High-speed air rudder integrally covered rudder surface heat shield and its integral molding method

By combining fiber preforms and closed-cell foam strain-coordination layers, the problems of localized ablation and molding precision of the air rudder heat shield were solved, achieving a high-stability and long-life overall thermal protection effect.

CN123104968APending Publication Date: 2026-11-17EAST CHINA UNIV OF SCI & TECH +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611618109.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing air rudder heat shields suffer from problems such as localized ablation, poor molding precision, high risk of thermal protection failure, and poor overall thermal protection structural stability.

Method used

An integrated, monolithic covering structure is prepared using fiber preforms. Combined with a closed-cell foam strain coordination layer and gradient density design, the air rudder metal skeleton is wrapped by stitching. A closed-cell foam strain coordination layer is set to buffer the difference in thermal expansion, and a continuous fiber structure and dense stitching area are used in the leading edge area to enhance the ablation resistance.

Benefits of technology

It achieves seamless overall coverage, improves molding accuracy and thermal protection consistency, reduces the risk of local ablation, and enhances the structural stability and service life of the air rudder in high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123104968A_ABST
    Figure CN123104968A_ABST
Patent Text Reader

Abstract

This invention relates to a heat shield sleeve for a high-speed air rudder that is integrally covered with the rudder surface and its integral molding method, belonging to the field of aerospace thermal protection materials technology. It solves at least one of the problems existing in current air rudder heat shield sleeves, including susceptibility to localized ablation, poor molding accuracy, easy thermal protection failure, and poor overall thermal protection structural stability. The fiber preform in the heat shield sleeve is an integral structure, integrally wrapping the air rudder metal skeleton by stitching. A closed-cell foam strain-coating layer is placed between the air rudder metal skeleton and the heat shield sleeve. The covering fiber structure corresponding to the lower end face between the rudder shaft and the air rudder leading edge is a continuous fiber structure. The density of the area corresponding to the thinned region of the heat shield sleeve and the air rudder leading edge is 1.10-1.20 g / cm³. 3 The thickness is 2-3 mm; the area corresponding to the heat shield and the main air rudder area has a gradient density. This heat shield is not prone to localized ablation, has high molding precision, is not prone to thermal protection failure, and has high overall thermal protection structural stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of aerospace thermal protection materials technology, and in particular to a high-speed air rudder integrally covered rudder surface heat protection sleeve and its integral molding method. Background Technology

[0002] During high-speed flight, the air rudder, as a key aerodynamic control component, is subjected to extreme thermal environments of high temperature, high-speed airflow scouring, and strong shearing for a long time. The surface will generate severe aerodynamic heating, which puts forward high requirements for the thermal protection performance, structural stability and dimensional accuracy of the air rudder.

[0003] Existing air rudder heat protection structures mostly adopt a split design, where the main body, rear end face, and leading edge of the rudder surface heat shield are processed separately and then assembled in a secondary process. Existing split air rudder heat protection structures are prone to localized ablation, have poor forming accuracy, a high risk of thermal protection failure, and poor overall thermal protection structure stability. Summary of the Invention

[0004] Based on the above analysis, the present invention aims to provide a high-speed air rudder integrally covered rudder surface heat shield and its integral molding method, in order to solve at least one of the problems of existing air rudder heat shields, such as easy local ablation, poor molding accuracy, high risk of thermal protection failure, and poor overall thermal protection structure stability.

[0005] On one hand, embodiments of the present invention provide a high-speed air rudder integrally wrapped rudder surface heat shield, the heat shield being an integral structure that wraps the air rudder, comprising a fiber preform and phenolic resin filled in the fiber preform; the fiber preform is an integral structure, and the fiber preform is stitched together to completely wrap the metal skeleton of the air rudder. A closed-cell foam strain-coordinating layer is provided between the heat-proof sleeve and the upper end face of the air rudder, and between the heat-proof sleeve and the rear end face of the air rudder. The fiber covering structure corresponding to the lower end face of the air rudder between the rudder shaft and the leading edge of the air rudder is an integral continuous fiber structure, while the fiber covering structures corresponding to other end faces are all covered by butt stitching. The region extending 20–35 mm from the leading edge of the air rudder to its rear end is defined as the air rudder leading edge thinning zone, and the remaining area of ​​the rudder surface is the main air rudder area; the density of the area corresponding to the heat shield and the air rudder leading edge thinning zone is 1.10–1.20 g / cm³. 3 The thickness is 2-3 mm; the area corresponding to the heat shield and the air rudder main body includes, from the outside to the inside, an ablation layer, a transition layer, and a heat insulation layer along the thickness direction of the heat shield; wherein, the thickness of the ablation layer is 2-3 mm, and the density is 1.10-1.20 g / cm³. 3The transition layer has a thickness of 2–3 mm and a density of 0.85–0.95 g / cm³. 3 The insulation layer has a thickness of 3–6 mm and a density of 0.50–0.55 g / cm³. 3 The fiber-reinforced structure in the region corresponding to the thinning area of ​​the leading edge of the heat shield and the air rudder is an integral continuous fiber structure with the fiber-reinforced structure in the ablation layer.

[0006] Preferably, the butt joint is made of quartz yarn.

[0007] Preferably, the area of ​​the heat shield near the root of the rudder shaft is a prefabricated dense stitching area, the stitch length of the prefabricated dense stitching area is 2-4 mm, and the spacing is 2-4 mm; the stitch length of the prefabricated sutures in the areas outside the prefabricated dense stitching area is 8-12 mm, and the spacing is 8-12 mm.

[0008] Preferably, the width of the prefabricated dense stitching area is 20-25 mm larger than the diameter of the rudder shaft ring heat shield, and the height extends 20-40 mm from the root of the rudder shaft to the upper surface of the air rudder.

[0009] Preferably, the closed-cell foam strain-coating layer is at least one of polyimide foam, polymethacrylimide foam, and polyvinylidene fluoride foam; And / or, the closed-cell rate of the closed-cell foam strain-coordinating layer is greater than 90%; And / or, the deformation temperature of the closed-cell foam strain-coordinating layer is not lower than 180°C.

[0010] Preferably, the phenolic resin is an organic-inorganic hybrid nanoporous phenolic resin.

[0011] Secondly, the present invention also provides an integral molding method for the above-mentioned high-speed air rudder integrally covering the rudder surface heat shield, the method comprising the following steps: Step S1: Adhere closed-cell foam strain-coordinating layers to the upper end face and the rear end face of the air rudder, respectively. Step S2: Prepare a powder with a density of 0.16–0.25 g / cm³. 3 A low-density fiber preform layer is formed; then, a fiber preform layer with a density of 0.45–0.55 g / cm³ is prepared on the low-density fiber preform layer. 3 A medium-density fiber prefabricated layer is obtained by repeatedly piercing a 2.5D woven fabric with a quartz fiber mesh to obtain a pierced fiber prefabricated layer. The pierced fiber prefabricated layer is then attached to the side of the medium-density fiber prefabricated layer away from the low-density fiber prefabricated layer. The pierced fiber prefabricated layer and the medium-density fiber prefabricated layer are then needle-punched together. The low-density fiber prefabricated layer, the medium-density fiber prefabricated layer, and the pierced fiber prefabricated layer are then stitched together with quartz yarn to obtain a variable-density flat fiber prefabricated body. Step S3: The variable density flat fiber preform is prepositioned on the air rudder metal frame. The lower end face of the air rudder between the rudder shaft and the leading edge of the air rudder is a continuous fiber. The edges of the fiber preforms corresponding to other end faces are covered by stitching. Before stitching the edges of the fiber preforms corresponding to the leading edge of the air rudder, the low-density fiber preform layer and the medium-density fiber preform layer corresponding to the thinned area of ​​the leading edge of the air rudder are first removed, leaving only the serrated fiber preform layer in this area. Then the stitching is performed to complete the overall coverage of the air rudder metal frame by the variable density flat fiber preform. Step S4: Place the air rudder covered with fiber preform into the air rudder heat shield molding mold, fully impregnate the fiber preform with phenolic resin, cure, dry, and machine to obtain the high-speed air rudder integrally covered heat shield.

[0012] Preferably, in step S2, the low-density fiber prefabricated layer, the medium-density fiber prefabricated layer, and the multi-spinned fiber prefabricated layer are integrally sutured, including: the area of ​​the heat shield near the root of the rudder shaft is the prefabricated dense suture area, the suture stitch length of the prefabricated dense suture area is 2-4 mm, and the spacing is 2-4 mm; the suture stitch length of the area outside the prefabricated dense suture area is 8-12 mm, and the spacing is 8-12 mm. And / or, the width of the prefabricated dense stitching area is 20-25 mm larger than the diameter of the rudder shaft ring heat shield, and the height extends 20-40 mm from the root of the rudder shaft to the upper surface of the air rudder.

[0013] Preferably, step S3 further includes: after completing the overall covering of the variable density flat fiber preform, needle-punch 1 to 2 layers of surface felt on the surface of the covered fiber preform.

[0014] Preferably, in step S4, the pressure inside the mold during the curing process is less than 0.2 MPa.

[0015] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects: 1. The heat shield of the present invention is an integrated structure that wraps around the air rudder. The fiber preform is an integrated structure. The heat shield wraps around the metal frame of the air rudder by stitching with quartz fiber thread. It abandons the traditional split assembly structure and achieves a seamless overall wrapping. Airflow is not easy to enter, which effectively solves the problems of easy airflow and local ablation failure of the existing split structure. The integrated structure heat shield of the present invention avoids secondary assembly, has high integral molding precision, and has good consistency.

[0016] 2. The present invention provides closed-cell foam strain coordination layers between the heat shield and the upper end face of the air rudder, and between the heat shield and the rear end face of the air rudder. By utilizing the buffer deformation capacity of the foam material, the thermal expansion difference between the metal skeleton and the composite material heat shield is effectively matched, avoiding the compression and damage of the heat shield by the thermal expansion of the metal under high temperature conditions, improving the stability and service life of the product under high temperature, and reducing the risk of thermal protection failure.

[0017] 3. The density of the region corresponding to the heat shield and the thinned area at the leading edge of the air rudder in this invention is 1.10–1.20 g / cm³. 3 The thickness is 2-3mm to ensure the compactness and shape retention of the front edge assembly area, ensure the aerodynamic shape accuracy, and avoid the problem of reduced protective performance and assembly performance after the front edge of the heat shield is thinned.

[0018] 4. The heat shield of this invention has a gradient density structure. The outer high-density ablation layer improves the resistance to erosion and high-temperature ablation, the middle transition layer buffers thermal stress, and the inner low-density layer achieves efficient heat insulation. The layered structure design is reasonable, and the overall thermal protection effect is good, improving the thermal protection capability of the air rudder. The heat shield has high structural stability. It has an outer strong ablation-resistant layer that does not deform under high heat and strong airflow, a transition layer that coordinates internal and external stresses and prevents mismatch of internal and external expansion coefficients, which could cause delamination and cracks, and an efficient heat insulation layer that reduces the temperature to a temperature at which the metal frame of the air rudder can maintain good working condition. The ablation layer, transition layer, and heat insulation layer complement each other, thereby improving the stability of the structure.

[0019] 5. The area near the root of the rudder shaft of the heat shield of the present invention is a prefabricated dense stitching area. The stitch length of the prefabricated dense stitching area is 2-4 mm and the spacing is 2-4 mm. The fiber prefabricated material near the root of the rudder shaft is locally densely stitched to strengthen the structural strength and density, improve the local ablation resistance of the heat shield, and achieve targeted enhanced protection.

[0020] 6. The heat shield of the present invention can be adapted to ultra-high temperature conditions of 1800℃. When flying at 1800℃ for more than 200 seconds, the rudder shaft temperature is below 565℃, the rudder surface ablation recedes by less than 0.65mm, the ablation depth of the heat shield at the root of the rudder shaft is less than 8.9mm, and the heat shield does not crack and the overall structure does not deform.

[0021] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description

[0022] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.

[0023] Figure 1 This is a schematic diagram of the high-speed air rudder integrally covered rudder surface heat shield structure of the present invention; Figure 2 This is a schematic diagram of the metal frame structure of the air rudder; Figure 3 The variable density flat fiber preform of the present invention.

[0024] Figure label: 1-Heatproof sleeve; 11-Variable density flat fiber preform; 12-Closed-cell foam strain coordination layer; 13-Preform dense stitching area; 14-Folding center line; 2-Air rudder metal skeleton; 21-Air rudder leading edge thinning area; 22-Air rudder main body area; 23-Air rudder upper end face; 24-Air rudder rear end face; 25-Rudder shaft; 26-Air rudder lower end face between rudder shaft and air rudder leading edge; 27-Rudder shaft ring heatproof sleeve; 28-Air rudder leading edge. Detailed Implementation

[0025] Preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which form part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.

[0026] In this invention, such as Figure 2 As shown, "lower end face of the air rudder" refers to the end face where the rudder shaft 25 is located, "upper end face of the air rudder 23" refers to the end face opposite to the end face where the rudder shaft 25 is located, and "rear end face of the air rudder 24" refers to the end face opposite to the leading edge 28 of the air rudder.

[0027] Research has revealed the following shortcomings in existing air rudder technologies: First, the modular assembly structure has assembly gaps and splicing breaks, allowing high-temperature, high-speed airflow to easily intrude through these gaps, causing localized ablation and thermal stress concentration. Second, the modular processing and secondary assembly process results in poor forming precision and significant accumulation of assembly errors, making it difficult to meet the high-precision aerodynamic shape requirements of high-speed aircraft. Third, the thermal expansion coefficients of the air rudder's metal frame and the composite material heat shield differ significantly. Under high-temperature conditions, the thermal expansion deformation of the air rudder's metal frame can compress and tear the heat shield, leading to cracking and detachment of the heat shield layer and a high risk of thermal protection failure. Fourth, the existing air rudder heat shield has a single density layer design, which cannot simultaneously meet the gradient performance requirements of surface ablation resistance, middle layer transition buffer, and inner layer efficient heat insulation, resulting in poor overall thermal protection performance.

[0028] Based on this, in a first aspect, the present invention provides a high-speed air rudder integrally covered with a heat shield for the rudder surface, such as... Figures 1 to 3As shown, the heat shield 1 is an integral structure that wraps around the air rudder metal frame 2, including a fiber preform and phenolic resin filled in the fiber preform; the fiber preform is an integral structure, and the fiber preform wraps around the air rudder metal frame 2 by stitching. A closed-cell foam strain-coordination layer 12 is provided between the heat-proof sleeve 1 and the upper end face 23 of the air rudder, and between the heat-proof sleeve 1 and the rear end face 24 of the air rudder. The fiber covering structure corresponding to the lower end face 26 of the air rudder between the rudder shaft 25 and the leading edge 28 of the air rudder is an integral continuous fiber structure, while the fiber covering structures corresponding to other end faces are all covered by butt stitching. The lower end face 26 of the air rudder between the rudder shaft 25 and the leading edge 28 of the air rudder is close to the incoming flow direction. This area has high heat and strong scouring force. The use of an integral continuous fiber structure in this area can avoid the suture line formed by the stitching method being damaged by high temperature and strong scouring force. The region extending 20-35 mm from the leading edge 28 of the air rudder to the rear end face 24 of the air rudder is defined as the leading edge thinning region 21 of the air rudder, and the other areas of the rudder surface are the main body region 22 of the air rudder; the density of the area corresponding to the leading edge thinning region 21 of the heat shield 1 is 1.10-1.20 g / cm³. 3 (e.g., 1.10 g / cm³) 3 1.12 g / cm 3 1.14 g / cm 3 1.16 g / cm 3 1.18 g / cm 3 1.20g / cm 3 The thickness of the heat shield 1 is 2-3 mm (e.g., 2 mm, 2.3 mm, 2.5 mm, 2.8 mm, 3 mm); the area corresponding to the air rudder body 22 of the heat shield 1 includes, from the outside to the inside, an ablation layer, a transition layer, and a heat insulation layer along the thickness direction of the heat shield 1; wherein, the thickness of the ablation layer is 2-3 mm (e.g., 2 mm, 2.3 mm, 2.5 mm, 2.8 mm, 3 mm), and the density is 1.10-1.20 g / cm³. 3 (e.g., 1.10 g / cm³) 3 1.12 g / cm 3 1.14 g / cm 3 1.16 g / cm 3 1.18 g / cm 3 1.20g / cm 3 The ablation layer possesses high strength and high density, directly resisting the erosion of hypersonic airflow and high-temperature ablation; the thickness of the transition layer is 2-3 mm (e.g., 2 mm, 2.3 mm, 2.5 mm, 2.8 mm, 3 mm), and the density is 0.85-0.95 g / cm³. 3(e.g., 0.85g / cm) 3 0.87g / cm 3 0.90g / cm 3 0.93g / cm 3 0.95g / cm 3 The transition layer serves to transition stress and buffer thermal stress, connecting the surface ablation layer and the inner insulation layer; the insulation layer has a thickness of 3–6 mm (e.g., 3 mm, 3.3 mm, 3.5 mm, 3.8 mm, 4 mm) and a density of 0.50–0.55 g / cm³. 3 (e.g., 0.50 g / cm) 3 0.52g / cm 3 0.54g / cm 3 0.55g / cm 3 The low-density insulation layer has a low thermal conductivity, achieving efficient heat insulation and blocking the transmission of high temperature to the air rudder metal frame 2; the fiber-reinforced structure in the region corresponding to the heat shield 1 and the leading edge thinning region 21 of the air rudder is an integral continuous fiber structure with the fiber-reinforced structure in the ablation layer.

[0029] Compared with the prior art, the high-speed air rudder integrally covered heat shield 1 of the present invention is an integrated structure that wraps the metal skeleton 2 of the air rudder. It has high molding precision, and airflow is not easy to enter the heat shield, resulting in a longer service life. The present invention provides closed-cell foam strain coordination layers 12 between the heat shield 1 and the upper end face 23 of the air rudder, and between the heat shield 1 and the rear end face 24 of the air rudder. The foam material's buffering deformation capability effectively buffers the thermal expansion deformation of the metal skeleton under high temperature, preventing the heat shield from being squeezed and damaged. Furthermore, the fiber reinforcement structure in the area corresponding to the leading edge thinning area 21 of the heat shield 1 and the fiber reinforcement structure in the ablation layer is an integral continuous fiber structure to ensure the compactness and shape retention of the leading edge assembly area, ensure the aerodynamic shape accuracy, and avoid the problem of reduced protection performance and assembly performance after the leading edge of the heat shield is thinned. The heat shield 1 of the present invention has a gradient density structure; the outer high-density ablation layer improves the resistance to erosion and high-temperature ablation performance, the middle transition layer buffers thermal stress, and the inner low-density layer achieves efficient heat insulation, resulting in high overall thermal protection performance.

[0030] For example, the butt joint is made of quartz yarn.

[0031] During the use of the air rudder, the airflow blows from the leading edge 28 of the air rudder and is blocked at the rudder shaft 25. After being blocked, thermal turbulence occurs at the root of the rudder shaft 25, where the temperature is 300-400°C higher than other areas. The high temperature and pressure of the turbulence can easily cause the heat shield at the root of the rudder shaft 25 to peel off, leading to ablation at the root of the rudder shaft 25. Therefore, to prevent the heat shield near the root of the rudder shaft 25 from peeling off, for example, the area of ​​the heat shield 1 near the root of the rudder shaft 25 is a prefabricated dense stitching area 13. The stitch spacing of the prefabricated dense stitching area 13 is 2-4 mm, and the spacing is 2-4 mm; the stitch spacing of the prefabricated ...

[0032] For example, the width of the prefabricated densified stitching area 13 is 20-25 mm larger than the diameter of the rudder shaft ring heat shield 27, and the height extends 20-40 mm (e.g., 20 mm, 25 mm, 30 mm, 35 mm, 40 mm) from the root of the rudder shaft 25 to the upper end face 23 of the air rudder, covering the high stress and high ablation risk area at the root of the rudder shaft 25, and achieving targeted enhanced protection.

[0033] It should be noted that the width of the prefabricated densified stitching area 13 is symmetrical about the center line of the rudder shaft 25.

[0034] For example, the closed-cell foam strain-coordinating layer 12 is at least one of polyimide foam, polymethacrylimide foam, and polyvinylidene fluoride foam.

[0035] For example, the closed-cell foam strain coordination layer 12 has a closed-cell rate of more than 90%; this closed-cell structure can ensure that the closed-cell foam strain coordination layer 12 has high heat insulation and buffering performance, while effectively preventing resin wetting and penetration, and ensuring structural stability.

[0036] For example, the deformation temperature of the closed-cell foam strain coordination layer 12 is not lower than 180°C, and more preferably 180-220°C, such as 180°C, 190°C, 200°C, 210°C, and 220°C. Deformation temperature refers to the temperature at which the closed-cell foam strain coordination layer 12 can deform. In this invention, the closed-cell foam strain coordination layer 12 is disposed on the upper end face 23 and the rear end face 24 of the air rudder. This region has a relatively mild thermal environment for the air rudder, and the temperature in this region will not exceed 350°C. The closed-cell foam strain coordination layer 12 has a good shape-maintaining effect in the early stage of flight. In the middle stage of flight, when the temperature of the air rudder metal frame 2 is too high, the air rudder metal frame 2 begins to expand, and the closed-cell foam strain coordination layer 12 will contract to alleviate the expansion force of the air rudder metal frame 2. In the later stage of flight, as the temperature of the air rudder metal frame 2 continues to rise and its volume continues to expand, the closed-cell foam strain coordination layer 12 will decompose itself to accommodate the expansion of the air rudder metal frame 2 within its own space. The deformation temperature of the closed-cell foam strain coordination layer 12 of the present invention is preferably 180-220°C. If the temperature is too high, it will not be able to decompose at high temperature, and the expansion of the air rudder metal skeleton 2 will not be released, which will cause local damage and cracking of the air rudder heat shield. If the deformation temperature is too low, it will deform or decompose prematurely and will not play an initial shaping role.

[0037] For example, the thickness of the closed-cell foam strain-coordinating layer 12 is 1.5–2.5 mm. This thickness refers to the thickness extending outward from the air rudder end face. If the thickness is too small, it will not be able to coordinate the expansion of the metal; if the thickness is too large, it will result in insufficient foam strength and heat insulation performance, leading to premature failure. The outer air rudder heat insulation sleeve will then lack support, and under the action of airflow, the stitched area will loosen and eventually fail.

[0038] For example, the phenolic resin is an organic-inorganic hybrid nanoporous phenolic resin.

[0039] For example, the phenolic resin is the organosilicon hybrid phenolic resin in CN110951210A, which has high resistance to high temperature, ablation, and airflow erosion.

[0040] Secondly, the present invention provides an integral molding method for the above-mentioned high-speed air rudder integrally covering the rudder surface heat shield, the method comprising the following steps: Step S1: Bond the closed-cell foam strain-coordination layer 12 to the upper end face 23 and the rear end face 24 of the air rudder, respectively. Step S2: Prepare a powder with a density of 0.16–0.25 g / cm³. 3 A low-density fiber preform layer is formed; then, a fiber preform layer with a density of 0.45–0.55 g / cm³ is prepared on the low-density fiber preform layer. 3A medium-density fiber prefabricated layer is obtained by repeatedly puncturing 2.5D woven fabric and quartz fiber mesh to obtain a punctured fiber prefabricated layer. The punctured fiber prefabricated layer is attached to the side of the medium-density fiber prefabricated layer away from the low-density fiber prefabricated layer. The punctured fiber prefabricated layer and the medium-density fiber prefabricated layer are needle-punched together. The low-density fiber prefabricated layer, the medium-density fiber prefabricated layer and the punctured fiber prefabricated layer are stitched together as a whole to obtain a variable-density flat fiber prefabricated body 11. Step S3: The variable density flat fiber preform 11 is pre-positioned on the air rudder metal frame 2. The lower end face 26 of the air rudder between the rudder shaft 25 and the leading edge 28 of the air rudder is a continuous fiber. The edges of the fiber preforms corresponding to other end faces are covered by stitching. Before stitching the edges of the fiber preforms corresponding to the leading edge 28 of the air rudder, the low-density fiber preform layer and the medium-density fiber preform layer corresponding to the thinning area 21 of the leading edge of the air rudder are first removed, leaving only the serrated fiber preform layer in this area. Then, the stitching is performed to complete the overall coverage of the air rudder metal frame 2 by the variable density flat fiber preform 11. The thinning area 21 of the leading edge of the air rudder is a pure woven fabric reinforcement structure, so that the density of this area after molding is 1.10~1.20g / cm³, ensuring the compactness and shape retention of the leading edge assembly area, and avoiding the problem of decreased protective performance and assembly performance after the leading edge is thinned. Step S4: Place the air rudder covered with fiber preform into the air rudder heat shield molding mold, fully impregnate the fiber preform with phenolic resin, cure, dry, and machine to obtain the high-speed air rudder integrally covered heat shield 1.

[0041] Compared with the prior art, the method of the present invention is an integral molding method, which avoids the secondary assembly process of split molding, has high molding accuracy, is simple, and prevents airflow from easily entering the heat shield, resulting in a longer service life.

[0042] For example, in step S1, high-temperature resistant silicone rubber is used as an adhesive to bond the closed-cell foam strain coordination layer 12 points to the upper end face 23 and the rear end face 24 of the air rudder. After bonding, mechanical pressure treatment and constant temperature curing are performed to ensure that the strain coordination layer is firmly bonded to the metal skeleton without delamination, providing a stable strain buffer foundation for subsequent overall encapsulation molding and high-temperature operation.

[0043] For example, the mechanical pressure treatment is 0.05 to 0.10 MPa, the constant temperature curing temperature is 20 to 30°C, and the time is 24 to 48 hours.

[0044] For example, in step S2, a low-density fiber preform layer is prepared by a 5-mesh-1-cloth lamination method.

[0045] Specifically, the lamination method of the 5 mesh 1 fabric includes: layering an 85-115g / m 2 The woven fabric is laid on a needle punching machine, and five layers of 55-75 g / m² are laid in sequence. 2 For mesh tires, the needle-punch density is controlled at 15-25 needles / cm. 2 Acupuncture was performed to obtain a low-density fiber preform layer.

[0046] For example, in step S2, a medium-density fiber preform layer is prepared on the low-density fiber preform layer using a 1-cloth-1-web lamination method.

[0047] Specifically, the stacking method of the 1-fabric-1-net includes: placing a layer of 200-240g / m 2 The woven fabric is laid on a needle punching machine, with one layer of 55-85 g / m² applied. 2 For mesh tires, the needle-punch density is controlled at 25-30 needles / cm. 2 Acupuncture was performed to obtain a medium-density fiber preform layer.

[0048] For example, in step S2, the low-density fiber prefabricated layer, the medium-density fiber prefabricated layer, and the multi-spinned fiber prefabricated layer are stitched together as a whole, including: the area of ​​the heat-resistant sleeve 1 near the root of the rudder shaft 25 is the prefabricated dense stitching area 13, the stitch distance of the prefabricated dense stitching area 13 is 2-4 mm, and the spacing is 2-4 mm, which improves the structural density and ablation resistance of this area; the stitch distance of the prefabricated dense stitching area 13 outside the prefabricated dense stitching area is 8-12 mm, and the spacing is 8-12 mm.

[0049] For example, the width of the prefabricated dense stitching area 13 is 20-25 mm larger than the diameter of the rudder shaft ring heat shield 27, and the height extends 20-40 mm from the root of the rudder shaft 25 to the upper end face 23 of the air rudder.

[0050] It should be noted that the width of the prefabricated densified stitching area 13 is symmetrical about the center line of the rudder shaft 25.

[0051] For example, 195tex quartz yarn is used to stitch together the low-density fiber preform layer, the medium-density fiber preform layer, and the serrated fiber preform layer to achieve integrated molding of the preform.

[0052] For example, the overall stitching is a straight stitch.

[0053] In step S2, the variable density flat fiber preform 11 is as follows: Figure 3 As shown, the overall shape of the variable density flat fiber preform 11 is a double-sided unfolded shape of the front and back of the air rudder metal skeleton 2.

[0054] In step S3, when covering the variable density flat fiber preform 11, the rudder shaft 25 is passed through the center of the preform dense stitching area 13 in the variable density flat fiber preform 11, thereby pre-positioning the variable density flat fiber preform 11 on the air rudder metal skeleton 2. The folding center line 14 corresponding to the rudder shaft 25 and the rear end face 24 of the air rudder is cut open, leaving only the folding center line 14 corresponding to the lower end face 26 of the air rudder between the rudder shaft 25 and the leading edge 28 of the air rudder as a whole continuous fiber; the lower end of the air rudder... The surface is pressed onto the folding center line 14, and the variable density flat fiber preform 11 is folded along the folding center line 14. The low-density fiber preform layer and the medium-density fiber preform layer corresponding to the thinning area 21 of the air rudder front edge are removed, and only the serrated fiber preform layer in this area is retained. Quartz yarn is used to cover and sew the fiber preform edges corresponding to the air rudder front edge 28, the air rudder upper end face 23, the air rudder rear end face 24, and the lower end face between the rudder shaft 25 and the air rudder rear end face 24 to achieve overall coverage.

[0055] For example, the butt joint is a Z-shaped suture.

[0056] For example, the stitch length of the covering and butt stitch is 5-8 mm and the spacing is 2-3 mm, which can balance the integrity of the covering and the structural strength.

[0057] For example, step S3 further includes: after completing the overall covering of the variable density flat fiber preform 11, needle-punch 1 to 2 layers of surface felt on the surface of the covered fiber preform to improve the surface smoothness and density.

[0058] For example, step S3 further includes: performing overlock stitching at the right-angled edge of the heat shield to prevent the edges from loosening or deforming, and to ensure the overall shape accuracy of the heat shield.

[0059] The present invention can use the organosilicon hybrid phenolic resin in CN110951210A as the impregnation resin. This resin is a solvent-based resin, with about 50% of the resin being solvent. The solvent will expand during the mold heating process. In order to balance the internal pressure of the mold and prevent the air rudder metal frame 2 from deforming due to excessive internal pressure, for example, in step S4, the pressure inside the mold during the curing process is less than 0.2 MPa.

[0060] For example, before curing, the mold outlet is opened to allow some resin to flow out, which is used to balance the molding pressure inside the mold, counteract pressure fluctuations during resin impregnation and curing, and effectively prevent the metal skeleton from deforming under pressure.

[0061] Specifically, before curing, a 3-5L resin collection tank is attached to the outside of the mold's outlet.

[0062] For example, in step S4, the curing temperature is 90-100°C and the time is 24-36 hours.

[0063] For example, in step S4, the drying includes: drying at 50-60°C for 6-8 hours, then heating to 90-100°C for 6-8 hours, and then heating to 120-130°C for 6-8 hours.

[0064] For example, in step S4, the machining includes: removing the glue injection holes and glue outlet marks on the surface of the heat shield and polishing the surface of the heat shield.

[0065] The following specific embodiments further illustrate the high-speed air rudder integral covering rudder surface heat shield and its integral molding method.

[0066] Example 1 This embodiment provides a high-speed air rudder integrally covered rudder surface heat shield and its preparation method.

[0067] A method for integrally molding a heat shield covering the entire rudder surface of a high-speed aerodynamic rudder, comprising: Step S1: Select polymethacrylimide foam with a closed-cell rate of 92% and a deformation temperature of 200℃ as the closed-cell foam strain coordination layer 12. The thickness of the closed-cell foam strain coordination layer 12 is 2mm. Assemble and fix the rudder shaft heat shield in the preset position of the air rudder metal frame 2. Use high-temperature resistant silicone rubber to apply the closed-cell foam strain coordination layer 12 to the upper end face 23 and the rear end face 24 of the air rudder. Apply a mechanical pressure of 0.05MPa and cure at room temperature for 1.5d.

[0068] Step S2, Preparation of variable density flat fiber preform 11: A 0.2 g / cm³ fiber preform is prepared using a 5-mesh, 1-cloth lamination method. 3 A low-density fiber preform layer is formed, and then a fiber mesh with a density of 0.5 g / cm³ is prepared on the low-density fiber preform layer using a 1-fabric-1-web lamination method. 3A medium-density fiber prefabricated layer is formed; a 2.5D quartz fiber woven fabric and a quartz fiber mesh are combined to form a serrated fiber prefabricated layer, which is then attached to the side of the medium-density fiber prefabricated layer away from the low-density fiber prefabricated layer. The serrated fiber prefabricated layer and the medium-density fiber prefabricated layer are needle-punched together; 195tex quartz yarn is used to stitch the low-density fiber prefabricated layer, the medium-density fiber prefabricated layer, and the serrated fiber prefabricated layer together in a straight line; a prefabricated dense stitching area 13 is provided with a width 22mm larger than the diameter of the rudder shaft ring heat shield, and extends 30mm from the root of the rudder shaft to the upper end face 23 of the air rudder. The width of the prefabricated dense stitching area 13 is symmetrically arranged about the center line of the rudder shaft 25. The stitch length of the prefabricated dense stitching area 13 is 3mm and the spacing is 3mm. The stitch length of the area outside the prefabricated dense stitching area 13 is 10mm and the spacing is 10mm. The overall shape of the variable density flat fiber preform 11 is a double-sided unfolded shape of the front and back of the air rudder metal skeleton 2.

[0069] Step S3, fiber preform covering: Pass the rudder shaft through the center of the preform dense stitching area 13 in the variable density flat fiber preform 11, thereby pre-positioning the variable density flat fiber preform 11 on the air rudder metal skeleton 2. Cut the folding center line 14 corresponding to the rudder shaft 25 and the air rudder rear end face 24, leaving only the folding center line 14 corresponding to the lower end face 26 of the air rudder between the rudder shaft 25 and the leading edge 28 of the air rudder as a whole continuous fiber; press the lower end face of the air rudder on the folding center line, fold the variable density flat fiber preform 11 along the folding center line 14, and thin the leading edge 21 of the air rudder (from the leading edge of the air rudder) The low-density fiber preform layer and medium-density fiber preform layer corresponding to the area extending 30mm from the rear end face 24 of the air rudder 28 are deleted, and only the serrated fiber preform layer in this area is retained; quartz yarn is used to perform Z-shaped wrapping and butt stitching on the fiber preform edges corresponding to the leading edge 28 of the air rudder, the upper end face 23 of the air rudder, the rear end face 24 of the air rudder, and the lower end face between the rudder shaft 25 and the rear end face 24 of the air rudder. The stitch length of the wrapping and butt stitching is 6mm and the spacing is 2.5mm; after the wrapping is completed, the right-angle edges are locked and shaped, and two layers of surface felt are needle-punched on the surface. Locking and sewing are performed at the right-angle edge of the heat-insulating sleeve 1.

[0070] Step S4, Composite Molding: The air rudder metal skeleton 2 covered with fiber preform is placed in the air rudder heat protection sleeve molding mold. A 4L resin collection tank is connected to the outside of the mold's glue outlet to balance the internal pressure. Organic-inorganic hybrid nanoporous phenolic resin (prepared using the method in CN110951210A) is fully impregnated with the fiber preform. The glue outlet of the mold is opened, and a 4L resin collection tank is connected to the outside of the mold's glue outlet. The pressure inside the mold is kept less than 0.2MPa during the curing process. The curing is carried out at 100℃ for 24 hours, dried at 60℃ for 6 hours, heated to 100℃ for 6 hours, and heated to 120℃ for 6 hours. The glue injection port and glue outlet marks are removed by machining. The surface of the heat protection sleeve is then polished to obtain the high-speed air rudder integrally covered heat protection sleeve 1.

[0071] The high-speed air rudder integral heat shield 1 prepared in this embodiment is an integrated structure that wraps around the air rudder metal skeleton 2, including a fiber preform and phenolic resin filled in the fiber preform; the fiber preform is an integral structure, and the fiber preform is integrally wrapped around the air rudder metal skeleton 2 by stitching with quartz fiber thread; the density of the area corresponding to the leading edge thinning region 21 of the heat shield 1 is 1.15 g / cm³. 3 The thickness is 2mm; the area corresponding to the air rudder main body area 22 of the heat shield 1 includes, from the outside to the inside, an ablation layer, a transition layer, and a heat insulation layer along the thickness direction of the heat shield 1; wherein, the thickness of the ablation layer is 2mm and the density is 1.15g / cm³. 3 The transition layer has a thickness of 2 mm and a density of 0.90 g / cm³. 3 The insulation layer has a thickness of 6 mm and a density of 0.52 g / cm³. 3 The fiber-reinforced structure in the region corresponding to the thinning area 21 at the leading edge of the heat shield 1 and the fiber-reinforced structure in the ablation layer is an integral continuous fiber structure. A closed-cell foam strain-coating layer 12 with a thickness of 2mm is provided between the heat shield 1 and the upper end face 23 of the air rudder, and between the heat shield 1 and the rear end face 24 of the air rudder. The covering fiber structure of the lower end face 26 of the air rudder between the rudder shaft 25 and the leading edge 28 of the air rudder is an integral continuous fiber structure; other end faces are covered by butt-stitching with quartz yarn. The region of the heat shield 1 near the root of the rudder shaft 25 is a prefabricated dense stitching area 13, with a stitch length of 3mm and a spacing of 3mm. The stitch length and spacing of the prefabricated stitches outside the prefabricated dense stitching area 13 are 10mm. The width of the prefabricated dense stitching area 13 is 22mm larger than the diameter of the rudder shaft ring heat shield 27, and the height is 30mm extending from the root of the rudder shaft 25 to the upper end face 23 of the air rudder.

[0072] Example 2 This embodiment provides a high-speed air rudder integrally covered rudder surface heat shield and its preparation method, similar to Embodiment 1. The difference lies in that the closed-cell foam strain-coating layer 12 is made of polyvinylidene fluoride closed-cell foam with a closed-cell rate of 91% and a deformation temperature of 220℃, and the mechanical pressure curing time is 1 day; the width of the prefabricated dense stitching area 13 is 20mm larger than the diameter of the rudder shaft ring heat shield 27, and its height extends 20mm from the root of the rudder shaft 25 to the upper end face 23 of the air rudder; the stitch spacing of the covering butt joint is 5mm, and the spacing is 2.5mm; the density of the area corresponding to the heat shield 1 and the thinned area 21 at the leading edge of the air rudder is 1.10 g / cm³. 3 The thickness of the ablation layer is 2 mm; the thickness of the ablation layer is 2 mm, and the density is 1.10 g / cm³. 3 The transition layer has a thickness of 3 mm and a density of 0.85 g / cm³. 3 The insulation layer has a thickness of 5 mm and a density of 0.50 g / cm³. 3 .

[0073] Example 3 This embodiment provides a high-speed air rudder integrally covered rudder surface heat shield similar to Embodiment 1 and its preparation method. The difference is that the closed-cell foam strain-coating layer 12 is a polyimide closed-cell foam with a closed-cell rate of 93% and a temperature resistance of 260℃, which is mechanically cured under pressure for 2 days; the width of the prefabricated dense stitching area 13 is the diameter of the rudder shaft ring heat shield 27 + 23mm, and the height is 30mm extending from the root of the rudder shaft 25 to the upper end face 23 of the air rudder; the stitch spacing of the covering butt joint is 8mm and the spacing is 3mm; the density of the area corresponding to the heat shield 1 and the thinning area 21 at the leading edge of the air rudder is 1.20g / cm³. 3 The ablation layer has a thickness of 2.5 mm and a density of 1.20 g / cm³. 3 The transition layer has a thickness of 3 mm and a density of 0.95 g / cm³. 3 The insulation layer has a thickness of 5 mm and a density of 0.55 g / cm³. 3 .

[0074] Example 4 This embodiment provides a high-speed air rudder integral covering rudder surface heat shield and its preparation method, which is similar to that of Embodiment 1. The difference is that the heat shield 1 does not have a prefabricated dense stitching area 13 in the area near the root of the rudder shaft 25. That is, the stitching distance in the area near the root of the rudder shaft 25 of the heat shield 1 is 10mm and the spacing is 10mm.

[0075] Comparative Example 1 This comparative example provides a high-speed air rudder integral covering rudder surface heat shield and its preparation method, similar to Example 1, except that a closed-cell foam strain coordination layer 12 is not provided.

[0076] Comparative Example 2 This comparative example provides a high-speed air rudder integrally covered rudder surface heat shield and its preparation method, similar to Example 1. The difference is that the density of the area corresponding to the heat shield 1 and the main air rudder area 22 is 1.15 g / cm³. 3 The uniform density.

[0077] Comparative Example 3 This comparative example provides a high-speed air rudder integrally covered rudder surface heat shield and its preparation method, which is similar to that of Example 1. The difference is that the covering fiber structure of the lower end face 26 of the air rudder between the rudder shaft 25 and the leading edge 28 of the air rudder is a butt-stitched covering.

[0078] Test case The heat resistance and corrosion resistance, cracking, and structural deformation of the high-speed air rudder integrally covered rudder surface heat shield of the test examples and comparative examples are shown in Table 1.

[0079] Table 1

[0080] As can be seen from Table 1, the heat shield of the present invention can be adapted to ultra-high temperature conditions of 1800℃. When flying at 1800℃ for more than 200 seconds, the rudder shaft temperature is below 565℃, the rudder surface ablation recedes by less than 0.65mm, the ablation depth of the heat shield at the root of the rudder shaft is less than 8.9mm, and the heat shield does not crack and the overall structure does not deform.

[0081] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. A high-speed air rudder integrally covered with a heat-resistant sleeve for the rudder surface, characterized in that, The heat shield is an integral structure that wraps around the air rudder, including a fiber preform and phenolic resin filled in the fiber preform; the fiber preform is an integral structure that wraps around the metal frame of the air rudder by stitching. A closed-cell foam strain-coordinating layer is provided between the heat-proof sleeve and the upper end face of the air rudder, and between the heat-proof sleeve and the rear end face of the air rudder. The fiber covering structure corresponding to the lower end face of the air rudder between the rudder shaft and the leading edge of the air rudder is an integral continuous fiber structure, while the fiber covering structures corresponding to other end faces are all covered by butt stitching. The region extending 20–35 mm from the leading edge of the air rudder to its rear end is defined as the air rudder leading edge thinning zone, and the remaining area of ​​the rudder surface is the main air rudder area; the density of the area corresponding to the heat shield and the air rudder leading edge thinning zone is 1.10–1.20 g / cm³. 3 The thickness is 2-3 mm; the area corresponding to the heat shield and the air rudder main body includes, from the outside to the inside, an ablation layer, a transition layer, and a heat insulation layer along the thickness direction of the heat shield; wherein, the thickness of the ablation layer is 2-3 mm, and the density is 1.10-1.20 g / cm³. 3 The transition layer has a thickness of 2–3 mm and a density of 0.85–0.95 g / cm³. 3 The insulation layer has a thickness of 3–6 mm and a density of 0.50–0.55 g / cm³. 3 The fiber-reinforced structure in the region corresponding to the thinning area of ​​the leading edge of the heat shield and the air rudder is an integral continuous fiber structure with the fiber-reinforced structure in the ablation layer.

2. The high-speed air rudder integrally covered rudder surface heat shield according to claim 1, characterized in that, The butt joint is made of quartz yarn.

3. The high-speed air rudder integrally covered rudder surface heat shield according to claim 1, characterized in that, The area near the root of the rudder shaft of the heat shield is the prefabricated dense stitching area. The stitch length of the prefabricated dense stitching area is 2-4 mm and the spacing is 2-4 mm. The stitch length of the prefabricated sutures in the areas outside the prefabricated dense stitching area is 8-12 mm and the spacing is 8-12 mm.

4. The high-speed air rudder integrally covered rudder surface heat shield according to claim 3, characterized in that, The width of the prefabricated dense stitching area is 20-25 mm larger than the diameter of the rudder shaft ring heat shield, and the height extends 20-40 mm from the root of the rudder shaft to the upper surface of the air rudder.

5. The high-speed air rudder integrally covered rudder surface heat shield according to claim 1, characterized in that, The closed-cell foam strain-coating layer is at least one of polyimide foam, polymethacrylimide foam, and polyvinylidene fluoride foam. And / or, the closed-cell rate of the closed-cell foam strain-coordinating layer is greater than 90%; And / or, the deformation temperature of the closed-cell foam strain-coordinating layer is not lower than 180°C.

6. The high-speed air rudder integrally covered rudder surface heat shield according to claim 1, characterized in that, The phenolic resin is an organic-inorganic hybrid nanoporous phenolic resin.

7. A method for integrally molding a heat shield covering the entire rudder surface of a high-speed air rudder according to any one of claims 1-6, characterized in that, The method includes the following steps: Step S1: Adhere closed-cell foam strain-coordinating layers to the upper end face and the rear end face of the air rudder, respectively. Step S2: Prepare a powder with a density of 0.16–0.25 g / cm³. 3 A low-density fiber preform layer is formed; then, a fiber preform layer with a density of 0.45–0.55 g / cm³ is prepared on the low-density fiber preform layer. 3 A medium-density fiber prefabricated layer is obtained by repeatedly piercing a 2.5D woven fabric with a quartz fiber mesh to obtain a pierced fiber prefabricated layer. The pierced fiber prefabricated layer is then attached to the side of the medium-density fiber prefabricated layer away from the low-density fiber prefabricated layer. The pierced fiber prefabricated layer and the medium-density fiber prefabricated layer are then needle-punched together. The low-density fiber prefabricated layer, the medium-density fiber prefabricated layer, and the pierced fiber prefabricated layer are then stitched together with quartz yarn to obtain a variable-density flat fiber prefabricated body. Step S3: The variable density flat fiber preform is prepositioned on the air rudder metal frame. The lower end face of the air rudder between the rudder shaft and the leading edge of the air rudder is a continuous fiber. The edges of the fiber preforms corresponding to other end faces are covered by stitching. Before stitching the edges of the fiber preforms corresponding to the leading edge of the air rudder, the low-density fiber preform layer and the medium-density fiber preform layer corresponding to the thinned area of ​​the leading edge of the air rudder are first removed, leaving only the serrated fiber preform layer in this area. Then the stitching is performed to complete the overall coverage of the air rudder metal frame by the variable density flat fiber preform. Step S4: Place the air rudder covered with fiber preform into the air rudder heat shield molding mold, fully impregnate the fiber preform with phenolic resin, cure, dry, and machine to obtain the high-speed air rudder integrally covered heat shield.

8. The method according to claim 7, characterized in that, In step S2, the low-density fiber prefabricated layer, the medium-density fiber prefabricated layer, and the multi-spinned fiber prefabricated layer are sutured together as a whole, including: the area of ​​the heat shield near the root of the rudder shaft is the prefabricated dense suture area, the suture stitch length of the prefabricated dense suture area is 2-4 mm, and the spacing is 2-4 mm; the suture stitch length of the area outside the prefabricated dense suture area is 8-12 mm, and the spacing is 8-12 mm. And / or, the width of the prefabricated dense stitching area is 20-25 mm larger than the diameter of the rudder shaft ring heat shield, and the height extends 20-40 mm from the root of the rudder shaft to the upper end face of the air rudder.

9. The method according to claim 7, characterized in that, Step S3 also includes: after completing the overall covering of the variable density flat fiber preform, needle-punch 1 to 2 layers of surface felt on the surface of the covered fiber preform.

10. The method according to claim 7, characterized in that, In step S4, during the curing process, the pressure inside the mold is less than 0.2 MPa.

Citation Information

Patent Citations

  • High-strength nanoporous ceramizable ablation heatproof composite material and preparation method thereof

    CN110951210A