements in cold environments. However, the real environment is highly dynamic, and single-function cooling or photothermal textiles face the contradiction of being too cold or too hot: cooling materials exacerbate heat loss in cold seasons, while photothermal materials may cause heatstroke in hot weather. Furthermore, in the practical application of functional textiles, waterproofness and breathability are key factors determining physiological comfort. If the fabric cannot timely expel sweat produced by metabolism, it will not only lead to stuffiness and skin stickiness, but in severe cases, it will also disrupt the microenvironment's thermal balance, inducing health risks. Existing technologies still have significant shortcomings in integrating thermal and moisture management. CN117587577A proposes a fluorine-free waterproof and breathable membrane, which is obtained by electrospinning and heat treatment of materials such as silicone-based polyurethane and polymethyl methacrylate to obtain a fiber membrane with certain water pressure resistance, moisture permeability and mechanical properties. However, this patent is limited to humidity regulation and lacks active control over solar radiation heat and infrared radiation heat. CN117822136A proposes a radiation-cooling fiber membrane and its wet blowing preparation method. Organic polymer materials are mixed with nanoparticles to form a spinning solution, and then blown and stretched into fibers by compressed air through a spray gun to prepare a fiber membrane with passive radiation cooling function. However, this patent is essentially a single radiation cooling material, which may accelerate the loss of human body heat in low temperature, cloudy days or seasonal changes. CN104805598B discloses a method for preparing a dual-mode composite nanofiber membrane. This method achieves certain dual-mode thermal management and directional sweat transport through a SiO2 / PAN cooling hydrophilic layer, an APTES / CNT intermediate conductive bonding layer, and an rGO / TPU heating hydrophobic layer. However, its cooling layer is hydrophilic, while the heating layer lacks sufficient hydrophobicity, making it difficult to meet the requirements of harsh outdoor environments in terms of water pressure resistance and moisture permeability. Furthermore, the process is lengthy. Therefore, there is an urgent need to develop a nanofiber membrane that combines dual-mode thermal regulation functions of radiative cooling and solar heating with excellent waterproof and breathable properties. Summary of the Invention
[0004] The present invention aims to at least solve one of the aforementioned technical problems existing in the prior art. To this end, the present invention provides a dual-mode thermal and humidity management nanofiber membrane, which integrates a radiative cooling layer and a photothermal conversion layer into one through a double-layer structure, enabling the material to simultaneously possess passive cooling in high-temperature environments, solar heating in low-temperature environments, and liquid water barrier and water vapor release functions, thereby improving the material's comprehensive applicability in outdoor wear and complex climatic environments.
[0005] The present invention also provides a method for preparing the dual-mode heat and humidity management nanofiber membrane.
[0006] The present invention also provides an application of the aforementioned dual-mode heat and humidity management nanofiber membrane.
[0007] A first aspect of the present invention provides a dual-mode heat and humidity management nanofiber membrane, comprising a radiative cooling layer and a solar heating layer stacked together; The radiation cooling layer comprises fluorinated polymers and nano-inorganic materials, and has a solar reflectivity of ≥95% in the 0.3μm~2.5μm wavelength band and an infrared emissivity of ≥90% in the 7μm~14μm wavelength band. The solar heating layer comprises fluorinated polymers and photothermal materials, and the solar heating layer has a solar light absorption rate of ≥80% in the 0.3μm~2.5μm wavelength band.
[0008] One of the technical solutions of the present invention concerning dual-mode thermal and humidity management nanofiber membranes has at least the following beneficial effects: This invention integrates a radiation cooling layer and a photothermal conversion layer into the same nanofiber membrane through a double-layer structure, enabling the material to simultaneously possess passive cooling in high-temperature environments, solar heating in low-temperature environments, and liquid water barrier and water vapor discharge functions, thereby improving the material's comprehensive applicability in outdoor wear and complex climatic environments.
[0009] This invention utilizes the different spectral selectivity and heat transfer characteristics on both sides of the nanofiber membrane to switch between radiative cooling and solar heating modes simply by physically flipping the front and back of the fiber membrane. No power supply, sensor or active control device is required, which can meet the dynamic thermal comfort regulation needs under day-night alternation, seasonal changes and cross-climate conditions.
[0010] The nanofiber membrane of the present invention can prevent the penetration of liquid water while allowing water vapor to pass through by relying on the microporous structure of the material itself, thus achieving a balance between waterproof and breathable properties and ensuring wearing comfort.
[0011] In the nanofiber membrane of the present invention, the radiation cooling layer comprises fluorinated polymers and nano-inorganic materials, and has high solar reflectivity and high infrared emissivity; the solar heating layer comprises fluorinated polymers and photothermal materials, and has high solar absorption.
[0012] According to some embodiments of the present invention, the hydrostatic pressure resistance of the nanofiber membrane is 80 kPa to 95 kPa.
[0013] According to some embodiments of the present invention, the hydrostatic pressure resistance of the nanofiber membrane is any value among 80 kPa, 82 kPa, 84 kPa, 85 kPa, 86 kPa, 88 kPa, 90 kPa, 92 kPa, 94 kPa, and 95 kPa, such as 85 kPa, or any range of two such values, such as 85 kPa to 90 kPa.
[0014] According to some embodiments of the present invention, the moisture permeability of the nanofiber membrane is 6.0 kg / m² / d to 7.5 kg / m² / d.
[0015] According to some embodiments of the present invention, the moisture permeability of the nanofiber membrane is any value among 6.0 kg / m² / d, 6.2 kg / m² / d, 6.4 kg / m² / d, 6.5 kg / m² / d, 6.8 kg / m² / d, 7.0 kg / m² / d, 7.2 kg / m² / d, and 7.5 kg / m² / d, such as 6.8 kg / m² / d, or any range formed by both, such as 6.5 kg / m² / d to 7.0 kg / m² / d.
[0016] According to some embodiments of the present invention, the solar reflectivity of the radiation cooling layer in the 0.3μm~2.5μm wavelength band is not less than 95%.
[0017] According to some embodiments of the present invention, the infrared emissivity of the radiation cooling layer in the 7μm~14μm band is not less than 90%.
[0018] According to some embodiments of the present invention, the solar heating layer has a solar light absorption rate of not less than 80% in the 0.3μm~2.5μm wavelength band.
[0019] According to some embodiments of the present invention, the fluorinated polymer is selected from at least one of fluorinated polyimide, polyvinylidene fluoride, fluorinated polyurethane, and polyvinylidene fluoride-hexafluoropropylene copolymer.
[0020] According to some embodiments of the present invention, the nano-inorganic material is selected from at least one of alumina, silicon dioxide and titanium dioxide.
[0021] According to some embodiments of the present invention, the photothermal material is selected from at least one of cesium tungsten bronze, carbon nanotubes, polypyrrole, polyaniline and copper oxide.
[0022] According to some embodiments of the present invention, the radiative cooling layer and the solar heating layer also independently comprise a thermoplastic polymer. The addition of the thermoplastic polymer can improve the mechanical flexibility and interlayer bonding of the fibrous membrane.
[0023] According to some embodiments of the present invention, the thermoplastic polymer is selected from at least one of styrene-ethylene-butene-styrene block copolymer, polyurethane, polycarbonate, polyethersulfone and polyethylene terephthalate.
[0024] The CAS number for the styrene-ethylene-butene-styrene block copolymer is 66070-58-4, and it can be purchased from Shanghai Haiyu Zhonglong Technology Co., Ltd.
[0025] According to some embodiments of the present invention, in the radiation cooling layer, the mass fraction of the fluorinated polymer is 8wt%~20wt%, and the mass fraction of the nano-inorganic material is 5wt%~9wt%.
[0026] According to some embodiments of the present invention, in the radiative cooling layer, the mass fraction of the fluorinated polymer is any value among 8wt%, 10wt%, 12wt%, 14wt%, 15wt%, 16wt%, 18wt%, and 20wt%, such as 12wt%, or any range of both, such as 12wt% to 15wt%.
[0027] According to some embodiments of the present invention, in the radiation cooling layer, the mass fraction of the nano-inorganic material is any value of 5wt%, 6wt%, 7wt%, 8wt%, or 9wt%, such as 8wt%, or any range of two, such as 7wt% to 8wt%.
[0028] According to some embodiments of the present invention, the mass fraction of the thermoplastic polymer in the radiative cooling layer is 1wt% to 5wt%.
[0029] According to some embodiments of the present invention, in the radiative cooling layer, the mass fraction of the thermoplastic polymer is any value of 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, such as 5wt%, or any range of two, such as 3wt% to 5wt%.
[0030] According to some embodiments of the present invention, in the solar heating layer, the mass fraction of the fluorinated polymer is 8wt%~20wt%, and the mass fraction of the photothermal material is 1wt%~3wt%.
[0031] According to some embodiments of the present invention, in the solar heating layer, the mass fraction of the fluorinated polymer is any value among 8wt%, 10wt%, 12wt%, 14wt%, 15wt%, 16wt%, 18wt%, and 20wt%, such as 12wt%, or any range of both, such as 12wt% to 15wt%.
[0032] According to some embodiments of the present invention, in the solar heating layer, the mass fraction of the photothermal material is any value among 1wt%, 1.5wt%, 2wt%, 2.5wt%, and 3wt%, such as 3wt%, or any range formed by both, such as 2wt% to 3wt%.
[0033] According to some embodiments of the present invention, the mass fraction of the thermoplastic polymer in the solar heating layer is 1wt% to 5wt%.
[0034] According to some embodiments of the present invention, the mass fraction of the thermoplastic polymer in the solar heating layer is any value of 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, such as 5wt%, or any range of two, such as 3wt% to 5wt%.
[0035] By controlling the mass fraction of each component, the microstructure, pore structure, and spectral selectivity of the fiber membrane can be optimized.
[0036] A second aspect of the present invention provides a method for preparing the dual-mode thermal and humidity management nanofiber membrane, comprising the following steps: S1: Dissolve the fluorinated polymer, photothermal material and optional thermoplastic polymer in a first organic solvent to prepare a solar heating layer spinning solution; S2: Dissolve fluorinated polymers, nano-inorganic materials and optional thermoplastic polymers in a second organic solvent to prepare a radiation-cooling layer spinning solution; S3: Using the receiving substrate as the receiving base, the solar heating layer spinning solution is spun onto the receiving substrate by electrospinning to obtain a solar heating layer fiber membrane. S4: The radiation cooling layer spinning solution is spun onto the solar heating layer fiber membrane by electrospinning to obtain a composite fiber membrane; S5: Dry the composite fiber membrane to obtain the dual-mode heat and humidity management nanofiber membrane.
[0037] One of the technical solutions regarding the preparation method of this invention has at least the following beneficial effects: The preparation method of this invention uses electrospinning technology, which has the characteristics of small fiber diameter, large specific surface area, easy functional modification, and large-scale production. Compared with traditional thin film preparation technology, it has the advantages of fewer steps, simple operation, and low cost, and can significantly improve production efficiency.
[0038] According to some embodiments of the present invention, the first organic solvent and the second organic solvent are each independently selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide and tetrahydrofuran.
[0039] According to some embodiments of the present invention, the receiving substrate is glossy paper.
[0040] According to some embodiments of the present invention, in step S3, the parameters of the electrospinning include: voltage 25kV~35kV, injection speed 1mL / h~3mL / h, receiving distance 15cm~25cm, temperature 20℃~30℃, and relative humidity 50%~70%.
[0041] According to some embodiments of the present invention, in step S3, the parameters of the electrospinning include: a voltage of any value among 25kV, 26kV, 28kV, 30kV, 32kV, 34kV, and 35kV, such as 30kV, or a range of any two, such as 28kV to 32kV.
[0042] According to some embodiments of the present invention, in step S3, the infusion rate is any value among 1 mL / h, 1.5 mL / h, 2 mL / h, 2.5 mL / h, and 3 mL / h, such as 2 mL / h, or any range formed by both, such as 1.5 mL / h to 2.5 mL / h.
[0043] According to some embodiments of the present invention, in step S3, the receiving distance is any value among 15cm, 18cm, 20cm, 22cm, and 25cm, such as 15cm, or a range of any two, such as 15cm to 20cm.
[0044] According to some embodiments of the present invention, in step S3, the temperature is any value among 20°C, 22°C, 25°C, 28°C, and 30°C, such as 25°C, or a range of any two, such as 23°C to 27°C.
[0045] According to some embodiments of the present invention, in step S3, the relative humidity is any value among 50%, 55%, 60%, 65%, and 70%, such as 50% to 60%, or a range of any two, such as 55% to 65%.
[0046] According to some embodiments of the present invention, in step S4, the parameters of the electrospinning include: voltage 25kV~35kV, injection speed 1mL / h~3mL / h, receiving distance 15cm~25cm, temperature 20℃~30℃, and relative humidity 50%~70%.
[0047] According to some embodiments of the present invention, in step S4, the parameters of the electrospinning include: a voltage of any value among 25kV, 26kV, 28kV, 30kV, 32kV, 34kV, and 35kV, such as 30kV, or a range of any two, such as 28kV to 32kV.
[0048] According to some embodiments of the present invention, in step S4, the infusion rate is any value among 1 mL / h, 1.5 mL / h, 2 mL / h, 2.5 mL / h, and 3 mL / h, such as 2 mL / h, or a range formed by any two, such as 1.5 mL / h to 2.5 mL / h.
[0049] According to some embodiments of the present invention, in step S4, the receiving distance is any value among 15cm, 18cm, 20cm, 22cm, and 25cm, such as 15cm, or a range of any two, such as 15cm to 20cm.
[0050] According to some embodiments of the present invention, in step S4, the temperature is any value among 20°C, 22°C, 25°C, 28°C, and 30°C, such as 25°C, or a range of any two, such as 23°C to 27°C.
[0051] According to some embodiments of the present invention, in step S4, the relative humidity is any value of 50%, 55%, 60%, 65%, or 70%, such as 50% to 60%, or a range of any two, such as 55% to 65%.
[0052] According to some embodiments of the present invention, in step S5, the drying temperature is 80℃~100℃ and the drying time is 1h~3h.
[0053] According to some embodiments of the present invention, in step S5, the drying temperature is any value among 80°C, 85°C, 90°C, 95°C, and 100°C, such as 90°C, or a range of any two, such as 85°C to 95°C.
[0054] According to some embodiments of the present invention, in step S5, the drying time is any value among 1h, 1.5h, 2h, 2.5h, and 3h, such as 2h, or a range of any two, such as 1.5h to 2.5h.
[0055] A third aspect of the invention provides the application of the dual-mode thermal and moisture management nanofiber membrane in the preparation of personal thermal management clothing, outdoor protective clothing, or building energy-saving materials.
[0056] One of the technical solutions of this invention regarding its application has at least the following beneficial effects: The dual-mode thermal and humidity management nanofiber membrane of this invention can be applied to the manufacture of outdoor protective clothing such as mountaineering suits, combat uniforms, and cycling suits. Through physical rotation, it achieves passive cooling at high temperatures and photothermal insulation at low temperatures, providing wearers with continuous and stable protection and thermal and humidity comfort under different seasons, diurnal variations, and complex climatic conditions. Simultaneously, this nanofiber membrane can also be used in the field of building energy-saving materials, as a smart window or exterior wall film, to achieve passive thermal regulation of building envelopes. Detailed Implementation
[0057] The following will describe the concept and technical effects of the present invention clearly and completely with reference to embodiments, so as to fully understand the purpose, features and effects of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are all within the scope of protection of the present invention.
[0058] In the description of this invention, the terms "one embodiment," "some embodiments," "illustrative embodiment," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0059] Unless otherwise specified, "room temperature" in this invention means 25℃±5℃.
[0060] Unless otherwise specified, "about" in this invention means that the allowable error is within ±2%.
[0061] Unless otherwise specified in the examples, the procedures should be performed under standard conditions or conditions recommended by the manufacturer. Reagents or instruments whose manufacturers are not specified are all commercially available products.
[0062] Fluorinated polyimide, CAS number 60842-76-4, was purchased from Fluorochemical Technology (Xiamen) New Materials Co., Ltd.
[0063] Polyvinylidene fluoride, CAS number 24937-79-9, was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0064] The polyvinylidene fluoride-hexafluoropropylene copolymer, CAS No. 9011-17-0, was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0065] Styrene-ethylene-butene-styrene block copolymer, CAS No. 66070-58-4, was purchased from Shanghai Haiyu Zhonglong Technology Co., Ltd.
[0066] Cesium tungsten bronze, CAS number 189619-69-0, was purchased from Shanghai Buwei Applied Materials Technology Co., Ltd.
[0067] Example 1 A dual-mode thermal and humidity management nanofiber membrane was prepared, and the steps were as follows: S1 is prepared by dissolving 12 wt% fluorinated polyimide, 5 wt% styrene-ethylene-butene-styrene block copolymer, and 3 wt% cesium tungsten bronze in N,N-dimethylformamide and stirring it evenly for 6-10 hours until it is uniform.
[0068] S2 is prepared by dissolving 12 wt% fluorinated polyimide, 5 wt% styrene-ethylene-butene-styrene block copolymer and 8 wt% alumina in N,N-dimethylformamide and stirring it evenly for 6-10 hours until it is uniform.
[0069] After the spinning solution in step S3 is completely dissolved, electrospinning is performed: a 60cm×60cm piece of glossy paper is cut as the receiving substrate for electrospinning. The heating layer spinning solution prepared in step one is used to prepare a heating layer nanofiber membrane by electrospinning technology. The spinning voltage is 30kV, the receiving distance is 15cm, the infusion rate is 2mL / h, the temperature is 25℃, and the relative humidity is 50%~60%.
[0070] S4 involves electrospinning the cooling layer spinning solution onto varnished paper on the heating layer fiber membrane. The spinning voltage is 30kV, the receiving distance is 15cm, the infusion rate is 2mL / h, the temperature is 25℃, and the relative humidity is 50%~60%.
[0071] S5 The prepared nanofiber membrane was removed and placed in a 90℃ drying oven for 2 hours to remove residual solvent, thus obtaining a dual-mode thermal and humidity management nanofiber membrane with a water pressure resistance of 85.2 kPa, a moisture permeability of 6.81 kg / m2 / d, a solar reflectance of 96.3% for the cooling layer, an infrared emissivity of 91.3%, a cooling temperature of 13.0℃, a solar absorptivity of 85.5% for the heating layer, and a heating temperature of 13.5℃.
[0072] Example 2 A dual-mode thermal and humidity management nanofiber membrane was prepared, and the steps were as follows: S1 is prepared by dissolving 14 wt% polyvinylidene fluoride, 5 wt% styrene-ethylene-butene-styrene block copolymer and 3 wt% cesium tungsten bronze in N,N-dimethylformamide and stirring it evenly for 6-10 hours until it is uniform.
[0073] S2 is prepared by dissolving 14 wt% polyvinylidene fluoride, 5 wt% styrene-ethylene-butene-styrene block copolymer and 8 wt% alumina in N,N-dimethylformamide and stirring it evenly for 6-10 hours until it is uniform.
[0074] After the spinning solution in step S3 is completely dissolved, electrospinning is performed: a 60cm×60cm piece of glossy paper is cut as the receiving substrate for electrospinning. The heating layer spinning solution prepared in step one is used to prepare a heating layer nanofiber membrane by electrospinning technology. The spinning voltage is 30kV, the receiving distance is 15cm, the infusion rate is 2mL / h, the temperature is 25℃, and the relative humidity is 50%~60%.
[0075] S4 involves electrospinning the cooling layer spinning solution onto varnished paper on the heating layer fiber membrane. The spinning voltage is 30kV, the receiving distance is 15cm, the infusion rate is 2mL / h, the temperature is 25℃, and the relative humidity is 50%~60%.
[0076] S5 The prepared nanofiber membrane was removed and placed in a 90℃ drying oven for 2 hours to remove residual solvent, thus obtaining a dual-mode thermal and humidity management nanofiber membrane with a water pressure resistance of 88.8 kPa, a moisture permeability of 6.65 kg / m2 / d, a solar reflectance of 96.6% for the cooling layer, an infrared emissivity of 92.0%, a cooling temperature of 13.2℃, a solar absorptivity of 85.6% for the heating layer, and a heating temperature of 13.4℃.
[0077] Example 3 A dual-mode thermal and humidity management nanofiber membrane was prepared, and the steps were as follows: S1 is prepared by dissolving 18 wt% polyvinylidene fluoride-hexafluoropropylene copolymer, 5 wt% styrene-ethylene-butene-styrene block copolymer, and 3 wt% cesium tungsten bronze in N,N-dimethylformamide and stirring it evenly for 6-10 hours until it is homogeneous.
[0078] S2 is prepared by dissolving 18 wt% polyvinylidene fluoride-hexafluoropropylene copolymer, 5 wt% styrene-ethylene-butene-styrene block copolymer, and 8 wt% alumina in N,N-dimethylformamide and stirring the solution evenly for 6-10 hours until homogeneous.
[0079] After the spinning solution in step S3 is completely dissolved, electrospinning is performed: a 60cm×60cm piece of glossy paper is cut as the receiving substrate for electrospinning. The heating layer spinning solution prepared in step one is used to prepare a heating layer nanofiber membrane by electrospinning technology. The spinning voltage is 30kV, the receiving distance is 15cm, the infusion rate is 2mL / h, the temperature is 25℃, and the relative humidity is 50%~60%.
[0080] S4 involves electrospinning the cooling layer spinning solution onto varnished paper on the heating layer fiber membrane. The spinning voltage is 30kV, the receiving distance is 15cm, the infusion rate is 2mL / h, the temperature is 25℃, and the relative humidity is 50%~60%.
[0081] S5 The prepared nanofiber membrane was removed and placed in a 90℃ drying oven for 2 hours to remove residual solvent, thus obtaining a dual-mode thermal and humidity management nanofiber membrane with a water pressure resistance of 90.2 kPa, a moisture permeability of 6.43 kg / m2 / d, a solar reflectance of 96.9% for the cooling layer, an infrared emissivity of 91.8%, a cooling temperature of 13.5℃, a solar absorptivity of 85.1% for the heating layer, and a heating temperature of 12.8℃.
[0082] Example 4 A dual-mode thermal and humidity management nanofiber membrane was prepared, and the steps were as follows: S1 is prepared by dissolving 12 wt% fluorinated polyimide, 5 wt% styrene-ethylene-butene-styrene block copolymer, and 3 wt% cesium tungsten bronze in N,N-dimethylformamide and stirring it evenly for 6-10 hours until it is uniform.
[0083] S2 prepares the spinning solution for the cooling layer by dissolving 12 wt% fluorinated polyimide, 5 wt% styrene-ethylene-butene-styrene block copolymer, and 8 wt% silica in N,N-dimethylformamide and stirring it evenly for 6-10 hours until it is homogeneous.
[0084] After the spinning solution in step S3 is completely dissolved, electrospinning is performed: a 60cm×60cm piece of glossy paper is cut as the receiving substrate for electrospinning. The heating layer spinning solution prepared in step one is used to prepare a heating layer nanofiber membrane by electrospinning technology. The spinning voltage is 30kV, the receiving distance is 15cm, the infusion rate is 2mL / h, the temperature is 25℃, and the relative humidity is 50%~60%.
[0085] S4 involves electrospinning the cooling layer spinning solution onto varnished paper on the heating layer fiber membrane. The spinning voltage is 30kV, the receiving distance is 15cm, the infusion rate is 2mL / h, the temperature is 25℃, and the relative humidity is 50%~60%.
[0086] S5 The prepared nanofiber membrane was removed and placed in a 90℃ drying oven for 2 hours to remove residual solvent, thus obtaining a dual-mode thermal and humidity management nanofiber membrane with a water pressure resistance of 85.4 kPa, a moisture permeability of 6.76 kg / m2 / d, a solar reflectance of 96.7% for the cooling layer, an infrared emissivity of 91.2%, a cooling temperature of 13.1℃, a solar absorptivity of 85.2% for the heating layer, and a heating temperature of 12.8℃.
[0087] Example 5 A dual-mode thermal and humidity management nanofiber membrane was prepared, and the steps were as follows: S1 is prepared by dissolving 12 wt% fluorinated polyimide, 5 wt% styrene-ethylene-butene-styrene block copolymer, and 3 wt% cesium tungsten bronze in N,N-dimethylformamide and stirring it evenly for 6-10 hours until it is uniform.
[0088] S2 prepares the spinning solution for the cooling layer by dissolving 12 wt% fluorinated polyimide, 5 wt% styrene-ethylene-butene-styrene block copolymer, and 8 wt% titanium dioxide in N,N-dimethylformamide and stirring it evenly for 6-10 hours until it is uniform.
[0089] After the spinning solution in step S3 is completely dissolved, electrospinning is performed: a 60cm×60cm piece of glossy paper is cut as the receiving substrate for electrospinning. The heating layer spinning solution prepared in step one is used to prepare a heating layer nanofiber membrane by electrospinning technology. The spinning voltage is 30kV, the receiving distance is 15cm, the infusion rate is 2mL / h, the temperature is 25℃, and the relative humidity is 50%~60%.
[0090] S4 involves electrospinning the cooling layer spinning solution onto varnished paper on the heating layer fiber membrane. The spinning voltage is 30kV, the receiving distance is 15cm, the infusion rate is 2mL / h, the temperature is 25℃, and the relative humidity is 50%~60%.
[0091] S5 The prepared nanofiber membrane was removed and placed in a 90℃ drying oven for 2 hours to remove residual solvent, thus obtaining a dual-mode thermal and humidity management nanofiber membrane with a water pressure resistance of 84.9 kPa, a moisture permeability of 6.98 kg / m2 / d, a solar reflectance of 97.1% for the cooling layer, an infrared emissivity of 91.4%, a cooling temperature of 13.5℃, a solar absorptivity of 84.8% for the heating layer, and a heating temperature of 12.2℃.
[0092] Example 6 A dual-mode thermal and humidity management nanofiber membrane was prepared, and the steps were as follows: S1 is prepared by dissolving 12 wt% fluorinated polyimide, 5 wt% styrene-ethylene-butene-styrene block copolymer and 3 wt% carbon nanotubes in N,N-dimethylformamide and stirring it evenly for 6-10 hours until it is uniform.
[0093] S2 is prepared by dissolving 12 wt% fluorinated polyimide, 5 wt% styrene-ethylene-butene-styrene block copolymer and 8 wt% alumina in N,N-dimethylformamide and stirring it evenly for 6-10 hours until it is uniform.
[0094] After the spinning solution in step S3 is completely dissolved, electrospinning is performed: a 60cm×60cm piece of glossy paper is cut as the receiving substrate for electrospinning. The heating layer spinning solution prepared in step one is used to prepare a heating layer nanofiber membrane by electrospinning technology. The spinning voltage is 30kV, the receiving distance is 15cm, the infusion rate is 2mL / h, the temperature is 25℃, and the relative humidity is 50%~60%.
[0095] S4 involves electrospinning the cooling layer spinning solution onto varnished paper on the heating layer fiber membrane. The spinning voltage is 30kV, the receiving distance is 15cm, the infusion rate is 2mL / h, the temperature is 25℃, and the relative humidity is 50%~60%.
[0096] S5 The prepared nanofiber membrane was removed and placed in a 90℃ drying oven for 2 hours to remove residual solvent, thus obtaining a dual-mode thermal and humidity management nanofiber membrane with a water pressure resistance of 85.8 kPa, a moisture permeability of 6.63 kg / m2 / d, a solar reflectance of 97.2% for the cooling layer, an infrared emissivity of 91.6%, a cooling temperature of 13.8℃, a solar absorptivity of 86.9% for the heating layer, and a heating temperature of 13.8℃.
[0097] Example 7 A dual-mode thermal and humidity management nanofiber membrane was prepared, and the steps were as follows: S1 prepares the spinning solution for the heating layer by dissolving 12 wt% fluorinated polyimide, 5 wt% polyurethane, and 3 wt% carbon nanotubes in N,N-dimethylformamide and stirring it evenly for 6-10 hours until it is homogeneous.
[0098] S2 prepares the spinning solution for the cooling layer by dissolving 12 wt% fluorinated polyimide, 5 wt% polyurethane, and 8 wt% alumina in N,N-dimethylformamide and stirring it evenly for 6-10 hours until it is homogeneous.
[0099] After the spinning solution in step S3 is completely dissolved, electrospinning is performed: a 60cm×60cm piece of glossy paper is cut as the receiving substrate for electrospinning. The heating layer spinning solution prepared in step one is used to prepare a heating layer nanofiber membrane by electrospinning technology. The spinning voltage is 30kV, the receiving distance is 15cm, the infusion rate is 2mL / h, the temperature is 25℃, and the relative humidity is 50%~60%.
[0100] S4 involves electrospinning the cooling layer spinning solution onto varnished paper on the heating layer fiber membrane. The spinning voltage is 30kV, the receiving distance is 15cm, the infusion rate is 2mL / h, the temperature is 25℃, and the relative humidity is 50%~60%.
[0101] S5 The prepared nanofiber membrane was removed and placed in a 90℃ drying oven for 2 hours to remove residual solvent, thus obtaining a dual-mode thermal and humidity management nanofiber membrane with a water pressure resistance of 86.2 kPa, a moisture permeability of 6.17 kg / m2 / d, a solar reflectance of 97.3% for the cooling layer, an infrared emissivity of 91.3%, a cooling temperature of 13.9℃, a solar absorptivity of 86.5% for the heating layer, and a heating temperature of 13.6℃.
[0102] Example 8 A dual-mode thermal and humidity management nanofiber membrane was prepared, and the steps were as follows: S1 is prepared by dissolving 12 wt% fluorinated polyimide, 5 wt% polyethylene terephthalate, and 3 wt% carbon nanotubes in N,N-dimethylformamide and stirring the solution evenly for 6-10 hours until homogeneous.
[0103] S2 prepares the spinning solution for the cooling layer by dissolving 12 wt% fluorinated polyimide, 5 wt% polyethylene terephthalate, and 8 wt% alumina in N,N-dimethylformamide and stirring it evenly for 6-10 hours until it is homogeneous.
[0104] After the spinning solution in step S3 is completely dissolved, electrospinning is performed: a 60cm×60cm piece of glossy paper is cut as the receiving substrate for electrospinning. The heating layer spinning solution prepared in step one is used to prepare a heating layer nanofiber membrane by electrospinning technology. The spinning voltage is 30kV, the receiving distance is 15cm, the infusion rate is 2mL / h, the temperature is 25℃, and the relative humidity is 50%~60%.
[0105] S4 involves electrospinning the cooling layer spinning solution onto varnished paper on the heating layer fiber membrane. The spinning voltage is 30kV, the receiving distance is 15cm, the infusion rate is 2mL / h, the temperature is 25℃, and the relative humidity is 50%~60%.
[0106] S5 The prepared nanofiber membrane was removed and placed in a 90℃ drying oven for 2 hours to remove residual solvent, thus obtaining a dual-mode thermal and humidity management nanofiber membrane with a water pressure resistance of 86.1 kPa, a moisture permeability of 6.28 kg / m2 / d, a solar reflectance of 97.0% for the cooling layer, an infrared emissivity of 91.4%, a cooling temperature of 13.6℃, a solar absorptivity of 86.8% for the heating layer, and a heating temperature of 13.5℃.
[0107] Performance testing The nanofiber membranes prepared in Examples 1-8 were subjected to performance tests, wherein: Hydrostatic pressure is an important indicator for evaluating the waterproof performance of fabrics, used to characterize the resistance encountered by liquid water when it permeates the fabric. This test is conducted according to GB / T4744-1997 standard: Three 18cm × 18cm square specimens are cut from the fiber membrane sample, placed in the disc position of the hydrostatic pressure tester, and covered with black fabric, with the pressure ring tightened to secure them. The test is started after setting the pressure increase rate to 6000 Pa / min. The test is stopped and the value is recorded when the third water droplet appears on the surface of the black fabric. Each sample is tested three times, and the average value is taken as the hydrostatic pressure resistance value of the fiber membrane.
[0108] Moisture permeation flux test procedure: First, pour approximately 30 mL of deionized water into the permeation cup. Cut the sample fiber membrane to the same size as the permeation cup, place the fiber membrane on the permeation cup, and secure it with rubber rings and washers, and nuts. After securing, set the instrument parameters: humidity 50%, constant temperature 38℃, and airflow speed 0.44 m / s. When the humidity and temperature in the constant temperature chamber reach the required levels, place the permeation cup inside and allow it to equilibrate in the constant temperature chamber for 1 hour. Quickly weigh the permeation cup and record the weight as m1. Then immediately place it in the testing instrument for 1 hour of experimentation, and weigh the permeation cup again, recording the weight as m2.
[0109] Finally, based on the moisture permeability flux formula WVT=24Δm / (St), the moisture permeability flux of each fiber membrane is calculated (WVT in the formula represents the moisture permeability flux per square meter per day, kg / m²). 2 / d;S(m) 2 The area of the fiber membrane during the test is 0.00283m². 2 Δm(g) represents the mass difference of the same fiber membrane, and t(h) represents the testing time of the fiber membrane.
[0110] UV-Vis-NIR (ultraviolet-visible-near-infrared) reflectance and absorptivity testing is used to characterize the light reflection and absorption capabilities of materials within a specific wavelength range. Before testing, the sample to be tested is cut to a suitable size with the cooling layer facing upwards, ensuring its surface is clean and flat. The UV-Vis-NIR reflectance meter is then started for preheating and calibration. Relevant parameters are set according to testing requirements, including a wavelength range of 0.3 μm-2.5 μm and a corresponding solar spectral power density range of 0 W / m². -2 / nm -1 -2W / m -2 / nm -1 After placing the sample in the instrument's testing position, reflectivity is measured according to the set parameters, and the spectral curve of reflectivity versus wavelength is recorded. For solar absorptivity, the testing surface is changed from having the cooling layer facing upwards to having the photothermal layer facing upwards, for subsequent analysis of the material's solar absorption performance.
[0111] The infrared emissivity of the samples was measured using a Fourier transform infrared spectrometer. Before testing, the instrument was powered on and preheated to ensure stable operation. The sample was then placed flat on the sampling system, and its position was adjusted to ensure proper alignment with the test optical path, guaranteeing accurate signal acquisition. The data acquisition and processing system was started, the spectral acquisition interface was accessed, and test parameters were set, including the wavelength range of 7μm-14μm. After parameter settings were completed, spectral data acquisition began, and the emissivity results of the samples in the corresponding infrared bands were obtained through system processing.
[0112] Solar absorptivity of the heating layer: The reflectivity (R) and transmittance (T) of the fiber membrane in the wavelength range of 0.3μm-2.5μm were measured using a UV-Vis-NIR Spectro photometer equipped with an integrating sphere attachment. Based on the law of conservation of energy, the absorptivity (A) at each wavelength was calculated as A(λ) = 1. R(λ) T(λ) is used to obtain the average solar absorptivity (α) of the sample across the entire solar spectrum. All samples were measured at room temperature and repeated at least three times to ensure data accuracy and repeatability.
[0113] Cooling / Heating Temperature Test: 5cm × 5cm nanofiber membranes and cotton fabrics were cut, with the cotton fabric serving as a control group. Each sample was flattened and placed on the surface of a human arm. Under the same environmental conditions, the surface temperature of the different fabric-covered areas was measured using an infrared thermal imager, and the temperature difference between the nanofiber membrane and the control sample was recorded to evaluate its radiative cooling or solar heating performance.
[0114] The test results are shown in Tables 1 to 4.
[0115] Table 1 Hydrostatic pressure resistance and moisture permeability of nanofiber membranes
[0116] Table 1 summarizes the hydrostatic pressure resistance and moisture permeability test results of the nanofiber membranes prepared in Examples 1 to 8. The data in the table show that the hydrostatic pressure resistance of each example ranges from 84.9 kPa to 90.2 kPa, with Example 3 exhibiting the highest hydrostatic pressure resistance at 90.2 kPa. The moisture permeability ranges from 6.17 kg / m² / d to 6.98 kg / m² / d, with Example 5 showing the highest moisture permeability at 6.98 kg / m² / d. This indicates that the nanofiber membranes prepared in each example of the present invention possess high hydrostatic pressure resistance and good moisture permeability.
[0117] The above results show that the nanofiber membrane constructed by electrospinning technology in this invention has excellent waterproof and breathable balance capabilities, effectively blocking liquid water intrusion while allowing water vapor to pass through, thus meeting the stringent requirements of outdoor protective clothing for waterproof and breathable performance.
[0118] Table 2 Solar reflectance and infrared emissivity of nanofiber membranes
[0119] Table 2 summarizes the test results of solar reflectance and infrared emissivity of the nanofiber membrane radiation cooling layers prepared in Examples 1 to 8. The data in the table show that the solar reflectance of each example is between 96.3% and 97.3%, with Example 7 having the highest at 97.3%; the infrared emissivity is between 91.2% and 92.0%, with Example 2 having the highest at 92.0%. This indicates that the radiation cooling layers prepared in each example of the present invention exhibit excellent spectral selectivity under different combinations of fluorinated polymers and nano-inorganic materials.
[0120] The above results show that the composite structure of fluorinated polymer and nano-inorganic materials in the radiation cooling layer of the present invention can effectively reflect solar radiation and enhance thermal emission in the atmospheric window band, providing a reliable spectral control basis for achieving efficient passive radiation cooling.
[0121] Table 3 Solar light absorption rate of nanofiber membranes
[0122] Table 3 summarizes the solar absorption rate test results of the nanofiber membrane solar heating layers prepared in Examples 1 to 8. The data in the table show that the solar absorption rate of each example is between 84.8% and 86.9%, with Example 6 having the highest at 86.9% and Example 5 having the lowest at 84.8%. This indicates that the solar heating layers prepared in each example of the present invention exhibit high and stable solar absorption capacity under different combinations of fluorinated polymers and photothermal materials.
[0123] The above results show that the photothermal material in the solar heating layer of the present invention is uniformly dispersed in the fluorinated polymer fiber matrix, and the constructed photothermal conversion network can achieve efficient broadband solar light absorption, providing reliable energy capture capability for photothermal conversion heating in low-temperature environments.
[0124] Table 4 Cooling and heating temperatures of nanofiber membranes compared to simulated bare skin
[0125] Table 4 summarizes the cooling and heating temperature test results of the nanofiber membranes prepared in Examples 1 to 8 relative to the cotton fabric control group. The data in the table show that the cooling temperatures of all examples ranged from 13.0 °C to 13.9 °C, with Example 7 achieving the highest temperature of 13.9 °C; the heating temperatures ranged from 12.2 °C to 13.8 °C, with Example 6 achieving the highest temperature of 13.8 °C. This indicates that all embodiments of the present invention can achieve significant temperature control effects in both radiative cooling and solar heating modes.
[0126] The above results demonstrate that by achieving high solar radiation reflection and high infrared emission in the radiative cooling layer and high solar radiation absorption in the solar heating layer, the nanofiber membrane can produce significant cooling or heating effects in both modes. This verifies the feasibility of achieving efficient passive cooling and photothermal insulation through physical flipping of the dual-mode thermal and humidity management nanofiber membrane.
[0127] This invention breaks through the technological barrier of traditional personal thermal management (PTM) materials with their single function, proposing a dual-mode nanofiber membrane system that integrates radiative cooling, photothermal conversion, and waterproofing / breathability. Unlike existing materials that often compromise between spectral control and wearability (waterproofing / breathability), this invention achieves interface decoupling and functional integration of "high reflectivity / high emission" and "efficient photothermal conversion" through structural design. While ensuring thermal balance regulation under extreme environments, it utilizes the surface chemistry and microporous properties of nanofibers to solve the common "stuffy" problem of thermal management materials, achieving a deep synergy between human thermal comfort and physiological moisture comfort.
[0128] Furthermore, this invention establishes a passive adaptive adjustment mechanism based on spectral differential response, endowing materials with survivability under extreme conditions through physical interface flipping. Utilizing the inherent difference in spectral selectivity between the cooling layer (high solar reflectance / high infrared emission) and the heating layer (broad-spectrum solar absorption), instantaneous switching between cooling and heating modes is achieved. This process completely eliminates dependence on sensors, power supplies, and actuators, overcoming the bottlenecks of complex systems, high maintenance costs, and inability to operate outdoors for extended periods in active thermal management devices, providing an efficient solution for achieving zero-energy, all-weather personal thermal management.
[0129] Furthermore, in the construction of the solar heating layer, this invention achieves highly efficient energy capture and retention through the precise design of a micro / nano fiber network. High-performance photothermal materials are uniformly anchored within a fluoropolymer fiber matrix using electrospinning technology, constructing a photothermal conversion network with a high specific surface area and multi-level scattering effects. This composite network not only achieves efficient broadband radiation absorption and in-situ conversion into heat energy through electron / phonon transitions, but also utilizes the static air layer between fibers and the low thermal conductivity matrix to achieve effective heat retention, significantly improving thermal compensation efficiency in low-temperature environments.
[0130] The present invention has been described in detail above with reference to the embodiments. However, the present invention is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present invention.
Claims
1. A dual-mode heat and humidity management nanofiber membrane, characterized in that, It includes a radiative cooling layer and a solar heating layer stacked together; The radiation cooling layer comprises fluorinated polymers and nano-inorganic materials, and has a solar reflectivity of ≥95% in the 0.3μm~2.5μm wavelength band and an infrared emissivity of ≥90% in the 7μm~14μm wavelength band. The solar heating layer comprises fluorinated polymers and photothermal materials, and the solar heating layer has a solar light absorption rate of ≥80% in the 0.3μm~2.5μm wavelength band.
2. The dual-mode thermal and humidity management nanofiber membrane according to claim 1, characterized in that, The nanofiber membrane has a hydrostatic pressure resistance of 80kPa to 95kPa and a moisture permeability of 6.0kg / m² / d to 7.5kg / m² / d.
3. The dual-mode thermal and humidity management nanofiber membrane according to claim 1, characterized in that, The fluorinated polymer is selected from at least one of fluorinated polyimide, polyvinylidene fluoride, fluorinated polyurethane, and polyvinylidene fluoride-hexafluoropropylene copolymer.
4. The dual-mode thermal and humidity management nanofiber membrane according to claim 1, characterized in that, The nano-inorganic material is selected from at least one of alumina, silicon dioxide, and titanium dioxide.
5. The dual-mode thermal and humidity management nanofiber membrane according to claim 1, characterized in that, The photothermal material is selected from at least one of cesium tungsten bronze, carbon nanotubes, polypyrrole, polyaniline, and copper oxide.
6. The dual-mode thermal and humidity management nanofiber membrane according to claim 1, characterized in that, In the radiative cooling layer, the mass fraction of fluorinated polymer is 8wt%~20wt%, and the mass fraction of nano-inorganic material is 5wt%~9wt%; in the solar heating layer, the mass fraction of fluorinated polymer is 8wt%~20wt%, and the mass fraction of photothermal material is 1wt%~3wt%.
7. The dual-mode thermal and humidity management nanofiber membrane according to claim 6, characterized in that, The radiative cooling layer and the solar heating layer also independently contain a thermoplastic polymer, the mass fraction of which is 1wt% to 5wt%.
8. A method for preparing a dual-mode thermal and humidity management nanofiber membrane as described in any one of claims 1 to 7, characterized in that, Includes the following steps: S1: Dissolve the fluorinated polymer, photothermal material and optional thermoplastic polymer in a first organic solvent to prepare a solar heating layer spinning solution; S2: Dissolve fluorinated polymers, nano-inorganic materials and optional thermoplastic polymers in a second organic solvent to prepare a radiation-cooling layer spinning solution; S3: Using the substrate as the receiving substrate, the solar heating layer spinning solution is spun onto the substrate by electrospinning to obtain a solar heating layer fiber membrane; S4: Electrospinning is used to spin the spinning solution of the radiation cooling layer onto the solar heating layer fiber membrane to obtain a composite fiber membrane; S5: Dry the composite fiber membrane to obtain the dual-mode heat and humidity management nanofiber membrane.
9. The method according to claim 8, characterized in that, In steps S3 and S4, the parameters of electrospinning each independently include: voltage 25kV~35kV, injection speed 1mL / h~3mL / h, receiving distance 15cm~25cm, temperature 20℃~30℃, and relative humidity 50%~70%.
10. The application of the dual-mode thermal and moisture management nanofiber membrane according to any one of claims 1 to 7 in the preparation of personal thermal management clothing, outdoor protective clothing or building energy-saving materials.
Citation Information
Patent Citations
A kind of electrospinning method for preparing vinyl polysiloxane nanofiber film
CN104805598B
Fluorine-free efficient waterproof moisture-permeable film and preparation method thereof
CN117587577A
Radiation refrigeration fiber membrane as well as preparation method and application thereof
CN117822136A